Tempered glass as well as preparation method and application thereof
By masking and various processing treatments on the base glass, the density balance of the strengthened glass is controlled, the problem of increased warpage during heat treatment is solved, and its light transmittance and stability are improved.
Patent Information
- Application Number
- CN202410740153.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-07
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2044-06-07
AI Technical Summary
Strengthened glass is prone to irregular deformation during heat treatment, leading to increased warpage and affecting its light transmittance and use effect.
By masking and various processing treatments on the base glass, including radiation treatment, heat treatment and strengthening treatment, the density difference between the exposed area and the non-exposed area is controlled within 0.01g/cm3 to achieve density balance and reduce warpage.
While maintaining the difference in light transmittance between the exposed area and the non-exposed area, it significantly reduces the warpage of the tempered glass and improves its heat treatment stability and light transmittance.
Smart Images

Figure CN118754441A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of glass technology, and in particular to a tempered glass and a preparation method and use thereof. Background Art
[0002] Tempered glass is a glass material that undergoes structural changes under the irradiation of light of a specific wavelength and exhibits special properties. When exposed to ultraviolet light, the structure of the tempered glass changes, and then a crystal nucleus is generated. After heat treatment at a certain temperature, glass with specific component microcrystals will be generated in the irradiated area. The component microcrystals in the irradiated area have the characteristics of weakening the intensity of the transmitted light and shielding the light source.
[0003] After UV exposure and heat treatment, tempered glass can form a light-shielding opaque area in the exposed area. The light transmittance of this area is low, and it has light-shielding performance compared to the unexposed part of the matrix glass. Therefore, when tempered glass is used in mobile phone covers, the structural design of the tempered glass can avoid the light emitted by adjacent LEDs from interfering with each other, thereby avoiding the formation of cross-light phenomenon.
[0004] Currently, research on strengthened glass is mainly focused on reducing the light transmittance of the material in the UV exposure area. However, during the heat treatment process of the substrate glass, large-sized substrate glass is prone to irregular deformation, resulting in increased warping and reduced yield.
[0005] It should be noted that this part of the present invention only provides background technology related to the present invention and does not necessarily constitute prior art or known technology. Summary of the invention
[0006] The purpose of the present application is to provide a tempered glass, which can achieve a balance in density between an exposed area and a non-exposed area, thereby reducing the warping of the glass while increasing the difference in light transmittance between the exposed area and the non-exposed area.
[0007] In order to achieve the above objectives, this application provides the following technical solutions:
[0008] In a first aspect, a tempered glass is provided, wherein the tempered glass is obtained by processing a substrate glass; the substrate glass comprises a first region and a second region, and after masking the first region, the first region and the second region are processed to obtain a non-exposed region and an exposed region, respectively, wherein the second region is a region that has not been masked; wherein the first region of the substrate glass corresponds to the first region of the tempered glass, and the second region of the substrate glass corresponds to the second region of the tempered glass;
[0009] The processing includes radiation treatment, heat treatment and strengthening treatment;
[0010] The tempered glass comprises the exposed area and the non-exposed area, the average density ρ1 of the exposed area is greater than the average density ρ2 of the non-exposed area, and the difference Δρ between the average density ρ1 of the exposed area and the average density ρ2 of the non-exposed area is ≤0.01 g / cm 3 , preferably the difference Δρ is ≤0.005g / cm 3 .
[0011] As an optional embodiment, the processing also includes one or more of cutting, CNC processing, grinding and polishing, cleaning, 3D hot bending and polishing before the chemical strengthening.
[0012] As an optional embodiment, the average density ρ1 of the exposure area satisfies 2.0000 g / cm 3 ≤ρ1≤3.0000g / cm 3 , preferably, 2.3000 g / cm 3 ≤ρ1≤2.7000g / cm 3 , more preferably, 2.3000 g / cm 3 ≤ρ1≤2.5000g / cm 3 and / or,
[0013] The average density ρ2 of the non-exposed area satisfies 2.0000 g / cm 3 ≤ρ2≤3.0000g / cm 3 , preferably, 2.3000 g / cm 3 ≤ρ2≤2.7000g / cm 3 , more preferably, 2.4000 g / cm 3 ≤ρ2≤2.5000g / cm 3 .
[0014] As an optional embodiment, the average density ρ1 of the exposed area is 2.4714 g / cm 3 , 2.4846g / cm 3 , 2.4896g / cm 3 , 2.4872g / cm 3 , 2.4918g / cm 3 , 2.4964g / cm 3 , 2.4753g / cm 3 or 2.4832 g / cm 3 and / or,
[0015] The average density ρ2 of the non-exposed area is 2.4709 g / cm 3 , 2.4796g / cm3 , 2.4826g / cm 3 , 2.4806g / cm 3 , 2.4893g / cm 3 , 2.4932g / cm 3 , 2.4704g / cm 3 or 2.4736 g / cm 3 .
[0016] As an optional embodiment, the difference Δρ between the average density ρ1 of the exposed area and the average density ρ2 of the non-exposed area is 0.0005 g / cm 3 , 0.005g / cm 3 , 0.007g / cm 3 , 0.0066g / cm 3 , 0.0025g / cm 3 , 0.0032g / cm 3 , 0.0049g / cm 3 or 0.0096 g / cm 3 .
[0017] As an optional embodiment, the average crystal content X in the exposed area is C1 Greater than the average crystal content X in the non-exposed area C2 and / or,
[0018] In terms of mass percentage, the average crystal content X in the exposure area is C1 Satisfy 3.00%≤X C1 ≤25.00%, preferably, 4.00%≤X C1 ≤20.00%, more preferably, 4.00%≤X C1 ≤15.00%; and / or,
[0019] In terms of mass percentage, the average crystal content X in the non-exposed area is C2 Satisfy 0.50%≤X C2 ≤20.00%, preferably, 1.00%≤X C2 ≤18.00%, more preferably, 1.40%≤X C2 ≤13.00%.
[0020] As an optional embodiment, the surface CS of the tempered glass is above 300 MPa, preferably above 350 MPa.
[0021] As an optional embodiment, the CS_50 of the tempered glass is 50 MPa to 100 MPa, preferably 55 MPa to 95 MPa.
[0022] As an optional embodiment, the average crystal content X in the exposure area is measured in mass percentage. C1 is 4.27%, 7.12%, 8.31%, 7.53%, 10.23%, 14.42%, 5.42% or 6.32%; and / or,
[0023] In terms of mass percentage, the average crystal content X in the non-exposed area is C2 It is 1.49%, 5.14%, 6.35%, 5.65%, 8.54%, 12.53%, 3.56% or 4.45%.
[0024] As an optional embodiment, the composition of the strengthened glass, in terms of the mass percentage of oxides, comprises: SiO2: 65.00% to 75.00%, Al2O3: 5.00% to 10.00%, Li2O: 7.00% to 13.00%, Na2O: 2.00% to 4.00%, K2O: 2.00% to 4.00%, ZrO2: 5.00% to 7.00%, X: 0.05% to 0.80%, CeO2: 0.05% to 0.13% and Sb2O3: 0% to 0.50%;
[0025] wherein X is Ag, Cu, Au, Bi and / or their respective oxides.
