Polyvinylidene fluoride trifluoroethylene-based composite membrane as well as preparation and application thereof
Through the polarization treatment and light control of the PVTF/photoelectric semiconductor nanoparticle composite film, the problem of insufficient electrical signal stimulation of PVTF materials in the early stage of tissue repair is solved, and dynamic regulation of cell behavior and precise control of electrical signals are achieved, which is suitable for biomedical applications. Implants to promote tissue repair.
Patent Information
- Application Number
- CN202410749807.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-12
- Publication Date
- 2024-10-08
AI Technical Summary
Existing polyvinylidene trifluoroethylene (PVTF) materials cannot meet the specific needs of electrical signals at different stages of tissue repair. Especially in the early stages of tissue repair, the mechanical signal stimulation is weak and cannot effectively regulate cell behavior.
The PVTF/optoelectronic semiconductor nanoparticle composite film is used to adjust the piezoelectric coefficient through polarization treatment, and use the wavelength and intensity of light to regulate the photogenerated potential to realize the coordinated regulation of cell behavior by bound charges and photogenerated carriers, providing force-electricity and light-electricity. Dual response characteristics.
It achieves dynamically controllable regulation of cell behavior, adapts to the electrical signal requirements at different stages, overcomes the bulkiness and tissue incompatibility of traditional electrical stimulation equipment, and improves the efficiency of photogenerated charges.
Smart Images

Figure HDA0004887516270000011 
Figure HDA0004887516270000012 
Figure HDA0004887516270000021
Abstract
Description
Technical Field
[0001] The invention relates to the field of biomedical materials, and in particular to a polyvinylidene fluoride trifluoroethylene composite film and a preparation method and application thereof. Background Art
[0002] Bioelectric phenomena exist in the normal physiological activities of the body. Under the physiological environment, electric potential (charge) plays an important role in transmitting signals and promoting tissue regeneration. Electroactive materials carrying surface potential (charge) are good carriers of exogenous electrical signals and can effectively regulate cell proliferation, adhesion and differentiation, and ultimately promote tissue repair and regeneration.
[0003] Polyvinylidene fluoride trifluoroethylene (PVTF) film has been proven to have excellent piezoelectricity, which originates from the orientation and arrangement of molecular dipoles, and generates electrical signals when subjected to mechanical stress or strain. After the PVTF material is deformed, the positive and negative charge centers in its crystal structure are reversely separated, and a certain surface potential is exhibited macroscopically. The surface potential generated by the PVTF material when it is strained can regulate cell behavior by affecting the state of cell integrins or ion channels. Therefore, PVTF materials can be used as medical implants to simulate electrophysiological microenvironments to regulate cell behavior. However, the electrical signals required at different stages of tissue repair are different. For example, in the early stages of tissue repair, the frequency and intensity of body activities are low, the mechanical signal stimulation applied to the piezoelectric material is weak, and the PVTF deformation is small. Since the bound charges on the PVTF surface are not variable, the specificity of the potential required at different stages of tissue repair cannot be met. Summary of the invention
[0004] In view of this, the object of the present invention is to provide a polyvinylidene fluoride trifluoroethylene (PVTF)-based composite film and its preparation and application. The composite film has both mechanical-electrical and photoelectrical response characteristics, and its piezoelectric coefficient can be regulated by adjusting the polarization treatment parameters. Moreover, the intensity of the photogenerated potential can be changed by adjusting the wavelength and intensity of the external light, and finally the bound charges and photogenerated carriers can be used as biomedical implants to dynamically and controllably regulate cell adhesion, proliferation and differentiation, and promote tissue repair and regeneration. The preparation method of the present invention is simple and easy to implement.
[0005] In order to achieve the above object, the present invention adopts the following technical solutions:
[0006] The invention provides a polyvinylidene fluoride trifluoroethylene-based composite film, which is a PVTF / photoelectric semiconductor nanoparticle composite film with a film thickness of 20 to 100 μm; at the same time, the composite film has a non-zero piezoelectric coefficient after polarization treatment.
