Graphene-based antistatic thermal insulation fabric, preparation method and application

Through the combination of modified hybrid reduction graphene oxide and modified polyester, combined with modified phase change fiber and electrospinning technology, the electrostatic and water-resistant problems of graphene knitted fabrics are solved, achieving efficient anti-static and warmth protection Performance improvement.

CN118685912BActive Publication Date: 2024-11-12ZHEJIANG KUQU NETWORK TECH CO LTD
View PDF 13 Cites 0 Cited by

Patent Information

Application Number
CN202411179192.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2024-11-12
Estimated Expiration
2044-08-27

AI Technical Summary

Technical Problem

Existing graphene knitted fabrics are prone to static electricity in dry environments, and due to poor smooth surface and agglomeration properties of graphene, they have poor adhesion, which affects their modification effect and water washing resistance.

Method used

By preparing hybrid reduced graphene oxide with zinc-aluminum-containing layered bimetallic hydroxide, and modifying it with silane coupling agent, agarose, etc., to form a composite modified polyester, and graphene fibers are obtained by melt spinning. Combined with modified phase-change fiber blending, electrospinning is used to form a hydrophobic fiber membrane to improve the antistatic and warmth of the fabric.

Benefits of technology

The permanent antistatic, hydrophilic and moisture-absorbing and breathable properties of graphene knitted fabrics are achieved, and its light-heat conversion effect and heat-conserving performance are improved, and the humidity and heat comfort and water-resistant performance are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118685912B_ABST
    Figure CN118685912B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of textile materials, and discloses an antistatic thermal insulation fabric based on graphene, a preparation method and an application. The preparation method of the antistatic thermal insulation fabric based on graphene comprises the following steps: preparing hybrid reduced graphene oxide, and then subjecting it to modification treatment to obtain modified hybrid reduced graphene oxide; subjecting polyester to modification treatment to obtain silane-modified polyester; reacting modified agarose with silane-modified polyester to obtain grafted modified polyester; reacting grafted modified polyester with modified hybrid reduced graphene oxide to obtain composite modified polyester; making graphene polyester yarn from composite modified polyester, and interweaving composite yarn obtained by blending with cotton fiber and modified phase change fiber to obtain graphene knitted fabric; electrostatic spinning is performed on one side of the graphene knitted fabric to form a hydrophobic fiber film to obtain antistatic thermal insulation fabric based on graphene. The antistatic thermal insulation fabric based on graphene of the present invention has good warmth retention, long-term antistatic properties and wet and hot comfort.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of textile materials, and in particular to a graphene-based antistatic thermal insulation fabric, a preparation method and an application thereof. Background Art

[0002] Traditional warm clothing worn in winter is generally thick and bloated, which is not beautiful and not conducive to the body's activities and stretching. In dry weather, it is very easy to generate static electricity, which affects the comfort of wearing. Graphene and ordinary fibers are used in fabrics to improve the antistatic and warmth retention of fabrics. For example, Chinese patent CN113308782B provides a graphene knitted fabric, including the following raw materials: blended yarn, spandex filament, the blended yarn is blended from the following raw materials: modal fiber and graphene modified fiber, the graphene knitted fabric has the advantages of fluffy and soft feel, excellent warmth retention, soft skin care, and comfortable skin-fitting. However, in the graphene knitted fabric, the graphene modified fiber is obtained by immersion. Since the surface of graphene is relatively smooth, there are almost no defect sites except for the edge, so that the interaction force with other substances is weak, and graphene is easy to agglomerate in the matrix material, resulting in an interface with poor adhesion, which will affect the modification effect of the graphene modified fiber and the water washing resistance of the fabric. Summary of the invention

[0003] In order to solve the above technical problems, the present invention provides a method for preparing an antistatic thermal insulation fabric based on graphene, comprising the following steps:

[0004] Step (1), preparing a hybrid reduced graphene oxide containing zinc-aluminum layered double metal hydroxide, and then modifying it with a silane coupling agent KH-560 to obtain a modified hybrid reduced graphene oxide;

[0005] Step (2), the polyester is subjected to hydroxylation treatment and γ-mercaptopropyltrimethoxysilane modification treatment to obtain a silane-modified polyester;

[0006] Step (3), modifying agarose with acryloyl chloride to obtain modified agarose; reacting the modified agarose with silane-modified polyester to obtain grafted modified polyester; reacting the grafted modified polyester with modified hybrid reduced graphene oxide to obtain composite modified polyester;

[0007] Step (4), melt spinning the composite modified polyester to obtain graphene polyester fiber, and then spinning to obtain graphene polyester yarn; blending cotton fiber and modified phase change fiber to obtain composite yarn; interweaving the graphene polyester yarn and the composite yarn to obtain graphene knitted fabric;

[0008] The method for preparing the modified phase change fiber comprises the following steps:

[0009] Step S1, reacting methacrylic acid with styrene to prepare carboxylated polystyrene;

[0010] Step S2, the nano-silica is activated and modified with 3-aminopropyltriethoxysilane to obtain hydrophilic modified nano-silica;

[0011] Step S3, carboxylated polystyrene, polyethylene glycol, hydrophilic modified nano-silica, and N,N-dimethylformamide are mixed to obtain a precursor solution, and electrospinning is performed to obtain a phase change fiber; the phase change fiber is modified with polydopamine to obtain a modified phase change fiber;

[0012] Step (5), mixing zein powder, glucose powder and ethanol aqueous solution into a spinning solution, and electrospinning on one side of the graphene knitted fabric to form a hydrophobic fiber membrane, thereby obtaining an antistatic thermal insulation fabric based on graphene.

[0013] Preferably, in step (1), the preparation method of the modified hybrid reduced graphene oxide is as follows: zinc nitrate hexahydrate and aluminum nitrate nonahydrate are dissolved in deionized water to obtain solution A; urea is dissolved in deionized water to obtain solution B; solution A and solution B are added to a 2 g / L graphene oxide aqueous dispersion, stirred at 90-110° C. for 10-14 h, then statically crystallized for 20-28 h, filtered, centrifuged, washed, and freeze-dried to obtain hybrid reduced graphene oxide; wherein the mass ratio of zinc nitrate hexahydrate, aluminum nitrate nonahydrate, urea, and graphene oxide is (1.6-2.2):1:(2.3-2.5):(3-6);

[0014] In the above process, firstly, a hybrid reduced graphene oxide containing zinc-aluminum hydrotalcite is prepared by a urea uniform coprecipitation assisted exfoliation self-assembly method, zinc ions and aluminum ions are adsorbed on the surface of graphene oxide through electrostatic interaction in an aqueous solution, and graphene oxide nanosheets are regarded as nucleation points, growing and forming zinc-aluminum layered double hydroxide crystals with high regularity, and the introduction of zinc-aluminum layered double hydroxide effectively prevents the agglomeration effect of reduced graphene oxide nanosheets, so that the reduced graphene oxide nanosheets are fully exfoliated by the zinc-aluminum layered double hydroxide;

