High-efficiency large-deposition high-toughness narrow-gap welding method and device for titanium alloy
Through the blunt edge U-shaped groove design and K-TIG welding process, combined with magnetic field swing and argon protection, the problems of unfused side walls and low cladding volume in large-thickness welding of titanium alloys are solved, and high-efficiency large cladding and High toughness welding to meet standard requirements.
Patent Information
- Application Number
- CN202411126803.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-16
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2044-08-16
AI Technical Summary
In the existing technology, high-efficiency and high-quality narrow-gap welding of large-thickness titanium alloys has problems such as unfused side walls, low single-layer cladding, and low joint impact toughness.
It adopts blunt edge U-shaped groove design, K-TIG welding process, introduces magnetic field to make the tungsten pole swing periodically, combined with argon gas protection, deep penetration argon arc welding, and arc preheating treatment on the welding groove surface to improve welding efficiency and joint toughness. .
It significantly improves the welding deposition efficiency, avoids pores and unfused sidewall defects, improves the impact toughness of the joint, reaches the same strength and toughness as the base metal, and meets the first-level qualification requirements of the NB/T 47013 standard.
Smart Images

Figure CN118744268A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of metal material welding, and in particular to a titanium alloy high-efficiency, large-deposition, high-toughness, narrow-gap welding method and device. Background Art
[0002] With the development of the marine economy, the thickness demand for titanium alloy structural parts is also increasing. The characteristics of titanium alloys used in marine engineering are "large and thick". High-strength titanium alloys are often used to weld structural parts. Traditional TIG welding requires more welding wire to fill the large-angle groove, resulting in large joint stress and welding deformation, low cladding efficiency, and slow welding speed. In addition, the wider heat-affected zone will reduce the performance of the joint. In contrast, the narrow gap welding method uses a small-angle groove to reduce the amount of weld beads and welding wire filling, thereby improving welding efficiency. Narrow gap welding provides an efficient solution for the manufacturing of titanium alloys in the marine engineering field, but conventional narrow gap TIG welding technology has the problems of low welding efficiency and easy side wall unfusion during welding, which makes it have great limitations in welding large-thickness titanium alloys.
[0003] In recent years, various welding technologies based on the narrow gap concept have emerged one after another. Narrow gap TIG welding has become one of the most widely used methods for complex large components due to its convenient operation, good welding quality and small deformation. However, it is limited by its disadvantages such as low efficiency and long cycle. Although many scholars have proposed different ideas and methods to solve the problems of unfused side walls and low welding efficiency, the improved welding equipment is complex and the welding efficiency is still low. Yoshiaki Arata of Osaka University in Japan and KW Carlson of the University of Illinois in the United States first proposed narrow gap laser wire welding in 1986. Subsequent scholars focused on how to deflect the laser to solve the problem of unfused side walls. The deflection electron microscope system was added. This method is more prone to defects such as welding pores and unfused due to the high energy density of the laser beam and the generation of keyholes. Similarly, narrow gap laser-arc hybrid welding has the same problem. Domestic researchers have proposed a series of innovative solutions to the above problems and applied for patents. Among the more representative existing technologies, the patent with application number CN202211330990.6 discloses a laser arc hybrid welding primer combined with arc control welding method and device, including a preheating device, a laser arc composite heat source, a combined arc heat source and a cooling device which are sequentially arranged above the workpiece to be welded and can move synchronously; the spacing between the preheating device, the laser arc composite heat source, the combined arc heat source and the cooling device can be adjusted. This patent can improve the shape and performance quality of the welding structure, but the composite heat source welding requires the simultaneous control of both laser and arc heat sources, which increases the complexity of process control and greatly increases the purchase and maintenance costs of the equipment; in addition, the mutual influence of the laser and the arc may lead to unstable welding quality, which requires precise regulation.
[0004] In addition, due to the characteristics of titanium alloy itself, the toughness of the joint after welding is reduced. The thermal conductivity of titanium alloy is very small, but the linear expansion coefficient is very large. Under the welding heat cycle of multi-layer and multi-pass welding, thick plates usually produce unevenly distributed three-dimensional stress, which greatly reduces the plasticity, toughness and other properties of the joint.