[0007] In some specific examples of the present invention, the optoelectronic semiconductor nanoparticles are at least one of bismuth sulfide (Bi2S3) nanoparticles, titanium dioxide (TiO2) nanoparticles or zinc oxide (ZnO) nanoparticles.
[0008] In some specific examples of the present invention, the piezoelectric coefficient d of the composite film is 33 Satisfy: -10pC / N≤d 33 <0pC / N or 0pC / N<d 33 ≤10pC / N.
[0009] In some specific examples of the present invention, the mass ratio of the optoelectronic semiconductor nanoparticles to PVTF is 1:10 to 1:30.
[0010] At the same time, the present invention also provides a method for preparing the above-mentioned polyvinylidene fluoride trifluoroethylene-based composite film, comprising the following steps:
[0011] (1) adding photoelectric semiconductor nanoparticles to an organic solvent and magnetically stirring for 2 to 6 hours to form a photoelectric semiconductor nanoparticle solution; adding PVTF powder thereto and magnetically stirring for 2 to 6 hours to obtain a PVTF / photoelectric semiconductor nanoparticle mixed solution; wherein the feed ratio of the organic solvent, the photoelectric semiconductor nanoparticles, and the PVTF powder is 3 mL: (5 to 50) mg: (250 to 500) mg;
[0012] (2) forming a film of the PVTF / photoelectric semiconductor nanoparticle mixed solution on a glass plate by a tape casting method, and then heat treating at 160° C. to 240° C. for 0.5 to 2 h to obtain a PVTF / photoelectric semiconductor nanoparticle composite film with a film thickness of 20 to 100 μm;
[0013] (3) The composite film obtained in step (2) is subjected to polarization treatment by a contact polarization method to obtain the polyvinylidene fluoride trifluoroethylene-based composite film.
[0014] In some specific examples of the present invention, in step (1), the photoelectric semiconductor nanoparticles are at least one of bismuth sulfide (Bi2S3) nanoparticles, titanium dioxide (TiO2) nanoparticles or zinc oxide (ZnO) nanoparticles.
[0015] In some specific examples of the present invention, in step (1), the organic solvent is at least one of N,N-dimethylformamide, acetone, dioxane, and dichloromethane.
[0016] In some specific examples of the present invention, in step (1), the mass ratio of the photoelectric semiconductor nanoparticles to the PVTF powder is 1:10 to 1:30.
[0017] In some specific examples of the present invention, in step (3), the piezoelectric coefficient d of the polyvinylidene fluoride trifluoroethylene composite film is 33 Satisfy: -10pC / N≤d 33 <0pC / N or 0pC / N<d 33 ≤10pC / N.
[0018] In some specific examples of the present invention, in step (3), in the polarization treatment, the polarization voltage is 3.5 to 6.0 kV or -6.0 to -3.5 kV, and the polarization time is 1 to 6 min.
[0019] In addition, the present invention also provides the application of the polyvinylidene fluoride trifluoroethylene-based composite film, which can be used as a biomedical implant in the field of tissue repair.
[0020] Compared with the prior art, the present invention has the following beneficial effects:
[0021] The polyvinylidene fluoride trifluoroethylene-based composite film of the present invention has both force-electric and light-electric dual response characteristics. On the one hand, under the stimulation of an external light field, the semiconductor optoelectronic material is triggered to generate an electrical signal, the photogenerated electrons and holes are separated by the built-in field, and the photogenerated surface charges are enriched on the surface of the composite film, which is manifested as a change in surface potential, thereby achieving dynamic and controllable regulation of the surface potential based on the variability of the light addition time and the wavelength of light; on the other hand, the internal electric field generated by PVTF under strain provides a driving force for the transmission of surface photoinduced charges, thereby promoting the separation of electron-hole pairs in semiconductor optoelectronic materials and inhibiting their recombination, thereby improving the efficiency of photogenerated charge action. The different types of electrical signals generated by the composite film of the present invention achieve the coordinated regulation of cell behavior by bound charges and photogenerated carriers.
[0022] Moreover, in the present invention, on the one hand, by adjusting the parameters of the polarization treatment, composite films with different piezoelectric coefficients can be obtained; on the other hand, the surface potential of the composite film of the present invention and the action time of the escaped carriers can be controllably adjusted by regulating the wavelength and intensity of the external light. Therefore, the composite film of the present invention can be more accurately regulated according to the intensity or time of the electrical stimulation required in different stages or situations.