[0015] In a nitrogen atmosphere, hybrid reduced graphene oxide, ethanol, deionized water, 25wt% ammonia water, and silane coupling agent KH-560 are mixed, stirred and reacted at 50-90° C. for 2-8 hours, centrifuged, washed, and dried to obtain modified hybrid reduced graphene oxide; wherein the mass ratio of hybrid reduced graphene oxide, ethanol, deionized water, 25wt% ammonia water, and silane coupling agent KH-560 is (2-10):100:(4-12):(1-8):(1-8);

[0016] In the above process, the silane coupling agent KH-560 combines with the hybrid reduced graphene oxide through the silanol bond after hydrolysis, and introduces epoxy groups on the hybrid reduced graphene oxide;

[0017] Preferably, in step (2), the preparation method of the silane-modified polyester comprises: crushing the polyester chips into polyester powder with a particle size of 30-80 μm, adding the polyester powder into a sodium hydroxide aqueous solution with a concentration of 200 g / L, stirring and reacting at 70-90° C. for 20-40 min, filtering, washing, and drying to obtain the hydroxylated polyester; wherein the mass ratio of the polyester powder to the sodium hydroxide aqueous solution is (10-15):(200-350);

[0018] Add γ-mercaptopropyltrimethoxysilane to an ethanol aqueous solution with a volume fraction of 80%, then add the hydroxylated polyester, stir and soak for 20-40 minutes at room temperature, filter, wash, and dry to obtain a silane-modified polyester; wherein the mass ratio of γ-mercaptopropyltrimethoxysilane, ethanol aqueous solution, and hydroxylated polyester is 1:(16-22):(0.34-0.44)

[0019] In the above process, part of the ester bonds of the polyester are broken in an alkaline sodium hydroxide aqueous solution to generate hydroxyl groups to form a hydroxylated polyester, and the γ-mercaptopropyltrimethoxysilane is hydrolyzed and reacts with the hydroxylated polyester to introduce mercapto groups into the polyester;

[0020] Preferably, in step (3), the preparation method of the modified agarose is as follows: at 80-100°C, agarose is dissolved in N,N-dimethylacetamide, and a dilution of acryloyl chloride in N,N-dimethylacetamide with a mass fraction of 7.7wt% is added dropwise at a rate of 0.5-1mL / min in an ice-water bath. After the addition is completed, the mixture is first reacted in an ice-water bath for 100-150min, then reacted at room temperature for 3.5-4.5h, concentrated by rotary evaporation, precipitated with acetone, washed, and dried; wherein the amount ratio of agarose, N,N-dimethylacetamide, and the dilution of acryloyl chloride in N,N-dimethylacetamide is (1.5-3)g:(50-100)g:(3.2-4.8)mL;

[0021] In the above process, the hydroxyl groups of agarose react with the acyl chloride of acryloyl chloride to introduce a carbon-carbon double bond structure into agarose;

[0022] Preferably, in step (3), the preparation method of the composite modified polyester is as follows: dispersing the silane modified polyester in ethanol under an ultrasonic power of 300-500 W, heating to 50-80° C., adding modified agarose, and then dripping a 0.4wt% azobisisobutyronitrile ethanol solution at a rate of 1.5-2.5 mL / min. After the dripping is completed, stirring and reacting for 2-4 hours, after the reaction is completed, centrifuging, washing, and drying to obtain the grafted modified polyester; wherein the mass ratio of the silane modified polyester, ethanol, modified agarose, and azobisisobutyronitrile ethanol solution is (10-15):(200-400):(1-4):(40-60);

[0023] In the above process, the carbon-carbon double bond of the modified agarose undergoes a thiol-ene click reaction with the thiol group of the silane-modified polyester to obtain a grafted modified polyester;

[0024] The grafted modified polyester is ultrasonically dispersed in toluene, heated to 60-80°C, and then modified hybrid reduced graphene oxide and boron trifluoride-ether are added, stirred for reaction for 1-3h, and after the reaction is completed, filtered, washed, and dried to obtain a composite modified polyester; wherein the mass ratio of the grafted modified polyester, toluene, modified hybrid reduced graphene oxide, and boron trifluoride-ether is (10-20):(200-300):(4-8):(0.01-0.03);

[0025] In the above process, the hydroxyl groups in the grafted modified polyester react with the epoxy groups of the modified hybrid reduced graphene oxide to obtain a composite modified polyester;

[0026] Preferably, in step (4), the fineness of the graphene polyester yarn is 20-30D; the ratio of cotton fiber to modified phase change fiber in the composite yarn is 1:(0.5-1), and the count of the composite yarn is 30-50 English count; in the graphene knitted fabric, the density of the graphene composite fiber yarn is (420-450) roots / 10cm, the density of the composite skin-friendly fiber yarn is (350-380) roots / 10cm, and the twist of the graphene polyester yarn and the composite yarn is 850-950 twists / m.

[0027] Preferably, in step (5), the preparation method of the graphene-based antistatic thermal insulation fabric comprises: mixing corn alcohol-soluble protein powder, glucose powder, and 75% ethanol aqueous solution in a mass ratio of (20-30): (5-10): (100-200), stirring in a water bath at 50-60°C for 12-16 hours, and cooling to obtain a spinning solution; electrospinning the spinning solution on one side of the graphene knitted fabric to form a hydrophobic fiber membrane, and then drying at 110-130°C for 2-4 hours to obtain the graphene-based antistatic thermal insulation fabric; wherein the electrospinning conditions are: spinning voltage of 15-20 kV, spinning distance of 14-18 cm, relative humidity of 35-45%, and spinning temperature of 23-27°C;

[0028] In the above process, zein is hydrophobic due to its rich non-polar amino acids (leucine, alanine and glycine). Zein and glucose are electrospun to form a hydrophobic fiber membrane on one side of the graphene knitted fabric. Then, zein and glucose are cross-linked through the Maillard reaction to improve the hydrophobicity and mechanical properties of the hydrophobic fiber membrane.

