Reflection type wavelength conversion device and preparation method thereof

By using a glass fluorescent layer of phosphor particles and glass powder particles in the wavelength conversion layer, combined with a metal reflective layer and a thermally conductive adhesive layer, the problem of insufficient thermal conductivity of the traditional wavelength conversion layer is solved, achieving efficient thermal conductivity and reliable device performance.

CN118752864APending Publication Date: 2024-10-11GUANGZHOU UNIONLUX ELECTRONICS TECH CO LTD

Patent Information

Application Number
CN202410886002.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-03
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

The traditional wavelength conversion layer has insufficient thermal conductivity and cannot meet the needs of high-power laser lighting and display scenarios. Moreover, the preparation of the ceramic fluorescent layer requires high-temperature sintering, which affects the adhesion of the reflective metal film layer.

Method used

The glass phosphor layer composed of phosphor particles and glass powder particles is used to increase the thermal conductivity by controlling the particle size and sintering temperature. It is combined with a metal reflective layer and a thermally conductive adhesive layer to reduce the interface thermal resistance and improve the overall thermal conductivity and heat dissipation capability.

Benefits of technology

It significantly improves the thermal conductivity of the wavelength conversion layer, reduces production energy consumption, ensures the firm adhesion of the metal reflective film and device reliability, and is suitable for high-power laser lighting and display applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004926072050000141
    Figure BDA0004926072050000141
Patent Text Reader

Abstract

The invention discloses a reflection type wavelength conversion device and a preparation method thereof. The reflection type wavelength conversion device comprises a glass fluorescent layer, a fluorescent reflection layer, a first heat conduction bonding layer, a middle layer substrate, a second heat conduction bonding layer and a bottom layer substrate which are sequentially stacked. The glass fluorescent layer is obtained by pressing a mixture of fluorescent powder particles and glass powder particles into a green body under the pressure of 80-200MPa and then sintering the green body at the temperature of Tm + k, the median diameter D50 of the fluorescent powder particles is 8-20 microns, and the median diameter D50 of the glass powder particles is 1-6 microns; tm is the lowest temperature of complete melting of the glass powder particles, and k is more than or equal to 80 DEG C and less than or equal to 120 DEG C. According to the scheme, by controlling the particle size of the fluorescent powder particles, the particle size of the glass powder particles, the pressing pressure and the sintering temperature, the heat conductivity coefficient of the glass fluorescent layer is remarkably increased, the high-power blue light resistance of the wavelength conversion layer is improved, the surface coating effect is good, a metal reflecting film can be firmly attached, and the use reliability of a device is good.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of laser lighting and display technology, and specifically relates to a reflective wavelength conversion device and a preparation method thereof. Background Art

[0002] The wavelength conversion components used in laser lighting and display are mainly composed of a wavelength conversion layer, a fluorescent reflection layer and a thermal conductive substrate. The blue laser excites the wavelength conversion layer, and part of the blue laser is converted into stimulated light, which is reflected by the fluorescent reflection layer at the bottom together with the remaining blue light and collected by the lens.

[0003] Traditional wavelength conversion layers mainly include organic fluorescent layers prepared by encapsulating phosphors with organic silicone and glass fluorescent layers prepared by encapsulating phosphors with glass powder. Organic silicone has low thermal conductivity (usually around 0.1W / (m·K)) and poor heat resistance (usually below 250°C). In many high-power laser lighting scenarios, the organic fluorescent layer suffers from severe thermal decay and yellowing, which greatly affects the reliability of luminescence. The thermal conductivity of the glass fluorescent layer is also not high (usually between 0.3 and 0.7W / (m·K)). The internal thermal decay is also severe under high blue light power, which cannot meet the needs of high-power laser lighting and display scenarios. It is necessary to develop wavelength conversion layer materials with better thermal conductivity and heat resistance.

[0004] At present, in addition to glass fluorescent layers, ceramic fluorescent layers are also wavelength conversion materials with great application prospects. Ceramic fluorescent layers are mainly made by sintering fluorescent ceramic raw material powder with rare earth additives. The preparation of ceramic fluorescent layers usually requires high-temperature sintering above 1500℃, otherwise its thermal conductivity will be severely weakened and the adhesion of the reflective metal film layer will be greatly affected.

[0005] Traditional reflective layers also have two categories: organic diffuse reflective layers prepared by organic silicone encapsulated diffuse reflective particles and glass diffuse reflective layers prepared by glass powder encapsulated diffuse reflective particles. Organic silicone and glass diffuse reflective layers also have the problem of low thermal conductivity mentioned in the wavelength conversion layer, and the thickness of the reflective layer is usually above 60μm, resulting in a large interface thermal resistance between the wavelength conversion layer and the diffuse reflection layer. The wavelength conversion component has poor thermal conductivity and cannot meet the application scenarios of high-power laser lighting and laser display. It is necessary to develop new reflective layer materials with good thermal conductivity, thin thickness and lower interface thermal resistance. Summary of the invention

[0006] The present invention aims to overcome at least one defect in the prior art and provide a reflective wavelength conversion device with high thermal conductivity, low manufacturing energy consumption and high wavelength conversion efficiency.

[0007] In order to solve the above technical problems, the following technical solutions are adopted:

[0008] In the first aspect, a reflective wavelength conversion device is provided. The device comprises a glass fluorescent layer, a fluorescent reflective layer, a first thermal conductive adhesive layer, an intermediate substrate, a second thermal conductive adhesive layer and a bottom substrate stacked in sequence. The glass fluorescent layer is a mixture of fluorescent powder particles and glass powder particles, which is first pressed into a blank under a pressure of 80 to 200 MPa and then pressed at T m The median diameter D50 of the phosphor particles sintered at +k temperature is 8-20 μm, and the median diameter D50 of the glass powder particles is 1-6 μm; m It is the lowest temperature at which the glass powder particles are completely melted, 80℃≤k≤120℃.

[0009] This solution significantly improves the thermal conductivity of the glass fluorescent layer (reaching more than 3w / (m·k)) by controlling the particle size of the phosphor particles, the particle size of the glass powder particles, the pressing pressure, and the sintering temperature in the glass fluorescent layer. This is much higher than the glass fluorescent layer prepared at conventional normal pressure, and greatly improves the ability of the wavelength conversion layer to withstand high-power blue light. Compared with the ceramic fluorescent layer, the glass fluorescent layer of the present application is made by sintering a glass powder raw material with a relatively low sintering temperature and a composite commercial phosphor. The glass powder raw material has a higher sintering activity than the ceramic powder raw material in the ceramic fluorescent layer, and is easier to sinter. The wavelength conversion layer can be prepared at a relatively low temperature (below 1000°C). Moreover, the surface coating effect of the prepared wavelength conversion layer is better, and it can be firmly attached by a metal reflective film, the bonding is more firm, and the device has better reliability in use.

[0010] The content of the phosphor particles in the glass phosphor layer is preferably 40 to 60 wt %.

[0011] The intermediate substrate is preferably a silver sheet, the first heat-conducting adhesive layer is preferably a silver glue, and the second heat-conducting adhesive layer is preferably an organic heat-conducting glue. The silver glue includes silver powder and epoxy resin, and the organic heat-conducting glue includes heat-conducting particles and silicone resin. There is a strong interaction force between the silver glue and the silver sheet, and the bonding is tighter, which can improve the reliability of the wavelength conversion device, and thus help to further improve the thermal conductivity and heat dissipation capacity of the reflective wavelength conversion device. The silver glue itself also has excellent thermal conductivity and can conduct heat faster. The second heat-conducting adhesive layer is preferably an organic heat-conducting glue because the intermediate substrate and the bottom substrate are both rigid structures. The use of organic heat-conducting glue can better eliminate the force between the rigid structures, making the two more firmly bonded.

[0012] The fluorescent reflective layer is preferably a metal reflective layer, and the material is preferably silver, aluminum or silver-aluminum alloy. The aforementioned metal single substance or alloy has high reflective performance in the visible light band of 400-800nm, and the reflectivity in the visible light band reaches more than 90%, which is equivalent to the reflectivity of the organic diffuse reflection layer or the glass diffuse reflection layer. Moreover, the thermal conductivity of the metal reflective layer is very high (more than 200w / (m·k)), which is much higher than the organic diffuse reflection layer or the glass diffuse reflection layer; and the thickness is very thin (less than 1000nm), which is much lower than the organic diffuse reflection layer or the glass diffuse reflection layer (more than 60μm); therefore, the wavelength conversion device using the metal reflective layer has a greatly reduced interface thermal resistance between the wavelength conversion layer and the fluorescent reflective layer, and the overall thermal conductivity and heat dissipation effect is greatly improved.