[0026] As an optional embodiment, the composition of the strengthened glass, measured in terms of mass percentage of oxides, comprises:
[0027] The mass percentage of SiO2 is 66.00% to 74.50%, preferably, the mass percentage of SiO2 is 66.50% to 74.00%; and / or,
[0028] The mass percentage of Al2O3 is 5.10% to 9.70%, preferably, the mass percentage of Al2O3 is 5.20% to 9.40%; and / or,
[0029] The mass percentage of Li2O is 7.10% to 12.80%, preferably, the mass percentage of Li2O is; and / or,
[0030] The mass percentage of Na2O is 2.10% to 3.80%, preferably, the mass percentage of Na2O is 2.10% to 3.60%; and / or,
[0031] The mass percentage of K2O is 2.10% to 3.95%, preferably, the mass percentage of K2O is 2.10% to 3.90%; and / or,
[0032] The mass percentage of ZrO2 is 5.10% to 6.90%, preferably, the mass percentage of ZrO2 is 5.10% to 6.80%; and / or,
[0033] The mass percentage of Ag2O is 0.05% to 0.80%, preferably, the mass percentage of Ag2O is 0.22% to 0.48%; and / or,
[0034] The mass percentage of CeO2 is 0.05% to 0.12%, preferably, the mass percentage of CeO2 is 0.06% to 0.12%; and / or,
[0035] The mass percentage of Sb2O3 is 0.06% to 0.48%, and preferably, the mass percentage of Sb2O3 is 0.07% to 0.46%.
[0036] As an optional embodiment, the composition of the strengthened glass, measured in terms of mass percentage of oxides, comprises:
[0037] The mass percentage of SiO2 is 66.93%, 68.16%, 70.07%, 72.61%, 70.01%, 73.52%, 69.94% or 72.40%; and / or,
[0038] The mass percentage of Al2O3 is 7.19%, 9.19%, 7.86%, 5.23%, 7.87%, 7.35%, 8.36% or 5.87%; and / or,
[0039] The mass percentage of Li2O is 12.32%, 11.56%, 8.95%, 10.25%, 8.93%, 7.33%, 9.77% or 9.80%; and / or,
[0040] The mass percentage of Na2O is 3.47%, 2.14%, 3.11%, 2.66%, 3.08%, 2.41%, 2.32% or 2.84%; and / or,
[0041] The mass percentage of K2O is 3.83%, 3.02%, 3.72%, 2.42%, 3.74%, 2.15%, 3.34% or 2.34%; and / or,
[0042] The mass percentage of ZrO2 is 5.62%, 5.12%, 5.74%, 6.25%, 5.71%, 6.78%, 5.54% or 5.77%; and / or,
[0043] The mass percentage of Ag2O is 0.25%, 0.41%, 0.37%, 0.35%, 0.39%, 0.33%, 0.28% or 0.43%; and / or,
[0044] The mass percentage of CeO2 is 0.12%, 0.08%, 0.09%, 0.11%, 0.06%, 0.10% or 0.12%; and / or,
[0045] The mass percentage of Sb2O3 is 0.27%, 0.32%, 0.09%, 0.12%, 0.16%, 0.07%, 0.35% or 0.43%.
[0046] As an optional embodiment, the exposed area has a low transmittance in the infrared wavelength range, and the non-exposed area has a high transmittance in the infrared wavelength range; and / or,
[0047] At a thickness of 0.70 mm, for light of 550 nm wavelength, the transmittance T1 of the exposed area is less than 20%, preferably the transmittance T1 is less than 10%, more preferably the transmittance T1 is less than 5%, more preferably T1 is 0, and the transmittance T2 of the non-exposed area is above 90%; and / or,
[0048] At a thickness of 0.70 mm, for light of 850 nm wavelength, the transmittance T3 of the exposed area is 0% to 10%, preferably the transmittance T3 is less than 5%, and the transmittance T4 of the non-exposed area is above 90%; and / or,
[0049] At a thickness of 0.70 mm, for light with a wavelength of 1000 nm, the transmittance T5 of the exposed area is 0% to 5%, and the transmittance T6 of the non-exposed area is above 90%.
[0050] As an optional embodiment, the crystalline phase of the exposure area includes one or more of lithium metasilicate, lithium disilicate, petalite, quartz, spodumene, eucryptite, zinc oxide, Ag nanocrystals, Cu nanocrystals, Au nanocrystals, and Bi nanocrystals; and / or,
[0051] The main crystalline phase of the non-exposed area includes one or more of lithium metasilicate, lithium disilicate, petalite, quartz, spodumene, eucryptite, zinc oxide, Ag nanocrystals, Cu nanocrystals, Au nanocrystals, and Bi nanocrystals.
[0052] In a second aspect, a method for preparing the tempered glass as described above is provided, the method comprising:
[0053] Obtaining substrate glass; performing masking treatment on a first region of the substrate glass, and not performing masking treatment on a second region of the substrate glass, and then performing processing on the first region and the second region to obtain a non-exposed region and an exposed region, respectively, wherein the processing includes radiation treatment, heat treatment, and strengthening treatment; wherein the first region of the substrate glass corresponds to the first region of the strengthened glass, and the second region of the substrate glass corresponds to the second region of the strengthened glass;
[0054] The tempered glass comprises the exposed area and the non-exposed area, the average density ρ1 of the exposed area is greater than the average density ρ2 of the non-exposed area, and the difference Δρ between the average density ρ1 of the exposed area and the average density ρ2 of the non-exposed area is ≤0.01 g / cm 3 , preferably the difference Δρ≤0.005g / cm 3 .
[0055] As an optional embodiment, the average density ρ1 of the exposure area satisfies 2.0000 g / cm 3 ≤ρ1≤3.0000g / cm 3 , preferably, 2.3000 g / cm 3 ≤ρ1≤2.7000g / cm 3 , more preferably, 2.3000 g / cm 3 ≤ρ1≤2.5000g / cm 3 and / or,
[0056] The average density ρ2 of the non-exposed area satisfies 2.0000 g / cm 3 ≤ρ2≤3.0000g / cm 3 , preferably, 2.3000 g / cm 3 ≤ρ2≤2.7000g / cm 3 , more preferably, 2.4000 g / cm 3 ≤ρ2≤2.5000g / cm 3 .
[0057] As an optional embodiment, the average crystal content X in the exposed area is C1 Greater than the average crystal content X in the non-exposed area C2 and / or,
[0058] In terms of mass percentage, the average crystal content X in the exposure area is C1 Satisfy 3.00%≤X C1 ≤25.00%, preferably, 4.00%≤X C1 ≤20.00%, more preferably, 4.00%≤X C1≤15.00%; and / or,
[0059] In terms of mass percentage, the average crystal content X in the non-exposed area is C2 Satisfy 0.50%≤X C2 ≤20.00%, preferably, 1.00%≤X C2 ≤18.00%, more preferably, 1.40%≤X C2 ≤13.00%.
[0060] As an optional embodiment, the composition of the substrate glass, in terms of the mass percentage of oxides, comprises: SiO2: 65.00% to 75.00%, Al2O3: 5.00% to 10.00%, Li2O: 7.00% to 13.00%, Na2O: 2.00% to 4.00%, K2O: 2.00% to 4.00%, ZrO2: 5.00% to 7.00%, X: 0.05% to 0.80%, CeO2: 0.05% to 0.13% and Sb2O3: 0% to 0.50%;
[0061] wherein X is Ag, Cu, Au, Bi and / or their respective oxides.
[0062] As an optional embodiment, the radiation treatment comprises ultraviolet irradiation treatment.
[0063] As an optional embodiment, the wavelength of the ultraviolet irradiation treatment is 300nm to 320nm; and / or,
[0064] The intensity of the ultraviolet irradiation treatment is 240mw / cm 2 ~260mw / cm 2 .
[0065] As an optional embodiment, the masking process includes masking using masking ink and / or a mask template.
[0066] As an optional embodiment, the heat treatment includes a nucleation treatment and a crystallization treatment.
[0067] As an optional embodiment, the heating rate of the nucleation treatment is 1°C / min to 10°C / min; and / or,
[0068] The temperature of the nucleation treatment is 450°C to 600°C; and / or,
[0069] The time of the nucleation treatment is 180 min to 300 min; and / or,
[0070] The heating rate of the crystallization treatment is 1°C / min to 10°C / min; and / or,
[0071] The temperature of the crystallization treatment is 550° C. to 800° C.; and / or,
[0072] The crystallization treatment time is 30 min to 180 min.