[0029] Furthermore, in step (4), the method for preparing the modified phase change fiber comprises the following steps:

[0030] Step S1, dissolving polyvinyl pyrrolidone in ethanol and ethylene glycol monomethyl ether, stirring at a speed of 200-300 r / min, then adding methacrylic acid, azobisisobutyronitrile and styrene, reacting at 45-55° C. for 10-30 min in a nitrogen atmosphere, and then reacting at 70-80° C. for 24-36 h. After the reaction is completed, cooling to room temperature, washing and drying the obtained solid to obtain carboxylated polystyrene; wherein the mass ratio of polyvinyl pyrrolidone, ethanol, ethylene glycol monomethyl ether, methacrylic acid, azobisisobutyronitrile and styrene is (1-2):(25-30):(15-20):(1.2-3):(1.2-1.5):(10.8-13.5);

[0031] In the above process, polyvinyl pyrrolidone is used as a dispersant, ethanol and ethylene glycol monomethyl ether are used as solvents, azobisisobutyronitrile is used as an initiator, and methacrylic acid is polymerized with styrene to obtain carboxylated polystyrene;

[0032] Step S2, mixing nano-silicon dioxide with a sodium hydroxide aqueous solution having a concentration of 1 mol / L, reacting at 65-75° C. for 20-30 hours, then neutralizing the sodium hydroxide with a hydrochloric acid aqueous solution having a concentration of 1 mol / L, centrifuging, washing, and drying to obtain activated nano-silicon dioxide; wherein the amount ratio of nano-silicon dioxide, sodium hydroxide aqueous solution, and hydrochloric acid aqueous solution is (4-10) g:(100-200) mL:(100-200) mL;

[0033] Add activated nano-silica to ethanol and homogenize for 45-50 hours, then add 3-aminopropyltriethoxysilane, react at room temperature for 5.5-6.5 hours, centrifuge, wash, and dry to obtain hydrophilic modified nano-silica; wherein the mass ratio of activated nano-silica, ethanol, and 3-aminopropyltriethoxysilane is (4-8):(100-200):(2-4);

[0034] In the above process, under the activation of sodium hydroxide, more hydrophilic hydroxyl groups are generated on the surface of nano-silica, and then 3-aminopropyltriethoxysilane is used to modify the activated nano-silica to further improve the hydrophilicity of the nano-silica;

[0035] Step S3, mixing carboxylated polystyrene, polyethylene glycol, hydrophilic modified nano-silica, and N,N-dimethylformamide in a mass ratio of (1-2):(0.5-1.5):(0.2-0.5):(5-10), stirring for 4-10 hours to obtain a precursor solution; maintaining the feed rate of the precursor solution at 2.5-3.5 mL / h, performing electrostatic spinning at a voltage of 20-30 kV and a spinning distance of 15-25 cm, and drying at room temperature for 10-12 hours to obtain a phase change fiber;

[0036] In the above process, carboxylated polystyrene, polyethylene glycol, and hydrophilic modified nano-silica are electrospun, and polyethylene glycol is encapsulated in the polystyrene fiber as a phase change material. The addition of hydrophilic modified nano-silica makes the polystyrene fiber produce more pores, which is helpful for the loading of polyethylene glycol. The solidification temperature of the phase change fiber varies around 24-26°C depending on the content of polyethylene glycol.

[0037] The phase change fiber is immersed in a dopamine hydrochloride solution with a mass fraction of 1 wt% at 27-33° C., the pH value is adjusted to 8.5 by using ammonia water with a mass fraction of 25 wt%, and the fiber is taken out after immersion treatment for 10-15 hours, washed, and dried to obtain a modified phase change fiber;

[0038] In the above process, dopamine polymerizes on the surface of the phase change fiber under alkaline conditions to form polydopamine, and the amino groups in the polydopamine and the carboxyl groups in the carboxylated polystyrene are combined through electrostatic interaction to achieve the encapsulation of the phase change fiber by polydopamine.

[0039] The graphene-based antistatic thermal insulation fabric is prepared by adopting the method for preparing the graphene-based antistatic thermal insulation fabric.

[0040] The graphene-based antistatic thermal insulation fabric is used in clothing.

[0041] Compared with the prior art, the present invention has the following beneficial effects:

[0042] 1. The present invention prepares phase change fibers by electrospinning carboxylated polystyrene, polyethylene glycol, and hydrophilic modified nano-silica. The phase change material is well encapsulated in the phase change fiber, so that the fabric has a better warming effect; the addition of hydrophilic modified nano-silica makes the polystyrene fiber produce more pores, which is helpful for the loading of polyethylene glycol; the polystyrene containing carboxyl groups can not only form hydrogen bonds with polyethylene glycol and hydrophilic modified nano-silica, improve the compatibility with polyethylene glycol and hydrophilic modified nano-silica, but also improve the hydrophilicity of the phase change fiber, and can react with polydopamine through electrostatic spinning. The combined effects can improve the encapsulation effect of polydopamine. Encapsulating polydopamine on the surface of phase change fiber can prevent leakage of phase change material on the one hand. On the other hand, due to the presence of a large number of conjugated double bonds in its aromatic structure, polydopamine can significantly enhance the absorption of ultraviolet light, visible light, and near-infrared short-wave regions. In collaboration with zinc-aluminum layered double hydroxides and reduced graphene oxide nanosheets, it can utilize full-spectrum sunlight and improve photothermal conversion efficiency, thereby achieving better warmth retention effect. In addition, polydopamine encapsulation can further improve the hydrophilicity of phase change fiber, thereby improving its antistatic property and moisture absorption and air permeability.

[0043] 2. The present invention prepares hybrid reduced graphene oxide nanosheets by inserting zinc aluminum layered double hydroxide into reduced graphene oxide nanosheets, and the hybrid modification improves the agglomeration of reduced graphene oxide nanosheets. More importantly, the zinc aluminum layered double hydroxide and reduced graphene oxide synergistically show excellent light-to-heat conversion effect, and due to the conductivity of reduced graphene oxide, it has good antistatic properties. Furthermore, by hydroxylating and silane-modifying the polyester, the modified agarose is grafted onto the polyester in the form of chemical bonds, and abundant hydroxyl groups are introduced to increase the hydrophilicity of the polyester. While improving the antistatic properties, the covalent bonding of the grafted modified polyester and the modified hybrid reduced graphene oxide is achieved to form a composite modified polyester, thereby solving the interface compatibility between the inorganic material modified hybrid reduced graphene oxide and the organic material polyester, and allowing the modified hybrid reduced graphene oxide to exert a permanent effect.

[0044] 3. The present invention obtains graphene polyester fiber by melt spinning of composite modified polyester, and then obtains graphene polyester yarn by spinning; cotton fiber and modified phase change fiber are blended to obtain composite yarn; graphene polyester yarn and composite yarn are interwoven to obtain graphene knitted fabric. The introduction of modified phase change fiber and composite modified polyester makes the graphene knitted fabric have permanent antistatic property, hydrophilicity and moisture absorption and breathability. Due to the light-heat conversion property of modified phase change fiber and composite modified polyester, they can efficiently absorb sunlight and convert it into heat, thereby achieving heating and warmth preservation of the fabric, and when the external temperature is lower than the phase change temperature of the phase change material, the phase change material solidifies. It releases heat and improves the heat-generating and warmth-keeping properties of the fabric. In addition, graphene can emit far-infrared rays, which has the same vibration frequency as the water molecules in human cells. It can easily cause resonance of the cell molecules on the surface of the human body, promote blood circulation in the subcutaneous tissue, and produce a thermal effect to achieve the warming function. Furthermore, a hydrophobic fiber membrane is formed on one side of the graphene knitted fabric through electrospinning, forming an anti-static and warm fabric based on graphene with significant wettability differences on both sides. This will generate anisotropic water penetration pressure, driving sweat to completely leave the skin surface, while preventing external moisture penetration, promoting the unidirectional transport of sweat to the environment, and improving the moisture and heat comfort of the fabric. BRIEF DESCRIPTION OF THE DRAWINGS