[0023] For example, at different stages of tissue repair, the required electrical signals are different. In particular, at the early stage of tissue repair, the frequency and intensity of body activities are low, and the mechanical signal stimulation applied to the piezoelectric material is weak. For example, the skin wound repair process is divided into an inflammatory phase, a proliferation phase, and a remodeling phase. The repair focus at different stages is different, and the required electrical signal strength and time are different. In view of this, you can choose a composite film with different piezoelectric coefficients of the present invention, or you can use the light field signal to regulate the surface electrical signal of the material during the use of the composite film of the present invention, and use the electrical signal generated by the photoelectric material as a supplement, in the early stage of tissue repair, to provide the body with the necessary external field electrical stimulation required for repair, thereby mediating cell behavior. Whether it is by adjusting the polarization treatment parameters to obtain PVTF-based composite films with different bound charge distribution states or by adjusting the wavelength and intensity of light to achieve the regulation of the escape concentration of photogenerated electrons or holes of optoelectronic semiconductor nanoparticles, it is possible to achieve the coordinated regulation of cell behavior by bound charges and photogenerated carriers, which is also very convenient to regulate; moreover, light is easily absorbed by photoresponsive materials rather than by water or other surrounding tissues, and the stimulation is more targeted; at the same time, the external electrical stimulation provided by the composite film of the present invention overcomes the shortcomings of traditional electrical stimulation equipment that is bulky, rigid electrodes are incompatible with tissues, and wounds are exposed, and overcomes the shortcomings of semiconductor nanoparticles that are directly implanted in the body and are easily accumulated in tissues.
[0024] In summary, the polyvinylidene fluoride trifluoroethylene-based composite membrane of the present invention can be implanted as an electroactive biological implant to construct an electrophysiological microenvironment in vivo and promote tissue repair. The polyvinylidene fluoride trifluoroethylene-based composite membrane of the present invention has clear practical significance. At the same time, the preparation method of the present invention is simple and easy to implement. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 It is the X-ray diffraction pattern of the target product obtained in Example 1 and the solid particles obtained in step (1).
[0026] Figure 2 It is the particle size analysis result of the solid particles obtained in step (1) in Example 1.
[0027] Figure 3 It is a comparison chart of the ultraviolet-visible spectra of the target product PVTF / Bi2S3 nanoparticle composite film obtained in Example 1 and the PVTF film obtained in Comparative Example 1.
[0028] Figure 4 This is a surface potential diagram of the target product PVTF / Bi2S3 nanoparticle composite film obtained in Example 1 under a Kelvin probe microscope in a dark environment.
[0029] Figure 5This is the surface potential diagram of the target product PVTF / Bi2S3 nanoparticle composite film obtained in Example 1 under 808nm light stimulation conditions using a Kelvin probe microscope.
[0030] Figure 6 This is a transient photocurrent response diagram of the composite film in Example 2 before and after polarization.
[0031] Figure 7 This is a comparison chart of the electrochemical impedance spectroscopy (EIS) of the target product PVTF / Bi2S3 nanoparticle composite film obtained in Example 2 in a dark environment and under 730nm light stimulation conditions. DETAILED DESCRIPTION
[0032] In order to better illustrate the present invention and facilitate understanding of the technical solution of the present invention, the present invention is further described in detail below in conjunction with the accompanying drawings and specific embodiments. It should be understood that the following embodiments are only used to illustrate the present invention and do not represent or limit the scope of protection of the present invention. The scope of protection of the present invention shall be subject to the claims.
[0033] In the following examples and comparative examples, the reagents or instruments used without indicating the manufacturer are all conventional products that can be purchased from the market. For example, the glass plate is a tempered glass plate, and the PVTF powder is produced by Piezotech of France. FC30, the molar ratio of vinylidene fluoride monomer to trifluoroethylene monomer in vinylidene fluoride trifluoroethylene copolymer is 7:3.
