A biomass remodelable triple shape memory epoxy resin and preparation method thereof
Through the epoxy compound reaction of tyramine and syringaldehyde, combined with a biomass anhydride curing agent, the problem that traditional thermosetting SMP cannot be reshaped and degraded is solved, and biomass with high heat resistance and mechanical properties can be reshaped into triple shapes. Memory epoxy resin achieves triple shape memory and degradable comprehensive properties.
Patent Information
- Application Number
- CN202410986355.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-23
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2044-07-23
AI Technical Summary
Traditional thermosetting shape memory materials (SMP) cannot be reshaped or degraded and recycled due to their irreversible three-dimensional network cross-linked structure, leading to environmental pollution and unsustainable development. It is also difficult to prepare reshapeable triple shape memory thermosetting resins.
Using tyramine and syringaldehyde as raw materials, biomass reshapeable triple shape memory epoxy resin is prepared through the reaction of epoxy compounds. Biomass acid anhydride is used as the curing agent, combined with specific molar ratios and reaction conditions, to achieve high heat resistance of the resin. and degradability.
The prepared biomass reshapeable triple shape memory epoxy resin has high heat resistance, mechanical strength, reshapeable and degradable properties, can achieve triple shape memory, and provides a reliable application foundation in cutting-edge fields.
Smart Images

Figure CN118515851B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a biomass epoxy compound, a remodelable triple shape memory resin based on the biomass epoxy compound and a preparation method thereof, and belongs to the technical field of functional polymer materials. Background Art
[0002] Shape memory polymers (SMPs) can recover their permanent shapes from temporary shapes under external stimuli such as heat, light, pressure, electric field, magnetic field, pH or solvents, and show good application prospects in aerospace self-deployment structures, flexible electronic devices, biomedical materials, intelligent robots and other fields. SMPs can be divided into two categories: thermoplastic SMPs (TP-SMPs) and thermosetting SMPs (TS-SMPs). Compared with TP-SMPs, TS-SMPs usually have relatively high glass transition temperature (Tg), shape recovery rate (Rr) and shape fixation rate (Rf), so TS-SMPs have greater application value. With the deepening of research, it has gradually expanded from the most common dual shape memory materials to triple and multiple shape memory materials to cope with more specific and complex environments. Traditional TS-SMPs cannot be reshaped or degraded and recycled due to their irreversible three-dimensional network cross-linked structure, and the treatment of waste TS-SMPs and related materials has caused irreversible environmental pollution, which has become the key to restricting sustainable development. Therefore, reshaping has become a new green indicator.
[0003] In summary, it is necessary to develop a reshapeable triple shape memory epoxy resin with good reshape performance, high heat resistance and full bio-based. Summary of the invention
[0004] The present invention aims at the deficiencies of the prior art and provides a biomass remodelable triple shape memory epoxy resin with high heat resistance and high mechanical strength and a preparation method thereof. Furthermore, the epoxy resin of the present invention has degradable properties. The present invention solves the problems of heat resistance and mechanical strength deviation of the existing thermosetting SMP, and especially overcomes the defect that it is difficult to prepare a remodelable triple shape memory thermosetting resin in the prior art.
[0005] In order to achieve the above object, the technical solution adopted by the present invention is:
[0006] A method for preparing a biomass remodelable triple shape memory epoxy resin comprises the following steps: epoxidizing tyramine and syringaldehyde to obtain an epoxy compound after reaction; and then curing the epoxy compound to obtain the biomass remodelable triple shape memory epoxy resin.
[0007] Preferably, the epoxy compound is subjected to a curing reaction with a curing agent to obtain the biomass remodelable triple shape memory epoxy resin.
[0008] The present invention reacts tyramine and syringaldehyde and then epoxidizes them to obtain a syringaldehyde epoxy compound; then the syringaldehyde epoxy compound is cured to obtain a biomass remodelable triple shape memory epoxy resin; preferably, the biomass remodelable triple shape memory epoxy resin is cured by the syringaldehyde epoxy compound and a curing agent; further preferably, the biomass remodelable triple shape memory epoxy resin is cured by the syringaldehyde epoxy compound and a biomass curing agent.
[0009] Preferably, the biomass curing agent is biomass acid anhydride; further preferably, the molar ratio of the epoxy group of the syringaldehyde epoxy compound to the anhydride group of the biomass acid anhydride is 1: (0.5-1.5), preferably 1: (0.75-1.25), such as 1:1.
[0010] The invention comprises the following steps: tyramine and syringaldehyde are reacted and then epoxidized to obtain an epoxy compound.
[0011] In the above technical scheme, the molar ratio of syringaldehyde to tyramine is 1: (0.9-1.5), preferably, the molar ratio of syringaldehyde to tyramine is 1: (0.9-1.2), preferably 1: 1.1; the reaction temperature is 40-70°C, and the time is 1-5h, preferably, the reaction temperature is 40-60°C, and the time is 1-3h, and further preferably, the reaction temperature is 45-55°C, and the time is 2-3h.
[0012] In the above technical solution, the reaction of tyramine and syringaldehyde is carried out in an alcohol solvent. Preferably, the alcohol solvent is a small molecule alcohol, such as ethanol.
[0013] In the above technical scheme, when preparing the syringaldehyde epoxy compound, epoxidation adopts the epoxy compound reaction method; the epoxy compound is a compound with a reactive group and an epoxy group, wherein the reactive group is a group that can react with a hydroxyl group, which can be a halogen or the like.
