Alloy coating material and preparation method thereof

By using 2,2-ethylenedithiodiethanol and nitrobenzotriazole in the copper-zinc alloy electroplating process, combined with temperature rate control, the problems of controllability of the coating composition and high power consumption are solved, and copper-zinc The mirror effect and low roughness of the alloy coating provide excellent decorative properties.

CN118745589APending Publication Date: 2024-10-08任益兵
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411102888.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-13
Publication Date
2024-10-08

AI Technical Summary

Technical Problem

The existing copper-zinc alloy electroplating process has problems such as poor controllability of coating composition and high power consumption. Especially in cyanide-free technology, it is difficult to achieve efficient copper-zinc alloy coating preparation.

Method used

2,2-Ethylenedithiodiethanol is used as the complexing agent, combined with nitrobenzotriazole to improve the stability of the plating solution, and by controlling the temperature rate parameters of electrodeposition, the mirror effect of copper-zinc co-deposition and coating is achieved.

Benefits of technology

It achieves uniformity, fine particles, and excellent mirror effect of the copper-zinc alloy coating, reduces power consumption, and obtains excellent decorative effects and low roughness.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118745589A_ABST
    Figure CN118745589A_ABST
Patent Text Reader

Abstract

According to the alloy coating material and the preparation method thereof, the bonding force of the whole coating and the base material is good, particularly, the temperature rate parameters for controlling electro-deposition are proposed for the first time, and the polished coating is smooth and fine in appearance, good in mirror surface effect, low in roughness and excellent in decoration effect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of metal surface electroplating alloys and relates to a high-mirror-surface and low-roughness copper-zinc alloy plating material and a preparation method thereof. Background Art

[0002] Since the electroplating of copper-zinc alloy became practical in the mid-to-late 19th century, it is still one of the most widely used alloy coatings. Copper-zinc alloys with a copper content higher than zinc content are called brass. The most widely used brass contains 68% to 75% copper. Copper-zinc alloys with a copper content higher than 70% to 80% are golden yellow and have excellent decorative effects. Generally, a 1 to 2 μm thick copper-zinc alloy layer is flash-plated on a bright nickel coating to achieve the decorative purpose. If you want to color or make patterns on the coating, you need to thicken the alloy coating according to the requirements of the parts.

[0003] Copper-zinc alloy is widely used in decorative electroplating and rust prevention of metal devices due to its bright golden color, good mechanical properties and corrosion resistance. It also has the function of promoting adhesion between rubber and steel. Copper-zinc alloy film can be prepared by electrochemical deposition, but the standard potential of Cu is far different from the standard potential of Zn, and direct electroplating cannot obtain copper-zinc alloy. Therefore, the assistance of a complexing agent is required to narrow the potential difference between Zn and Cu, so that copper ions and zinc ions can be co-deposited. At present, cyanide is generally used as a complexing agent in the electrochemical deposition of copper-zinc alloy in industry. Although the copper-zinc alloy coating produced has uniform structure and fine and tight particles, cyanide and its compounds are highly toxic and will cause great harm to humans and the ecology. In order to find a substitute for cyanide plating solution, many scholars have studied the copper-zinc alloy electrodeposition complexing system.

[0004] For example, CN104120468B discloses a cyanide-free cuprous copper-zinc alloy electroplating solution. The present invention relates to the preparation and use of a cyanide-free cuprous copper-zinc alloy electroplating solution. The present invention aims to solve the problem of controllable coating composition during the electroplating of copper-zinc alloy and the problem of high power consumption caused by the use of divalent copper in the current cyanide-free technology. A cyanide-free cuprous copper-zinc alloy electroplating solution is prepared using cuprous compounds, zinc chloride, cuprous non-cyanide complexing agents, auxiliary complexing agents, plating solution stabilizers, brighteners and sodium acetate. The solution is heated to 30-75°C and 0.1-3.0A / dm 2 It can be used under the conditions of ruthenium titanium anode or copper-zinc alloy anode. A cyanide-free cuprous copper-zinc alloy electroplating solution can control the copper-zinc ratio in the coating by selective complexation of cuprous ions, and the use of cuprous ions in the plating solution can reduce power consumption, which is beneficial to energy conservation.