[0073] In a third aspect, a cover glass is provided, wherein the cover glass is made of the tempered glass as described in any embodiment of the first aspect.
[0074] In a fourth aspect, an electronic device is provided, wherein the electronic device comprises the tempered glass as described in any embodiment of the first aspect.
[0075] As an optional embodiment, the electronic device includes a housing assembled on the outside of the electronic device, and the housing includes the tempered glass as described in any embodiment of the first aspect.
[0076] As an optional embodiment, the electronic device also includes a camera assembly located inside the housing, the housing includes a camera protection cover, the camera protection cover is covered on the camera assembly, and the camera protection cover includes the tempered glass as described in any embodiment of the first aspect.
[0077] In some embodiments, the housing may be partially or entirely made of tempered glass.
[0078] In a fifth aspect, a use of tempered glass in components for mobile phones, smart watches, wearable devices, camera modules or vehicles is provided, wherein the tempered glass is the tempered glass as described in any embodiment of the first aspect or the tempered glass prepared by the method for preparing the tempered glass as described in any embodiment of the second aspect.
[0079] One or more of the above technical solutions provided by the present application have the following advantages compared with the prior art:
[0080] The present invention controls the difference Δρ between the average density ρ1 of the exposed area of the tempered glass and the average density ρ2 of the non-exposed area to be less than or equal to 0.01 g / cm 3 Within the range, the density of the exposed area and the non-exposed area is balanced, thereby increasing the difference in light transmittance between the exposed area and the non-exposed area, reducing the deformation of the tempered glass during the heat treatment process, and reducing the warping of the tempered glass. BRIEF DESCRIPTION OF THE DRAWINGS
[0081] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the drawings required for use in the embodiments will be briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present application and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without paying creative work.
[0082] Figure 1 A schematic diagram of the structure of a mask provided in an embodiment of the present application.
[0083] Figure 2 A schematic diagram of the structure of a single hole in a mask provided in an embodiment of the present application.
[0084] Figure 3 A schematic diagram of the structure of the tempered glass provided in an embodiment of the present application.
[0085] Figure 4 This is a schematic diagram of the rear structure of the electronic device mentioned in the implementation mode of this application.
[0086] Figure 5 The structure of the electronic device mentioned in the embodiment of this application is schematically shown. Figure 1 .
[0087] Figure 6 The structure of the electronic device mentioned in the embodiment of this application is schematically shown. Figure 2 .
[0088] Figure 7 This is a comparison diagram of the XRD diffraction curves of the exposed area and the non-exposed area of the tempered glass provided in Example 1 of the present application.
[0089] Figure 8 This is a comparison chart of the transmittance curves of the exposed area and the non-exposed area of the tempered glass provided in Example 7 of the present application.
[0090] Figure numerals: 1-housing; 12-back cover; 13-camera protection cover; 2-camera assembly; 3-middle frame; 4-display module; 5-mask; 51-light-transmitting area; 52-light-shielding area; 6-tempered glass; 61-exposure area; 62-non-exposure area. DETAILED DESCRIPTION
[0091] The embodiments of the present application will be described in detail below in conjunction with the examples, but it will be appreciated by those skilled in the art that the following examples are only used to illustrate the present application and should not be considered as limiting the scope of the present application. In the examples, if specific conditions are not specified, they are carried out according to normal conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.
[0092] The endpoints and any values of the ranges disclosed in this article are not limited to the precise range or value, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article. Among them, the terms "optional" and "optional" all refer to being included or not (or being included or not). "And / or" as referred to herein is inclusive, for example, "A and / or B" means only A, or only B, or both A and B.
[0093] Explanation of terms and test methods:
[0094] In the present application, the main surface refers to the surface with the largest surface area, such as the upper surface or the lower surface of a horizontally placed strengthened glass sheet.
[0095] In the present application, the infrared wavelength range refers to 750nm to 1000nm.
[0096] In the present application, when light of a certain wavelength is irradiated onto the main surface of the tempered glass, the light will be reflected, absorbed and transmitted, wherein the ratio of the intensity of the transmitted part to the intensity of the incident light is the transmittance.
[0097] In the present application, the crystallized glass raw material refers to the glass raw material which has reached a certain degree of crystallinity after a period of heat treatment, but has not yet reached the target crystallinity, and can continue to crystallize to reach the target crystallinity when heated.
[0098] In this application, surface CS refers to surface compressive stress or surface compression stress. After the substrate glass is chemically strengthened, the alkali metal ions with a smaller radius on the surface are replaced by alkali metal ions with a larger radius. Due to the crowding effect of the alkali metal ions with a larger radius, compressive stress is generated on the glass surface, which is called surface compressive stress.
[0099] In the present application, CS_50 refers to the compressive stress value at a depth of 50 μm from the glass surface.
[0100] In this application, the thickness of the glass is measured by a micrometer.
[0101] In this application, the density test uses the electronic density balance SD-200L of ALFAMIRAGE of Japan to test the density of the tempered glass. In this application, the density of different positions of the same piece of glass is tested and the average density is taken.
[0102] In this application, the size specifications of the glass sheets are tested using a two-dimensional measuring machine (instrument model: MiyuMY-YXCL-4030).
[0103] In the present application, the warpage of the glass is obtained by testing with a laser thickness gauge.
[0104] The surface CS was tested using FSM-6000 manufactured by Orihara, Japan. Test conditions: light source wavelength 596 nm, SOC = 28.6 (nm / cm) / MPa, refractive index = 1.52.
[0105] CS_50 was tested using a stress meter SLP-2000 from Luceo (Japan Orihara). The test conditions were: light source wavelength 518nm, SOC = 28.6 (nm / cm) / MPa, refractive index = 1.52, exposure time: 5000usec.
[0106] In this application, the crystal phase and crystal content of the glass are confirmed by XRD test as follows:
[0107] (1) XRD test: The tempered glass of the present application was crushed and ground into a sample with a particle size of less than 75 μm, and the ground sample was tested using an X-ray diffractometer to obtain an XRD diffraction peak curve and XRD diffraction data. The X-ray diffractometer used in the present application is Shimadzu XRD-6100, the target material is copper, 2θ=10°-50°, the scanning speed is 6° / min, the operating voltage is 40 kV, and the operating current is 30 mA.
[0108] (2) Determination of crystalline phase: XRD diffraction data were analyzed using Jade software (JADE Standard 8.6) to determine the crystalline phase in the sample.
[0109] (3) Determination of crystal content (also known as crystallinity): The XRD test results (RAW format) are imported into the X-ray diffraction data Rietveld refinement software Jade for fitting and calculation to determine the crystallinity of the sample. Specifically, the ratio of the fitted crystal phase peak area to the fitted total peak area is recorded as the crystal content of the sample. This application tests the crystal content at different positions of the same piece of glass and takes the average crystal content.
[0110] In the present application, an ultraviolet-visible spectrophotometer is used to test the transmittance of the exposed area and the non-exposed area of the tempered glass of the present application. Specifically, the ultraviolet-visible spectrophotometer is used to test the transmittance of the exposed area and the non-exposed area of 5 tempered glasses of the same batch to light of different wavelengths. The average value of the transmittance measured in the exposed area and the non-exposed area of the 5 tempered glasses under light of different wavelengths is taken, and recorded as the transmittance result of the exposed area and the non-exposed area of the tempered glass under the light of the wavelength. The ultraviolet-visible spectrophotometer used in the test of the present application is Shimadzu's UV-2000 ultraviolet-visible spectrophotometer.
[0111] The present application achieves density balance in the exposed and non-exposed areas by controlling the difference between the average density of the exposed area and the average density of the non-exposed area of the tempered glass within a certain range, thereby achieving the goal of reducing the deformation of the tempered glass during the heat treatment process while expanding the difference in light transmittance between the exposed and non-exposed areas, thereby reducing the warping of the tempered glass.