[0034] The polarization device includes: a base copper plate and an upper copper sheet, which are connected to the two poles of a high-voltage DC power supply through wires. The electric field between the surface conductive copper sheet and the base conductive copper sheet can be regulated by adjusting the voltage. The entire device is immersed in dimethyl silicone oil for insulation and prevention of breakdown. The above polarization device can be homemade or purchased from the market.
[0035] The process of polarization treatment using the above polarization device and contact polarization method is as follows: 2 The upper copper sheet is covered with 1×1cm 2 The film to be polarized is placed on the film layer to be polarized, and then the whole device is transferred to the polarization device, and the whole device is immersed in dimethyl silicone oil. A certain voltage (polarization voltage) is applied between the upper copper sheet and the base copper plate, and after a period of time (polarization time), the film layer is taken out and cleaned with anhydrous ethanol and ultrapure water for standby use.
[0036] Example 1
[0037] (1) dissolving bismuth nitrate pentahydrate in ethylene glycol to form a clear solution, and obtaining a bismuth nitrate pentahydrate solution with a concentration of 0.6 mol / L; dissolving sodium sulfide nonahydrate in ethylene glycol to form a clear solution, and obtaining a sodium sulfide nonahydrate solution with a concentration of 0.9 mol / L; mixing the bismuth nitrate pentahydrate solution and the sodium sulfide nonahydrate solution in a volume ratio of 1:1 and stirring for 20 minutes, stirring evenly, placing in an 80° C. water bath and stirring for 60 minutes; after cooling, centrifuging to separate a solid phase, washing, drying in an oven at 50° C., and grinding to obtain solid particles;
[0038] (2) adding 25 mg of the solid particles obtained in step (1) above to 3 mL of N,N-dimethylformamide solvent, and magnetically stirring for 2 h, then adding 250 mg of PVTF powder, and magnetically stirring for 6 h to obtain a mixed solution;
[0039] (3) forming a film on a clean glass plate by a casting method using the mixed solution obtained in step (2) (the specific operation of the casting method is: dropping the solution on the glass plate, and then using a film applicator to evenly disperse the solution on the glass plate to form a film, the film applicator height can be set to 0.5-1.5 mm, and is set to 1 mm here), and then heat-treating in a muffle furnace at 210° C. for 0.5 h to obtain a composite film with a thickness of 80 μm;
[0040] (4) The composite film obtained in step (3) was polarized by contact polarization method, the polarization voltage was set to -4.0 kV, the polarization time was set to 3 min, and the target product was obtained.
[0041] The target product obtained in Example 1 and the solid particles obtained in step (1) were subjected to X-ray diffraction analysis, and their XRD patterns were as follows: Figure 1 As shown in the two spectrum curves. Among them, the peak of 19.9° corresponds to the (110) and (200) crystal planes in PVTF, and the peaks of 22.40°, 24.92°, 28.60°, 31.80° and 45.66° correspond to the (220), (130), (211), (221) and (002) crystal planes of Bi2S3, respectively. It can be seen that the solid particles obtained in step (1) are Bi2S3 particles, and PVTF and Bi2S3 are effectively present in the target product obtained in this embodiment 1. Therefore, the target product is a PVTF / Bi2S3 particle composite film, and the PVTF has good crystallinity.
[0042] The particle size of the Bi2S3 particles obtained in step (1) was tested using a multifunctional nanoparticle size analyzer. Figure 2 As shown, the average particle size is about 435nm.
[0043] The piezoelectric coefficient of the PVTF / Bi2S3 nanoparticle composite film obtained in Example 1 was tested, and its piezoelectric coefficient d 33 It is -5pC / N and has force-electric response characteristics.
[0044] The absorbance of the PVTF / Bi2S3 nanoparticle composite film obtained in Example 1 was tested using a UV-visible spectrophotometer. The test results are as follows: Figure 3 As shown in the curve marked as PVTF / Bi2S3 in FIG. 1 , it can be seen that the PVTF / Bi2S3 nanoparticle composite film shows obvious absorption, and the absorption peak is around 730nm, indicating that the PVTF / Bi2S3 nanoparticle composite film has obvious light absorption.