[0005] For example, CN105154937A discloses a copper-zinc alloy electroplating solution and an electroplating method thereof. The copper-zinc alloy electroplating solution contains 40-60 g / L copper sulfate, 6-10 g / L copper pyrophosphate, 6-10 g / L diammine palladium chloride, 20-40 g / L zinc sulfate, 20-30 g / L potassium citrate, 5-10 g / L amino acid, 4-8 g / L saccharin, and 10-15 g / L sodium acetate. The coating obtained by electroplating with the copper-zinc alloy electroplating solution has no cracks and has good corrosion resistance and wear resistance.

[0006] For example, CN105543914A discloses an electroplating method of a decorative copper-zinc alloy electroplating solution, comprising the following steps: first preparing a copper-zinc alloy electroplating solution, then activating a workpiece to be plated, placing the activated workpiece as a cathode in the electroplating solution prepared in step (1), using stainless steel as an anode, linearly increasing the current density to 4-6A / dm2, and then continuing electroplating under a constant current to obtain a copper-zinc alloy coating. The electroplating method of the decorative copper-zinc alloy electroplating solution of the present invention has simple steps, adopts a linearly increasing small current density for electroplating, and then adopts a constant current density for electroplating, the electroplating method has high electroplating efficiency, the obtained coating is bright and flat, has good impact resistance and high temperature resistance, and has strong bonding with the substrate.

[0007] For example, JP2007-304376 discloses a copper-zinc alloy electroplating bath with excellent productivity. The copper-zinc alloy electroplating bath does not use cyanide and can form a uniform and shiny alloy layer with a target composition even at a current density higher than before. The copper-zinc alloy electroplating bath contains a copper salt, a zinc salt, and at least one selected from an alkali metal pyrophosphate salt, an amino acid or a salt thereof, and has a pH value of 8.5 to 14. Preferably, the pH value is 10.5 to 11.8, and the concentration of the amino acid or a salt thereof is preferably 0.08 mol / L to 0.22 mol / L, and more preferably 0.1 mol / L to 0.13 mol / L. As the amino acid or a salt thereof, histidine or a salt thereof can be preferably used. Summary of the invention

[0008] The invention provides an alloy coating material and a preparation method thereof. The 2,2-ethylenedithiodiethanol complexing agent used in the coating preparation process significantly realizes copper-zinc co-deposition, nitrobenzotriazole improves the stability of the plating solution, and the coating as a whole has good bonding strength with a substrate. In particular, a temperature rate parameter for controlling electrodeposition is proposed for the first time, so that the coating after polishing has a smooth and delicate morphology, a good mirror effect, and low roughness, thereby obtaining an excellent decorative effect.

[0009] Specifically: A method for preparing an alloy coating material comprises the following steps: (1) grinding, degreasing, alkali washing and drying the metal substrate, wherein the alkali washing solution used is composed of sodium silicate, sodium hydroxide, sodium carbonate, sodium phosphate and deionized water; (2) The surface pretreated metal substrate is used as the working electrode, the inert platinum metal is used as the auxiliary electrode, the reference electrode is the mercuric oxide electrode, and the plating solution includes 0.16 mol / L copper sulfate pentahydrate, 0.07 mol / L zinc sulfate heptahydrate, 0.3 mol / L potassium pyrophosphate, 0.05 mol / L potassium citrate, 0.6 mol / L sodium hydroxide, 2.5 g 2,2-ethylenedithiodiethanol, 1.3 g nitrobenzotriazole, the starting temperature of the electroplating temperature is 7 ° C, the heating rate is 0.9-1.4 ° C / min, the temperature is raised to 14 ° C, the maintenance time is 3 minutes, and then the heating equipment is turned off. The current density is 2.8 A / dm 2 , time 15min; (3) Washing and drying; (4) Polishing with 1500 mesh SiC sandpaper for 3-8 min to obtain a mirror alloy with a roughness of 35.47±4.9 nm.