[0112] In some embodiments of the present application, a tempered glass is provided, wherein the tempered glass is obtained by processing a substrate glass; the substrate glass comprises a first region and a second region, and after masking the first region, the first region and the second region are processed to obtain a non-exposed region and an exposed region, respectively, wherein the second region is a region that has not been masked, wherein the first region of the substrate glass corresponds to the first region of the tempered glass, and the second region of the substrate glass corresponds to the second region of the tempered glass; the processing comprises radiation treatment, heat treatment, and strengthening treatment;
[0113] The tempered glass comprises the exposed area and the non-exposed area, the average density ρ1 of the exposed area is greater than the average density ρ2 of the non-exposed area, and the difference Δρ between the average density ρ1 of the exposed area and the average density ρ2 of the non-exposed area is ≤0.01 g / cm 3 , preferably the difference Δρ is ≤0.005g / cm 3 .
[0114] In some embodiments of the present application, the difference Δρ between the average density ρ1 of the exposed area and the average density ρ2 of the non-exposed area is 0.0001 g / cm 3 , 0.0005g / cm 3 , 0.0010g / cm 3 , 0.0050g / cm 3 , 0.0070g / cm 3 , 0.0066g / cm 3 , 0.0025g / cm 3 , 0.0032g / cm 3 , 0.0049g / cm 3 , 0.0070g / cm 3 , 0.0080g / cm 3 , 0.0096g / cm 3 or 0.01g / cm 3 , or a value within a numerical range consisting of any two of the above specific values as endpoints, as long as the tempered glass with the desired performance of the present application can be obtained. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the tempered glass with the desired performance of the present application can be obtained.
[0115] In some embodiments of the present application, the average density ρ1 of the exposure area satisfies 2.0000 g / cm 3 ≤ρ1≤3.0000g / cm 3 , preferably, 2.3000 g / cm 3 ≤ρ1≤2.7000g / cm 3 , more preferably, 2.3000 g / cm 3 ≤ρ1≤2.5000g / cm 3 .
[0116] In some embodiments, the average density ρ1 of the exposed area is 2.1000 g / cm 3 , 2.2000g / cm 3 , 2.3000g / cm 3 , 2.4000g / cm 3 , 2.5000g / cm 3 , 2.6000g / cm 3 , 2.7000g / cm 3 , 2.8000g / cm 3 , 2.9000g / cm 3 3.0000g / cm 3 , 2.4714g / cm 3 , 2.4846g / cm 3 , 2.4896g / cm 3 , 2.4872g / cm 3 , 2.4918g / cm 3 , 2.4964g / cm 3 , 2.4753g / cm 3 or 2.4832 g / cm 3 , or a value within a numerical range consisting of any two of the above specific values as endpoints, as long as the tempered glass with the desired performance of the present application can be obtained. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the tempered glass with the desired performance of the present application can be obtained.
[0117] In some embodiments of the present application, the average density ρ2 of the non-exposed area satisfies 2.0000 g / cm 3 ≤ρ2≤3.0000g / cm 3 , preferably, 2.3000 g / cm 3 ≤ρ2≤2.7000g / cm 3 , more preferably, 2.4000 g / cm 3 ≤ρ2≤2.5000g / cm3 .
[0118] In some embodiments, the average density ρ2 of the non-exposed area is 2.1000 g / cm 3 , 2.2000g / cm 3 , 2.3000g / cm 3 , 2.4000g / cm 3 , 2.5000g / cm 3 , 2.6000g / cm 3 , 2.7000g / cm 3 , 2.8000g / cm 3 , 2.9000g / cm 3 3.0000g / cm 3 , 2.4709g / cm 3 , 2.4796g / cm 3 , 2.4826g / cm 3 , 2.4806g / cm 3 , 2.4893g / cm 3 , 2.4932g / cm 3 , 2.4704g / cm 3 , 2.4736g / cm 3 , 2.4900g / cm 3 or 2.4950g / cm 3 , or a value within a numerical range consisting of any two of the above specific values as endpoints, as long as the tempered glass with the desired performance of the present application can be obtained. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the tempered glass with the desired performance of the present application can be obtained.
[0119] In some embodiments of the present application, the average crystal content X in the exposed area of the strengthened glass C1 Greater than the average crystal content X in the non-exposed area C2 .
[0120] In some embodiments of the present application, the average crystal content X in the exposure area is, in terms of mass percentage. C1 Satisfy 3.00%≤X C1 ≤25.00%, preferably, 4.00%≤X C1 ≤20.00%, more preferably, 4.00%≤X C1 ≤15.00%.
[0121] In some embodiments, the average crystal content X in the exposed area is C1The content of the tempered glass may be 3.00%, 4.00%, 5.00%, 6.00%, 7.00%, 8.00%, 9.00%, 10.00%, 11.00%, 12.00%, 13.00%, 14.00%, 15.00%, 16.00%, 17.00%, 18.00%, 19.00%, 20.00%, 21.00%, 22.00%, 23.00%, 24.00%, 25.00%, 4.27%, 7.12%, 8.31%, 7.53%, 10.23%, 14.42%, 5.42% or 6.32%, or a value within a numerical range consisting of any two of the above specific values as endpoints, as long as the tempered glass having the desired properties of the present application can be obtained. It should be understood that, in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the tempered glass with the desired properties of the present application can be obtained.
[0122] In some embodiments of the present application, the average crystal content X in the non-exposed area is, in terms of mass percentage, C2 Satisfy 0.50%≤X C2 ≤20.00%, preferably, 1.00%≤X C2 ≤18.00%, more preferably, 1.40%≤X C2 ≤13.00%.
[0123] In some embodiments, the average crystal content X in the non-exposed area is C2 It is 0.50%, 1.00%, 2.00%, 3.00%, 4.00%, 5.00%, 6.00%, 7.00%, 8.00%, 9.00%, 10.00%, 11.00%, 12.00%, 13.00%, 14.00%, 15.00%, 16.00%, 17.00%, 18.00%, 19.00%, 20.00%, 1.49%, 5.14%, 6.35%, 5.65%, 8.54%, 12.53%, 3.56% or 4.45%.
[0124] It should be understood that the tempered glass in the present application is obtained by subjecting the substrate glass to processing including radiation treatment, heat treatment (including nucleation treatment and crystallization treatment) and strengthening treatment, and the composition of the substrate glass is the same or substantially the same as that of the tempered glass in terms of the mass percentage of oxides.
[0125] In some embodiments of the present application, the composition of the strengthened glass, in terms of mass percentage of oxides, comprises: SiO2: 65.00% to 75.00%, Al2O3: 5.00% to 10.00%, Li2O: 7.00% to 13.00%, Na2O: 2.00% to 4.00%, K2O: 2.00% to 4.00%, ZrO2: 5.00% to 7.00%, X: 0.05% to 0.80%, CeO2: 0.05% to 0.13% and Sb2O3: 0% to 0.50%;
[0126] Wherein X is Ag (silver), Cu (copper), Au (gold), Bi (bismuth) and / or their respective oxides. It should be noted that X is Ag, Cu, Au, Bi and / or their respective oxides means that X is at least one of Ag, Cu, Au, Bi, AgO, CuO, AuO and BiO.
[0127] In this application, SiO2 is a glass-forming oxide, which forms an irregular continuous network with the structural unit of silicon-oxygen tetrahedron, and is the skeleton of glass. Increasing the SiO2 content can increase the T g Temperature, so that the thermal stability is enhanced, which is conducive to inhibiting the phase separation of glass heat treatment process, but too much will lead to high viscosity of glass and high melting temperature. Reducing the SiO2 content is conducive to lowering the melting temperature of glass and inhibiting the volatilization of components in the glass melting process, but too little will lead to easy phase separation in the glass heat treatment process and T g The temperature will decrease accordingly, and the thermal stability will deteriorate. In some embodiments of the present application, in terms of the mass percentage of oxides, the mass percentage of SiO2 in the composition of the tempered glass or the base glass used to prepare the tempered glass is 65.00% to 75.00%, preferably 66.00% to 74.50%, and more preferably 66.50% to 74.00%.