[0005] In summary, the existing technology for efficient and high-quality narrow gap welding of thick titanium alloys has problems such as unfused side walls, low single-layer cladding, and low impact toughness of the joint.
[0006] In view of this, the present invention is proposed. Summary of the invention
[0007] The purpose of the present invention is to propose a titanium alloy high-efficiency, large-cladding, high-toughness, narrow-gap welding method and device, so as to solve the problems of unfused side walls, low single-layer cladding amount and low impact toughness of joints in the prior art for high-efficiency, high-quality, narrow-gap welding of thick titanium alloys.
[0008] To achieve the above object, the technical solution of the present invention is achieved as follows:
[0009] A titanium alloy high-efficiency large-deposition high-toughness narrow-gap welding method, comprising:
[0010] S1. Welding groove design:
[0011] The root length of the welding groove is 4-6 mm, the groove angle is 3-6°, the blunt edge thickness is 8-12 mm, and the root radius R is 1-2 mm;
[0012] S2. Welding process:
[0013] The base welding is K-TIG welding, the welding current is 390-450A, and the welding speed is 90-110mm / min;
[0014] The filling welding is K-TIG wire welding, the welding current is 400-500A, and the welding speed is 90-100mm / min;
[0015] The cap welding is automatic TIG wire welding, the welding current is 180-200A, and the welding speed is 70-90mm / min;
[0016] During the welding process, a magnetic field is introduced to cause the tungsten electrode to oscillate periodically;
[0017] Argon is used as shielding gas during welding.
[0018] The titanium alloy high-efficiency large-cladding high-toughness narrow-gap welding method described in the present invention avoids defects such as pores and unfused side walls during large-cladding, thereby improving welding efficiency, welding deposition efficiency and impact toughness of welded joints.
[0019] Furthermore, the intensity of the magnetic field is 0 to 20 mT, and the stirring frequency of the magnetic field is 0 to 30 Hz.
[0020] Furthermore, the groove surface is arc preheated before welding.
[0021] Furthermore, during filling welding, the diameter of the welding wire is 1.6 to 3.0 mm, and the wire feeding speed is 20 to 50 mm / s.
[0022] Furthermore, during cap welding, the diameter of the welding wire is 1.6 mm and the wire feeding speed is 15 to 20 mm / s.
[0023] Furthermore, the flow rate of the protective gas is 30 L / min, and the purity of the protective gas is 99.999%.
[0024] Furthermore, before welding, a protective gas is passed around the tungsten electrode, and a protective drag hood is used behind the tungsten electrode.
[0025] In a second aspect of the present invention, a titanium alloy high-efficiency large deposition high-toughness narrow gap welding device is provided, wherein the welding device is used for welding in the above-mentioned titanium alloy high-efficiency large deposition high-toughness narrow gap welding method, and the welding device comprises:
[0026] Welding gun;
[0027] A welding power source connected to the welding gun;
[0028] A wire feeder, which feeds wire to the welding gun;
[0029] The magnetron device is arranged on one side of the welding gun, and can introduce a magnetic field during welding to cause the tungsten pole to oscillate periodically.
[0030] Compared with the prior art, the titanium alloy high-efficiency large-deposition high-toughness narrow-gap welding method and device described in the present invention have the following beneficial effects:
[0031] The titanium alloy high-efficiency large deposition high-toughness narrow gap welding method and device described in the present invention solve the problems of low welding efficiency and unfused side walls in narrow gap welding, and can increase the welding deposition efficiency to 3.0Kg / h, which is more than 7 times that of existing traditional narrow gap welding. At the same time, it can ensure that the flaw detection of the welded joint meets the first-level qualification requirements of the NB / T 47013 standard, and the strength and toughness of the joint reach the same level as the parent material, thereby realizing titanium alloy high-efficiency large deposition high-toughness narrow gap welding. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 A schematic diagram of a titanium alloy high-efficiency, large-deposition, high-toughness, narrow-gap welding device according to an embodiment of the present invention;
[0033] Figure 2 A schematic diagram of a groove structure of a titanium alloy high-efficiency large deposition high-toughness narrow gap welding method according to an embodiment of the present invention;
[0034] Figure 3 A metallographic diagram of a joint welded by a titanium alloy high-efficiency large-deposition high-toughness narrow-gap welding method according to an embodiment of the present invention;
[0035] Figure 4 This is the metallographic diagram of the traditional titanium alloy high-efficiency large deposition and high-toughness narrow gap weld joint.