[0013] The side of the fluorescent reflective layer facing the glass fluorescent layer is provided with an adhesive modification layer, and the material of the adhesive modification layer is preferably aluminum oxide, silicon oxide, metal titanium or metal chromium, so as to further improve the adhesive firmness between the fluorescent reflective layer and the glass fluorescent layer. The side of the fluorescent reflective layer facing away from the glass fluorescent layer is provided with a fluorescent protection layer, and the material of the fluorescent protection layer is preferably gold, nickel or platinum.

[0014] The thickness of the glass fluorescent layer is preferably 0.07 to 0.2 mm.

[0015] The thickness of the fluorescent reflective layer is preferably 100 to 1000 nm, more preferably 200 to 500 nm.

[0016] The thickness of the adhesion improvement layer is preferably 10 to 100 nm, more preferably 20 to 50 nm.

[0017] The thickness of the fluorescent protective layer is preferably 10 to 100 nm, more preferably 20 to 50 nm.

[0018] The thickness of the intermediate substrate is preferably 0.2 to 1 mm.

[0019] The thickness of the first thermally conductive adhesive layer is preferably 20 to 50 μm.

[0020] The thickness of the second thermally conductive adhesive layer is preferably 20 to 50 μm.

[0021] The bottom substrate is preferably a heat dissipation turntable, and the material is preferably aluminum. The heat dissipation turntable can timely discharge the heat generated by the wavelength conversion device during operation by rotating.

[0022] The surface of the glass fluorescent layer facing the fluorescent reflecting layer is set as a polished surface with a surface roughness Ra≤0.02 μm.

[0023] In a second aspect, a method for preparing the above-mentioned reflective wavelength conversion device is proposed. The method comprises the following steps:

[0024] Making a glass fluorescent layer: mixing fluorescent powder particles and glass powder particles evenly, loading them into a mold, and then pressing them into a green body at a pressure of 80 to 200 MPa, and then sintering them at a temperature 80 to 120°C higher than the full melting temperature of the glass powder particles (i.e., the lowest temperature at which the glass powder particles are completely melted) for 30 to 90 minutes, and finally polishing them to obtain a glass fluorescent layer;

[0025] Making the fluorescent reflective layer: firstly, coating the polished surface of the glass fluorescent layer with a bonding modification layer, then coating the fluorescent reflective layer on the side of the bonding modification layer facing away from the glass fluorescent layer, and finally coating the fluorescent protective layer on the side of the fluorescent reflective layer facing away from the bonding modification layer;

[0026] Bonding the intermediate substrate: coating silver glue on one side of the intermediate substrate and the side of the fluorescent protective layer facing away from the fluorescent reflective layer, so that the fluorescent protective layer and the silver glue-coated surface of the intermediate substrate are relatively attached, curing the silver glue, and forming a first thermal conductive adhesive layer between the fluorescent protective layer and the intermediate substrate;

[0027] Bonding the bottom substrate: coating organic thermally conductive adhesive on one side of the bottom substrate and the side of the intermediate substrate facing away from the first thermally conductive adhesive layer, so that the surfaces of the intermediate substrate and the bottom substrate coated with the organic thermally conductive adhesive are relatively fitted, and curing the organic thermally conductive adhesive to form a second thermally conductive adhesive layer between the intermediate substrate and the bottom substrate.

[0028] In the above-mentioned step of making the glass fluorescent layer, the fluorescent powder particles and the glass powder particles can be evenly mixed by ball milling. The specific process is: put the fluorescent powder particles and the glass powder particles into a ball mill, add anhydrous ethanol as the ball milling medium, and ball mill for 24 hours under the conditions of a ball-to-material ratio of 5:1 and a rotation speed of 120-150rpm / min to obtain a fluorescent slurry in which all raw materials are evenly dispersed. The fluorescent slurry is placed in a high-temperature oven and dried at 70°C for 24 hours to remove the anhydrous ethanol to obtain a fluorescent dry powder. The fluorescent dry powder is crushed with a mortar and passed through a 200-mesh sieve to obtain a mixed fluorescent powder in which the fluorescent powder particles and the glass powder particles are evenly mixed.

[0029] In the above steps of making the glass fluorescent layer, the product obtained after sintering can be called a glass fluorescent body. If the thickness of the glass fluorescent body is equivalent to the target thickness of the glass fluorescent layer, it can be polished after sintering. If the thickness of the glass fluorescent body is significantly greater than the target thickness of the glass fluorescent layer, it needs to be cut into thin slices after sintering and then polished.

[0030] In the above-mentioned step of making the fluorescent reflective layer, the bonding modification layer, the fluorescent reflective layer and the fluorescent protective layer can be obtained by plating in a manner such as evaporation and sputtering.

[0031] In the above-mentioned step of bonding the intermediate layer substrate, the surfaces of the intermediate layer substrate and the fluorescent protective layer can be coated with silver glue by steel screen printing, dispensing, scraping, etc.; after the fluorescent protective layer and the intermediate layer substrate are relatively attached, they can be baked at 200-300°C to achieve the purpose of curing the silver glue.

[0032] In the above-mentioned step of bonding the bottom substrate, the surfaces of the bottom substrate and the middle substrate can be coated with organic thermal conductive adhesive by steel screen printing, dispensing, scraping, etc.; after the middle substrate and the bottom substrate are relatively bonded, they can be placed at room temperature for a period of time to achieve the purpose of curing the organic thermal conductive adhesive.

[0033] Compared with the prior art, the present solution has the following beneficial effects: by controlling the particle size of the phosphor particles, the particle size of the glass powder particles, the pressing pressure and the sintering temperature in the glass phosphor layer, the thermal conductivity of the glass phosphor layer is significantly improved (reaching above 3w / (m·k)), which is much higher than that of the glass phosphor layer prepared at conventional normal pressure, and the ability of the wavelength conversion layer to withstand high-power blue light is greatly improved. The production energy consumption is significantly lower than that of the ceramic phosphor layer. The surface coating effect of the prepared wavelength conversion layer (glass phosphor layer) is better, and it can be firmly attached by a metal reflective film, the bonding is more firm, and the device has better reliability in use. DETAILED DESCRIPTION

[0034] The reflective wavelength conversion device proposed in this solution includes a glass fluorescent layer, a fluorescent reflective layer, a first thermal conductive adhesive layer, an intermediate substrate, a second thermal conductive adhesive layer and a bottom substrate which are stacked in sequence.

[0035] The glass fluorescent layer is used as a wavelength conversion layer to generate stimulated fluorescence when stimulated by laser light. Coarse-grained fluorescent powder particles with a median diameter D50 of 8 to 20 μm are selected as the fluorescent generation phase, and glass powder particles with a median diameter D50 of 1 to 6 μm are selected as the matrix phase. This combination of particle sizes allows the glass powder particles to fill the gaps formed by the bridges of the fluorescent powder particles. The fluorescent powder particles can be selected from (Y, Gd)3(Al, Ga)5O 12 :Ce, α-Sialon:Eu and other yellow powders, LuAG, GaYAG, β-Sialon:Eu and other green powders, and CaAlSiN3:Eu and other red powders, preferably 40-60wt% in the glass fluorescent layer. Glass powder particles can be selected from Si-BO system, Zn-B-Si-O system and Al-Si-BKO system, etc., with a full melting temperature of 700-900℃, a visible light transmittance of more than 90% in the 450-700nm band, a refractive index of 1.44-1.68, and a room temperature linear expansion coefficient of (40-90)*10 -7 / ℃, which is between the phosphor particles and metal. In the preparation process of the glass phosphor layer, it is first pressed into a blank at a pressure of 80-200MPa, and then sintered at a temperature 80-120℃ higher than the full melting temperature of the glass powder particles (i.e., the lowest temperature at which the glass powder particles are completely melted). During the pressing process, the glass powder particles filled in the gaps between the phosphor particles are compressed. During the sintering process at this temperature, the glass powder particles melt into a flowing state with moderate viscosity, and the phosphor particles evenly dispersed therein are evenly wrapped to form a spatial network skeleton.