[0010] The metal is selected from titanium or titanium alloy materials.

[0011] The alkaline washing solution is composed of 10wt.% sodium silicate, 15wt.% sodium hydroxide, 1wt.% sodium carbonate, 4wt.% sodium phosphate and deionized water. The alkaline washing temperature is 40-45°C and the washing time is 5-7min.

[0012] The heating rate is 1.1-1.2°C / min, preferably 1.15°C / min.

[0013] After being polished with sandpaper, the alloy has lower roughness, higher mirror effect, and a dense surface without cracks.

[0014] The alloy has a thickness of 7-15 μm.

[0015] Beneficial technical effects: (1) As is well known, the standard potential of Cu is far different from the standard potential of Zn, and direct electrodeposition cannot obtain a copper-zinc alloy. Therefore, a complexing agent is needed to narrow the potential difference between Zn and Cu so that copper ions and zinc ions can be co-deposited. The present invention uses 2,2-ethylenedithiodiethanol (also called 2,2'-ethylenedithiodiethanol, CAS: 5244-34-8) as a complexing agent. Since 2,2-ethylenedithiodiethanol has a multi-hydroxyl and sulfur structure, it can coordinate with copper ions to form a stable complex, thereby improving the cathode polarization of copper ions in the plating solution. At the same time, zinc ions in the alkaline solution will be converted into Zn(OH) 4 2-The deposition potential will also shift to the positive direction, and finally the deposition potential of copper ions and zinc ions will be brought closer to each other, thus achieving the purpose of co-deposition. Figure 2 The energy spectrum of the copper and zinc elements can be clearly removed and evenly distributed, effectively forming an alloy structure. Referring to the corresponding SEM image, it can be seen that if polishing is not performed, the copper-zinc alloy coating has a uniform structure and fine and tight particles; (2) See the attached Figure 1 , attached Figure 1 The surface morphology of Example 2 and Comparative Examples 1-3 was characterized. After electroplating, the surface roughness of Comparative Example 1 was uneven and there were obvious cracks. Although there were no obvious cracks on the surface of Comparative Example 2, the reasonable size was larger and the roughness was high. Although the surface deposited particles of Comparative Example 3 were smaller, there were more cracks. In comparison, the surface of Example 2 was crack-free and the corresponding grains were smaller. (3) After polishing the Examples and Comparative Examples 1-3, it can be seen that the base color of Comparative Examples 1-2 is darker, while the base colors of Comparative Examples 3 and Example 2 are whiter. Obviously, after polishing, the overall mirror effect of Examples 2 and Comparative Examples 3 is better than that of Comparative Examples 1-2. For details, see the attached Figure 3 Polishing morphology and attachment Figure 4 According to the roughness test, the surface roughness of Comparative Example 1 is 284.6 nm, that of Comparative Example 2 is 123.4 nm, that of Comparative Example 3 is 70.83 nm, and that of Example 2 is 35.47 nm. The surface of Example 2 has obvious ripples and flaws. Although the surface roughness of Comparative Example 3 is reduced, the corresponding ripples are obvious. In comparison, the surface of Example 2 is smooth, dense and smooth as a whole, and there are only inevitable scratches on the surface during the polishing process (caused by polishing, not the coating morphology). It can be seen that the coating surface of Example 2 is smoother after polishing; (4) The dosage of the reagents used in the present invention is all point values, that is, the range of the plating solution formula is strictly screened, and the main findings are the influence of the heating rate on the coating morphology and the internal coating morphology after polishing. It has a very high display guiding significance for obtaining a smooth, delicate coating morphology with good mirror effect, low roughness, and excellent decorative effect. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Attached Figure 1 SEM images of the embodiments of the present invention and comparative examples.

[0017] Attached Figure 2 Energy spectrum diagram of Example 2 of the present invention.

[0018] Attached Figure 3 The morphology after polishing of the present invention.