[0128] In some embodiments of the present application, the content of SiO2 in the composition of the strengthened glass or the substrate glass used to prepare the strengthened glass can be 65.00%, 66.00%, 67.00%, 68.00%, 69.00%, 70.00%, 71.00%, 72.00%, 73.00%, 74.00%, 75.00%, 66.93%, 68.16%, 70.07%, 72.61%, 70.01%, 73.52%, 69.94% or 72.40%, or can be a value within a numerical range consisting of any two of the above specific values as endpoints, as long as the strengthened glass or substrate glass with the desired performance of the present application can be obtained. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the strengthened glass or substrate glass with the desired performance of the present application can be obtained.
[0129] In this application, Al2O3 is a glass network intermediate, and enters the glass network structure as [AlO4] tetrahedron. The increase of Al2O3 can improve the T g Temperature, thermal stability is enhanced, and it is beneficial to inhibit phase separation during the heat treatment of glass, but too much will increase the melting temperature of the glass. In some embodiments of the present application, the mass percentage of Al2O3 in the composition of the tempered glass or the substrate glass used to prepare the tempered glass is 5.00% to 10.00%, preferably 5.10% to 9.70%, and more preferably 5.20% to 9.40%, calculated as the mass percentage of oxides.
[0130] In some embodiments of the present application, the content of Al2O3 in the composition of the strengthened glass or the substrate glass used to prepare the strengthened glass can be 5.00%, 5.50%, 6.00%, 6.50%, 7.00%, 7.50%, 8.00%, 8.50%, 9.00%, 9.50%, 10.00%, 7.19%, 9.19%, 7.86%, 5.23%, 7.87%, 7.35%, 8.36% or 5.87%, or can be a value within a numerical range consisting of any two of the above specific values as endpoints, as long as the strengthened glass or substrate glass with the desired performance of the present application can be obtained. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the strengthened glass or substrate glass with the desired performance of the present application can be obtained.
[0131] In the present application, the alkali metal oxide Li2O is the main component of the crystals formed by the strengthened glass material, and can also reduce the chemical temperature of the glass. In some embodiments of the present application, the mass percentage of Li2O in the composition of the strengthened glass or the base glass used to prepare the strengthened glass is 7.00% to 13.00%, preferably 7.10% to 12.80%, and more preferably 7.10% to 12.80%, calculated by the mass percentage of the oxide.
[0132] In some embodiments of the present application, the content of Li2O in the composition of the strengthened glass or the substrate glass used to prepare the strengthened glass can be 7.00%, 7.50%, 8.00%, 8.50%, 9.00%, 9.50%, 10.00%, 10.50%, 11.00%, 11.50%, 12.00%, 12.50%, 13.00%, 12.32%, 11.56%, 8.95%, 10.25%, 8.93%, 7.33%, 9.77% or 9.80%, or can be a value within a numerical range consisting of any two of the above specific values as endpoints, as long as the strengthened glass or substrate glass with the desired performance of the present application can be obtained. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the strengthened glass or substrate glass with the desired performance of the present application can be obtained.
[0133] In this application, Na2O and K2O are glass network exogenous bodies and serve as co-solvents, which can reduce the melting temperature of glass. + , K + Existing situation, Na + , K + It will preferentially enter the aluminum-silicon-oxygen network to compensate for the electricity price, which maintains the lithium content in the lithium-rich area to a certain extent, making the Si / Li ratio in the lithium-rich area closer to the chemical ratio of Li2SiO3. As a result, it is shown that the crystal phase precipitated from the tempered glass containing Na2O and K2O is lithium metasilicate. However, too much Na2O and K2O will cause the glass to be easily separated and opaque during the heat treatment process, increase the light absorption coefficient, and T g The temperature also decreases, and the thermal stability deteriorates. In some embodiments of the present application, the mass percentage of Na2O in the composition of the strengthened glass or the substrate glass used to prepare the strengthened glass is 2.00% to 4.00%, preferably 2.10% to 3.80%, and more preferably 2.10% to 3.60%. In some embodiments of the present application, the mass percentage of K2O in the composition of the strengthened glass or the substrate glass used to prepare the strengthened glass is 2.00% to 4.00%, preferably 2.10% to 3.95%, and more preferably 2.10% to 3.90%.
[0134] In some embodiments of the present application, the content of Na2O in the composition of the strengthened glass or the substrate glass used to prepare the strengthened glass may be 2.00%, 2.10%, 2.20%, 2.30%, 2.40%, 2.50%, 2.60%, 2.70%, 2.80%, 2.90%, 3.00%, 3.10%, 3.20%, 3.30%, 3.40%, 3.50%, 3.60%, 3.70%, 3.80%, 3.90%, 4.00%, 3.47%, 2.14%, 3.11%, 2.66%, 3.08%, 2.41%, 2.32% or 2.84%, or may be a value within a numerical range consisting of any two of the above specific values as endpoints, as long as the strengthened glass or substrate glass having the desired performance of the present application can be obtained. It should be understood that, in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the strengthened glass or substrate glass with the desired performance of the present application can be obtained.
[0135] In some embodiments of the present application, the content of K2O in the composition of the strengthened glass or the substrate glass used to prepare the strengthened glass may be 2.00%, 2.10%, 2.20%, 2.30%, 2.40%, 2.50%, 2.60%, 2.70%, 2.80%, 2.90%, 3.00%, 3.10%, 3.20%, 3.30%, 3.40%, 3.50%, 3.60%, 3.70%, 3.80%, 3.90%, 4.00%, 3.83%, 3.02%, 3.72%, 2.42%, 3.74%, 2.15%, 3.34% or 2.34%, or may be a value within a numerical range consisting of any two of the above specific values as endpoints, as long as the strengthened glass or substrate glass having the desired performance of the present application can be obtained. It should be understood that, in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the strengthened glass or substrate glass with the desired performance of the present application can be obtained.
[0136] In the present application, ZrO2 can increase the crystal content of the glass and refine the grain size. If the ZrO2 content is too little, it will not act as a nucleating agent, while if the content is too high, it will easily deposit during the high-temperature melting process, affecting the crystallization performance of the strengthened glass material. In some embodiments of the present application, in terms of the mass percentage of the oxide, the mass percentage of ZrO2 in the composition of the strengthened glass or the substrate glass used to prepare the strengthened glass is 5.00% to 7.00%, preferably 2.10% to 3.95%, and more preferably 2.10% to 3.90%.
[0137] In some embodiments of the present application, the content of ZrO2 in the composition of the strengthened glass or the substrate glass used to prepare the strengthened glass may be 5.00%, 5.10%, 5.20%, 5.30%, 5.40%, 5.50%, 5.60%, 5.70%, 5.80%, 5.90%, 6.00%, 6.10%, 6.20%, 6.30%, 6.40%, 6.50%, 6.60%, 6.70%, 6.80%, 6.90%, 7.00%, 5.62%, 5.12%, 5.74%, 6.25%, 5.71%, 6.78%, 5.54% or 5.77%, or may be a value within the numerical range consisting of any two of the above specific values as endpoints, as long as the strengthened glass or substrate glass having the desired performance of the present application can be obtained. It should be understood that, in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the strengthened glass or substrate glass with the desired performance of the present application can be obtained.
[0138] In the present application, X is Ag, Cu, Au, Bi and / or their respective oxides. In some embodiments of the present application, in terms of the mass percentage of the oxide, the content of X in the composition of the strengthened glass or the substrate glass used to prepare the strengthened glass may be 0.05%, 0.1%, 0.20%, 0.22%, 0.24%, 0.26%, 0.28%, 0.30%, 0.32%, 0.34%, 0.36%, 0.38%, 0.40%, 0.42%, 0.44%, 0.46%, 0.48%, 0.50%, 0.60%, 0.70% or 0.80%, or may be a value within a numerical range consisting of any two of the above specific values as endpoints, as long as the strengthened glass or substrate glass with the desired performance of the present application can be obtained. It should be understood that in a specific embodiment, any of the above ranges may be combined with any other ranges, as long as the strengthened glass or substrate glass with the desired performance of the present application can be obtained.