[0045] Figure 1 It is a process flow chart of a method for preparing the graphene-based antistatic thermal fabric of the present invention;

[0046] Figure 2 It is a comparison chart of the initial half-life and half-life after 50 washings of the graphene-based antistatic thermal insulation fabrics of Examples 2-4 of the present invention and Comparative Examples 3-8;

[0047] Figure 3 It is a comparison chart of the thermal insulation rate test of the graphene-based antistatic thermal fabrics of Examples 2-4 of the present invention and Comparative Examples 3-8. DETAILED DESCRIPTION

[0048] The technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0049] Example 1

[0050] This embodiment discloses a method for preparing a modified phase change fiber, comprising the following steps:

[0051] Step S1, dissolving 1.5 g of polyvinyl pyrrolidone in 27.5 g of ethanol and 17.5 g of ethylene glycol monomethyl ether, stirring at a speed of 250 r / min, then adding 2.1 g of methacrylic acid, 1.4 g of azobisisobutyronitrile, and 12.2 g of styrene, reacting at 50° C. for 20 min and then at 75° C. for 30 h in a nitrogen atmosphere, cooling to room temperature after the reaction is completed, washing and drying the obtained solid to obtain carboxylated polystyrene;

[0052] Step S2, mixing 7g of nano-silica with 150mL of a 1mol / L sodium hydroxide aqueous solution, reacting at 70°C for 25h, then neutralizing the sodium hydroxide with 150mL of a 1mol / L hydrochloric acid aqueous solution, centrifuging, washing, and drying to obtain activated nano-silica; adding 6g of activated nano-silica to 150g of ethanol and homogenizing for 48h, then adding 3g of 3-aminopropyltriethoxysilane, reacting at room temperature for 6h, centrifuging, washing, and drying to obtain hydrophilic modified nano-silica;

[0053] Step S3, carboxylated polystyrene, polyethylene glycol, hydrophilic modified nano-silica, and N,N-dimethylformamide are mixed in a mass ratio of 1.5:1:0.4:8, and stirred for 7 hours to obtain a precursor solution; the feed rate of the precursor solution is maintained at 3 mL / h, and electrospinning is performed under the conditions of a voltage of 25 kV and a spinning distance of 20 cm, and the phase change fiber is dried at room temperature for 11 hours;

[0054] The phase change fiber was immersed in a 1 wt % dopamine hydrochloride solution at 30° C., the pH value was adjusted to 8.5 by using 25 wt % ammonia water, and after immersion for 12 h, the fiber was taken out, washed, and dried to obtain a modified phase change fiber.

[0055] Example 2

[0056] This embodiment discloses a method for preparing an antistatic thermal insulation fabric based on graphene, comprising the following steps:

[0057] Step (1), dissolving zinc nitrate hexahydrate and aluminum nitrate nonahydrate in deionized water to obtain solution A; dissolving urea in deionized water to obtain solution B; adding solution A and solution B to a 2 g / L graphene oxide aqueous dispersion, stirring at 90° C. for 14 h, then statically crystallizing for 20 h, filtering, centrifuging, washing, and freeze-drying to obtain hybrid reduced graphene oxide; wherein the mass ratio of zinc nitrate hexahydrate, aluminum nitrate nonahydrate, urea, and graphene oxide is 1.6:1:2.3:3;

[0058] In a nitrogen atmosphere, hybrid reduced graphene oxide, ethanol, deionized water, 25 wt% ammonia water, and silane coupling agent KH-560 were mixed, stirred and reacted at 50° C. for 8 h, centrifuged, washed, and dried to obtain modified hybrid reduced graphene oxide; wherein the mass ratio of hybrid reduced graphene oxide, ethanol, deionized water, 25 wt% ammonia water, and silane coupling agent KH-560 was 2:100:4:1:1;

[0059] Step (2), crushing the polyester chips into polyester powder with a particle size of 30 μm, adding 10-15 g of the polyester powder into 200 g of a 200 g / L sodium hydroxide aqueous solution, stirring and reacting at 70° C. for 40 min, filtering, washing, and drying to obtain a hydroxylated polyester;

[0060] Adding γ-mercaptopropyltrimethoxysilane to an ethanol aqueous solution with a volume fraction of 80%, then adding the hydroxylated polyester, stirring and soaking for 20 minutes at room temperature, filtering, washing, and drying to obtain a silane-modified polyester; wherein the mass ratio of γ-mercaptopropyltrimethoxysilane, the ethanol aqueous solution, and the hydroxylated polyester is 1:16:0.34;

[0061] Step (3), at 80° C., dissolving 1.5 g of agarose in 50 g of N,N-dimethylacetamide, adding 3.2 mL of a 7.7 wt% N,N-dimethylacetamide dilution of acryloyl chloride at a rate of 0.5 mL / min in an ice-water bath, reacting in an ice-water bath for 100 min after the addition, and then reacting at room temperature for 3.5 h, concentrating the reaction mixture by rotary evaporation to a volume of 20 mL, precipitating with acetone, washing, and drying to obtain modified agarose;

[0062] 10 g of silane-modified polyester was dispersed in 200 g of ethanol under an ultrasonic power of 300 W, heated to 50° C., 1 g of modified agarose was added, and then 40 g of 0.4 wt% azobisisobutyronitrile ethanol solution was added dropwise at a rate of 1.5 mL / min. After the addition was completed, stirring was continued for 2 h. After the reaction was completed, centrifugation, washing, and drying were performed to obtain a grafted modified polyester.

[0063] 10 g of grafted modified polyester was ultrasonically dispersed in 200 g of toluene, heated to 60° C., and then 4 g of modified hybrid reduced graphene oxide and 0.01 g of boron trifluoride-ether were added, and stirred for reaction for 3 h. After the reaction was completed, the mixture was filtered, washed, and dried to obtain a composite modified polyester;

[0064] Step (4), melt spinning the composite modified polyester to obtain graphene polyester fiber, and spinning the graphene polyester fiber to obtain graphene polyester yarn with a fineness of 20D; mixing cotton fiber and modified phase change fiber in a ratio of 1:0.5 and blending to obtain a composite yarn with a count of 30; using the graphene polyester yarn as a warp and the composite yarn as a weft, interweaving through a knitting device to obtain a graphene knitted fabric, wherein the density of the graphene composite fiber yarn is 450 strands / 10cm, the density of the composite skin-friendly fiber yarn is 380 strands / 10cm, and the twist of the graphene polyester yarn and the composite yarn is 850 twists / m;

[0065] Step (5), dissolving 20g of corn protein powder and 5g of glucose powder in 100g of 75% by volume ethanol aqueous solution, stirring in a 50°C water bath for 16h, cooling to obtain a spinning solution; electrospinning the spinning solution on one side of the graphene knitted fabric to form a hydrophobic fiber membrane, and then drying at 110°C for 4h to obtain an antistatic thermal insulation fabric based on graphene; wherein the electrospinning conditions are: spinning voltage of 15kV, spinning distance of 14cm, relative humidity of 35%, and spinning temperature of 23°C.