[0014] The invention discloses a biomass remodelable triple shape memory epoxy resin or epoxy compound prepared according to the method.
[0015] The present invention discloses a deformation recovery method of the above-mentioned biomass remodelable triple shape memory epoxy resin, comprising the following steps:
[0016] (1) At a deformation temperature, the biomass reshapeable triple shape memory epoxy resin with an original shape is changed to obtain a biomass reshapeable triple shape memory epoxy resin with a new shape, thereby completing the shape change;
[0017] (2) The biomass reshapeable triple shape memory epoxy resin with a new shape is placed back at the deformation temperature, and the biomass reshapeable triple shape memory epoxy resin with a new shape returns to its original shape, completing shape recovery.
[0018] Preferably, the deformation temperature is 20-40°C below and 10-60°C above the glass transition temperature of the biomass reshapeable triple shape memory epoxy resin; and the deformation recovery is multiple deformation recovery.
[0019] Most of the existing shape memory epoxy resins have dual shape memory. The present invention discloses a biomass remodelable triple shape memory epoxy resin with high heat resistance and high mechanical strength. The triple shape memory method comprises the following steps:
[0020] (1) At deformation temperature II, the biomass reshapeable triple shape memory epoxy resin with an original shape is changed into a shape II biomass reshapeable triple shape memory epoxy resin, thereby completing the shape change;
[0021] (2) At deformation temperature I, the biomass reshapeable triple shape memory epoxy resin having shape II is changed in shape to obtain the biomass reshapeable triple shape memory epoxy resin having shape I, thereby completing the shape change;
[0022] (3) The biomass reshapeable triple shape memory epoxy resin with shape I is placed under deformation temperature I again, and the biomass reshapeable triple shape memory epoxy resin with shape I is restored to shape II, thus completing shape recovery;
[0023] (4) The biomass reshapeable triple shape memory epoxy resin with shape II is placed under deformation temperature II, and the biomass reshapeable triple shape memory epoxy resin with shape II is restored to its original shape, completing shape recovery.
[0024] Preferably, the material is heated to the deformation temperature and kept warm for 3 to 30 seconds. Preferably, the keeping warm time is 5 to 20 seconds. More preferably, the keeping warm time is 10 to 15 seconds.
[0025] Preferably, the deformation temperature I and the deformation temperature II are 20 to 40°C below and 10 to 60°C above the glass transition temperature of the biomass reshapeable triple shape memory epoxy resin, respectively, which, as common sense, is lower than the initial thermal decomposition temperature (5%); preferably, the deformation temperature I and the deformation temperature II are 30 to 40°C below and 10 to 40°C above the glass transition temperature of the biomass reshapeable triple shape memory epoxy resin, respectively.
[0026] The present invention discloses a method for reshaping the above-mentioned biomass reshapeable triple shape memory epoxy resin, comprising the following steps: hot pressing the crushed biomass reshapeable triple shape memory epoxy resin to complete the reshaping of the biomass reshapeable triple shape memory epoxy resin. The hot pressing temperature is 160-250°C, the pressure is 1-100MPa, and the time is 1-10h; preferably, the hot pressing temperature is 180-230°C, the pressure is 5-50MPa, and the time is 2-8h; further preferably, the hot pressing temperature is 190-210°C, the pressure is 10-20MPa, and the time is 2-4h.
[0027] The present invention discloses a method for degrading the above-mentioned biomass reshapeable triple shape memory epoxy resin, wherein the biomass reshapeable triple shape memory epoxy resin is mixed with alcohol to achieve its degradation. Preferably, the alcohol is a small molecule alcohol, such as ethylene glycol; preferably, the degradation is carried out at room temperature to 200°C.
[0028] The invention discloses the application of the epoxy compound or biomass remodelable triple shape memory epoxy resin in the preparation or as epoxy resin material.
[0029] In the present invention, when preparing the syringaldehyde epoxy compound, epoxidation adopts the method of epoxy compound reaction, and the reaction product of tyramine and syringaldehyde is reacted with the epoxy compound to obtain the epoxy compound, i.e., the syringaldehyde epoxy compound; the epoxy compound is a compound with a reactive group and an epoxy group, wherein the reactive group is a group capable of reacting with a hydroxyl group, which may be a halogen, etc.; preferably, the reactive group and the epoxy group are connected by an alkyl chain, and the alkyl chain may be a straight chain or a branched chain; further preferably, the number of carbon atoms of the alkyl chain is 1 to 10, preferably 1 to 5, and further preferably 1 to 3; such as epichlorohydrin, epichlorohydrin, etc. Halogen is used to react with the hydroxyl groups on the reaction product of tyramine and syringaldehyde, and an epoxy group is introduced to obtain the syringaldehyde epoxy compound. During the reaction, it is necessary to be in an inert gas atmosphere, preferably nitrogen.
[0030] Preferably, the epoxidation is first carried out in the presence of a catalyst, wherein the molar ratio of the product of the reaction of tyramine and syringaldehyde, the epoxide compound, and the catalyst is 1: (5-15): (0.05-0.15), preferably 1: 10: 0.1; the reaction temperature is 80-100°C, the time is 3-5h, preferably, the reaction temperature is 80-90°C, and the time is 4-5h; the catalyst is an organic ammonium compound, such as tetrabutylammonium bromide (TBAB). Then the epoxidation reaction is carried out in the presence of an inorganic base, preferably, the inorganic base is sodium hydroxide; the molar ratio of the product of the reaction of tyramine and syringaldehyde to the inorganic base is 1: (3-6), preferably 1: 4; the reaction temperature is 30-50°C, the time is 3-5h, preferably, the reaction temperature is 35-45°C, and the time is 4-5h.