[0139] In some embodiments of the present application, the mass percentage of Ag2O is 0.05% to 0.80%, preferably 0.21% to 0.49%, and more preferably 0.22% to 0.48%. In some embodiments of the present application, the content of Ag2O in the composition of the strengthened glass or the substrate glass used to prepare the strengthened glass may be 0.05%, 0.1%, 0.20%, 0.22%, 0.24%, 0.26%, 0.28%, 0.30%, 0.32%, 0.34%, 0.36%, 0.38%, 0.40%, 0.42%, 0.44%, 0.46%, 0.48%, 0.50%, 0.25%, 0.41%, 0.37%, 0.35%, 0.39%, 0.33%, 0.43%, 0.50%, 0.60%, 0.70% or 0.80%, calculated as a percentage by mass of the oxide, or may be a value within a numerical range consisting of any two of the above specific values as endpoints, as long as the strengthened glass or substrate glass having the desired performance of the present application can be obtained. It should be understood that, in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the strengthened glass or substrate glass with the desired performance of the present application can be obtained.
[0140] In this application, CeO2 is a photosensitizer and Ag + Provide electrons. When the CeO2 content is lower than 0.05%, it cannot provide enough electrons, resulting in too low a crystal content, increasing the light transmittance of the glass in the exposure area. When the CeO2 content is higher than 0.13%, the transmittance of the glass in the ultraviolet exposure band decreases, and the penetration depth of ultraviolet light decreases, resulting in a large increase in the density of the exposure area. In some embodiments of the present application, in terms of the mass percentage of oxide, the mass percentage of CeO2 in the composition of the strengthened glass or the substrate glass used to prepare the strengthened glass is 0.05% to 0.13%, preferably 0.05% to 0.12%, and more preferably 0.06% to 0.12%.
[0141] In some embodiments of the present application, the CeO2 content in the composition of the strengthened glass or the substrate glass used to prepare the strengthened glass can be 0.05%, 0.06%, 0.07%, 0.08%, 0.09%, 0.10%, 0.11%, 0.12% or 0.13%, or can be a value within a numerical range consisting of any two of the above specific values as endpoints, as long as the strengthened glass or substrate glass with the desired performance of the present application can be obtained. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the strengthened glass or substrate glass with the desired performance of the present application can be obtained.
[0142] In this application, Sb2O3 is a weak reducing agent and also acts as a clarifier. 3+ During the glass melting process, Ce 4+ Oxidation-reduction reaction occurs to maintain Ce 3+ In some embodiments of the present application, the mass percentage of Sb2O3 in the composition of the strengthened glass or the substrate glass used to prepare the strengthened glass is 0.05% to 0.50%, preferably 0.06% to 0.48%, and more preferably 0.07% to 0.46%, calculated as the mass percentage of the oxide.
[0143] In some embodiments of the present application, the content of Sb2O3 in the composition of the strengthened glass or the substrate glass used to prepare the strengthened glass can be 0.05%, 0.10%, 0.15%, 0.20%, 0.25%, 0.30%, 0.35%, 0.40%, 0.45%, 0.50%, 0.27%, 0.32%, 0.09%, 0.12%, 0.16%, 0.07% or 0.43%, or can be a value within a numerical range consisting of any two of the above specific values as endpoints, as long as the strengthened glass or substrate glass with the desired performance of the present application can be obtained. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the strengthened glass or substrate glass with the desired performance of the present application can be obtained.
[0144] In some embodiments of the present application, the exposure area has a low transmittance in the infrared wavelength range, and the non-exposure area has a high transmittance in the infrared wavelength range. Tempered glass that meets this transmittance can ensure that the non-exposure area has good light transmittance and a good transparent effect, while the exposure area has a lower light transmittance and a good shielding effect, and is suitable for use in cover glass that needs to shield the light source. The "infrared wavelength range" here refers to light with a wavelength of 750nm to 1000nm.
[0145] In some embodiments of the present application, at a thickness of 0.70 mm, for light of 550 nm wavelength, the transmittance T1 of the exposed area is less than 20%, preferably the transmittance T1 is less than 10%, preferably the transmittance T1 is less than 5%, preferably the transmittance T1 is 0%, and the transmittance T2 of the non-exposed area is above 90%.
[0146] In some embodiments, at a thickness of 0.70 mm, for light with a wavelength of 550 nm, the transmittance T2 of the non-exposed area may be 90.00%, 90.10%, 90.20%, 90.30%, 90.40%, 90.50%, 91.00%, 92.00%, 91.05%, 90.98%, 90.73%, 90.83%, 90.65%, 90.51%, 91.02% or 91.02%, or may be a value within a numerical range consisting of any two of the above specific values as endpoints, as long as the tempered glass with the desired performance of the present application can be obtained. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the tempered glass with the desired performance of the present application can be obtained.
[0147] In some embodiments of the present application, at a thickness of 0.70 mm, for light of 850 nm wavelength, the transmittance T3 of the exposed area is 0% to 10%, preferably less than 5%, and the transmittance T4 of the non-exposed area is above 90%.
[0148] In some embodiments, at a thickness of 0.70 mm, for light with a wavelength of 850 nm, the transmittance T4 of the non-exposed area may be 90.00%, 90.10%, 90.20%, 90.30%, 90.40%, 90.50%, 91.00%, 92.00%, 92.23%, 91.54%, 91.35%, 91.46%, 91.21%, 91.15%, 92.09% or 91.76%, or may be a value within a numerical range consisting of any two of the above specific values as endpoints, as long as the tempered glass with the desired performance of the present application can be obtained. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the tempered glass with the desired performance of the present application can be obtained.
[0149] In some embodiments, the crystalline phase of the exposed area includes one or more of lithium metasilicate, lithium disilicate, petalite, quartz, spodumene, eucryptite, zinc oxide, Ag nanocrystals, Cu nanocrystals, Au nanocrystals, and Bi nanocrystals.
[0150] In some embodiments, the crystalline phase of the non-exposed area includes one or more of lithium metasilicate, lithium disilicate, petalite, quartz, spodumene, eucryptite, zinc oxide, Ag nanocrystals, Cu nanocrystals, Au nanocrystals, and Bi nanocrystals.
[0151] In some embodiments, the strengthened glass is single-strengthened glass, double-strengthened glass, or glass-ceramics (including single-strengthened glass-ceramics, double-strengthened glass-ceramics, or multi-strengthened glass-ceramics).
[0152] In some embodiments, the substrate glass may also be plain glass, nucleated glass (eg, glass that has only been nucleated but not crystallized), or microcrystalline glass (eg, single crystallized microcrystalline glass, double crystallized microcrystalline glass, or multi-crystallized microcrystalline glass).
[0153] It can be understood that the crystallinity of the once-strengthened glass-ceramics, the twice-strengthened glass-ceramics, the multiply-strengthened glass-ceramics, the once-crystallized glass-ceramics, the twice-crystallized glass-ceramics or the multiply-crystallized glass-ceramics can all be 10%-100%.
[0154] In some embodiments of the present application, the exposed area and the non-exposed area may both be microcrystalline glass, or the exposed area may be microcrystalline glass and the non-exposed area may not be microcrystalline glass.