[0036] Description of reference numerals:
[0037] 1. Welding gun; 2. Welding power source; 3. Wire feeder; 4. Magnetron device; 5. Workpiece. DETAILED DESCRIPTION
[0038] It should be noted that, in the absence of conflict, the embodiments of the present invention and the features in the embodiments can be combined with each other. The descriptions of "first", "second", etc. mentioned in the embodiments of the present invention are only for descriptive purposes, and cannot be understood as indicating or implying their relative importance or implicitly indicating the number of technical features indicated. Therefore, the features defined as "first" and "second" may explicitly or implicitly include at least one of the features. In addition, the technical solutions between the various embodiments can be combined with each other, but they must be based on the ability of ordinary technicians in the field to implement them. When the combination of technical solutions is contradictory or cannot be implemented, it should be deemed that such a combination of technical solutions does not exist and is not within the scope of protection required by the present invention.
[0039] The present invention will be described in detail below with reference to the accompanying drawings and in conjunction with embodiments.
[0040] In the prior art, efficient and high-quality narrow-gap welding of thick titanium alloys has problems such as unfused side walls, low single-layer cladding, and low impact toughness of the joint.
[0041] The purpose of the present invention is to solve the above problems. Aiming at the demand for high-efficiency, high-quality and narrow-gap welding of thick titanium alloys, a high-efficiency, large-cladding, high-toughness and narrow-gap welding method for titanium alloys is proposed. A magnetic field is introduced during the welding process to make the tungsten electrode oscillate periodically, effectively solving the problem of unfused side walls. At the same time, the magnetic field is used to stir the molten pool to effectively avoid the generation of welding defects. The columnar crystals in the weld can also be broken, and the weld grains can be refined to improve the toughness and plasticity of the weld. In addition, through deep-melting argon arc welding, a strong arc force is generated by a large current to push the molten pool to form a keyhole effect. By concentrating the welding energy, deep-melting welding is achieved, and the cladding efficiency can reach more than 3.0kg / h.
[0042] Specifically, Figures 1 to 3 As shown, the applicant aims at the demand for high-efficiency, high-quality and narrow-gap welding of thick titanium alloys, and the present invention provides a titanium alloy high-efficiency, large-deposition, high-toughness and narrow-gap welding method, the welding method comprising the following steps:
[0043] S1. Welding groove design:
[0044] The design of welding groove needs to minimize the cross-sectional area of the groove to reduce the amount of cladding metal filling and increase the welding speed. Figure 2 As shown, a U-shaped double-sided groove with a blunt edge is processed on the titanium alloy thick plate to be welded, the root length d of the welding groove is 4 to 6 mm, the welding groove angle β is 3 to 6°, and the blunt edge thickness 2c is 8 to 12 mm.
[0045] The root radius R is 1 to 2 mm, which increases the space at the root of the groove and allows the weld metal to spread better to facilitate penetration of the root.
[0046] S2. Welding process:
[0047] Before welding, the groove surface is arc preheated to make the groove surface temperature reach above the β phase transformation point, and then cooled to room temperature. The structure of the welded joint can be intertwined with the structure formed by preheating. This organizational feature is conducive to improving the impact toughness of the joint.
[0048] The base welding is K-TIG welding, the welding current is 390~450A, and the welding speed is 90~110mm / min. This setting can realize deep penetration welding of the base weld of titanium alloy with a thickness of less than 15mm, and on the other hand, it can realize high-efficiency large cladding filling of 3.0Kg / h per pass, thus ensuring high-efficiency welding of thick titanium alloy;
[0049] For base welding, different base welding processes are used for different welding materials to ensure high toughness of the joint.