[0036] By controlling the particle size of the phosphor particles in the glass phosphor layer, the particle size of the glass powder particles, the pressing pressure and the sintering temperature, the thermal conductivity of the glass phosphor layer is significantly improved (reaching more than 3w / (m·k)), which is much higher than the glass phosphor layer prepared at conventional normal pressure, and the ability of the wavelength conversion layer to withstand high-power blue light is greatly improved. Compared with the ceramic phosphor layer, the glass phosphor layer is made by sintering a glass powder raw material with a relatively low sintering temperature and a composite commercial phosphor. Compared with the ceramic powder raw material in the ceramic phosphor layer, the glass powder raw material has a high sintering activity and is easier to sinter. The wavelength conversion layer can be prepared at a relatively low temperature (below 1000°C). Moreover, the surface coating effect of the prepared wavelength conversion layer is better, and it can be firmly attached by the metal reflective film, the bonding is more firm, and the device has better reliability in use. The thickness of the glass phosphor layer is preferably 0.07 to 0.2mm. The glass phosphor layer can be polished on one side or on both sides, and the surface roughness of the polished surface Ra≤0.02μm, and the surface roughness of the non-polished surface Ra≥5μm.

[0037] The fluorescent reflection layer can be a metal reflection layer. The metal reflection layer can be made of a material with a high reflectivity in the visible light band, preferably silver, aluminum or silver-aluminum alloy, and the thickness is preferably 100-1000nm, and more preferably 200-500nm. The above-mentioned metal single substance or alloy has high reflectivity in the visible light band of 400-800nm, and the reflectivity in the visible light band reaches more than 90%, which is equivalent to the reflectivity of the organic diffuse reflection layer or the glass diffuse reflection layer. Moreover, the thermal conductivity of the metal reflection layer is very high (more than 200w / (m·k)), which is much higher than that of the organic diffuse reflection layer or the glass diffuse reflection layer; and the thickness is very thin (less than 1000nm). The thickness of the metal reflection layer prepared by sputtering or evaporation is about 100-500nm, which is much lower than that of the organic diffuse reflection layer or the glass diffuse reflection layer (more than 60μm); therefore, the wavelength conversion device using the metal reflection layer has a greatly reduced interface thermal resistance between the wavelength conversion layer and the fluorescent reflection layer, and the overall thermal conductivity and heat dissipation effect is greatly improved.

[0038] An adhesive modification layer is provided on the side of the fluorescent reflective layer facing the glass fluorescent layer to further improve the adhesive strength between the fluorescent reflective layer and the glass fluorescent layer. The material of the adhesive modification layer is preferably aluminum oxide, silicon oxide, metal titanium or metal chromium, and the thickness is preferably 10 to 100 nm, more preferably 20 to 50 nm. A fluorescent protective layer is provided on the side of the fluorescent reflective layer facing away from the glass fluorescent layer. The fluorescent protective layer can be made of a metal or alloy material with good chemical stability in an air environment, preferably gold, nickel, platinum, etc., and the thickness is preferably 10 to 100 nm, more preferably 20 to 50 nm.

[0039] The intermediate substrate plays a role in heat dissipation, and timely conducts away the heat generated by the glass fluorescent layer when it is working, so as to prevent the heat from accumulating inside the glass fluorescent layer and the thermal decay and thermal saturation of the fluorescent powder. The first thermal conductive adhesive layer mainly plays a bonding role between the fluorescent reflective layer and the intermediate substrate, so that the heat generated by the glass fluorescent layer when it is working can be timely conducted to the intermediate substrate through the fluorescent reflective layer. The second thermal conductive adhesive layer mainly plays a bonding role between the intermediate substrate and the bottom substrate, so that the heat in the intermediate substrate can be conducted to the bottom substrate through the second thermal conductive adhesive layer. The intermediate substrate is preferably made of silver sheet, and the thickness is preferably 0.2 to 1 mm. The material of the first thermal conductive adhesive layer is preferably silver glue, and the thickness is preferably 20 to 50 μm. The material of the second thermal conductive adhesive layer is preferably organic thermal conductive glue, and the thickness is preferably 20 to 50 μm. The main components of the silver glue are silver powder and epoxy resin, which have a strong interaction force with the silver sheet, and the bonding is tighter, which can improve the reliability of the wavelength conversion device, and the silver glue itself has excellent thermal conductivity and can conduct heat faster. The second thermally conductive adhesive layer uses organic thermally conductive adhesive to effectively eliminate the force between the middle substrate of the rigid structure and the bottom substrate of the rigid structure, making the two more firmly bonded.

[0040] The bottom substrate plays a role in heat dissipation, discharging the heat generated by the wavelength conversion device. The bottom substrate preferably adopts a heat dissipation turntable, which can timely discharge the heat generated by the wavelength conversion device by rotating. The material of the bottom substrate is preferably metal aluminum.

[0041] The present invention also proposes a method for preparing the above-mentioned reflective wavelength conversion device, comprising the following steps:

[0042] 1. Making a glass fluorescent layer: Evenly mix the fluorescent powder particles and the glass powder particles, put them into a mold, and then press them into a green body under a pressure of 80 to 200 MPa, and then sinter them at a temperature 80 to 120°C higher than the full melting temperature of the glass powder particles for 30 to 90 minutes, and finally polish them to obtain a glass fluorescent layer. The fluorescent powder particles and the glass powder particles can be evenly mixed by ball milling. The specific process is as follows: put the fluorescent powder particles and the glass powder particles into a ball milling jar, add anhydrous ethanol as a ball milling medium, and ball mill for 24 hours at a ball-to-material ratio of 5:1 and a rotation speed of 120 to 150 rpm / min to obtain a fluorescent slurry in which all raw materials are evenly dispersed; put the fluorescent slurry in a high-temperature oven, dry it at 70°C for 24 hours, remove the anhydrous ethanol, and obtain a fluorescent dry powder; crush the fluorescent dry powder with a mortar, and pass it through a 200-mesh screen to obtain a mixed fluorescent powder in which the fluorescent powder particles and the glass powder particles are evenly mixed. The product obtained after sintering can be called a glass phosphor; if the thickness of the glass phosphor is equivalent to the target thickness of the glass phosphor layer, it can be polished after sintering; if the thickness of the glass phosphor is significantly greater than the target thickness of the glass phosphor layer, it needs to be cut into thin slices after sintering and then polished. Specifically, a multi-wire cutting process can be used.

[0043] 2. Making the fluorescent reflective layer: firstly, the bonding modification layer is plated on the polished surface of the glass fluorescent layer, then the fluorescent reflective layer is plated on the side of the bonding modification layer facing away from the glass fluorescent layer, and finally the fluorescent protective layer is plated on the side of the fluorescent reflective layer facing away from the bonding modification layer. The bonding modification layer, the fluorescent reflective layer and the fluorescent protective layer can be plated by evaporation, sputtering or the like.

[0044] 3. Bonding the intermediate substrate: Silver glue is applied on one side of the intermediate substrate and the side of the fluorescent protective layer facing away from the fluorescent reflective layer, so that the fluorescent protective layer and the silver-coated surface of the intermediate substrate are relatively fitted, and the silver glue is cured to form a first thermally conductive adhesive layer between the fluorescent protective layer and the intermediate substrate. The surfaces of the intermediate substrate and the fluorescent protective layer can be coated with silver glue by steel screen printing, dispensing, scraping, etc. After the fluorescent protective layer and the intermediate substrate are relatively fitted, they can be baked at 200-300°C to achieve the purpose of curing the silver glue.

[0045] 4. Bonding the bottom substrate: Coat organic thermally conductive adhesive on one side of the bottom substrate and the side of the middle substrate facing away from the first thermally conductive adhesive layer, so that the middle substrate and the bottom substrate with the organic thermally conductive adhesive are relatively attached, and the organic thermally conductive adhesive is cured to form a second thermally conductive adhesive layer between the middle substrate and the bottom substrate. The surfaces of the bottom substrate and the middle substrate can be coated with organic thermally conductive adhesive by steel screen printing, dispensing, scraping, etc. After the middle substrate and the bottom substrate are relatively attached, they can be left at room temperature for a period of time to achieve the purpose of curing the organic thermally conductive adhesive.

[0046] In order to enable those skilled in the art to better understand the present solution, the present solution is further described in detail below in conjunction with specific embodiments.

[0047] The silver glue described in the following examples comes from Shenzhen Xinyuan New Materials Co., Ltd., and its model is PF-01B91A.

[0048] The organic thermally conductive adhesive described in the following examples is from Shenzhen Jinling Tongda Electronics Co., Ltd., model number is XK-S65.

[0049] Example 1

[0050] The reflective wavelength conversion device of this embodiment includes a glass fluorescent layer, a fluorescent reflective layer, a first thermal conductive adhesive layer, an intermediate substrate, a second thermal conductive adhesive layer and a bottom substrate which are stacked in sequence.