[0031] In the present invention, the curing temperature is 120-160°C and the curing time is 6-10 hours. Preferably, the curing is a step-by-step heating method, the heat preservation time at each step temperature is not less than 2 hours, and the temperature difference between adjacent steps does not exceed 30°C.
[0032] Compared with the prior art, the present invention has the following beneficial effects:
[0033] 1. The present invention uses tyramine and syringaldehyde as raw materials, and the syringaldehyde epoxy compound prepared by curing obtains a biomass remodelable triple shape memory epoxy resin, which has outstanding heat resistance and a glass transition temperature (T g ) is 161°C, and it also has high flexural modulus (4.29GPa) and strength (120.5MPa), which provides a reliable basis for its application in cutting-edge fields. In particular, the tyramine, syringaldehyde and curing agent used are all biomass raw materials.
[0034] 2. The epoxy resin obtained by the method of the present invention has a wide glass transition temperature range, so it can change its shape twice as needed to achieve triple shape memory, overcoming the defect that the existing biomass epoxy resin can only achieve double shape memory.
[0035] 3. The biomass-based epoxy thermosetting shape memory resin prepared by the present invention has the advantage of triple shape memory, and the shape recovery rate of the prepared biomass remodelable triple shape memory epoxy resin is as high as 97%. At the same time, the epoxy resin of the present invention also has remodelable and degradable properties. These application methods overcome the defect that traditional cross-linked polymers cannot be processed again after molding. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] FIG. 1 is a synthetic reaction formula and chemical structural formula for preparing intermediates and epoxy compounds in Example 1 of the present invention.
[0037] FIG. 2 is a hydrogen nuclear magnetic resonance spectrum of the intermediate in Example 1 of the present invention ( 1 H-NMR).
[0038] FIG3 is a high-resolution mass spectrum of the intermediate in Example 1 of the present invention.
[0039] FIG. 4 is a hydrogen nuclear magnetic resonance spectrum of the epoxy compound in Example 1 of the present invention ( 1 H-NMR).
[0040] FIG5 is a high-resolution mass spectrum of the epoxy compound prepared in Example 1 of the present invention.
[0041] FIG6 is a thermal gravimetric analysis (TGA) curve of the biomass remodelable triple shape memory epoxy resin prepared in Example 1 of the present invention, 10° C. / min, nitrogen.
[0042] FIG. 7 is a dynamic thermal mechanical analysis (DMA) curve of the biomass remodelable triple shape memory epoxy resin prepared in Example 1 of the present invention, 3° C. / min.
[0043] FIG8 is a tensile stress-strain curve of the biomass remodelable triple shape memory epoxy resin prepared in Example 1 of the present invention.
[0044] FIG. 9 is a triple shape memory electron image of the biomass remodelable triple shape memory epoxy resin prepared in Example 1 of the present invention.
[0045] FIG. 10 is a reshaped electron image of the biomass reshapeable triple shape memory epoxy resin prepared in Example 1 of the present invention.
[0046] FIG. 11 is an electronic image of the degradation of the biomass remodelable triple shape memory epoxy resin prepared in Example 1 of the present invention.
[0047] Fig.12 is the nuclear magnetic resonance hydrogen spectrum of the intermediate in Comparative Example 1 of the present invention ( 1 H-NMR).
[0048] Fig.13 This is a degradation electronic image of the biomass epoxy resin prepared in Comparative Example 1 of the present invention. DETAILED DESCRIPTION
[0049] In the present invention, the chemical structural formula of the epoxy compound is as follows:
[0050]
[0051] When preparing epoxy compounds, epoxidation is carried out by means of epoxy compound reaction, such as using epoxy halogen compounds to achieve epoxidation.
[0052] The epoxy compound is then cured to obtain a biomass remodelable triple shape memory epoxy resin; preferably, the biomass remodelable triple shape memory epoxy resin is obtained by curing the epoxy compound and a curing agent.
[0053] The shape memory method of the biomass remodelable triple shape memory epoxy resin of the present invention comprises the following steps:
[0054] (1) At a deformation temperature, the biomass reshapeable triple shape memory epoxy resin with an original shape is changed to obtain a biomass reshapeable triple shape memory epoxy resin with a new shape, thereby completing the shape change;
[0055] (2) The biomass reshapeable triple shape memory epoxy resin with a new shape is placed back at the deformation temperature, and the biomass reshapeable triple shape memory epoxy resin with a new shape returns to its original shape, completing shape recovery.
[0056] As an example, the triple shape memory method of the biomass-reshaped triple shape memory epoxy resin of the present invention comprises the following steps:
[0057] (1) At deformation temperature II, the biomass reshapeable triple shape memory epoxy resin having an original shape is changed into shape II; the biomass reshapeable triple shape memory epoxy resin having shape II is obtained, and the shape change is completed;
[0058] (2) at a deformation temperature I, the biomass reshapeable triple shape memory epoxy resin having shape II is changed into shape I, thereby obtaining a biomass reshapeable triple shape memory epoxy resin having shape I, and the shape change is completed;
[0059] (3) The biomass reshapeable triple shape memory epoxy resin with shape I is placed back under deformation temperature I, and the biomass reshapeable triple shape memory epoxy resin with shape I is restored to shape II, thus completing shape recovery;
[0060] (4) The biomass reshapeable triple shape memory epoxy resin with shape II is placed at a deformation temperature II, and the biomass reshapeable triple shape memory epoxy resin with shape II is restored to its original shape, completing shape recovery.