[0045] The surface potential of the PVTF / Bi2S3 nanoparticle composite film obtained in Example 1 was analyzed using a Kelvin probe microscope under light stimulation (808 nm) and in a dark environment. The potential diagrams are shown as follows: Figure 4 and Figure 5 As shown. In a dark environment, the surface potential of the PVTF / Bi2S3 nanoparticle composite film with a piezoelectric coefficient of -5pC / N is -177mV; while under the condition of applying light stimulation (808nm), the surface potential of the PVTF / Bi2S3 nanoparticle composite film with a piezoelectric coefficient of -5pC / N is -431mV. This shows that: under an external light field, the surface potential of the composite film is variable and has photo-electric responsiveness.
[0046] It can be seen that the target product obtained in this Example 1 is a PVTF / Bi2S3 nanoparticle composite film having both mechano-electrical and photo-electrical response characteristics.
[0047] Comparative Example 1
[0048] (1) Add 250 mg of PVTF powder to 3 mL of N,N-dimethylformamide solvent and stir magnetically for 6 h to obtain a PVTF solution;
[0049] (2) The PVTF solution obtained in step (1) is formed into a film on a clean glass plate by a casting method (specifically: the solution is dropped on the glass plate, and then the solution is evenly dispersed on the glass plate by a film applicator to form a film, and the film applicator height is set to 1 mm), and then heat treated in a muffle furnace at 210° C. for 0.5 h to obtain a PVTF film with a thickness of 80 μm;
[0050] (3) The PVTF film obtained in step (2) was polarized by contact polarization method, the polarization voltage was set to -3.5 kV, the polarization time was set to 3 min, and a control PVTF film was obtained.
[0051] The piezoelectric coefficient of the PVTF film obtained in this comparative example 1 was tested, and its piezoelectric coefficient d 33 It is -5pC / N and has force-electric response characteristics.
[0052] The absorbance of the PVTF film obtained in Comparative Example 1 was tested using an ultraviolet-visible spectrophotometer, and the test graph is as follows: Figure 3 As shown in the curve marked as Pure PVTF in FIG. 1 , it can be seen that in the range of 400 to 900 nm, the PVTF film does not show an obvious absorption peak. This indicates that the PVTF film obtained in Comparative Example 1 does not have a photo-electric response characteristic.
[0053] Example 2
[0054] (1) dissolving bismuth nitrate pentahydrate in ethylene glycol to form a clear solution, and obtaining a bismuth nitrate pentahydrate solution with a concentration of 0.6 mol / L; dissolving sodium sulfide nonahydrate in ethylene glycol to form a clear solution, and obtaining a sodium sulfide nonahydrate solution with a concentration of 0.9 mol / L; mixing the bismuth nitrate pentahydrate solution and the sodium sulfide nonahydrate solution in a volume ratio of 1:1 and stirring for 20 minutes, stirring evenly, placing in an 80° C. water bath and stirring for 60 minutes; after cooling, centrifuging to separate a solid phase, washing, drying in an oven at 50° C., and grinding to obtain solid particles;
[0055] (2) 12.5 mg of the solid particles obtained in step (1) above were added to 3 mL of N,N-dimethylformamide solvent, and magnetically stirred for 2 h. Then, 250 mg of PVTF powder was added thereto, and magnetically stirred for 6 h to obtain a mixed solution;
[0056] (3) forming a film on a clean glass plate by a casting method using the mixed solution obtained in step (2) (specifically, dropping the solution on the glass plate, and then using a film applicator to evenly disperse the solution on the glass plate to form a film, and the film applicator height is set to 1 mm), and then heat treating in a muffle furnace at 210° C. for 0.5 h to obtain a composite film with a thickness of 80 μm;
[0057] (4) The composite film obtained in step (3) was polarized by contact polarization method, the polarization voltage was set to -6.0 kV, the polarization time was set to 3 min, and the target product was obtained.
[0058] The test results show that the solid particles obtained in step (1) are Bi2S3 particles with an average particle size of about 435nm; the target product obtained in Example 2 is a PVTF / Bi2S3 nanoparticle composite film, and the PVTF has good crystallinity and the piezoelectric coefficient d of the composite film is 33 It is -10pC / N and has force-electric response characteristics.