[0066] Example 3

[0067] This embodiment discloses a method for preparing an antistatic thermal insulation fabric based on graphene, comprising the following steps:

[0068] Step (1), dissolving zinc nitrate hexahydrate and aluminum nitrate nonahydrate in deionized water to obtain solution A; dissolving urea in deionized water to obtain solution B; adding solution A and solution B to a 2 g / L graphene oxide aqueous dispersion, stirring at 110° C. for 10 h, then statically crystallizing for 28 h, filtering, centrifuging, washing, and freeze-drying to obtain hybrid reduced graphene oxide; wherein the mass ratio of zinc nitrate hexahydrate, aluminum nitrate nonahydrate, urea, and graphene oxide is 2.2:1:2.5:6;

[0069] In a nitrogen atmosphere, hybrid reduced graphene oxide, ethanol, deionized water, 25 wt% ammonia water, and silane coupling agent KH-560 were mixed, stirred and reacted at 90° C. for 2 h, centrifuged, washed, and dried to obtain modified hybrid reduced graphene oxide; wherein the mass ratio of hybrid reduced graphene oxide, ethanol, deionized water, 25 wt% ammonia water, and silane coupling agent KH-560 was 10:100:12:8:8;

[0070] Step (2), crushing the polyester chips into polyester powder with a particle size of 80 μm, adding 15 g of the polyester powder into 350 g of a 200 g / L sodium hydroxide aqueous solution, stirring and reacting at 90° C. for 20 min, filtering, washing, and drying to obtain a hydroxylated polyester;

[0071] Adding γ-mercaptopropyltrimethoxysilane to an ethanol aqueous solution with a volume fraction of 80%, then adding the hydroxylated polyester, stirring and soaking for 40 minutes at room temperature, filtering, washing, and drying to obtain a silane-modified polyester; wherein the mass ratio of γ-mercaptopropyltrimethoxysilane, the ethanol aqueous solution, and the hydroxylated polyester is 1:22:0.44;

[0072] Step (3), at 100° C., dissolving 3 g of agarose in 100 g of N,N-dimethylacetamide, and adding 4.8 mL of a 7.7 wt% N,N-dimethylacetamide dilution of acryloyl chloride dropwise at a rate of 1 mL / min in an ice-water bath. After the addition is completed, reacting in an ice-water bath for 150 min, and then reacting at room temperature for 4.5 h. After concentrating the reaction mixture by rotary evaporation to a volume of 30 mL, precipitating with acetone, washing, and drying to obtain modified agarose;

[0073] 15 g of silane-modified polyester was dispersed in 400 g of ethanol under an ultrasonic power of 500 W, and then heated to 80° C., 4 g of modified agarose was added, and then 60 g of azobisisobutyronitrile ethanol solution with a mass fraction of 0.4 wt% was added dropwise at a rate of 2.5 mL / min. After the addition was completed, stirring was continued for 4 h. After the reaction was completed, centrifugation, washing, and drying were performed to obtain a grafted modified polyester;

[0074] 20 g of grafted modified polyester was ultrasonically dispersed in 300 g of toluene, heated to 80°C, and then 8 g of modified hybrid reduced graphene oxide and 0.03 g of boron trifluoride-ether were added, and stirred for reaction for 3 h. After the reaction was completed, the mixture was filtered, washed, and dried to obtain a composite modified polyester;

[0075] Step (4), melt spinning the composite modified polyester to obtain graphene polyester fiber, and spinning the graphene polyester fiber to obtain graphene polyester yarn with a fineness of 30D; mixing cotton fiber and modified phase change fiber in a ratio of 1:1 and blending to obtain a composite yarn with a count of 50 English count; using the graphene polyester yarn as a warp and the composite yarn as a weft, interweaving through a knitting device to obtain a graphene knitted fabric, wherein the density of the graphene composite fiber yarn is 420 strands / 10 cm, the density of the composite skin-friendly fiber yarn is 350 strands / 10 cm, and the twist of the graphene polyester yarn and the composite yarn is 950 twists / m;

[0076] Step (5), dissolving 30g of corn protein powder and 10g of glucose powder in 200g of 75% by volume ethanol aqueous solution, stirring in a 60°C water bath for 12h, and cooling to obtain a spinning solution; electrospinning the spinning solution on one side of the graphene knitted fabric to form a hydrophobic fiber membrane, and then drying at 130°C for 2h to obtain an antistatic thermal insulation fabric based on graphene; wherein the electrospinning conditions are: spinning voltage of 20kV, spinning distance of 18cm, relative humidity of 45%, and spinning temperature of 27°C.

[0077] Example 4

[0078] This embodiment discloses a method for preparing an antistatic thermal insulation fabric based on graphene, comprising the following steps:

[0079] Step (1), dissolving zinc nitrate hexahydrate and aluminum nitrate nonahydrate in deionized water to obtain solution A; dissolving urea in deionized water to obtain solution B; adding solution A and solution B to a graphene oxide aqueous dispersion having a concentration of 2 g / L, stirring at 100° C. for 12 h, then statically crystallizing for 24 h, filtering, centrifuging, washing, and freeze-drying to obtain hybrid reduced graphene oxide; wherein the mass ratio of zinc nitrate hexahydrate, aluminum nitrate nonahydrate, urea, and graphene oxide is 1.9:1:2.4:4.5;

[0080] In a nitrogen atmosphere, hybrid reduced graphene oxide, ethanol, deionized water, 25 wt% ammonia water, and silane coupling agent KH-560 were mixed, stirred and reacted at 70° C. for 5 h, centrifuged, washed, and dried to obtain modified hybrid reduced graphene oxide; wherein the mass ratio of hybrid reduced graphene oxide, ethanol, deionized water, 25 wt% ammonia water, and silane coupling agent KH-560 was 6:100:8:4.5:4.5;

[0081] Step (2), crushing the polyester chips into polyester powder with a particle size of 60 μm, adding 12.5 g of the polyester powder into 275 g of a 200 g / L sodium hydroxide aqueous solution, stirring and reacting at 80° C. for 30 min, filtering, washing, and drying to obtain a hydroxylated polyester;