[0050] For high-strength titanium alloy, due to its poor plasticity and toughness, the base welding is K-TIG wire welding, the welding current is 390~450A, and the speed is 90~110mm / min.
[0051] The welding wire is a low-matching or pure titanium welding wire, and high plasticity and toughness welding of the weld joint is achieved through welding fusion of the welding wire and the material to be welded.
[0052] Among them, high-strength titanium alloy refers to titanium alloy materials with tensile strength ≥840MPa and yield strength ≥740MPa.
[0053] For high plasticity and high toughness titanium alloy materials, the base welding is K-TIG self-melting welding without wire, the welding current is 390~450A, and the speed is 90~110mm / min.
[0054] Among them, high plasticity and high toughness titanium alloy materials refer to those with elongation after fracture A≥10% and impact toughness>47J / cm 2 , fracture toughness ≥70MPa·m 1 / 2 Titanium alloy material.
[0055] The filling welding is K-TIG filling wire welding. The welding wire uses a matching welding wire with similar composition to the base material. The welding current is 400-500A and the welding speed is 90-100mm / min.
[0056] K-TIG is used as the welding heat source for the filling layer, and the welding current is between 400 and 500A, which can achieve a high-efficiency large cladding filling of 3.0Kg / h for a single pass, thereby ensuring the efficient welding of thick titanium alloys.
[0057] If K-TIG is still used for cap welding, the surface of the welding sample will be burned and not beautiful. Therefore, in the present invention, the cap welding is automatic TIG welding, the welding current is 180-200A, the welding speed is 70-90mm / min, and when cap welding, the welding wire uses a matching welding wire with similar composition to the base material, the diameter of the welding wire is 1.6mm, and the wire feeding speed is 15-20mm / s, so as to obtain a weld with good surface forming, beautiful and flat surface, and smooth transition with the base material.
[0058] The cover welding uses automatic TIG as the welding heat source, which can ensure the accuracy and consistency of welding, significantly improve the efficiency, fast welding speed and beautiful weld.
[0059] Since titanium alloys are very easy to absorb nitrogen, hydrogen, and oxygen at high welding temperatures, which reduces the plasticity and toughness of the weld and causes weld embrittlement, titanium alloys must be effectively protected during welding.
[0060] In the present invention, argon is used as a shielding gas during the welding process. Argon is an inert gas that effectively prevents titanium alloy from being oxidized in a high-temperature welding environment. The cost of production, storage, and transportation is also low, and the safety is higher. The shielding gas can also stabilize the arc and increase the depth of penetration.
[0061] Before welding, a protective gas is passed around the tungsten electrode, and a protective hood is used behind the tungsten electrode to prevent gas overflow and isolate the air to prevent oxidation in the welding area. The protective gas flow rate is 30L / min, and the purity of the protective gas is 99.999% high-purity argon.
[0062] In order to effectively improve welding efficiency and avoid defects such as pores and unfused side walls during large cladding, a magnetic field is introduced during the entire welding process to cause the tungsten electrode to oscillate periodically, and the arc oscillates periodically to stir the molten pool.
[0063] During the welding process, a transverse magnetic field is introduced, and the magnetic flux lines are arranged along the direction of the weld. The arc swings periodically to stir the molten pool. The intensity of the magnetic field is 0-20mT, and the stirring frequency of the magnetic field is 0-30Hz. The tungsten pole heat source and magnetic control guided arc deflection are used to improve the spreading effect of the liquid metal and accelerate the internal movement of the molten pool, reduce the surface tension and the weld defects caused by insufficient internal molten pool movement, and thus innovatively achieve large cladding, high-speed, and high-efficiency welding of titanium alloys.