[0059] For the composite film before and after polarization in Example 2, i.e., the composite film (NoPolarization) obtained in step (3) and the target product (Polarization) obtained in step (4), transient photocurrent response tests were performed respectively. The test graphs are shown in FIG. Figure 6 As shown. It can be seen that obvious photocurrent response can be observed in the composite film before and after polarization under 730nm light stimulation. Moreover, the absolute value of the photocurrent response of the composite film after polarization under 730nm light stimulation is significantly increased compared with the composite film before polarization. Therefore, the target product obtained in Example 2 is a PVTF / Bi2S3 nanoparticle composite film with both force-electric and photo-electric response characteristics, and, compared with the composite film before polarization, the target product composite film obtained in Example 2 has better photo-electric response characteristics.
[0060] The PVTF / Bi2S3 nanoparticle composite film obtained in Example 2 was subjected to electrochemical impedance spectroscopy (EIS) analysis in a dark environment and under 730nm light stimulation conditions. The test graph is as follows: Figure 7 As shown. The diameter of the semicircle or arc represents the charge transfer resistance (Rct), and the smaller the Rct, the faster the charge transfer process. It can be seen that compared with the dark environment, the photogenerated carriers of Bi2S3 in the PVTF / Bi2S3 nanoparticle composite film are excited under the stimulation of 730nm light, and the interface resistance is reduced. This shows that the PVTF / Bi2S3 nanoparticle composite film obtained in Example 2 generates more electrons and holes under the stimulation of 730nm light, and the separation efficiency of electrons and holes is improved, which proves that the internal electric field of PVTF is conducive to the generation and separation of electrons and holes.
[0061] Example 3
[0062] (1) dissolving zinc nitrate hexahydrate in ultrapure water to form a clear solution to obtain a zinc nitrate hexahydrate solution with a concentration of 8 mol / L; adding 10 mL of a 25% by volume ammonia solution thereto, mixing evenly, and placing in an 85° C. water bath pot and stirring for 2 h; after cooling, centrifuging to separate a solid phase, washing it, and then heat treating it in a muffle furnace at 400° C. for 2 h at a heating rate of 2° C. / min to obtain solid particles;
[0063] (2) 12.5 mg of the solid particles obtained in step (1) above were added to 3 mL of N,N-dimethylformamide solvent, and magnetically stirred for 2 h. Then, 250 mg of PVTF powder was added thereto, and magnetically stirred for 6 h to obtain a mixed solution;
[0064] (3) forming a film on a clean glass plate by a casting method using the mixed solution obtained in step (2) (specifically, dropping the solution on the glass plate, and then using a film applicator to evenly disperse the solution on the glass plate to form a film, and the film applicator height is set to 1 mm), and then heat treating in a muffle furnace at 210° C. for 0.5 h to obtain a composite film with a thickness of 80 μm;
[0065] (4) The composite membrane obtained in step (3) was polarized by contact polarization method, the polarization voltage was set to 6.0 kV, the polarization time was set to 3 min, and the target product was obtained.
[0066] The test results show that the solid particles obtained in step (1) are ZnO nanoparticles, the target product is a PVTF / ZnO nanoparticle composite film, and the PVTF has good crystallinity; the piezoelectric coefficient of the composite film is d 33 The PVTF / ZnO nanoparticle composite film has obvious light absorption and photoelectric response. It can be seen that the target product obtained in Example 3 is a PVTF / ZnO nanoparticle composite film with both mechano-electric and photo-electric response characteristics.