[0051] The glass fluorescent layer is mainly composed of fluorescent powder particles and glass powder particles, with the fluorescent powder particles accounting for 50wt%. The fluorescent powder particles and glass powder particles are mixed evenly and loaded into a mold, first pressed into a green body at a pressure of 140MPa, and then sintered at a temperature 100℃ higher than the full melting temperature of the glass powder particles. The fluorescent powder particles are (Y, Gd)3(Al, Ga)5O 12 :Ce, median diameter D50 is 14μm. The glass powder particles are selected from Si-BO system, with a median diameter D50 of 3μm, a full melting temperature of about 800℃, a visible light transmittance of more than 90% in the 450-700nm band, a refractive index of 1.44-1.68, and a room temperature linear expansion coefficient of about 70*10 -7 / ℃. The thickness of the glass fluorescent layer is 0.13mm, double-sided polishing, and the surface roughness of the polished surface Ra≤0.02μm.

[0052] The fluorescent reflection layer is a metal reflection layer, and the material is silver with high reflectivity in the visible light band, and the thickness is 300nm. The side of the fluorescent reflection layer facing the glass fluorescent layer is provided with an adhesive modification layer, and the material of the adhesive modification layer is metal titanium, and the thickness is 30nm. The side of the fluorescent reflection layer facing away from the glass fluorescent layer is provided with a fluorescent protection layer, and the material of the fluorescent protection layer is gold with good chemical stability in the air environment, and the thickness is 30nm.

[0053] The middle layer substrate is made of silver sheet with a thickness of 0.6mm. The first thermal conductive adhesive layer is made of silver glue with a thickness of 30μm. The second thermal conductive adhesive layer is made of organic thermal conductive glue with a thickness of 30μm. The bottom substrate is made of aluminum heat dissipation turntable.

[0054] The reflective wavelength conversion device is prepared according to the following steps:

[0055] 1. Preparation of glass fluorescent layer: Put the fluorescent powder particles and glass powder particles into a ball mill, add anhydrous ethanol as the ball milling medium, and ball mill for 24 hours at a ball-to-material ratio of 5:1 and a rotation speed of 135rpm / min to obtain a fluorescent slurry in which all raw materials are evenly dispersed. The fluorescent slurry is placed in a high-temperature oven and dried at 70°C for 24 hours to remove the anhydrous ethanol to obtain a fluorescent dry powder. The fluorescent dry powder is crushed with a mortar and passed through a 200-mesh sieve to obtain a mixed fluorescent powder. The mixed fluorescent powder is loaded into a mold, first pressed into a green body under a pressure of 140MPa, and then sintered for 60 minutes at a temperature 100°C higher than the full melting temperature of the glass powder particles to obtain a glass fluorescent body. The glass fluorescent body is cut into thin slices, and then single-sided or double-sided polishing is obtained to obtain a glass fluorescent layer.

[0056] 2. Making a fluorescent reflective layer: coating the polished surface of the glass fluorescent layer with a bonding modification layer by evaporation, coating the fluorescent reflective layer on the side of the bonding modification layer facing away from the glass fluorescent layer by evaporation, and coating the fluorescent protective layer on the side of the fluorescent reflective layer facing away from the bonding modification layer by evaporation.

[0057] 3. Bonding the intermediate substrate: Silver glue is applied on one side of the intermediate substrate and the side of the fluorescent protective layer facing away from the fluorescent reflective layer by scraping, so that the fluorescent protective layer and the silver-coated surface of the intermediate substrate are relatively fitted together, and baked at 250°C to solidify the silver glue, thereby forming a first thermally conductive adhesive layer between the fluorescent protective layer and the intermediate substrate.

[0058] 4. Bonding the bottom substrate: Use a scraping method to apply organic thermally conductive adhesive on one side of the bottom substrate and the side of the middle substrate facing away from the first thermally conductive adhesive layer, so that the surfaces of the middle substrate and the bottom substrate covered with the organic thermally conductive adhesive are relatively fitted together, and the organic thermally conductive adhesive is allowed to solidify at room temperature for a period of time to form a second thermally conductive adhesive layer between the middle substrate and the bottom substrate.

[0059] Example 2

[0060] The reflective wavelength conversion device of this embodiment includes a glass fluorescent layer, a fluorescent reflective layer, a first thermal conductive adhesive layer, an intermediate substrate, a second thermal conductive adhesive layer and a bottom substrate which are stacked in sequence.

[0061] The glass phosphor layer is mainly composed of phosphor particles and glass powder particles, with the phosphor particles accounting for 50wt%. The phosphor particles and glass powder particles are mixed evenly and loaded into a mold, first pressed into a green body at a pressure of 80MPa, and then sintered at a temperature 120℃ higher than the full melting temperature of the glass powder particles. The phosphor particles are (Y, Gd)3(Al, Ga)5O 12:Ce, median diameter D50 is 8μm. The glass powder particles are selected from Si-BO system, with a median diameter D50 of 1μm, a full melting temperature of about 800℃, a visible light transmittance of more than 90% in the 450-700nm band, a refractive index of 1.44-1.68, and a room temperature linear expansion coefficient of about 70*10 -7 / ℃. The thickness of the glass fluorescent layer is 0.13mm, double-sided polishing, and the surface roughness of the polished surface Ra≤0.02μm.

[0062] The fluorescent reflection layer is a metal reflection layer, and the material is silver with high reflectivity in the visible light band, and the thickness is 300nm. The side of the fluorescent reflection layer facing the glass fluorescent layer is provided with an adhesive modification layer, and the material of the adhesive modification layer is metal titanium, and the thickness is 30nm. The side of the fluorescent reflection layer facing away from the glass fluorescent layer is provided with a fluorescent protection layer, and the material of the fluorescent protection layer is gold with good chemical stability in the air environment, and the thickness is 30nm.

[0063] The middle layer substrate is made of silver sheet with a thickness of 0.6mm. The first thermal conductive adhesive layer is made of silver glue with a thickness of 30μm. The second thermal conductive adhesive layer is made of organic thermal conductive glue with a thickness of 30μm. The bottom substrate is made of aluminum heat dissipation turntable.

[0064] The reflective wavelength conversion device is prepared according to the following steps:

[0065] 1. Preparation of glass fluorescent layer: Put the fluorescent powder particles and glass powder particles into a ball mill, add anhydrous ethanol as the ball milling medium, and ball mill for 24 hours at a ball-to-material ratio of 5:1 and a rotation speed of 135rpm / min to obtain a fluorescent slurry in which all raw materials are evenly dispersed. Place the fluorescent slurry in a high-temperature oven and dry it at 70℃ for 24 hours to remove the anhydrous ethanol to obtain a fluorescent dry powder. Crush the fluorescent dry powder with a mortar and pass it through a 200-mesh sieve to obtain a mixed fluorescent powder. Put the mixed fluorescent powder into a mold, first press the mixed fluorescent powder into a green body under a pressure of 80MPa, and then sinter the green body for 60 minutes at a temperature 120℃ higher than the full melting temperature of the glass powder particles to obtain a glass fluorescent body. Cut the glass fluorescent body into thin slices, and then polish them on one side or both sides to obtain a glass fluorescent layer.

[0066] 2. Making a fluorescent reflective layer: coating the polished surface of the glass fluorescent layer with a bonding modification layer by evaporation, coating the fluorescent reflective layer on the side of the bonding modification layer facing away from the glass fluorescent layer by evaporation, and coating the fluorescent protective layer on the side of the fluorescent reflective layer facing away from the bonding modification layer by evaporation.

[0067] 3. Bonding the intermediate substrate: Silver glue is applied on one side of the intermediate substrate and the side of the fluorescent protective layer facing away from the fluorescent reflective layer by scraping, so that the fluorescent protective layer and the silver-coated surface of the intermediate substrate are relatively fitted together, and baked at 250°C to solidify the silver glue, thereby forming a first thermally conductive adhesive layer between the fluorescent protective layer and the intermediate substrate.

[0068] 4. Bonding the bottom substrate: Use a scraping method to apply organic thermally conductive adhesive on one side of the bottom substrate and the side of the middle substrate facing away from the first thermally conductive adhesive layer, so that the surfaces of the middle substrate and the bottom substrate covered with the organic thermally conductive adhesive are relatively fitted together, and the organic thermally conductive adhesive is allowed to solidify at room temperature for a period of time to form a second thermally conductive adhesive layer between the middle substrate and the bottom substrate.