[0061] As is common sense, each shape change can be achieved by external force, and the new shape can be maintained by cooling after deformation. The cooling time is conventional technology, such as 1 second to 10 minutes, preferably 5 seconds to 1 minute.
[0062] The present invention places conventional crushed biomass remodelable triple shape memory epoxy resin in a mold for hot pressing to complete the remodeling of the biomass remodelable triple shape memory epoxy resin.
[0063] The present invention mixes the above biomass remodelable triple shape memory epoxy resin with ethylene glycol to achieve its degradation; preferably, the degradation is carried out at room temperature to 180° C. As an example, the present invention places the resin block in ethylene glycol, and the resin can be completely degraded after 9 hours.
[0064] The technical solution of the present invention is further described below in conjunction with the accompanying drawings and embodiments; all raw materials are commercially available, and the specific preparation operations and testing methods involved are conventional methods in the art. A universal testing machine (MTS CMT-4104, China) is used to test the mechanical properties. The test standard for the tensile test refers to the American material testing standard ASTM-D882, and the test standard for the bending test refers to the Chinese material testing standard GBT2570-1995. The molecular weight of the epoxy compound is tested using a high-resolution mass spectrometer (HRMS, MICRO TOF-QIII, Germany, ESI+). A nuclear magnetic resonance spectrometer (Bruker 400-600mhz, Germany) is used for testing 1 H-NMR spectrum, solvent is DMSO-d6. The thermal stability of the resin under N2 atmosphere was studied using a thermogravimetric analyzer (TGA, Discovery, USA), and the sample was heated from room temperature to 800°C at a heating rate of 10°C / min. The dynamic thermomechanical properties of the material were tested using a dynamic thermomechanical analyzer (DMA, TA Q800, USA), with a frequency of 1Hz, and a heating rate of 3°C / min from 25°C to 250°C. The sample size was 32mm×3mm×1mm.
[0065] As an example, the biomass remodelable triple shape memory epoxy resin preparation process disclosed in the present invention is as follows:
[0066] (1) After heating tyramine and syringaldehyde to react, an intermediate is obtained;
[0067] (2) heating the intermediate and epichlorohydrin in the presence of an organic ammonium to react, then adding an inorganic base and continuing the reaction to obtain a syringaldehyde epoxy compound;
[0068] (3) The syringaldehyde epoxy compound is cured to obtain a biomass reshapeable triple shape memory epoxy resin.
[0069] In the above step (1), the molar ratio of syringaldehyde to tyramine is 1:(0.9-1.2), preferably 1:1.1; the heating reaction is carried out in an alcohol solvent, preferably, the alcohol solvent is ethanol; the heating reaction temperature is 40-60°C, the time is 1-3h, preferably, the heating reaction temperature is 45-55°C, and the time is 2-3h.
[0070] In the above step (2), the molar ratio of the intermediate to epichlorohydrin is 1: (5-15), preferably 1: 10; the molar ratio of the intermediate to the organic ammonium is 1: (0.05-0.15), preferably 1: 0.1; the reaction is carried out in an inert gas atmosphere, preferably, the inert gas is nitrogen; the heating reaction temperature is 80-100°C, the time is 3-5h, preferably, the heating reaction temperature is 80-90°C, the time is 4-5h, and the organic ammonium is tetrabutylammonium bromide; then the reaction is carried out in the presence of an inorganic base, preferably, the inorganic base is sodium hydroxide; the molar ratio of the intermediate to the inorganic base is 1: (3-6), preferably 1: 4; the temperature for continuing the reaction is 30-50°C, the time is 3-5h, preferably, the temperature for continuing the reaction is 35-45°C, and the time is 4-5h.
[0071] In the above step (3), the curing agent is a biomass anhydride, such as citraconic anhydride, and the molar ratio of the epoxy group of the syringaldehyde epoxy compound to the anhydride group of the biomass anhydride is 1: (0.5-1.5), preferably 1: (0.75-1.25), such as 1: 1; the curing temperature is 120-160°C, and the time is 6-10h. Preferably, the curing is a step-by-step heating method, and the insulation time at each step temperature is not less than 2h, and the temperature difference between adjacent steps does not exceed 30°C.
[0072] Specifically, the preparation method of the biomass reshapeable shape memory epoxy resin of the present invention is as follows:
[0073] (1) By mole, 110 parts of tyramine and 100 parts of syringaldehyde were mixed in ethanol, and then stirred at 45-55°C for 2-3 hours, cooled naturally to room temperature, filtered and dried to obtain an intermediate;
[0074] (2) On a molar basis, 100 parts of the intermediate, 1000 parts of epichlorohydrin and 10 parts of tetrabutylammonium bromide were mixed, reacted at 80-90°C for 4-5 hours in a nitrogen atmosphere, and then an aqueous sodium hydroxide solution (3-6 equivalents per mole of the intermediate) was added dropwise to the mixture, reacted at 35-45°C for 4-5 hours, cooled naturally to room temperature, filtered, and then the mixture was mixed with dichloromethane, washed with deionized water, and the solvent was removed by rotary evaporation. The syringaldehyde epoxy compound was obtained by vacuum distillation;
[0075] (3) The syringaldehyde epoxy compound obtained in step (2) is mixed with a biomass curing agent, citraconic anhydride, degassed, prepolymerized, and then cured to obtain a biomass reshapeable triple shape memory epoxy resin.