[0155] In some embodiments of the present application, the crystalline phase of the exposed area includes one or more of lithium metasilicate, lithium disilicate, petalite, quartz, spodumene, eucryptite, zinc oxide, Ag nanocrystals, Cu nanocrystals, Au nanocrystals, and Bi nanocrystals; the crystalline phase of the non-exposed area includes one or more of lithium metasilicate, lithium disilicate, petalite, quartz, spodumene, eucryptite, zinc oxide, Ag nanocrystals, Cu nanocrystals, Au nanocrystals, and Bi nanocrystals.
[0156] In the present application, the warpage refers to the warpage caused by the shrinkage or expansion caused by the precipitation of crystals in different regions during the heat treatment of the substrate glass. In some embodiments of the present application, the warpage is not greater than 100 μm, preferably not greater than 90 μm, and more preferably not greater than 80 μm.
[0157] In some embodiments, the warpage of the tempered glass may be 5 μm, 10 μm, 15 μm, 20 μm, 25 μm, 30 μm, 35 μm, 40 μm, 45 μm, 50 μm, 55 μm, 60 μm, 65 μm, 70 μm, 75 μm, 80 μm, 85 μm, 90 μm, 95 μm or 100 μm, or may be a value within a numerical range consisting of any two of the above specific values as endpoints, as long as the tempered glass with the desired performance of the present application can be obtained. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the tempered glass with the desired performance of the present application can be obtained.
[0158] In some embodiments of the present application, the strengthened glass is flat or curved.
[0159] In some embodiments of the present application, the thickness of the tempered glass described in the present application is not particularly limited, for example, it can be 0.4 to 2.0 mm; preferably 0.4 to 1.0 mm. In some embodiments of the present invention, the thickness of the tempered glass described in the present application can be 0.4 mm, 0.5 mm, 0.6 mm, 0.7 mm, 0.8 mm, 0.9 mm, 1.0 mm, 1.1 mm, 1.2 mm, 1.3 mm, 1.4 mm, 1.5 mm or 2.0 mm, or it can be a value within the numerical range formed by any two of the above specific values as endpoints, as long as the tempered glass with the desired performance of the present application can be obtained. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the tempered glass with the desired performance of the present application can be obtained.
[0160] In the present application, chemical strengthening can be performed by existing known methods; for example, chemical strengthening includes single-step chemical strengthening or multi-step chemical strengthening. In some embodiments of the present application, the single-step chemical strengthening uses a salt bath containing NaNO3; preferably, the content of NaNO3 is 30-100wt%; preferably, the single-step chemical strengthening uses a mixed salt bath containing NaNO3 and KNO3, preferably, the content of KNO3 in the mixed salt bath is 80-100wt%, and the content of NaNO3 is 0-20wt%.
[0161] In some embodiments of the present application, the temperature of the single-step chemical strengthening is 380-480° C., and preferably, the ion exchange time of the single-step chemical strengthening is 5-10 h.
[0162] In some embodiments of the present application, the multi-step chemical strengthening includes two steps of chemical strengthening, wherein the first step of chemical strengthening uses a salt bath containing NaNO3, preferably the content of NaNO3 is 30-100wt%; the second step of chemical strengthening uses a salt bath containing KNO3, preferably the content of KNO3 is 60-100wt%.
[0163] In some embodiments of the present application, the temperature of the first step chemical strengthening is 380-480°C, and the time of the first step chemical strengthening is preferably 3-10h; preferably, the temperature of the second step chemical strengthening is 380-480°C, and the time of the second step chemical strengthening is preferably 5-30min.
[0164] In some embodiments of the present application, the CS_50 of the tempered glass described in the present application is 50MPa to 100MPa, preferably, CS_50 is 55MPa to 95MPa. In some embodiments of the present invention, the CS_50 of the colored chemically tempered glass described in the present invention is 50MPa, 55MPa, 60MPa, 65MPa, 70MPa, 75MPa, 80MPa, 82MPa, 84MPa, 86MPa, 88MPa, 90MPa, 92MPa, 94MPa, 96MPa, 98MPa or 100MPa, or can be a value within the numerical range consisting of any two of the above specific values as endpoints, as long as the tempered glass with the desired performance of the present application can be obtained. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the tempered glass with the desired performance of the present application can be obtained.
[0165] In some embodiments of the present application, the surface CS of the tempered glass described in the present application is 300 MPa or more, preferably 350 MPa or more, and more preferably the surface CS is 300 MPa to 600 MPa. In some embodiments of the present application, the surface CS of the chemically tempered glass described in the present application is 350 MPa, 380 MPa, 400 MPa, 450 MPa, 500 MPa or 600 MPa, or can be a value within a numerical range consisting of any two of the above specific values as endpoints, as long as the tempered glass with the desired performance of the present application can be obtained. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the tempered glass with the desired performance of the present application can be obtained.
[0166] The preparation method of the tempered glass in the present application includes: obtaining a substrate glass; performing a masking treatment on a first area of the substrate glass, and not performing a masking treatment on a second area of the substrate glass, and then performing a processing treatment on the first area and the second area to obtain a non-exposed area and an exposed area respectively, wherein the processing treatment includes radiation treatment, heat treatment and tempering treatment; wherein the first area of the substrate glass corresponds to the first area of the tempered glass, and the second area of the substrate glass corresponds to the second area of the tempered glass.
[0167] In the present application, the substrate glass can be prepared by a molding method in the prior art, and the present application has no limitation on this. For example, the molding method of the substrate glass can include but is not limited to float, overflow, rolling or casting processes. For example, the substrate glass can be obtained by uniformly mixing the components according to the formula, melting and molding, cooling and annealing.
[0168] Exemplarily, each raw material (conventional industrial raw material) is configured according to the formula ratio, a clarifier is added, and then mixed for a period of time to obtain a uniform raw material mixture. The raw material mixture is placed in a platinum crucible, heated to 1250°C to 1680°C, preferably the melting temperature is 1480°C to 1680°C, and preferably kept warm for 3 to 12 hours under this temperature condition, and then poured into a molding mold for cooling and molding, preferably cooled to 750°C to 1000°C, and then placed in an annealing furnace for annealing treatment, preferably the annealing temperature is 400°C to 650°C, and the annealing time is preferably 10 to 48 hours; then cooled to room temperature with the furnace, the substrate glass can be obtained. Those skilled in the art can select the type and amount of clarifier according to needs, and they do not need to pay creative labor. Further, the clarifier may include but is not limited to one or more of sodium chloride, tin oxide, antimony oxide or arsenic oxide, and the amount of clarifier added may be 0wt%-1wt% of the total amount of each raw material.
[0169] In some embodiments of the present application, the radiation treatment method includes ultraviolet irradiation treatment, wherein the wavelength of the ultraviolet irradiation treatment is 300nm to 320nm, and the intensity of the ultraviolet irradiation treatment is 240mw / cm 2 ~260mw / cm 2 In some embodiments of the present application, before the radiation treatment, the substrate glass is subjected to a masking treatment to form the non-exposed area after the radiation treatment and the heat treatment. The masking treatment includes masking the substrate glass using a masking ink and / or a mask. The structure of the mask 5 is shown in FIG. Figure 1 , one of the 36 compound circular holes, 48 compound circular holes or 90 compound circular holes, wherein the compound circular hole has a light-transmitting area 51 of the inner diameter and a light-shielding area 52 other than the inner diameter, and the schematic diagram of the compound circular hole structure is shown in Figure 2 As shown, the structure of the corresponding strengthened glass 6 is shown in FIG. Figure 3 The position corresponding to the light-transmitting area 51 forms an exposure area 61, and the position corresponding to the light-shielding area 52 forms a non-exposure area 62.
[0170] In some embodiments of the present application, the heat treatment process of the substrate glass may include a nucleation treatment and / or a crystallization treatment, preferably a nucleation treatment and a crystallization treatment. In some embodiments, the crystallization treatment includes a one-step crystallization treatment or a multi-step crystallization treatment. In some embodiments, in order to prepare a curved tempered glass, a two-step crystallization treatment may be used. When a two-step crystallization treatment is used, the second step of the crystallization treatment is to place the crystallized glass raw material obtained by the first step of the crystallization treatment into a hot bending mold, heat it to the crystallization temperature and perform a 3D hot bending forming process.