[0069] Example 3

[0070] The reflective wavelength conversion device of this embodiment includes a glass fluorescent layer, a fluorescent reflective layer, a first thermal conductive adhesive layer, an intermediate substrate, a second thermal conductive adhesive layer and a bottom substrate which are stacked in sequence.

[0071] The glass fluorescent layer is mainly composed of fluorescent powder particles and glass powder particles, with the fluorescent powder particles accounting for 50wt%. The fluorescent powder particles and glass powder particles are mixed evenly and loaded into a mold, first pressed into a green body at a pressure of 200MPa, and then sintered at a temperature 80℃ higher than the full melting temperature of the glass powder particles. The fluorescent powder particles are (Y, Gd)3(Al, Ga)5O 12 :Ce, median diameter D50 is 20μm. The glass powder particles are selected from Si-BO system, with a median diameter D50 of 6μm, a full melting temperature of about 800℃, a visible light transmittance of more than 90% in the 450-700nm band, a refractive index of 1.44-1.68, and a room temperature linear expansion coefficient of about 70*10 -7 / ℃. The thickness of the glass fluorescent layer is 0.13mm, double-sided polishing, and the surface roughness of the polished surface Ra≤0.02μm.

[0072] The fluorescent reflection layer is a metal reflection layer, and the material is silver with high reflectivity in the visible light band, and the thickness is 300nm. The side of the fluorescent reflection layer facing the glass fluorescent layer is provided with an adhesive modification layer, and the material of the adhesive modification layer is metal titanium, and the thickness is 30nm. The side of the fluorescent reflection layer facing away from the glass fluorescent layer is provided with a fluorescent protection layer, and the material of the fluorescent protection layer is gold with good chemical stability in the air environment, and the thickness is 30nm.

[0073] The middle layer substrate is made of silver sheet with a thickness of 0.6mm. The first thermal conductive adhesive layer is made of silver glue with a thickness of 30μm. The second thermal conductive adhesive layer is made of organic thermal conductive glue with a thickness of 30μm. The bottom substrate is made of aluminum heat dissipation turntable.

[0074] The reflective wavelength conversion device is prepared according to the following steps:

[0075] 1. Preparation of glass fluorescent layer: Put the fluorescent powder particles and glass powder particles into a ball mill, add anhydrous ethanol as the ball milling medium, and ball mill for 24 hours at a ball-to-material ratio of 5:1 and a rotation speed of 135rpm / min to obtain a fluorescent slurry in which all raw materials are evenly dispersed. The fluorescent slurry is placed in a high-temperature oven and dried at 70°C for 24 hours to remove the anhydrous ethanol to obtain a fluorescent dry powder. The fluorescent dry powder is crushed with a mortar and passed through a 200-mesh sieve to obtain a mixed fluorescent powder. The mixed fluorescent powder is loaded into a mold, first pressed into a green body at a pressure of 200MPa, and then sintered for 60 minutes at a temperature 80°C higher than the full melting temperature of the glass powder particles to obtain a glass fluorescent body. The glass fluorescent body is cut into thin slices, and then single-sided or double-sided polishing is obtained to obtain a glass fluorescent layer.

[0076] 2. Making a fluorescent reflective layer: coating the polished surface of the glass fluorescent layer with a bonding modification layer by evaporation, coating the fluorescent reflective layer on the side of the bonding modification layer facing away from the glass fluorescent layer by evaporation, and coating the fluorescent protective layer on the side of the fluorescent reflective layer facing away from the bonding modification layer by evaporation.

[0077] 3. Bonding the intermediate substrate: Silver glue is applied on one side of the intermediate substrate and the side of the fluorescent protective layer facing away from the fluorescent reflective layer by scraping, so that the fluorescent protective layer and the silver-coated surface of the intermediate substrate are relatively fitted together, and baked at 250°C to solidify the silver glue, thereby forming a first thermally conductive adhesive layer between the fluorescent protective layer and the intermediate substrate.

[0078] 4. Bonding the bottom substrate: Use a scraping method to apply organic thermally conductive adhesive on one side of the bottom substrate and the side of the middle substrate facing away from the first thermally conductive adhesive layer, so that the surfaces of the middle substrate and the bottom substrate covered with the organic thermally conductive adhesive are relatively fitted together, and the organic thermally conductive adhesive is allowed to solidify at room temperature for a period of time to form a second thermally conductive adhesive layer between the middle substrate and the bottom substrate.

[0079] Example 4

[0080] The reflective wavelength conversion device of this embodiment includes a glass fluorescent layer, a fluorescent reflective layer, a first thermal conductive adhesive layer, an intermediate substrate, a second thermal conductive adhesive layer and a bottom substrate which are stacked in sequence.

[0081] The glass fluorescent layer is mainly composed of fluorescent powder particles and glass powder particles, with the fluorescent powder particles accounting for 45wt%. After the fluorescent powder particles and glass powder particles are evenly mixed, they are first pressed into a blank at a pressure of 120MPa, and then sintered at a temperature 110℃ higher than the full melting temperature of the glass powder particles. The fluorescent powder particles are (Y, Gd)3(Al, Ga)5O 12:Ce, median diameter D50 is 10μm. The glass powder particles are selected from the Zn-B-Si-O system, the median diameter D50 is 2μm, the full melting temperature is about 750℃, the transmittance of visible light in the 450-700nm band is more than 90%, the refractive index is 1.44-1.68, and the room temperature linear expansion coefficient is about 70*10 -7 / ℃. The thickness of the glass fluorescent layer is 0.11mm, double-sided polishing, and the surface roughness of the polished surface Ra≤0.02μm.

[0082] The fluorescent reflective layer is a metal reflective layer, and the material is aluminum with high reflectivity in the visible light band, and the thickness is 200nm. The side of the fluorescent reflective layer facing the glass fluorescent layer is provided with an adhesive modification layer, and the material of the adhesive modification layer is metal chromium, and the thickness is 20nm. The side of the fluorescent reflective layer facing away from the glass fluorescent layer is provided with a fluorescent protective layer, and the material of the fluorescent protective layer is nickel with good chemical stability in the air environment, and the thickness is 20nm.

[0083] The middle substrate is made of silver sheet with a thickness of 0.4mm. The first thermal conductive adhesive layer is made of silver glue with a thickness of 30μm. The second thermal conductive adhesive layer is made of organic thermal conductive glue with a thickness of 30μm. The bottom substrate is made of aluminum heat dissipation turntable.

[0084] The reflective wavelength conversion device is prepared according to the following steps:

[0085] 1. Preparation of glass fluorescent layer: Put the fluorescent powder particles and glass powder particles into a ball mill, add anhydrous ethanol as the ball milling medium, and ball mill for 24 hours at a ball-to-material ratio of 5:1 and a rotation speed of 130rpm / min to obtain a fluorescent slurry in which all raw materials are evenly dispersed. The fluorescent slurry is placed in a high-temperature oven and dried at 70°C for 24 hours to remove the anhydrous ethanol to obtain a fluorescent dry powder. The fluorescent dry powder is crushed with a mortar and passed through a 200-mesh sieve to obtain a mixed fluorescent powder. The mixed fluorescent powder is loaded into a mold, first pressed into a green body under a pressure of 120MPa, and then sintered at a temperature 110°C higher than the full melting temperature of the glass powder particles for 45 minutes to obtain a glass fluorescent body. The glass fluorescent body is cut into thin slices, and then single-sided or double-sided polishing is obtained to obtain a glass fluorescent layer.

[0086] 2. Making a fluorescent reflective layer: coating the polished surface of the glass fluorescent layer with a bonding modification layer by sputtering, coating the fluorescent reflective layer on the side of the bonding modification layer facing away from the glass fluorescent layer by sputtering, and coating the fluorescent protective layer on the side of the fluorescent reflective layer facing away from the bonding modification layer by sputtering.

[0087] 3. Bonding the intermediate substrate: Use steel screen printing to coat silver glue on one side of the intermediate substrate and the side of the fluorescent protective layer facing away from the fluorescent reflective layer, so that the fluorescent protective layer and the surface of the intermediate substrate covered with silver glue are relatively fitted together, and bake at 300°C to solidify the silver glue to form a first thermally conductive adhesive layer between the fluorescent protective layer and the intermediate substrate.