[0064] In the titanium alloy high-efficiency large-deposition high-toughness narrow-gap welding method described in the present invention, the welding groove design of step S1 and the welding process of step S2 are interrelated and cooperate with each other to play multiple roles:
[0065] 1. In the welding process, a magnetic field is introduced to make the tungsten electrode swing periodically, so that the arc heat distribution is reasonable and uniform, which plays a role in controlling the arc heat distribution. At the same time, the arc is made to swing periodically. The periodic swing of the arc stirs the molten pool, accelerates the movement inside the molten pool, and makes the solidification structure of the molten pool more evenly distributed, and refines the joint structure. On the one hand, it can effectively avoid defects such as pores and unfused side walls during the large cladding process. On the other hand, it improves the strength and impact toughness of the welded joint. In addition, it also improves the welding efficiency.
[0066] 2. During the process of base welding and filling welding, deep-melting argon arc welding is used to generate a strong arc force with a large current to push the molten pool to form a keyhole effect. By concentrating the welding energy, deep-melting welding is achieved, which improves the cladding efficiency. The cladding efficiency can reach more than 3.0kg / h, which is more than 7 times that of existing traditional narrow gap welding.
[0067] 3. Before welding, the groove surface is preheated with arc to make the groove surface temperature reach above the β phase transformation point, and then cooled to room temperature. The structure of the welded joint can be intertwined with the structure formed by preheating. This organizational feature is conducive to improving the impact toughness of the joint.
[0068] 4. During the welding process, high plasticity and toughness welding of the welded joint is achieved through welding fusion of the welding wire and the material to be welded.
[0069] The present invention also provides a titanium alloy high-efficiency large deposition high-toughness narrow gap welding device, the welding device is used for the titanium alloy high-efficiency large deposition high-toughness narrow gap welding method, such as Figure 1 As shown, the welding device comprises:
[0070] Welding gun 1, the electrode of the welding gun 2 is a tungsten electrode;
[0071] A welding power source 2, which is connected to the welding gun 1, and forms a welding arc at the end of the welding gun 2. The heat generated by the welding arc can heat the welding wire, melt the welding wire, and form a molten pool;
[0072] A wire feeder 3, which feeds welding wire to the welding gun 1;
[0073] The magnetron device 4 is arranged on one side of the welding gun 1 , and can introduce a magnetic field during welding to cause the tungsten pole to oscillate periodically.
[0074] The workpiece 5 is welded by the welding device.
[0075] The magnetron device 4 is a device that adds an electromagnet near the tungsten pole and winds an electromagnetic wire around it. When an alternating current is passed through the electromagnetic wire, an electromagnetic field is generated. The magnetic lines of force promote the arc to swing periodically at the narrow gap groove, so that the arc heat distribution is reasonably uniform, which plays a role in controlling the arc heat distribution and can effectively avoid defects such as pores and unfused side walls during large cladding. At the same time, the swinging welding pool of the arc has a uniformly distributed solidified structure, which refines the weld structure and improves the impact toughness and plasticity of the joint.
[0076] In this application, large thickness refers to a plate thickness range of 20 to 100 mm.
[0077] The present invention describes a titanium alloy high-efficiency, large-deposition, high-toughness, narrow-gap welding method and device. The welding method and the welding device are interrelated and work together to not only solve the problems of low welding efficiency and unfused side walls in narrow gap welding, but also increase the welding deposition efficiency to 3.0Kg / h, which is more than 7 times that of existing traditional narrow gap welding. At the same time, it can ensure that the flaw detection of the welded joint meets the first-level qualification requirements of the NB / T47013 standard, and the strength and toughness of the joint reach the same level as the parent material, thereby achieving titanium alloy high-efficiency, large-deposition, high-toughness narrow gap welding.
[0078] Example 1
[0079] In this embodiment, the applicant proposes a titanium alloy high-efficiency large deposition high-toughness narrow gap welding method. In this embodiment, the titanium alloy is Ti80 alloy with a thickness of 60 mm;
[0080] The welding method comprises the following steps:
[0081] S1. Welding groove design: Figure 2 As shown, a U-shaped double-sided groove with a blunt edge is processed on the titanium alloy thick plate to be welded: the root length of the welding groove d = 5mm, the root radius R = 2mm, the groove angle β = 3°, and the blunt edge thickness 2c = 10mm;
[0082] exist Figure 2 In the figure, c is half of the blunt edge thickness, d is the root length, R is the root radius, and β is the groove angle.