[0076] The present invention discloses a method for shape change and recovery of the above-mentioned biomass remodelable triple shape memory epoxy resin, comprising the following steps:
[0077] (1) At deformation temperature II, the biomass reshapeable triple shape memory epoxy resin with the original shape is changed into a new shape II, thereby obtaining a biomass reshapeable triple shape memory epoxy resin with shape II, and completing the shape change; as common sense, the deformation is achieved under the action of a conventional external force;
[0078] (2) placing the biomass reshapeable triple shape memory epoxy resin having shape II at a deformation temperature I, changing the biomass reshapeable triple shape memory epoxy resin having shape II into a new shape I, obtaining a biomass reshapeable triple shape memory epoxy resin having shape I, and completing the shape change; as common sense, the deformation is achieved under the action of a conventional external force;
[0079] (3) heating the biomass reshapeable triple shape memory epoxy resin having shape I to deformation temperature I and keeping the temperature for 5 to 20 seconds, wherein the biomass reshapeable triple shape memory epoxy resin having shape I is restored to shape II, thereby completing shape recovery; this step does not require external force;
[0080] (4) The biomass reshapeable triple shape memory epoxy resin with shape II is heated to deformation temperature II and kept warm for 5 to 20 seconds, and the biomass reshapeable triple shape memory epoxy resin with shape II is restored to its original shape, completing shape recovery; this step does not require external force.
[0081] In the above technical solution, the deformation temperature I and the deformation temperature II are respectively 20-40°C below and 10-60°C above the glass transition temperature of the biomass reshapeable triple shape memory epoxy resin. As common sense, the temperature lower than the initial thermal decomposition temperature (Td 5% ); Preferably, the deformation temperature I and the deformation temperature II are respectively 30-40°C below and 10-40°C above the glass transition temperature of the biomass reshapeable triple shape memory epoxy resin.
[0082] Example 1
[0083] (1) Preparation of intermediates
[0084] 15.09 g of tyramine (CAS#: 51-67-2) and 18.22 g of syringaldehyde (CAS#: 134-96-3) were mixed in ethanol, and then stirred at 50°C for 2 h, and then naturally cooled to room temperature, filtered and dried to obtain an intermediate with a yield of 89%. Its H NMR spectrum ( 1 H-NMR) and high-resolution mass spectrometry are shown in the attached Figure 2 , Attachment Figure 3 .
[0085] (2) Preparation of syringaldehyde epoxy compounds
[0086] Under nitrogen atmosphere, 29 g of the intermediate was mixed with 75 mL of epichlorohydrin and 3.15 g of tetrabutylammonium bromide, and reacted at 80 ° C for 4 h, and then sodium hydroxide aqueous solution (50 wt%, 4 times equivalent per mole of intermediate) was added dropwise to the mixture. After the addition was completed (1 minute), the mixture was reacted at 40 ° C for 4 h, and then naturally cooled to room temperature, filtered, and the obtained mixture was mixed with 90 mL of dichloromethane, and then washed with 100 mL of deionized water, and then rotary evaporated (80 ° C, 0.08 MPa) to remove dichloromethane and part of epichlorohydrin, and then vacuum distilled (110 ° C) to obtain syringaldehyde epoxy compound with a yield of 90%; Figure 4 Its H NMR spectrum ( 1 H-NMR); Figure 5 This is its high-resolution mass spectrum.
[0087] The above reaction is schematically shown in Figure 1 .
[0088] (3) Preparation of biomass reshapeable triple shape memory epoxy resin
[0089] 10.0 g of syringaldehyde epoxy compound and 5.4 g of citraconic anhydride were mixed uniformly at 65 ° C and degassed (65 ° C, 10 min, 0.1 MPa), and then prepolymerized at 65 ° C for 4 h, transferred to a mold and hot-pressed at 8 MPa, and cured in sequence according to the process of 120 ° C / 2 h + 140 ° C / 2 h + 160 ° C / 2 h; after the curing, the resin was naturally cooled to obtain a biomass reshapeable triple shape memory epoxy resin. Its thermogravimetric (TGA) curve, dynamic thermomechanical analysis (DMA) curve, and tensile stress-strain curve are shown in Figure 6 , Figure 7 , Figure 8 .
[0090] It can be seen that the above biomass can reshape the glass transition temperature (T g DMA) is 161°C, T d5% The temperature of the biomass reshapeable triple shape memory epoxy resin is 256° C. Furthermore, the bending modulus, bending strength and tensile strength of the biomass reshapeable triple shape memory epoxy resin at room temperature are 4.29 GPa, 120.5 MPa and 54.49 MPa, respectively, which has outstanding mechanical properties.
[0091] See also Fig. 9 The specific steps of the shape change and recovery method of the above-mentioned biomass-remodelable triple shape memory epoxy resin are as follows:
[0092] (1) 175°C (deformation temperature II), under the action of external force, the resin with the original shape is changed into a new shape II;
[0093] (2) 130°C (deformation temperature I), the shape described in step (1) is fixed to become a new permanent shape II of the biomass reshapeable triple shape memory epoxy resin;
[0094] (3) 130°C (deformation temperature I), under the action of external force, the biomass reshapeable triple shape memory epoxy resin in permanent shape II is changed into a new shape I;
[0095] (4) cooling naturally to room temperature, the shape I described in step (3) is fixed to become another new permanent shape I of the biomass remodelable triple shape memory epoxy resin;
[0096] (5) placing the biomass reshapeable triple shape memory epoxy resin having a new permanent shape I at 130° C. (without external force) for 10 seconds, and the resin automatically recovers from the permanent shape I in step (4) to the permanent shape II in step (2);
[0097] (6) The biomass reshapeable triple shape memory epoxy resin having permanent shape II is placed at 175° C. (without external force) for 10 seconds, and the resin automatically returns to its original shape from permanent shape II in step (2).