[0082] Adding γ-mercaptopropyltrimethoxysilane to an ethanol aqueous solution with a volume fraction of 80%, then adding the hydroxylated polyester, stirring and soaking for 30 minutes at room temperature, filtering, washing, and drying to obtain a silane-modified polyester; wherein the mass ratio of γ-mercaptopropyltrimethoxysilane, the ethanol aqueous solution, and the hydroxylated polyester is 1:19:0.39;

[0083] Step (3), at 90° C., dissolving 2.8 g of agarose in 80 g of N,N-dimethylacetamide, and adding 4 mL of a 7.7 wt% N,N-dimethylacetamide dilution of acryloyl chloride dropwise at a rate of 0.8 mL / min in an ice-water bath. After the addition is completed, reacting in an ice-water bath for 120 min, then reacting at room temperature for 4 h, concentrating the reaction mixture by rotary evaporation to a volume of 25 mL, precipitating with acetone, washing, and drying to obtain modified agarose;

[0084] 12.5 g of silane-modified polyester was dispersed in 300 g of ethanol under an ultrasonic power of 400 W, and then heated to 65° C., and then 2.5 g of modified agarose was added, and then 50 g of azobisisobutyronitrile ethanol solution with a mass fraction of 0.4 wt% was added dropwise at a rate of 2 mL / min. After the addition was completed, stirring was continued for 3 h. After the reaction was completed, centrifugation, washing, and drying were performed to obtain a grafted modified polyester;

[0085] 15 g of grafted modified polyester was ultrasonically dispersed in 250 g of toluene, heated to 70° C., and then 6 g of modified hybrid reduced graphene oxide and 0.02 g of boron trifluoride-ether were added, and stirred for reaction for 2 h. After the reaction was completed, the mixture was filtered, washed, and dried to obtain a composite modified polyester;

[0086] Step (4), melt spinning the composite modified polyester to obtain graphene polyester fiber, and spinning the graphene polyester fiber to obtain graphene polyester yarn with a fineness of 25D; mixing cotton fiber and modified phase change fiber in a ratio of 1:0.8 and blending to obtain a composite yarn with a count of 40 English count; using the graphene polyester yarn as a warp and the composite yarn as a weft, interweaving through a knitting device to obtain a graphene knitted fabric, wherein the density of the graphene composite fiber yarn is 440 strands / 10 cm, the density of the composite skin-friendly fiber yarn is 370 strands / 10 cm, and the twist of the graphene polyester yarn and the composite yarn is 900 twists / m;

[0087] Step (5), dissolving 25g of corn protein powder and 7.5g of glucose powder in 150g of 75% by volume ethanol aqueous solution, stirring in a 55°C water bath for 14h, cooling to obtain a spinning solution; electrospinning the spinning solution on one side of the graphene knitted fabric to form a hydrophobic fiber membrane, and then drying at 120°C for 3h to obtain an antistatic thermal insulation fabric based on graphene; wherein the electrospinning conditions are: spinning voltage of 18kV, spinning distance of 16cm, relative humidity of 40%, and spinning temperature of 25°C.

[0088] The phase change fibers in the above Examples 2-4 are the phase change fibers prepared in Example 1.

[0089] Comparative Example 1

[0090] Comparative Example 1 Compared with Example 1, in the process of preparing the phase change fiber in Comparative Example 1, no hydrophilic modified nano-silica was added, and other conditions remained unchanged.

[0091] Comparative Example 2

[0092] Comparative Example 2 Compared with Example 1, in the process of preparing the phase change fiber in Comparative Example 2, styrene is used instead of carboxylated polystyrene, and other conditions remain unchanged.

[0093] Comparative Example 3

[0094] Compared with Example 1, in the process of preparing graphene knitted fabric, Comparative Example 3 uses the modified phase change fiber prepared in Comparative Example 1, and other conditions remain unchanged.

[0095] Comparative Example 4

[0096] Comparative Example 4 Compared with Example 4, in the process of preparing graphene knitted fabric, Comparative Example 4 uses the modified phase change fiber prepared in Comparative Example 2, and other conditions remain unchanged.

[0097] Comparative Example 5

[0098] Compared with Example 4, in the process of preparing the graphene knitted fabric in Comparative Example 5, phase change fiber is used instead of modified phase change fiber, and other conditions remain unchanged.

[0099] Comparative Example 6

[0100] Compared with Example 4, Comparative Example 6 uses reduced graphene oxide instead of hybrid modified reduced graphene oxide, and other conditions remain unchanged.

[0101] Comparative Example 7

[0102] Compared with Example 4, in Comparative Example 7, during the preparation of the composite modified polyester, the grafted modified polyester and the modified hybrid reduced graphene oxide are directly mixed, and other conditions remain unchanged.

[0103] Comparative Example 8

[0104] Comparative Example 8 Compared with Example 4, in the process of preparing the composite modified polyester in Comparative Example 8, silane-modified polyester was used instead of graft-modified polyester, and other conditions remained unchanged.

[0105] In the above embodiments and comparative examples, graphene oxide, with a thickness of 0.55-1.2 nm and a diameter of 0.5-3 μm, is from Zhongke Leiming (Beijing) Technology Co., Ltd.; polyester chips, with a melting point of 180°C, are used for spinning and blowing, with a melt index of 3.3 g / 10 min, a tensile strength of 62 MPa, an elongation at break of 4.5%, and a density of 1.17 g / cm 3, from Dongguan Siyezi Plastic Co., Ltd.; agarose, CAS number is 9012-36-6, molecular formula is C 24 H 38 O 19 , from Hubei Xinyuhong Biotechnology Co., Ltd.; corn alcohol-soluble protein powder, with an active ingredient content of 99%, is a yellow powder in appearance, with the model number LY8493, from Hubei Xinyuhong Biotechnology Co., Ltd.; polyethylene glycol, with a molecular weight of 900-1000, comes from Nantong Yongle Chemical Co., Ltd.; nano-silicon dioxide, with a particle size of 30nm, with the model number DK-SiO2-30, comes from Beijing Dekedaojin Technology Co., Ltd.

[0106] Experimental example

[0107] The performance of the graphene-based antistatic thermal insulation fabrics of Examples 2-4 and Comparative Examples 3-8 was tested.

[0108] 1. Antistatic test: According to GB / T12703 standard, the half-life is recorded by the half-life method, and the initial half-life and the half-life after 50 washings are tested. The shorter the half-life, the better the antistatic performance of the fabric.

[0109] 2. Warmth test: Test the thermal insulation rate of the fabric according to GB / T11048 "Test method for thermal insulation performance of textiles" to characterize the warmth retention of the fabric.