[0067] Example 4
[0068] (1) TiCl4 was added to a mixed solvent of ultrapure water / anhydrous ethanol (v / v, 3:7), and stirred in an ice water bath for 30 min to obtain a TiCl4 solution with a volume fraction of 10%, and the TiCl4 solution was poured into a reactor liner, and the reactor liner was placed in a reactor, and then kept warm at 200° C. for 2 h; after cooling to room temperature (26° C.), the white precipitate in the reactor liner was washed and dried, and then annealed at 400° C. for 1 h to obtain solid particles;
[0069] (2) 6 mg of the solid particles obtained in step (1) above were added to 3 mL of N,N-dimethylformamide solvent, and magnetically stirred for 2 h. Then, 250 mg of PVTF powder was added thereto, and magnetically stirred for 6 h to obtain a mixed solution;
[0070] (3) forming a film on a clean glass plate by a casting method using the mixed solution obtained in step (2) (specifically, dropping the solution on the glass plate, and then using a film applicator to evenly disperse the solution on the glass plate to form a film, and the film applicator height is set to 1 mm), and then heat treating in a muffle furnace at 210° C. for 0.5 h to obtain a composite film with a thickness of 80 μm;
[0071] (4) The composite membrane obtained in step (3) was polarized by contact polarization method, the polarization voltage was set to 6.0 kV, the polarization time was set to 3 min, and the target product was obtained.
[0072] The test results show that the solid particles obtained in step (1) are titanium dioxide nanoparticles, the target product is a PVTF / TiO2 nanoparticle composite film, and the PVTF has good crystallinity; the piezoelectric coefficient of the composite film is d 33 The PVTF / TiO2 nanoparticle composite film has obvious light absorption and photoelectric response. It can be seen that the target product obtained in Example 4 is a PVTF / TiO2 nanoparticle composite film with both mechano-electric and photo-electric response characteristics.
[0073] It can be seen that the polyvinylidene fluoride trifluoroethylene-based composite film of the present invention has both force-electric and light-electric dual response characteristics. On the one hand, under the stimulation of an external light field, the semiconductor optoelectronic material is triggered to generate electrical signals, photogenerated electrons and holes are separated by the built-in field, and the photogenerated surface charges are enriched on the surface of the composite film, which is manifested as a change in surface potential, thereby achieving dynamic and controllable regulation of the surface potential based on the variability of the light addition time and the wavelength of light; on the other hand, the internal electric field generated by PVTF under strain provides a driving force for the transmission of surface photoinduced charges, thereby promoting the separation of electron-hole pairs in semiconductor optoelectronic materials and inhibiting their recombination, thereby improving the efficiency of photogenerated charge action. The different types of electrical signals generated by the composite film of the present invention achieve the coordinated regulation of cell behavior by bound charges and photogenerated carriers.
[0074] Moreover, in the present invention, on the one hand, by adjusting the parameters of the polarization treatment, composite films with different piezoelectric coefficients can be obtained; on the other hand, the surface potential of the composite film of the present invention and the action time of the escaped carriers can be controllably adjusted by regulating the wavelength and intensity of the external light. Therefore, the composite film of the present invention can be more accurately regulated according to the intensity or time of the electrical stimulation required in different stages or situations.
[0075] For example, at different stages of tissue repair, the required electrical signals are different. In particular, at the early stage of tissue repair, the frequency and intensity of body activities are low, and the mechanical signal stimulation applied to the piezoelectric material is weak. For example, the skin wound repair process is divided into an inflammatory phase, a proliferation phase, and a remodeling phase. The repair focus at different stages is different, and the required electrical signal strength and time are different. In view of this, you can choose a composite film with different piezoelectric coefficients of the present invention, or you can use the light field signal to regulate the surface electrical signal of the material during the use of the composite film of the present invention, and use the electrical signal generated by the photoelectric material as a supplement, in the early stage of tissue repair, to provide the body with the necessary external field electrical stimulation required for repair, thereby mediating cell behavior. Whether it is by adjusting the polarization treatment parameters to obtain PVTF-based composite films with different bound charge distribution states or by adjusting the wavelength and intensity of light to achieve the regulation of the escape concentration of photogenerated electrons or holes of optoelectronic semiconductor nanoparticles, it is possible to achieve the coordinated regulation of cell behavior by bound charges and photogenerated carriers, which is also very convenient to regulate; moreover, light is easily absorbed by photoresponsive materials rather than by water or other surrounding tissues, and the stimulation is more targeted; at the same time, the external electrical stimulation provided by the composite film of the present invention overcomes the shortcomings of traditional electrical stimulation equipment that is bulky, rigid electrodes are incompatible with tissues, and wounds are exposed, and overcomes the shortcomings of semiconductor nanoparticles that are directly implanted in the body and are easily accumulated in tissues.