[0098] The shape recovery rate Rr = θ2 / θ1 × 100%, θ1 is the initial angle, and θ2 is the final shape recovery angle. In the shape change and recovery method of the biomass remodelable triple shape memory epoxy resin, θ1 is 180° and Rr = 97%.
[0099] This embodiment uses a conventional mold to provide external force. In actual production or application, other methods that can deform the resin strip can also be used, which are conventional technologies.
[0100] As a comparison, the inventor's research group previously disclosed a biomass recyclable shape memory epoxy resin (CN2023109638801), which requires 30 minutes of external force to restore the permanent shape III resin to its original shape. If the external force is removed, it cannot be restored to its original shape and cannot achieve triple memory. The present invention realizes the true triple memory of thermosetting resin, and can achieve shape recovery without external force. In addition, the product has excellent heat resistance and mechanical properties, which is beyond the expectations of those skilled in the art.
[0101] The remodeling performance test of the above biomass remodelable triple shape memory epoxy resin is as follows Fig.10 After the resin is crushed, it is poured into a mold and hot-pressed at 15 MPa and 200°C for 2.5 hours to obtain the reshaped resin.
[0102] The biodegradable properties of the above biomass remodelable triple shape memory epoxy resin are tested as follows Fig.11A small piece of resin (weight 0.25g) was placed in ethylene glycol (15mL) at 180℃, and the resin was completely degraded after 9h.
[0103] It can be seen from the above that the all-biomass reshapeable triple shape memory epoxy resin prepared by the present invention has excellent heat resistance, mechanical properties, reshape and degradation properties, which solves the problem that the Tg of the prior art biomass triple shape memory resin is less than 100°C, and also overcomes the defect that the prior art biomass triple shape memory resin needs to rely on external force to restore the original shape.
[0104] Comparative Example 1
[0105] (1) Preparation of intermediates
[0106] 15.09 g of tyramine and 15.21 g of vanillin were mixed in ethanol, and then stirred at 50 °C for 2 h, and then naturally cooled to room temperature, filtered and dried to obtain an intermediate with a yield of 87%; its H NMR spectrum ( 1 H-NMR) see Appendix Fig.12 .
[0107] (2) Preparation of vanillin epoxide
[0108] Under nitrogen atmosphere, 27 g of the intermediate, 75 mL of epichlorohydrin and 3.15 g of tetrabutylammonium bromide were mixed and reacted at 80 ° C for 4 h, and then an aqueous sodium hydroxide solution (50 wt%, 4 times the equivalent per mole of intermediate) was added dropwise to the mixture. After the addition was completed (1 minute), the mixture was reacted at 40 ° C for 4 h, and then naturally cooled to room temperature, filtered, and the obtained mixture was mixed with 90 mL of dichloromethane, washed with 100 mL of deionized water, and then rotary evaporated (80 ° C, 0.08 MPa) to remove dichloromethane and part of epichlorohydrin, and then vacuum distilled (110 ° C) to obtain vanillin epoxide with a yield of 89%.
[0109] (3) Preparation of biomass epoxy resin
[0110] 10.0g of vanillin epoxy compound and 5.8g of citraconic anhydride were mixed evenly at 65℃ and degassed (65℃, 10min, 0.1MPa). Then, they were prepolymerized at 65℃ for 4h and transferred to a mold and hot-pressed at 8MPa. The resin was cured in the process of 120℃ / 2h+140℃ / 2h+160℃ / 2h. After the curing, the resin was naturally cooled to obtain a biomass epoxy resin. The flexural modulus and flexural strength at room temperature were 3.91GPa and 91.21MPa, respectively.
[0111] The biodegradability test of the above biomass epoxy resin is as follows: Fig.13A small piece of resin (weight 0.246 g) was placed in ethylene glycol (15 mL) at 180°C. The resin was not completely degraded after 9 hours. After filtration and drying, the residual content was 3.8%.
[0112] Example 2
[0113] (1) Preparation of intermediates
[0114] 13.72 g of tyramine and 18.22 g of syringaldehyde were mixed in ethanol, and then stirred at 50° C. for 2 h, and then naturally cooled to room temperature, filtered and dried to obtain an intermediate.
[0115] (2) Preparation of syringaldehyde epoxy compounds
[0116] Under nitrogen atmosphere, 29 g of the intermediate, 75 mL of epichlorohydrin and 3.15 g of tetrabutylammonium bromide were mixed and reacted at 80 ° C for 4 h, and then sodium hydroxide aqueous solution (50 wt%, 4 times equivalent per mole of intermediate) was added dropwise to the mixture. After the addition was completed (1 minute), the mixture was reacted at 40 ° C for 4 h, and then naturally cooled to room temperature, filtered, and the obtained mixture was mixed with 90 mL of dichloromethane, washed with 100 mL of deionized water, and then rotary evaporated (80 ° C, 0.08 MPa) to remove dichloromethane and part of epichlorohydrin, and then vacuum distilled (110 ° C) to obtain syringaldehyde epoxy compound.