[0088] 4. Bonding the bottom substrate: Use steel screen printing to coat organic thermal conductive adhesive on one side of the bottom substrate and the side of the middle substrate facing away from the first thermal conductive adhesive layer, so that the surfaces of the middle substrate and the bottom substrate covered with organic thermal conductive adhesive are relatively fitted together, and left at room temperature for a period of time to allow the organic thermal conductive adhesive to solidify, thereby forming a second thermal conductive adhesive layer between the middle substrate and the bottom substrate.

[0089] Example 5

[0090] The reflective wavelength conversion device of this embodiment includes a glass fluorescent layer, a fluorescent reflective layer, a first thermal conductive adhesive layer, an intermediate substrate, a second thermal conductive adhesive layer and a bottom substrate which are stacked in sequence.

[0091] The glass fluorescent layer is mainly composed of fluorescent powder particles and glass powder particles, with the fluorescent powder particles accounting for 40wt%. After the fluorescent powder particles and glass powder particles are evenly mixed, they are first pressed into a blank under a pressure of 100MPa, and then sintered at a temperature 90℃ higher than the full melting temperature of the glass powder particles. The fluorescent powder particles are (Y, Gd)3(Al, Ga)5O 12 :Ce, median diameter D50 is 12μm. The glass powder particles are selected from the Zn-B-Si-O system, the median diameter D50 is 3μm, the full melting temperature is 750℃, the transmittance of visible light in the 450-700nm band is more than 90%, the refractive index is 1.44-1.68, and the room temperature linear expansion coefficient is 70*10 -7 / ℃. The thickness of the glass fluorescent layer is 0.07mm, double-sided polishing, and the surface roughness of the polished surface Ra≤0.02μm.

[0092] The fluorescent reflection layer is a metal reflection layer, and the material is silver-aluminum alloy with high reflectivity in the visible light band, and the thickness is 100nm. The side of the fluorescent reflection layer facing the glass fluorescent layer is provided with an adhesive modification layer, and the material of the adhesive modification layer is aluminum oxide, and the thickness is 50nm. The side of the fluorescent reflection layer facing away from the glass fluorescent layer is provided with a fluorescent protection layer, and the material of the fluorescent protection layer is platinum with good chemical stability in the air environment, and the thickness is 10nm.

[0093] The middle substrate is made of silver sheet with a thickness of 0.2mm. The first thermal conductive adhesive layer is made of silver glue with a thickness of 20μm. The second thermal conductive adhesive layer is made of organic thermal conductive glue with a thickness of 20μm. The bottom substrate is made of aluminum heat dissipation turntable.

[0094] The reflective wavelength conversion device is prepared according to the following steps:

[0095] 1. Preparation of glass fluorescent layer: Put the fluorescent powder particles and glass powder particles into a ball mill, add anhydrous ethanol as the ball milling medium, and ball mill for 24 hours at a ball-to-material ratio of 5:1 and a rotation speed of 120rpm / min to obtain a fluorescent slurry in which all raw materials are evenly dispersed. The fluorescent slurry is placed in a high-temperature oven and dried at 70°C for 24 hours to remove the anhydrous ethanol to obtain a fluorescent dry powder. The fluorescent dry powder is crushed with a mortar and passed through a 200-mesh sieve to obtain a mixed fluorescent powder. The mixed fluorescent powder is loaded into a mold, first pressed into a green body under a pressure of 100MPa, and then sintered at a temperature 90°C higher than the full melting temperature of the glass powder particles for 30 minutes to obtain a glass fluorescent body. The glass fluorescent body is cut into thin slices, and then single-sided or double-sided polishing is obtained to obtain a glass fluorescent layer.

[0096] 2. Making a fluorescent reflective layer: coating the polished surface of the glass fluorescent layer with a bonding modification layer by sputtering, coating the fluorescent reflective layer on the side of the bonding modification layer facing away from the glass fluorescent layer by sputtering, and coating the fluorescent protective layer on the side of the fluorescent reflective layer facing away from the bonding modification layer by sputtering.

[0097] 3. Bonding the middle layer substrate: Use a dispensing method to apply silver glue on one side of the middle layer substrate and the side of the fluorescent protective layer facing away from the fluorescent reflective layer, so that the fluorescent protective layer and the surface of the middle layer substrate covered with silver glue are relatively fitted together, and bake at 200°C to solidify the silver glue to form a first thermally conductive adhesive layer between the fluorescent protective layer and the middle layer substrate.

[0098] 4. Bonding the bottom substrate: Use a dispensing method to apply organic thermally conductive adhesive on one side of the bottom substrate and the side of the middle substrate facing away from the first thermally conductive adhesive layer, so that the surfaces of the middle substrate and the bottom substrate covered with the organic thermally conductive adhesive are relatively fitted together, and are placed at room temperature for a period of time to allow the organic thermally conductive adhesive to solidify, thereby forming a second thermally conductive adhesive layer located between the middle substrate and the bottom substrate.

[0099] Example 6

[0100] The reflective wavelength conversion device of this embodiment includes a glass fluorescent layer, a fluorescent reflective layer, a first thermal conductive adhesive layer, an intermediate substrate, a second thermal conductive adhesive layer and a bottom substrate which are stacked in sequence.

[0101] The glass fluorescent layer is mainly composed of fluorescent powder particles and glass powder particles, with the fluorescent powder particles accounting for 60wt%. After the fluorescent powder particles and glass powder particles are evenly mixed, they are first pressed into a green body at a pressure of 180MPa, and then sintered at a temperature 110°C higher than the full melting temperature of the glass powder particles. The fluorescent powder particles are LuAG and CaAlSiN3:Eu, with a median diameter D50 of 16μm. The glass powder particles are Zn-B-Si-O system, with a median diameter D50 of 4μm, a full melting temperature of about 750°C, a visible light transmittance of more than 90% in the 450-700nm band, a refractive index of 1.44-1.68, and a room temperature linear expansion coefficient of about 70*10 -7 / ℃. The thickness of the glass fluorescent layer is 0.2mm, double-sided polishing, and the surface roughness of the polished surface Ra≤0.02μm.

[0102] The fluorescent reflection layer is a metal reflection layer, and the material is silver-aluminum alloy with high reflectivity in the visible light band, and the thickness is 500nm. The side of the fluorescent reflection layer facing the glass fluorescent layer is provided with an adhesive modification layer, and the material of the adhesive modification layer is silicon oxide, and the thickness is 50nm. The side of the fluorescent reflection layer facing away from the glass fluorescent layer is provided with a fluorescent protection layer, and the material of the fluorescent protection layer is platinum with good chemical stability in the air environment, and the thickness is 50nm.

[0103] The middle layer substrate is made of silver sheet with a thickness of 1mm. The first thermal conductive adhesive layer is made of silver glue with a thickness of 50μm. The second thermal conductive adhesive layer is made of organic thermal conductive glue with a thickness of 50μm. The bottom substrate is made of aluminum heat dissipation turntable.

[0104] The reflective wavelength conversion device is prepared according to the following steps:

[0105] 1. Preparation of glass fluorescent layer: Put the fluorescent powder particles and glass powder particles into a ball mill, add anhydrous ethanol as the ball milling medium, and ball mill for 24 hours at a ball-to-material ratio of 5:1 and a rotation speed of 150rpm / min to obtain a fluorescent slurry in which all raw materials are evenly dispersed. The fluorescent slurry is placed in a high-temperature oven and dried at 70°C for 24 hours to remove the anhydrous ethanol to obtain a fluorescent dry powder. The fluorescent dry powder is crushed with a mortar and passed through a 200-mesh sieve to obtain a mixed fluorescent powder. The mixed fluorescent powder is loaded into a mold, first pressed into a green body under a pressure of 180MPa, and then sintered at a temperature 110°C higher than the full melting temperature of the glass powder particles for 90 minutes to obtain a glass fluorescent body. The glass fluorescent body is cut into thin slices, and then single-sided or double-sided polishing is obtained to obtain a glass fluorescent layer.

[0106] 2. Making a fluorescent reflective layer: coating the polished surface of the glass fluorescent layer with a bonding modification layer by sputtering, coating the fluorescent reflective layer on the side of the bonding modification layer facing away from the glass fluorescent layer by sputtering, and coating the fluorescent protective layer on the side of the fluorescent reflective layer facing away from the bonding modification layer by sputtering.

[0107] 3. Bonding the middle layer substrate: Use a dispensing method to apply silver glue on one side of the middle layer substrate and the side of the fluorescent protective layer facing away from the fluorescent reflective layer, so that the fluorescent protective layer and the surface of the middle layer substrate covered with silver glue are relatively fitted together, and bake at 200°C to solidify the silver glue to form a first thermally conductive adhesive layer between the fluorescent protective layer and the middle layer substrate.