[0110] The test results are shown in Table 1:

[0111] Table 1

[0112] Initial half-life / s Washing 50 times half-life / s Insulation rate / % Example 2 1.32 1.56 50.1 Example 3 1.21 1.41 51.4 Example 4 1.27 1.50 50.6 Comparative Example 3 1.33 1.58 49.2 Comparative Example 4 1.36 1.74 49.9 Comparative Example 5 1.58 1.83 47.7 Comparative Example 6 1.29 1.53 48.0 Comparative Example 7 1.41 1.77 48.8 Comparative Example 8 1.56 1.82 49.7

[0113] It can be seen from the test results in Table 1 that the graphene-based antistatic thermal fabrics prepared in Examples 2-4 of the present invention have good thermal insulation and long-term antistatic properties. From the comparison between Comparative Example 3 and Example 4, it can be seen that the hydrophilic modified nano-silica makes the polystyrene fiber produce more pores, which is helpful for the loading of polyethylene glycol, and can improve the hydrophilicity of the phase change fiber, thereby improving the antistatic and warmth retention of the fabric; from the comparison between Comparative Example 4 and Example 4, it can be seen that compared with the polystyrene without carboxyl groups, the introduction of carboxyl groups in the polystyrene containing carboxyl groups can not only form hydrogen bonds with polyethylene glycol and hydrophilic modified nano-silica, improve the compatibility with polyethylene glycol and hydrophilic modified nano-silica, but also improve the hydrophilicity of the phase change fiber, and can combine with polydopamine through electrostatic action to improve the encapsulation effect of polydopamine, thereby having a positive effect on the warmth retention and lasting antistatic properties of the fabric; from the comparison between Comparative Example 5 and Example 4, it can be seen that encapsulating polydopamine on the surface of the phase change fiber can prevent the leakage of the phase change material and improve the hydrophilicity of the phase change fiber on the one hand, and on the other hand, polydopamine and zinc-aluminum layered double metal The synergy of zinc-aluminum layered double metal hydroxide and reduced graphene oxide nanosheets can utilize full-spectrum sunlight to improve the photothermal conversion efficiency, thereby improving the antistatic and warmth retention of the fabric; from the comparison of comparative example 6 with example 4, it can be seen that the zinc-aluminum layered double metal hydroxide and reduced graphene oxide synergistically show excellent photothermal conversion effect, improve the warmth retention of the fabric, and improve the agglomeration of reduced graphene oxide nanosheets, thereby having a slight effect on the antistatic property of the fabric; from the comparison of comparative example 7 with example 4, it can be seen that combining the grafted modified polyester and the modified hybrid reduced graphene oxide in a direct mixing manner will affect the dispersibility and durability of the modified hybrid reduced graphene oxide, thereby affecting the performance of the fabric; from the comparison of comparative example 8 with example 4, it can be seen that introducing agarose into polyester can introduce more abundant hydroxyl groups, improve the hydrophilicity of polyester, and increase the grafting amount of modified hybrid reduced graphene oxide, thereby improving the antistatic and warmth retention of the fabric.

[0114] 3. One-way sweat transport test: The water contact angles on both sides of the graphene-based antistatic thermal insulation fabrics of Examples 2-4 were tested using a water contact angle meter. The test results are shown in Table 2:

[0115] Table 2

[0116] Water contact angle on the hydrophobic fiber membrane side / ° Water contact angle on the side of graphene knitted fabric / ° Example 2 122.3 15.7 Example 3 124.1 14.5 Example 4 123.5 15.0

[0117] It can be seen from Table 2 that the graphene-based antistatic thermal insulation fabrics prepared in Examples 2-4 have significant wettability differences on both sides, which will produce anisotropic water penetration pressure, driving sweat to completely leave the skin surface while preventing external moisture penetration, so that the fabrics of the present invention have good moisture and heat comfort.

[0118] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A method for preparing antistatic thermal insulation fabric based on graphene, It is characterized in that The following steps are involved: Step (1), preparing a hybrid reduced graphene oxide containing zinc-aluminum layered double metal hydroxide, and then modifying it with a silane coupling agent KH-560 to obtain a modified hybrid reduced graphene oxide; Step (2), the polyester is subjected to hydroxylation treatment and γ-mercaptopropyltrimethoxysilane modification treatment to obtain silane-modified polyester, the method is as follows: The polyester chips are crushed into polyester powder with a particle size of 30-80 μm, the polyester powder is added into a sodium hydroxide aqueous solution with a concentration of 200 g / L, stirred and reacted at 70-90° C. for 20-40 min, filtered, washed, and dried to obtain a hydroxylated polyester; wherein the mass ratio of the polyester powder to the sodium hydroxide aqueous solution is (10-15):(200-350); Add γ-mercaptopropyltrimethoxysilane to an ethanol aqueous solution with a volume fraction of 80%, then add the hydroxylated polyester, stir and soak for 20-40 minutes at room temperature, filter, wash, and dry to obtain a silane-modified polyester; wherein the mass ratio of γ-mercaptopropyltrimethoxysilane, ethanol aqueous solution, and hydroxylated polyester is 1:(16-22):(0.34-0.44); Step (3), modifying agarose with acryloyl chloride to obtain modified agarose; reacting the modified agarose with silane-modified polyester to obtain grafted modified polyester; reacting the grafted modified polyester with modified hybrid reduced graphene oxide to obtain a composite modified polyester: The preparation method of the modified agarose comprises: dissolving agarose in N,N-dimethylacetamide at 80-100° C., adding a dilution of N,N-dimethylacetamide with a mass fraction of 7.7 wt% of acryloyl chloride at a rate of 0.5-1 mL / min in an ice water bath, reacting in an ice water bath for 100-150 min after the addition is completed, and then reacting at room temperature for 3.5-4.5 h, concentrating by rotary evaporation, precipitating with acetone, washing, and drying; wherein the amount ratio of agarose, N,N-dimethylacetamide, and the dilution of N,N-dimethylacetamide of acryloyl chloride is (1.5-3) g:(50-100) g:(3.2-4.8) mL; The preparation method of the composite modified polyester comprises the following steps: dispersing the silane modified polyester in ethanol under an ultrasonic power of 300-500 W, heating to 50-80° C., adding modified agarose, and then dripping a 0.4wt% azobisisobutyronitrile ethanol solution at a rate of 1.5-2.5 mL / min, stirring and reacting for 2-4 hours after the dripping is completed, centrifuging, washing, and drying to obtain the grafted modified polyester; wherein the mass ratio of the silane modified polyester, ethanol, modified agarose, and azobisisobutyronitrile ethanol solution is (10-15):(200-400):(1-4):(40-60); The grafted modified polyester is ultrasonically dispersed in toluene, heated to 60-80°C, and then modified hybrid reduced graphene oxide and boron trifluoride-ether are added, stirred for reaction for 1-3h, and after the reaction is completed, filtered, washed, and dried to obtain a composite modified polyester; wherein the mass ratio of the grafted modified polyester, toluene, modified hybrid reduced graphene oxide, and boron trifluoride-ether is (10-20):(200-300):(4-8):(0.01-0.03); Step (4), melt spinning the composite modified polyester to obtain graphene polyester fiber, and then spinning to obtain graphene polyester yarn; blending cotton fiber and modified phase change fiber to obtain composite yarn; interweaving the graphene polyester yarn and the composite yarn to obtain graphene knitted fabric; The method for preparing the modified phase change fiber comprises the following steps: Step S1, reacting methacrylic acid with styrene to prepare carboxylated polystyrene; Step S2, the nano-silica is activated and modified with 3-aminopropyltriethoxysilane to obtain hydrophilic modified nano-silica; Step S3, carboxylated polystyrene, polyethylene glycol, hydrophilic modified nano-silica, and N,N-dimethylformamide are mixed to obtain a precursor solution, and electrospinning is performed to obtain a phase change fiber; the phase change fiber is modified with polydopamine to obtain a modified phase change fiber; Step (5), mixing zein powder, glucose powder and ethanol aqueous solution into a spinning solution, and electrospinning on one side of the graphene knitted fabric to form a hydrophobic fiber membrane, thereby obtaining an antistatic thermal insulation fabric based on graphene.