[0117] (3) Preparation of biomass reshapeable triple shape memory epoxy resin
[0118] 10.0g of syringaldehyde epoxy compound and 5.4g of citraconic anhydride were mixed evenly at 65℃ and degassed (65℃, 10min, 0.1MPa), and then prepolymerized at 65℃ for 4h, transferred to a mold and hot-pressed at 8MPa, and cured in sequence according to the process of 120℃ / 2h+140℃ / 2h+160℃ / 2h; after curing, the hot press reduced the pressure by half and cooled naturally with the hot press to obtain a biomass reshapeable triple shape memory epoxy resin.
[0119] Example 3
[0120] (1) Preparation of intermediates
[0121] 15.09 g of tyramine and 18.22 g of syringaldehyde were mixed in ethanol, and then stirred at 50° C. for 2 h, and then naturally cooled to room temperature, filtered and dried to obtain an intermediate.
[0122] (2) Preparation of syringaldehyde epoxy compounds
[0123] Under nitrogen atmosphere, 29 g of the intermediate, 75 mL of epichlorohydrin and 3.15 g of tetrabutylammonium bromide were mixed and reacted at 80 ° C for 4 h, and then sodium hydroxide aqueous solution (50 wt%, 4 times equivalent per mole of intermediate) was added dropwise to the mixture. After the addition was completed (1 minute), the mixture was reacted at 40 ° C for 4 h, and then naturally cooled to room temperature, filtered, and the obtained mixture was mixed with 90 mL of dichloromethane, washed with 100 mL of deionized water, and then rotary evaporated (80 ° C, 0.08 MPa) to remove dichloromethane and part of epichlorohydrin, and then vacuum distilled (110 ° C) to obtain syringaldehyde epoxy compound.
[0124] (3) Preparation of biomass reshapeable triple shape memory epoxy resin
[0125] 10.0g of syringaldehyde epoxy compound and 2.7g of citraconic anhydride were mixed evenly at 65℃ and degassed (65℃, 10min, 0.1MPa), and then prepolymerized at 65℃ for 4h, moved to a mold and hot-pressed at 8MPa, and cured in sequence according to the process of 120℃ / 2h+140℃ / 2h+160℃ / 2h; after curing, the hot press reduced the pressure by half and cooled naturally with the hot press to obtain a biomass reshapeable triple shape memory epoxy resin.
[0126] Example 4
[0127] (1) Preparation of intermediates
[0128] 15.09 g of tyramine and 18.22 g of syringaldehyde were mixed in ethanol, and then stirred at 50° C. for 2 h, and then naturally cooled to room temperature, filtered and dried to obtain an intermediate.
[0129] (2) Preparation of syringaldehyde epoxy compounds
[0130] Under nitrogen atmosphere, 29 g of the intermediate, 75 mL of epichlorohydrin and 3.15 g of tetrabutylammonium bromide were mixed and reacted at 80 ° C for 4 h, and then sodium hydroxide aqueous solution (50 wt%, 4 times equivalent per mole of intermediate) was added dropwise to the mixture. After the addition was completed (1 minute), the mixture was reacted at 40 ° C for 4 h, and then naturally cooled to room temperature, filtered, and the obtained mixture was mixed with 90 mL of dichloromethane, washed with 100 mL of deionized water, and then rotary evaporated (80 ° C, 0.08 MPa) to remove dichloromethane and part of epichlorohydrin, and then vacuum distilled (110 ° C) to obtain syringaldehyde epoxy compound.
[0131] (3) Preparation of biomass reshapeable triple shape memory epoxy resin
[0132] 10.0g of syringaldehyde epoxy compound and 4.1g of citraconic anhydride were mixed evenly at 65℃ and degassed (65℃, 10min, 0.1MPa), and then prepolymerized at 65℃ for 4h, transferred to a mold and hot-pressed at 8MPa, and cured in sequence according to the process of 120℃ / 2h+140℃ / 2h+160℃ / 2h; after curing, the hot press reduced the pressure by half and cooled naturally with the hot press to obtain a biomass reshapeable triple shape memory epoxy resin.
[0133] Example 5
[0134] (1) Preparation of intermediates
[0135] 15.09 g of tyramine and 18.22 g of syringaldehyde were mixed in ethanol, and then stirred at 50° C. for 2 h, and then naturally cooled to room temperature, filtered and dried to obtain an intermediate.
[0136] (2) Preparation of syringaldehyde epoxy compounds
[0137] Under nitrogen atmosphere, 29 g of the intermediate, 75 mL of epichlorohydrin and 3.15 g of tetrabutylammonium bromide were mixed and reacted at 80 ° C for 4 h, and then sodium hydroxide aqueous solution (50 wt%, 4 times equivalent per mole of intermediate) was added dropwise to the mixture. After the addition was completed (1 minute), the mixture was reacted at 40 ° C for 4 h, and then naturally cooled to room temperature, filtered, and the obtained mixture was mixed with 90 mL of dichloromethane, washed with 100 mL of deionized water, and then rotary evaporated (80 ° C, 0.08 MPa) to remove dichloromethane and part of epichlorohydrin, and then vacuum distilled (110 ° C) to obtain syringaldehyde epoxy compound.