[0083] S2. Welding process:
[0084] The groove surface is arc preheated before welding.
[0085] Ti80 material is a high plasticity and high toughness material. The base welding is K-TIG self-melting welding without wire. The welding current is 400A and the welding speed is 90mm / min.
[0086] The filling welding is K-TIG filler wire welding, the welding wire is Ti80A, the welding wire diameter is 3.0mm, the wire feeding speed is 50mm / s, the welding wire Ti80A has a meshing effect with the base material Ti80, which improves the strength of the welded joint, the welding current is 450A, and the welding speed is 100mm / min;
[0087] The cap welding is automatic TIG wire welding, the welding wire is Ti80A, the welding wire diameter is 1.6mm, the welding current is 200A, the welding speed is 90mm / min, and the wire feeding speed is 10mm / s, obtaining a well-formed weld with a smooth transition with the base material.
[0088] During the welding process, argon is used as the shielding gas, the flow rate of the shielding gas is 30L / min, and the purity of the shielding gas is 99.999%.
[0089] Before welding, a protective gas is passed around the tungsten electrode, and a protective hood is used behind the tungsten electrode.
[0090] Example 2
[0091] In this embodiment, a titanium alloy high-efficiency large deposition high-toughness narrow gap welding device is proposed, and the welding device is used for welding of any one of the titanium alloy high-efficiency large deposition high-toughness narrow gap welding methods, such as Figure 1 As shown, the welding device comprises:
[0092] Welding gun 1;
[0093] A welding power source 2 connected to the welding gun 1;
[0094] A wire feeder 3, which feeds wire to the welding gun 1;
[0095] The magnetron device 4 is arranged on one side of the welding gun 1 , and can introduce a magnetic field during welding to cause the tungsten pole to oscillate periodically.
[0096] Performance Testing
[0097] 1. The welded joint formed by the titanium alloy high-efficiency large deposition, high-toughness and narrow gap welding method described in Example 1 is subjected to non-destructive testing by X-ray, penetration and ultrasound.
[0098] Through testing, the applicant found that the welded joint formed by the titanium alloy high-efficiency large deposition, high-toughness and narrow gap welding method described in the present invention is well formed, and no macroscopic pores, cracks, undercuts and other welding defects are found in the welded joint, meeting the NB / T 47013 standard Level I qualification requirements.
[0099] 2. Metallographic tests were performed on the welded joints formed by the titanium alloy high-efficiency large deposition high-toughness narrow gap welding method described in Example 1 and the welded joints formed by the traditional narrow gap welding method. The metallographic samples were sampled in the direction perpendicular to the weld, and after being corroded by Kroll reagent, metallographic observation was performed under an OLYMPUS GX71 metallographic microscope. The metallographic morphology characterization results are shown in Figure 3 and Figure 4 .
[0100] like Figure 4 As shown, using traditional narrow gap welding, 27 layers need to be welded. Figure 3 As shown, the welded joint formed by the titanium alloy high-efficiency, large-deposition, high-toughness, narrow-gap welding method described in Example 1 only requires 11 layers of welding to complete, greatly improving the welding efficiency.
[0101] like Figure 3 As shown, metallographic observation shows that the welded joint formed by the titanium alloy high-efficiency, large-deposition, high-toughness, narrow-gap welding method described in the present invention is free of welding defects such as pores, lack of fusion and cracks.
[0102] 3. For the weld, fusion line and heat affected zone of the weld joint formed by the titanium alloy high-efficiency, large-deposition, high-toughness and narrow-gap welding method described in Example 1, the Charpy impact toughness tests were carried out three times on each area and the surface, 1 / 4 thickness, 1 / 2 thickness, 3 / 4 thickness and bottom layer of the base material. The results are shown in Table 1.