[0019] Attached Figure 4 The roughness after polishing of the present invention. DETAILED DESCRIPTION Example 1

[0020] A method for preparing an alloy coating material comprises the following steps: (1) The metal substrate is polished, degreased, alkali-washed, and blow-dried, wherein the alkali washing solution used for alkali washing is composed of sodium silicate, sodium hydroxide, sodium carbonate, sodium phosphate, and deionized water, the metal is selected from titanium alloy material, the alkali washing solution is composed of 10wt.% sodium silicate, 15wt.% sodium hydroxide, 1wt.% sodium carbonate, 4wt.% sodium phosphate, and deionized water, the alkali washing temperature is 40°C, and the time is 5 minutes.

[0021] (2) The metal substrate after surface pretreatment is used as the working electrode, the inert platinum metal is used as the auxiliary electrode, and the reference electrode is the mercuric oxide electrode. The plating solution includes 0.16 mol / L copper sulfate pentahydrate, 0.07 mol / L zinc sulfate heptahydrate, 0.3 mol / L potassium pyrophosphate, 0.05 mol / L potassium citrate, 0.6 mol / L sodium hydroxide, 2.5 g 2,2-ethylenedithiodiethanol, 1.3 g nitrobenzotriazole, and the starting temperature of the electroplating temperature is 7 ° C, the heating rate is 0.9 ° C / min, the temperature is raised to 14 ° C, the maintenance time is 3 minutes, and then the heating equipment is turned off. The current density is 2.8 A / dm 2 , time 15 minutes.

[0022] (3) Wash and blow dry.

[0023] (4) Polish with 1500-grit SiC sandpaper for 5 min to obtain a mirror-finished alloy. Example 2

[0024] A method for preparing an alloy coating material comprises the following steps: (1) The metal substrate is polished, degreased, alkali-washed, and blow-dried, wherein the alkali washing solution used for alkali washing is composed of sodium silicate, sodium hydroxide, sodium carbonate, sodium phosphate, and deionized water, the metal is selected from titanium alloy material, the alkali washing solution is composed of 10wt.% sodium silicate, 15wt.% sodium hydroxide, 1wt.% sodium carbonate, 4wt.% sodium phosphate, and deionized water, the alkali washing temperature is 42.5°C, and the time is 6 minutes.

[0025] (2) The surface pretreated metal substrate is used as the working electrode, the inert platinum metal is used as the auxiliary electrode, and the reference electrode is the mercuric oxide electrode. The plating solution includes 0.16 mol / L copper sulfate pentahydrate, 0.07 mol / L zinc sulfate heptahydrate, 0.3 mol / L potassium pyrophosphate, 0.05 mol / L potassium citrate, 0.6 mol / L sodium hydroxide, 2.5 g 2,2-ethylenedithiodiethanol, 1.3 g nitrobenzotriazole, and the starting temperature of the electroplating temperature is 7 ° C, the heating rate is 1.15 ° C / min, the temperature is raised to 14 ° C, the maintenance time is 3 min, and then the heating equipment is turned off. The current density is 2.8 A / dm 2, time 15 minutes.

[0026] (3) Wash and blow dry.

[0027] (4) Polish with 1500-grit SiC sandpaper for 5 min to obtain a mirror-finished alloy. Example 3

[0028] A method for preparing an alloy coating material comprises the following steps: (1) The metal substrate is polished, degreased, alkali-washed, and blow-dried, wherein the alkali washing solution used for alkali washing is composed of sodium silicate, sodium hydroxide, sodium carbonate, sodium phosphate, and deionized water, the metal is selected from titanium alloy material, the alkali washing solution is composed of 10wt.% sodium silicate, 15wt.% sodium hydroxide, 1wt.% sodium carbonate, 4wt.% sodium phosphate, and deionized water, the alkali washing temperature is 45°C, and the time is 7 minutes.

[0029] (2) The metal substrate after surface pretreatment is used as the working electrode, the inert platinum metal is used as the auxiliary electrode, and the reference electrode is the mercuric oxide electrode. The plating solution includes 0.16 mol / L copper sulfate pentahydrate, 0.07 mol / L zinc sulfate heptahydrate, 0.3 mol / L potassium pyrophosphate, 0.05 mol / L potassium citrate, 0.6 mol / L sodium hydroxide, 2.5 g 2,2-ethylenedithiodiethanol, 1.3 g nitrobenzotriazole, and the starting temperature of the electroplating temperature is 7 ° C, the heating rate is 1.4 ° C / min, the temperature is raised to 14 ° C, the maintenance time is 3 min, and then the heating equipment is turned off. The current density is 2.8 A / dm 2 , time 15 minutes.