2. The method for preparing the graphene-based antistatic thermal insulation fabric according to claim 1, It is characterized in that In the step (1), the preparation method of the modified hybrid reduced graphene oxide comprises: dissolving zinc nitrate hexahydrate and aluminum nitrate nonahydrate in deionized water to obtain a solution A; Dissolve urea in deionized water to obtain solution B; add solution A and solution B to a graphene oxide aqueous dispersion having a concentration of 2 g / L, stir at 90-110° C. for 10-14 h, then statically crystallize for 20-28 h, filter, centrifuge, wash, and freeze-dry to obtain hybrid reduced graphene oxide; wherein the mass ratio of zinc nitrate hexahydrate, aluminum nitrate nonahydrate, urea, and graphene oxide is (1.6-2.2):1:(2.3-2.5):(3-6); In a nitrogen atmosphere, hybrid reduced graphene oxide, ethanol, deionized water, 25wt% ammonia water, and silane coupling agent KH-560 are mixed, stirred and reacted at 50-90°C for 2-8h, centrifuged, washed, and dried to obtain modified hybrid reduced graphene oxide; wherein the mass ratio of hybrid reduced graphene oxide, ethanol, deionized water, 25wt% ammonia water, and silane coupling agent KH-560 is (2-10):100:(4-12):(1-8):(1-8).

3. The method for preparing the graphene-based antistatic thermal insulation fabric according to claim 1, It is characterized in that In the step (4), the fineness of the graphene polyester yarn is 20-30D; the ratio of cotton fiber to modified phase change fiber in the composite yarn is 1:(0.5-1), and the count of the composite yarn is 30-50 English count.

4. The method for preparing the graphene-based antistatic thermal insulation fabric according to claim 1, It is characterized in that In the step (5), the preparation method of the graphene-based antistatic thermal insulation fabric is as follows: corn alcohol-soluble protein powder, glucose powder, and 75% ethanol aqueous solution by volume fraction are mixed in a mass ratio of (20-30):(5-10):(100-200), stirred in a water bath at 50-60°C for 12-16 hours, and cooled to obtain a spinning solution; the spinning solution is electrostatically spun on one side of the graphene knitted fabric to form a hydrophobic fiber membrane, and then dried at 110-130°C for 2-4 hours to obtain the graphene-based antistatic thermal insulation fabric; wherein the electrostatic spinning conditions are as follows: the spinning voltage is 15-20 kV, the spinning distance is 14-18 cm, the relative humidity is 35-45%, and the spinning temperature is 23-27°C.

5. The method for preparing the graphene-based antistatic thermal insulation fabric according to claim 1, It is characterized in that In the step (4), the method for preparing the modified phase change fiber comprises the following steps: Step S1, dissolving polyvinyl pyrrolidone in ethanol and ethylene glycol monomethyl ether, stirring at a speed of 200-300 r / min, then adding methacrylic acid, azobisisobutyronitrile and styrene, reacting at 45-55° C. for 10-30 min in a nitrogen atmosphere, and then reacting at 70-80° C. for 24-36 h. After the reaction is completed, cooling to room temperature, washing and drying the obtained solid to obtain carboxylated polystyrene; wherein the mass ratio of polyvinyl pyrrolidone, ethanol, ethylene glycol monomethyl ether, methacrylic acid, azobisisobutyronitrile and styrene is (1-2):(25-30):(15-20):(1.2-3):(1.2-1.5):(10.8-13.5); Step S2, mixing nano-silicon dioxide with a sodium hydroxide aqueous solution having a concentration of 1 mol / L, reacting at 65-75° C. for 20-30 hours, then neutralizing the sodium hydroxide with a hydrochloric acid aqueous solution having a concentration of 1 mol / L, centrifuging, washing, and drying to obtain activated nano-silicon dioxide; wherein the amount ratio of nano-silicon dioxide, sodium hydroxide aqueous solution, and hydrochloric acid aqueous solution is (4-10) g:(100-200) mL:(100-200) mL; Add activated nano-silica to ethanol and homogenize for 45-50 hours, then add 3-aminopropyltriethoxysilane, react at room temperature for 5.5-6.5 hours, centrifuge, wash, and dry to obtain hydrophilic modified nano-silica; wherein the mass ratio of activated nano-silica, ethanol, and 3-aminopropyltriethoxysilane is (4-8):(100-200):(2-4); Step S3, mixing carboxylated polystyrene, polyethylene glycol, hydrophilic modified nano-silica, and N,N-dimethylformamide in a mass ratio of (1-2):(0.5-1.5):(0.2-0.5):(5-10), stirring for 4-10 hours to obtain a precursor solution; maintaining the feed rate of the precursor solution at 2.5-3.5 mL / h, performing electrostatic spinning at a voltage of 20-30 kV and a spinning distance of 15-25 cm, and drying at room temperature for 10-12 hours to obtain a phase change fiber; The phase change fiber is immersed in a dopamine hydrochloride solution with a mass fraction of 1wt% at 27-33°C, the pH is adjusted to 8.5 by using ammonia water with a mass fraction of 25wt%, and after immersion for 10-15h, it is taken out, washed, and dried to obtain a modified phase change fiber.

6. A graphene-based antistatic thermal insulation fabric prepared by the method for preparing a graphene-based antistatic thermal insulation fabric as described in any one of claims 1 to 5.

7. Application of the graphene-based antistatic thermal insulation fabric according to claim 6 in clothing.

Citation Information

Patent Citations

  • A graphene knitted fabric and its preparation method

    CN113308782B

  • Preparation method of functionalized graphene intercalated in-situ polymerized polyester composite fibers

    CN112458568A

  • Modified graphene oxide, preparation method thereof and coating

    CN114381160A

  • Antistatic fabric and preparation method thereof

    CN115058896A

  • Anti-cracking micro-electrostatic filter element material and preparation method thereof

    CN115646063A