[0103] Table 1 Impact toughness of the joint of the present invention
[0104]
[0105] As shown in Table 1, the impact toughness of each area of the welded joint and the parent material formed by the titanium alloy high-efficiency large deposition high-toughness narrow gap welding method of the present invention is 47 J / cm 2 The above indicates that the welded joint formed by the titanium alloy high-efficiency large deposition, high-toughness and narrow-gap welding method described in the present invention has good impact toughness. This patent can be used to achieve high-efficiency large deposition, high-toughness and narrow-gap welding of thick titanium alloys.
[0106] Although the present invention is disclosed as above, the present invention is not limited thereto. Any person skilled in the art can make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, the protection scope of the present invention shall be subject to the scope defined by the claims.
Claims
1. A titanium alloy high-efficiency large-deposition high-toughness narrow-gap welding method, It is characterized in that include: S1. Welding groove design: The root length of the welding groove is 4-6 mm, the groove angle is 3-6°, the blunt edge thickness is 8-12 mm, and the root radius is 1-2 mm; S2. Welding process: The base welding is K-TIG welding, the welding current is 390-450A, and the welding speed is 90-110mm / min; The filling welding is K-TIG wire welding, the welding current is 400-500A, and the welding speed is 90-100mm / min; The cap welding is automatic TIG wire welding, the welding current is 180-200A, and the welding speed is 70-90mm / min; During the welding process, a magnetic field is introduced to cause the tungsten electrode to oscillate periodically; Argon is used as shielding gas during welding.
2. A titanium alloy high-efficiency large deposition high-toughness narrow gap welding method according to claim 1, It is characterized in that The intensity of the magnetic field is 0 to 20 mT, and the stirring frequency of the magnetic field is 0 to 30 Hz.
3. A titanium alloy high-efficiency, large-deposition, high-toughness, narrow-gap welding method according to claim 1, It is characterized in that The groove surface is arc preheated before welding.
4. A titanium alloy high-efficiency, large-deposition, high-toughness, narrow-gap welding method according to claim 1, It is characterized in that During filling welding, the diameter of the welding wire is 1.6~3.0mm and the wire feeding speed is 20~50mm / s.
5. A titanium alloy high-efficiency, large-deposition, high-toughness, narrow-gap welding method according to claim 1, It is characterized in that When cap welding, the diameter of the welding wire is 1.6mm and the wire feeding speed is 15-20mm / s.
6. A titanium alloy high-efficiency, large-deposition, high-toughness, narrow-gap welding method according to claim 1, It is characterized in that The flow rate of the protective gas is 30 L / min, and the purity of the protective gas is 99.999%.
7. A titanium alloy high-efficiency, large-deposition, high-toughness, narrow-gap welding method according to claim 1, It is characterized in that Before welding, a protective gas is passed around the tungsten electrode, and a protective hood is used behind the tungsten electrode.
8. A titanium alloy high-efficiency, large-deposition, high-toughness, narrow-gap welding device, It is characterized in that The welding device is used for welding in a titanium alloy high-efficiency large-deposition high-toughness narrow-gap welding method as described in any one of claims 1 to 7, and the welding device comprises: Welding gun (1); A welding power source (2), which is connected to the welding gun (1); A wire feeder (3) for feeding wire to the welding gun (1); A magnetron device (4) is arranged on one side of the welding gun (1), and the magnetron device (4) can introduce a magnetic field during welding to cause the tungsten pole to oscillate periodically.
Citation Information
Patent Citations
Magnetic control TIG (Tungsten Inert Gas) welding process for narrow gap of thick plate titanium alloy
CN102601501A
Repair method for weld fusion penetration defect of automatic welding of narrow gap of nuclear power main pipeline
CN108480825A
Narrow gap welding method for titanium alloy thick plate
CN116174858A
Welding wire vibration and magnetic control narrow gap GTAW composite device and using method thereof
CN117001116A
Tig welding torch
JP1995040053A
Cited By
Strengthening and toughening control method for high-strength titanium alloy welded joint
CN120244340A
Tungsten electrode self-adaptive swing GTAW narrow-gap weld intelligent welding system
CN121156441A
Intelligent welding system for tungsten electrode adaptive oscillation GTAW narrow gap weld
CN121156441B