[0030] (3) Wash and blow dry.

[0031] (4) Polish with 1500-grit SiC sandpaper for 5 min to obtain a mirror-finished alloy.

[0032] Comparative Example 1. A method for preparing an alloy coating material, comprising the following preparation steps: (1) The metal substrate is polished, degreased, alkali-washed, and blow-dried, wherein the alkali washing solution used for alkali washing is composed of sodium silicate, sodium hydroxide, sodium carbonate, sodium phosphate, and deionized water, the metal is selected from titanium alloy material, the alkali washing solution is composed of 10wt.% sodium silicate, 15wt.% sodium hydroxide, 1wt.% sodium carbonate, 4wt.% sodium phosphate, and deionized water, the alkali washing temperature is 42.5°C, and the time is 6 minutes.

[0033] (2) The surface pretreated metal substrate is used as the working electrode, the inert platinum metal is used as the auxiliary electrode, the reference electrode is the mercuric oxide electrode, and the plating solution includes 0.16 mol / L copper sulfate pentahydrate, 0.07 mol / L zinc sulfate heptahydrate, 0.3 mol / L potassium pyrophosphate, 0.05 mol / L potassium citrate, 0.6 mol / L sodium hydroxide, 1.3 g nitrobenzotriazole, and the starting temperature of the electroplating temperature is 7 ° C, the heating rate is 1.15 ° C / min, the temperature is raised to 14 ° C, the maintenance time is 3 minutes, and then the heating equipment is turned off. The current density is 2.8 A / dm 2 , time 15 minutes.

[0034] (3) Wash and blow dry.

[0035] (4) Polish with 1500-grit SiC sandpaper for 5 min to obtain a mirror-finished alloy.

[0036] Comparative Example 2, a method for preparing an alloy coating material, comprising the following preparation steps: (1) The metal substrate is polished, degreased, alkali-washed, and blow-dried, wherein the alkali washing solution used for alkali washing is composed of sodium silicate, sodium hydroxide, sodium carbonate, sodium phosphate, and deionized water, the metal is selected from titanium alloy material, the alkali washing solution is composed of 10wt.% sodium silicate, 15wt.% sodium hydroxide, 1wt.% sodium carbonate, 4wt.% sodium phosphate, and deionized water, the alkali washing temperature is 42.5°C, and the time is 6 minutes.

[0037] (2) The surface pretreated metal substrate is used as the working electrode, the inert platinum metal is used as the auxiliary electrode, the reference electrode is the mercuric oxide electrode, and the plating solution includes 0.16 mol / L copper sulfate pentahydrate, 0.07 mol / L zinc sulfate heptahydrate, 0.3 mol / L potassium pyrophosphate, 0.05 mol / L potassium citrate, 0.6 mol / L sodium hydroxide, 2.5 g 2,2-ethylenedithiodiethanol, 1.3 g nitrobenzotriazole, the plating temperature is constant at 14 °C, and the current density is 2.8 A / dm 2 , time 15 minutes.

[0038] (3) Wash and blow dry.

[0039] (4) Polish with 1500-grit SiC sandpaper for 5 min to obtain a mirror-finished alloy.

[0040] Comparative Example 3, a method for preparing an alloy coating material, comprising the following preparation steps: (1) The metal substrate is polished, degreased, alkali-washed, and blow-dried, wherein the alkali washing solution used for alkali washing is composed of sodium silicate, sodium hydroxide, sodium carbonate, sodium phosphate, and deionized water, the metal is selected from titanium alloy material, the alkali washing solution is composed of 10wt.% sodium silicate, 15wt.% sodium hydroxide, 1wt.% sodium carbonate, 4wt.% sodium phosphate, and deionized water, the alkali washing temperature is 42.5°C, and the time is 6 minutes.