[0108] 4. Bonding the bottom substrate: Use a dispensing method to apply organic thermally conductive adhesive on one side of the bottom substrate and the side of the middle substrate facing away from the first thermally conductive adhesive layer, so that the surfaces of the middle substrate and the bottom substrate covered with the organic thermally conductive adhesive are relatively fitted together, and are placed at room temperature for a period of time to allow the organic thermally conductive adhesive to solidify, thereby forming a second thermally conductive adhesive layer located between the middle substrate and the bottom substrate.

[0109] Comparative Example 1

[0110] The reflective wavelength conversion device of this comparative example 1 comprises a glass fluorescent layer, a fluorescent reflective layer, a first thermal conductive adhesive layer, an intermediate substrate, a second thermal conductive adhesive layer and a bottom substrate which are stacked in sequence. Except that the fluorescent powder particles and the glass powder particles are evenly mixed and then pressed into a green body at a pressure of 50 MPa and then sintered, the rest is the same as in Example 1.

[0111] Comparative Example 2

[0112] The reflective wavelength conversion device of this comparative example 2 comprises a glass fluorescent layer, a fluorescent reflective layer, a first thermal conductive adhesive layer, an intermediate substrate, a second thermal conductive adhesive layer and a bottom substrate which are stacked in sequence. Except that the fluorescent powder particles and the glass powder particles are evenly mixed and then pressed into a green body at a pressure of 250 MPa and then sintered, the rest is the same as in Example 1.

[0113] Comparative Example 3

[0114] The reflective wavelength conversion device of this comparative example 3 comprises a glass fluorescent layer, a fluorescent reflective layer, a first thermal conductive adhesive layer, an intermediate substrate, a second thermal conductive adhesive layer and a bottom substrate which are stacked in sequence. Except that the sintering temperature is 50° C. higher than the full melting temperature of the glass powder particles, the rest is the same as in Example 1.

[0115] Comparative Example 4

[0116] The reflective wavelength conversion device of this comparative example 4 comprises a glass fluorescent layer, a fluorescent reflective layer, a first thermal conductive adhesive layer, an intermediate substrate, a second thermal conductive adhesive layer and a bottom substrate stacked in sequence. Except that the sintering temperature is 150° C. higher than the full melting temperature of the glass powder particles, the rest is the same as in Example 1.

[0117] Comparative Example 5

[0118] The reflective wavelength conversion device of this comparative example 5 comprises a glass fluorescent layer, a fluorescent reflective layer, a first thermal conductive adhesive layer, an intermediate substrate, a second thermal conductive adhesive layer and a bottom substrate stacked in sequence. Except that the median diameter D50 of the fluorescent powder particles is 25 μm, the other parts are the same as those of Example 1.

[0119] Comparative Example 6

[0120] The reflective wavelength conversion device of this comparative example 6 comprises a glass fluorescent layer, a fluorescent reflective layer, a first thermal conductive adhesive layer, an intermediate substrate, a second thermal conductive adhesive layer and a bottom substrate stacked in sequence. Except that the median diameter D50 of the glass powder particles is 8 μm, the rest is the same as in Example 1.

[0121] Comparative Example 7

[0122] Comparative Example 7 includes a glass fluorescent layer, a fluorescent reflective layer, a first thermal conductive adhesive layer, an intermediate substrate, a second thermal conductive adhesive layer and a bottom substrate stacked in sequence. Except that the first thermal conductive adhesive layer is made of organic thermal conductive adhesive, the rest is the same as Example 1.

[0123] The reflective wavelength conversion devices prepared in the above embodiments and comparative examples were assembled on a laser light source system for testing. The laser light source system uses a blue laser light source with a maximum blue light output power of 120W and a laser spot size of Φ1mm. The test items include: extreme blue light power resistance, extreme luminous flux, luminous flux at a low blue light power of 10W, and aging cycle reliability test.

[0124] 1. Test of blue light power tolerance: adjust the blue light power to a lower range, then continuously increase the blue light power and observe the change in luminous flux. When the luminous flux stops increasing or even decreases, record the blue light power, which is the limit value of the blue light power tolerance of the wavelength conversion device.

[0125] 2. Luminous flux test: Light up the light source and align the light outlet of the light source with the entrance of the integrating sphere so that the light completely enters the integrating sphere. Test the luminous flux of the reflective wavelength conversion device at the extreme blue light power and the luminous flux at the low blue light power of 10w.

[0126] 3. Aging cycle reliability test: Test the change in the luminous flux of the wavelength conversion device before and after high and low temperature aging. After aging, the luminous flux drops to less than 90% of that before aging, which is the tolerable limit aging time. Calculate the number of cycles to evaluate its reliability. High and low temperature test environment: high temperature 85℃, low temperature -40℃. One cycle 2h.

[0127] Table 1 Test results of Examples 1 to 6 and Comparative Examples 1 to 7

[0128]

[0129] It can be seen from Table 1 that the reflective wavelength conversion device prepared in the present application can withstand an extreme blue light power ≥108W, an extreme luminous flux of 17040 / lm, a luminous flux of ≥1660lm at a low blue light power of 10W, and can withstand high and low temperature cycles of up to 1000 times. It can be seen that the reflective wavelength conversion device described in the present application has high wavelength conversion efficiency and good thermal conductivity.

[0130] From the comparison between Example 1 and Comparative Examples 1 and 2, it can be seen that in the process of initially pressing the phosphor particles and the glass powder particles into a blank, when the pressure is too small or too large, the ultimate blue light power, the ultimate luminous flux and the luminous flux at a low blue light power of 10W of the prepared reflective wavelength conversion device are significantly reduced. The reason may be that: when the pressing pressure is too small, the gaps between the phosphor particles and between the phosphor particles and the glass powder particles are large. In the subsequent sintering process, it is difficult for the glass melt to fill the gaps between the phosphor particles. On the one hand, this leads to a low thermal conductivity of the glass phosphor layer, and on the other hand, the surface of the glass phosphor layer is The surface polishing quality is poor, and the subsequent coating effect of the fluorescent reflective layer (silver film) is poor. The adhesion between the fluorescent reflective layer and the glass fluorescent sheet deteriorates, further resulting in the wavelength conversion device's ability to withstand blue light power deteriorating. When the pressing pressure is too large, the excessive pressure will cause the fluorescent powder particles to break, the particle size of the fluorescent powder particles is different from the original particle size, the arrangement state between the particles changes, and the fine glass powder particles cannot fill the gaps between the coarse fluorescent powder particles, resulting in the prepared glass fluorescent layer The thermal conductivity is low, the effect of the reflective silver film on the glass fluorescent layer is also deteriorated, and the wavelength conversion device's ability to withstand blue light power deteriorates.

[0131] From the comparison between Example 1 and Comparative Examples 3 and 4, it can be seen that when the phosphor particles and the glass powder particles are sintered, if the sintering temperature is too low or too high, the ultimate blue light power and the ultimate luminous flux of the prepared reflective wavelength conversion device will be significantly reduced. The reasons may be:

[0132] When the sintering temperature is too high, the glass powder melts and changes from a solid state to a flowing liquid state. The higher the temperature, the lower the viscosity of the liquid glass slurry and the stronger the fluidity. When the viscosity of the glass slurry is very low, the fluorescent particles with high volume density and the glass melt with low volume density inside the glass fluorescent layer will be separated into layers. The fluorescent particles with high density are distributed in the lower layer, and the glass melt with low density is distributed in the upper layer. Since the lower layer of the glass fluorescent layer lacks glass melt, the gaps between the fluorescent particles cannot be well filled by the glass melt, resulting in low density and low thermal conductivity of the glass fluorescent layer. The wavelength conversion device finally obtained has poor blue light power resistance.

[0133] When the sintering temperature is too low, although the glass powder particles also melt, due to the low sintering temperature, the viscosity of the glass powder particle melt is high and the fluidity of the glass slurry is poor. When the glass fluorescent layer is sintered, the driving force for the rearrangement of the fluorescent particles is insufficient, resulting in the inability of the glass melt to completely fill the gaps between the fluorescent powder particles and low thermal conductivity. In addition, the quality of the polished surface of the glass fluorescent layer deteriorates, the effect of the fluorescent reflective layer covering the polished surface deteriorates, the adhesion between the fluorescent reflective layer and the polished surface of the glass fluorescent sheet deteriorates, and the wavelength conversion device's ability to withstand blue light power deteriorates.