[0138] (3) Preparation of biomass reshapeable triple shape memory epoxy resin
[0139] 10.0g of syringaldehyde epoxy compound and 6.8g of citraconic anhydride were mixed evenly at 65℃ and degassed (65℃, 10min, 0.1MPa), and then prepolymerized at 65℃ for 4h, moved to a mold and hot-pressed at 8MPa, and cured in sequence according to the process of 120℃ / 2h+140℃ / 2h+160℃ / 2h; after curing, the hot press reduced the pressure by half and cooled naturally with the hot press to obtain a biomass reshapeable triple shape memory epoxy resin.
[0140] Example 6
[0141] (1) Preparation of intermediates
[0142] 15.09 g of tyramine and 18.22 g of syringaldehyde were mixed in ethanol, and then stirred at 50° C. for 2 h, and then naturally cooled to room temperature, filtered and dried to obtain an intermediate.
[0143] (2) Preparation of syringaldehyde epoxy compounds
[0144] Under nitrogen atmosphere, 29 g of the intermediate, 75 mL of epichlorohydrin and 3.15 g of tetrabutylammonium bromide were mixed and reacted at 80 ° C for 4 h, and then sodium hydroxide aqueous solution (50 wt%, 4 times equivalent per mole of intermediate) was added dropwise to the mixture. After the addition was completed (1 minute), the mixture was reacted at 40 ° C for 4 h, and then naturally cooled to room temperature, filtered, and the obtained mixture was mixed with 90 mL of dichloromethane, washed with 100 mL of deionized water, and then rotary evaporated (80 ° C, 0.08 MPa) to remove dichloromethane and part of epichlorohydrin, and then vacuum distilled (110 ° C) to obtain syringaldehyde epoxy compound.
[0145] (3) Preparation of biomass reshapeable triple shape memory epoxy resin
[0146] 10.0g of syringaldehyde epoxy compound and 8.1g of citraconic anhydride were mixed evenly at 65℃ and degassed (65℃, 10min, 0.1MPa), and then prepolymerized at 65℃ for 4h, transferred to a mold and hot-pressed at 8MPa, and cured in sequence according to the process of 120℃ / 2h+140℃ / 2h+160℃ / 2h; after curing, the hot press reduced the pressure by half and cooled naturally with the hot press to obtain a biomass reshapeable triple shape memory epoxy resin.
[0147] The present invention uses tyramine and syringaldehyde as raw materials and biomass acid anhydride as curing agent to prepare an epoxy resin containing an ester bond. The tyramine and syringaldehyde used are both biomass raw materials. The prepared biomass reshapeable triple shape memory epoxy resin has outstanding heat resistance and a glass transition temperature (T g ) is 161°C, and it also has high flexural modulus (4.29GPa) and strength (120.5MPa). Compared with the prior art, the present invention realizes the preparation of biomass epoxy resin from all biomass raw materials, and the resin has very excellent comprehensive properties, thus providing a reliable foundation for its application in cutting-edge fields.
Claims
1. A method for preparing a biomass remodelable triple shape memory epoxy resin, characterized in that: The method comprises the following steps: epoxidizing tyramine and syringaldehyde to obtain an epoxy compound after reaction; and then curing the epoxy compound to obtain a biomass remodelable triple shape memory epoxy resin.
2. The method according to claim 1, characterized in that: The epoxy compound is subjected to a curing reaction with a curing agent to obtain a biomass remodelable triple shape memory epoxy resin.
3. A method for preparing an epoxy compound, characterized in that: The method comprises the following steps: epoxidizing tyramine and syringaldehyde after reaction to obtain an epoxy compound.
4. The method according to claim 1 or 3, characterized in that The molar ratio of syringaldehyde to tyramine is 1: (0.9-1.5); the reaction temperature is 40-70°C, and the reaction time is 1-5h.
5. The biomass remodelable triple shape memory epoxy resin or epoxy compound prepared according to the method of claim 1 or 3.
6. The deformation recovery method of the biomass remodelable triple shape memory epoxy resin according to claim 5, characterized in that: The following steps are involved: (1) At a deformation temperature, the biomass reshapeable triple shape memory epoxy resin with an original shape is changed to obtain a biomass reshapeable triple shape memory epoxy resin with a new shape, thereby completing the shape change; (2) The biomass reshapeable triple shape memory epoxy resin with a new shape is placed back at the deformation temperature, and the biomass reshapeable triple shape memory epoxy resin with a new shape returns to its original shape, completing shape recovery.
7. The deformation recovery method of biomass remodelable triple shape memory epoxy resin according to claim 6, characterized in that: The deformation temperature is 20-40°C below and 10-60°C above the glass transition temperature of the biomass reshapeable triple shape memory epoxy resin; and the deformation recovery is multiple deformation recovery.
8. The method for reshaping the biomass reshapeable triple shape memory epoxy resin according to claim 5, comprising the following steps: The crushed biomass remodelable triple shape memory epoxy resin is hot-pressed to complete the remodeling of the biomass remodelable triple shape memory epoxy resin.
9. The method for degrading the biomass remodelable triple shape memory epoxy resin according to claim 5, comprising mixing the biomass remodelable triple shape memory epoxy resin with alcohol to achieve its degradation.
10. Use of the epoxy compound or biomass remodelable triple shape memory epoxy resin according to claim 5 in the preparation or as epoxy resin material.
Citation Information
Cited By
Thermotropic shape memory epoxy resin material based on polycaprolactone and preparation method thereof
CN119899493A
A polycaprolactone-based thermotropic shape memory epoxy resin material and a preparation method thereof
CN119899493B