[0041] (2) The surface pretreated metal substrate is used as the working electrode, the inert platinum metal is used as the auxiliary electrode, the reference electrode is the mercuric oxide electrode, and the plating solution includes 0.16 mol / L copper sulfate pentahydrate, 0.07 mol / L zinc sulfate heptahydrate, 0.3 mol / L potassium pyrophosphate, 0.05 mol / L potassium citrate, 0.6 mol / L sodium hydroxide, 2.5 g 2,2-ethylenedithiodiethanol, 1.3 g nitrobenzotriazole, the starting temperature of the plating temperature is 7 ° C, the temperature is increased to 14 ° C, the heating rate is 2 ° C / min, and the current density is 2.8 A / dm 2 , time 15 minutes.

[0042] (3) Wash and blow dry.

[0043] (4) Polish with 1500-grit SiC sandpaper for 5 min to obtain a mirror-finished alloy.

[0044] The main difference between Comparative Examples 1-3 is that Comparative Example 1 does not have a complexing agent, Comparative Example 2 is a constant temperature electroplating, and the electroplating heating rate of Comparative Example 3 is outside the scope of protection of the present invention. Figure 1-4 The corresponding characterization shows that the surface morphology of Comparative Example 3 and Example 2 is similar, but the corresponding internal polishing effect is significantly different. By controlling the heating rate of electrodeposition, the polishing effect is better, that is, the heating rate will affect the internal morphology of the coating, especially the formation of internal ripples. The main difference between Comparative Example 1 and Example 2 is whether a complexing agent is added. The presence of the complexing agent affects the co-deposition process, resulting in poor overall morphology of Comparative Example 1, but there are no ripples inside the coating of Comparative Example 1, but some faults or gaps; the difference between Comparative Example 2 and Example 2 is the constant temperature state, and there are a large number of defects and ripples inside the coating of Comparative Example 2.

[0045] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing an alloy coating material, comprising the following preparation steps: (1) grinding, degreasing, alkali washing and drying the metal substrate, wherein the alkali washing solution used is composed of sodium silicate, sodium hydroxide, sodium carbonate, sodium phosphate and deionized water; (2) The surface pretreated metal substrate is used as the working electrode, the inert platinum metal is used as the auxiliary electrode, the reference electrode is the mercuric oxide electrode, and the plating solution includes 0.16 mol / L copper sulfate pentahydrate, 0.07 mol / L zinc sulfate heptahydrate, 0.3 mol / L potassium pyrophosphate, 0.05 mol / L potassium citrate, 0.6 mol / L sodium hydroxide, 2.5 g 2,2-ethylenedithiodiethanol, 1.3 g nitrobenzotriazole, the starting temperature of the electroplating temperature is 7 ° C, the heating rate is 0.9-1.4 ° C / min, the temperature is raised to 14 ° C, the maintenance time is 3 minutes, and then the heating equipment is turned off. The current density is 2.8 A / dm 2 , time 15min; (3) Washing and drying; (4) Polishing with 1500 mesh SiC sandpaper for 3-8 min to obtain a mirror alloy with a roughness of 35.47±4.9 nm.

2. A method for preparing an alloy coating material as claimed in claim 1, Features The metal is selected from titanium or titanium alloy materials.

3. A method for preparing an alloy coating material as claimed in claim 1, Features The alkaline washing solution is composed of 10wt.% sodium silicate, 15wt.% sodium hydroxide, 1wt.% sodium carbonate, 4wt.% sodium phosphate and deionized water. The alkaline washing temperature is 40-45°C and the washing time is 5-7min.

4. A method for preparing an alloy coating material as claimed in claim 1, Features The heating rate is 1.1-1.2°C / min, preferably 1.15°C / min.

5. The alloy material obtained by the method for preparing an alloy coating material according to claim 1, Features After being polished with sandpaper, the alloy has lower roughness, higher mirror effect, and a dense surface without cracks.

6. A method for preparing an alloy coating material as claimed in claim 1, Features The alloy has a thickness of 7-15 μm.