[0076] In summary, the polyvinylidene fluoride trifluoroethylene-based composite membrane of the present invention can be implanted as an electroactive biological implant to construct an electrophysiological microenvironment in vivo and promote tissue repair. The polyvinylidene fluoride trifluoroethylene-based composite membrane of the present invention has clear practical significance. At the same time, the preparation method of the present invention is simple and easy to implement.
[0077] It can be seen that the purpose of the present invention has been completely and effectively achieved. The functional and structural principles of the present invention have been demonstrated and explained in the embodiments. Without departing from the principles, the implementation methods can be modified arbitrarily. Therefore, the present invention includes all modified implementation methods based on the spirit and scope of the claims.
Claims
1. A polyvinylidene fluoride trifluoroethylene-based composite film, which is a PVTF / photoelectric semiconductor nanoparticle composite film with a film thickness of 20 to 100 μm; at the same time, the composite film has a non-zero piezoelectric coefficient after polarization treatment.
2. The polyvinylidene fluoride trifluoroethylene-based composite film according to claim 1, characterized in that: The photoelectric semiconductor nanoparticles are at least one of bismuth sulfide nanoparticles, titanium dioxide nanoparticles or zinc oxide nanoparticles.
3. The polyvinylidene fluoride trifluoroethylene-based composite film according to claim 1, characterized in that: The piezoelectric coefficient d of the composite film 33 Satisfy: -10pC / N≤d 33 <0pC / N or 0pC / N<d 33 ≤10pC / N.
4. The method for preparing the polyvinylidene fluoride trifluoroethylene-based composite film according to any one of claims 1 to 3, comprising the following steps: (1) adding photoelectric semiconductor nanoparticles to an organic solvent and magnetically stirring for 2 to 6 hours to form a photoelectric semiconductor nanoparticle solution; adding PVTF powder thereto and magnetically stirring for 2 to 6 hours to obtain a PVTF / photoelectric semiconductor nanoparticle mixed solution; wherein the feed ratio of the organic solvent, the photoelectric semiconductor nanoparticles, and the PVTF powder is 3 mL: (5 to 50) mg: (250 to 500) mg; (2) forming a film of the PVTF / photoelectric semiconductor nanoparticle mixed solution on a glass plate by a tape casting method, and then heat treating at 160° C. to 240° C. for 0.5 to 2 h to obtain a PVTF / photoelectric semiconductor nanoparticle composite film with a film thickness of 20 to 100 μm; (3) The composite film obtained in step (2) is subjected to polarization treatment by a contact polarization method to obtain the polyvinylidene fluoride trifluoroethylene-based composite film.
5. The method for preparing a polyvinylidene fluoride trifluoroethylene-based composite film according to claim 4, characterized in that: The piezoelectric coefficient d 33 Satisfy: -10pC / N≤d 33 <0pC / N or 0pC / N<d 33 ≤10pC / N.
6. The method for preparing a polyvinylidene fluoride trifluoroethylene-based composite film according to claim 4, characterized in that: The photoelectric semiconductor nanoparticles are at least one of bismuth sulfide nanoparticles, titanium dioxide nanoparticles or zinc oxide nanoparticles.
7. The method for preparing a polyvinylidene fluoride trifluoroethylene-based composite film according to claim 4, characterized in that: The organic solvent is at least one of N,N-dimethylformamide, acetone, dioxane and dichloromethane.
8. The method for preparing a polyvinylidene fluoride trifluoroethylene-based composite film according to claim 4, characterized in that: In step (1), the mass ratio of the photoelectric semiconductor nanoparticles to the PVTF powder is 1:10 to 1:
30.
9. The method for preparing a polyvinylidene fluoride trifluoroethylene-based composite film according to claim 5, characterized in that: In step (3), in the polarization treatment, the polarization voltage is 3.5 to 6.0 kV or -6.0 to -3.5 kV, and the polarization time is 1 to 6 minutes.
10. Use of the polyvinylidene fluoride trifluoroethylene based composite membrane as claimed in any one of claims 1 to 3.