[0134] From the comparison between Example 1 and Comparative Example 5, it can be seen that when the particle size of the phosphor particles is too large, the ultimate blue light power and ultimate luminous flux of the prepared reflective wavelength conversion device are significantly reduced. The reason may be that when the phosphor particles are too coarse, the gaps between the phosphor particles are too large. Although the glass powder particles can fill the gaps to a certain extent, the particle size of the glass powder particles is relatively small and the particle fluidity is relatively poor. Therefore, there will be gaps in some areas that cannot be filled by the glass powder particles, resulting in uneven internal structure of the glass phosphor sheet, low thermal conductivity of the glass phosphor sheet, and poor surface polishing quality, resulting in poor adhesion between the fluorescent reflective layer and the glass fluorescent layer, increased interface thermal resistance, and poor blue light power resistance of the wavelength conversion device.

[0135] From the comparison between Example 1 and Comparative Example 6, it can be seen that when the particle size of the glass powder particles is too large, the ultimate blue light power and the ultimate luminous flux of the prepared reflective wavelength conversion device are significantly reduced. The reason may be that when the particle size of the glass powder particles is relatively large, a large number of gaps cannot be effectively filled by the glass powder particles, resulting in a relatively low density of the glass fluorescent layer and a low thermal conductivity. It also makes the polished surface quality of the glass fluorescent layer poor, the adhesion between the polished surface and the fluorescent reflective layer is low, the thermal resistance at the interface between the fluorescent reflective layer and the glass fluorescent layer increases, and the wavelength conversion device's ability to withstand blue light power is reduced.

[0136] From the comparison between Example 1 and Comparative Example 7, it can be seen that when the first thermally conductive adhesive layer uses organic thermally conductive glue, the ultimate blue light power and ultimate luminous flux of the prepared reflective wavelength conversion device are significantly reduced, and the number of high and low temperature cycles that can be withstood is also significantly reduced. The reason may be that the thermal conductivity of the organic thermally conductive glue is not enough, and the heat generated by the glass fluorescent layer during operation cannot be promptly conducted to the intermediate substrate in time, and the bonding performance of the organic thermally conductive glue is not as good as that of silver glue, which results in a loose bonding between the glass fluorescent layer and the intermediate substrate at high and low temperatures.

[0137] Obviously, the above embodiments of the present invention are merely examples for clearly illustrating the present invention, and are not intended to limit the implementation methods of the present invention. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all implementation methods here. Any modifications, equivalent substitutions, and improvements made within the spirit and principles of the present invention shall be included in the protection scope of the claims of the present invention.

Claims

1. A reflective wavelength conversion device, It is characterized in that The invention comprises a glass fluorescent layer, a fluorescent reflective layer, a first heat-conducting adhesive layer, an intermediate substrate, a second heat-conducting adhesive layer and a bottom substrate which are stacked in sequence; the glass fluorescent layer is a mixture of fluorescent powder particles and glass powder particles which is first pressed into a blank under a pressure of 80 to 200 MPa and then pressed at T m +k temperature; the median diameter D50 of the phosphor particles is 8 to 20 μm, the median diameter D50 of the glass powder particles is 1 to 6 μm; the T m It is the lowest temperature at which the glass powder particles are completely melted, 80℃≤k≤120℃.

2. The reflective wavelength conversion device according to claim 1, It is characterized in that The intermediate layer substrate is a silver sheet, the first thermally conductive adhesive layer is silver glue, and the second thermally conductive adhesive layer is an organic thermally conductive glue. The silver glue includes silver powder and epoxy resin, and the organic thermally conductive glue includes thermally conductive particles and silicone resin.

3. The reflective wavelength conversion device according to claim 1, It is characterized in that The content of the phosphor particles in the glass phosphor layer is 40-60 wt %.

4. The reflective wavelength conversion device according to any one of claims 1 to 3, It is characterized in that The material of the fluorescent reflective layer is silver, aluminum or silver-aluminum alloy; A bonding modification layer is provided on one side of the fluorescent reflective layer facing the glass fluorescent layer, and the bonding modification layer is made of aluminum oxide, silicon oxide, metal titanium or metal chromium; A fluorescent protection layer is disposed on a side of the fluorescent reflection layer facing away from the glass fluorescent layer. The material of the fluorescent protection layer is gold, nickel or platinum.

5. The reflective wavelength conversion device according to claim 4, It is characterized in that The thickness of the glass fluorescent layer is 0.07-0.2 mm; and / or The thickness of the fluorescent reflective layer is 100-1000 nm; and / or The thickness of the adhesion modification layer is 10 to 100 nm; and / or The thickness of the fluorescent protective layer is 10 to 100 nm; and / or The thickness of the intermediate substrate is 0.2-1 mm; and / or The thickness of the first thermally conductive adhesive layer is 20 to 50 μm; and / or The thickness of the second thermally conductive adhesive layer is 20-50 μm.

6. The reflective wavelength conversion device according to claim 5, It is characterized in that The thickness of the fluorescent reflection layer is 200-500 nm; and / or The thickness of the adhesion modification layer is 20 to 50 nm; and / or The thickness of the fluorescent protection layer is 20-50 nm.

7. The reflective wavelength conversion device according to any one of claims 1 to 3, It is characterized in that The bottom substrate is a heat dissipation turntable; and / or The bottom substrate is made of aluminum.

8. The reflective wavelength conversion device according to any one of claims 1 to 3, It is characterized in that The surface of the glass fluorescent layer facing the fluorescent reflective layer is set as a polished surface with a surface roughness Ra≤0.02 μm.

9. A method for preparing the reflective wavelength conversion device according to any one of claims 1 to 8, It is characterized in that include: Making a glass fluorescent layer: mixing fluorescent powder particles and glass powder particles evenly, loading them into a mold, and then pressing them into a green body at a pressure of 80 to 200 MPa, and then sintering them at a temperature 80 to 120°C higher than the full melting temperature of the glass powder particles for 30 to 90 minutes, and finally polishing them to obtain a glass fluorescent layer; Making the fluorescent reflective layer: firstly, coating the polished surface of the glass fluorescent layer with a bonding modification layer, then coating the fluorescent reflective layer on the side of the bonding modification layer facing away from the glass fluorescent layer, and finally coating the fluorescent protective layer on the side of the fluorescent reflective layer facing away from the bonding modification layer; Bonding the intermediate substrate: coating silver glue on one side of the intermediate substrate and the side of the fluorescent protective layer facing away from the fluorescent reflective layer, so that the fluorescent protective layer and the silver glue-coated surface of the intermediate substrate are relatively attached, curing the silver glue, and forming a first thermal conductive adhesive layer between the fluorescent protective layer and the intermediate substrate; Bonding the bottom substrate: coating organic thermally conductive adhesive on one side of the bottom substrate and the side of the intermediate substrate facing away from the first thermally conductive adhesive layer, so that the surfaces of the intermediate substrate and the bottom substrate coated with the organic thermally conductive adhesive are relatively fitted, and curing the organic thermally conductive adhesive to form a second thermally conductive adhesive layer between the intermediate substrate and the bottom substrate.

10. The method for preparing the reflective wavelength conversion device according to claim 9, It is characterized in that In the step of making the glass fluorescent layer, the fluorescent powder particles and the glass powder particles are evenly mixed by ball milling, and after sintering, they are first cut into thin slices and then polished; and / or In the step of making the fluorescent reflective layer, the bonding modification layer, the fluorescent reflective layer and / or the fluorescent protective layer are plated by evaporation or sputtering; and / or In the step of bonding the intermediate substrate, the silver paste is applied by screen printing, dispensing or scraping, and the silver paste is cured by baking at 200-300° C.; and / or In the step of bonding the bottom substrate, the organic thermal conductive adhesive is applied by means of steel screen printing, dispensing or scraping, and is left to cure at room temperature.

Citation Information

Patent Citations

  • Manufacturing method of wavelength conversion device

    CN104061531A

  • Wavelength conversion device, and light source system and projection system thereof

    CN104566230A

  • Fluorescent lithium silicate glass material and preparation method and applications thereof

    CN110981204A

  • Wavelength conversion device, preparation method thereof, light-emitting device and projection device

    CN111123630A

  • Wavelength conversion member and light-emitting device using same

    CN111448489A

Cited By

  • Reflection type wavelength conversion device and preparation method thereof

    CN119427849A

  • Reflective wavelength conversion device and method of manufacturing the same

    CN119427849B

  • Reflection type wavelength conversion device and preparation method thereof

    CN119820970A