[0171] In some embodiments of the present application, in order to obtain the desired physical and chemical properties of the tempered glass, when the substrate glass is heat treated, a one-step heat treatment may be performed, or a two-step or multi-step heat treatment may be performed. If a one-step heat treatment is performed, it means that a nucleation treatment (i.e., nucleation treatment) is not performed separately, and a one-step heating is performed directly, and nucleation and target crystal growth are performed at the temperature reached in the one-step heating process, which can be understood as a direct crystallization treatment. If a two-step heat treatment is performed, it means that a two-step heating process is performed, first a nucleation treatment, i.e., nucleation treatment, is performed, and then a target crystal growth treatment, i.e., crystallization treatment, is performed.
[0172] In order to make the tempered glass precipitate the desired crystalline phase and obtain the desired physical and chemical properties, further, the temperature of the nucleation treatment can be 450℃~600℃, and the time of the nucleation treatment can be 180min~300min, preferably 210min~270min; the temperature of the crystallization treatment can be 550℃~800℃, and the time of the crystallization treatment can be 30min~180min, preferably 60min~120min. When performing heat treatment, it is preferred to control the heating rate to 1℃ / min~10℃ / min, and more preferably the heating rate is 10℃ / min. Among them, the temperature of the nucleation treatment refers to the temperature at which the crystal nucleus can be formed. The temperature of the crystallization treatment refers to the temperature at which the target crystal is suitable for controllable growth.
[0173] Before and / or after the heat treatment, those skilled in the art may also perform other conventional steps to obtain a strengthened glass sample that meets the required specifications or requirements, such as shaping, cutting (such as cutting with a multi-wire saw), CNC machining (computer numerical control, i.e., CNC machine tools), thinning, or polishing. In the present application, there is no limitation on the size of the substrate glass or strengthened glass sample, such as 50 mm×50 mm×1.0 mm, 300 mm×120 mm×0.7 mm, etc.
[0174] The tempered glass with excellent performance provided in the present application can be used in electronic devices, including but not limited to mobile phones, tablet computers, handheld game consoles, portable digital devices (such as digital cameras), smart homes, smart wearables (such as smart bracelets, smart watches, smart glasses), and can also be used in vehicles, aircraft or aircraft, and can also be used in any glass device that requires tempered glass. For example, it can be used for the back cover glass of mobile phones, the back cover glass of smart watches, etc.; for example, it can be used for the windshield of vehicles, aircraft or aircraft, such as the front windshield or the side windshield. For example, it can be used for work surfaces, other surfaces, appliance doors, floor tiles, wall panels or storage containers. Other surfaces can include but are not limited to exterior wall surfaces, stair tread surfaces, column veneers or counter surfaces, etc., and storage containers can include but are not limited to cups, plates, medicine bottles or beverage bottles, etc.
[0175] For example, the tempered glass with excellent performance provided in the present application can be used to manufacture glass devices. The glass devices referred to here can be regular or irregular, and those skilled in the art can manufacture them according to requirements.
[0176] For example, the tempered glass with excellent performance provided by the present application can be used to manufacture cover glass, and the cover glass can be a back cover or camera protection cover of an electronic device such as a mobile phone. For example, the tempered glass with excellent performance provided by the present application can be used in electronic devices. Figure 4 , Figure 5 and Figure 6 In some embodiments of the present application, an electronic device is provided, which may be a mobile phone (such as Figure 5 As shown), it can also be a tablet computer, a smart wearable device (such as Figure 6 As shown, the tempered glass can be used as the back cover of a smart watch) and other electronic products, the electronic device includes a housing 1 assembled on the outside of the electronic device, the housing 1 includes a display screen cover assembled on the front side and a back cover 12 assembled on the back side, the display screen cover is covered on the display module 4, wherein the back cover 12 adopts the aforementioned tempered glass. In the present application, the back cover 12 may be entirely made of the aforementioned tempered glass, or only partially made of the aforementioned tempered glass. In the present application, the display screen may be a touch display screen, and the display screen cover may be a protective cover provided on the touch display screen. In the present application, the back cover 12 may cover only the back side (and the side away from the display screen) of the electronic device, or may cover both the back side and the side frame of the electronic device, optionally, the back cover 12 may cover all the side frames around the electronic device, or may cover part of the side frames.
[0177] In some implementation modes of the present application, Figure 4 As shown, the electronic device also includes a camera assembly 2 located inside the housing 1, and the housing 1 may include a camera protection cover 13, and the camera protection cover 13 is covered on the camera assembly 2 to protect the camera assembly 2, and the camera protection cover 13 adopts the aforementioned tempered glass. In the present application, the camera protection cover 13 may be partially made of the aforementioned tempered glass, or may be entirely made of the aforementioned tempered glass. In the present application, the setting position of the camera protection cover 13 is determined according to the setting position of the camera assembly 2, and may be located on the front side of the electronic device, or may be located on the back side of the electronic device. In some embodiments of the present application, the camera protection cover 13 may be a separate structure from the back cover 12. In other embodiments of the present application, the camera protection cover 13 may also be an integrated structure with the back cover 12.
[0178] In some embodiments of the present application, Figure 5As shown, the electronic device may further include a middle frame 3 located between the display module 4 and the housing 1 , and the middle frame 3 may include the aforementioned tempered glass.
[0179] In the embodiments of the present application, the back cover plate and the camera protection cover plate in the electronic device may be either one of them using the aforementioned tempered glass, or both of them may be using the aforementioned tempered glass.
[0180] The technical solution of the present application is further described in detail below in conjunction with the embodiments. The embodiments of the present application described in detail below are exemplary and are only used to explain the present application, and cannot be understood as limiting the present application.
[0181] Example 1
[0182] A tempered glass, the preparation process of which is as follows:
[0183] (1) Preparation of substrate glass:
[0184] The raw materials (conventional industrial raw materials) were prepared according to the proportions of the components in Table 1. The total mass of the prepared raw materials was 5000 g. 10 g of clarifier sodium chloride (NaCl) was added to the prepared raw materials, and then mixed with a V-type mixer for 30 minutes to obtain a uniform raw material mixture.
[0185] The raw material mixture is transferred to a melting furnace and then melted at 1500°C. The melt is stirred with a platinum stirring rod for 12 hours, and then pulled into shape and continuously drawn into glass bricks of the required specifications. The glass bricks are quickly placed in an annealing furnace at 450°C for 5 hours, and then naturally cooled to room temperature to obtain the base glass bricks.
[0186] The obtained substrate glass bricks are subjected to cold working treatments of cutting, CNC processing (the CNC equipment model used in this application is: RCG500S), and polishing in sequence, and substrate glass samples that meet the required specifications and requirements can be obtained. In Examples 1 to 8 of this application, the substrate glass sample bricks are subjected to the aforementioned cold working treatment to produce glass substrates with a size of 300 mm×120 mm×0.7 mm.
[0187] (2) Preparation of tempered glass: The glass substrate was ultrasonically cleaned in deionized water, anhydrous ethanol, propanol and deionized water for 10 min in sequence, and then dried in a drying oven; the glass substrate and the mask were fixed together and placed horizontally in a predetermined line of ultraviolet parallel light spot, with the mask on the top and the glass substrate on the bottom. The wavelength of ultraviolet irradiation was 310 nm and the irradiation intensity was 250 mw / cm 2, the exposure time is 10min; the glass substrate is separated from the mask after exposure; and then heat-treated according to the heat treatment process in Table 1 to obtain a crystallized glass. The mask used has 90 composite circular holes, and the composite circular holes have a light-transmitting area and a light-shielding area, and the structure is as follows Figure 2 The heat treatment includes nucleation treatment and crystallization treatment, and the heating rates of nucleation treatment and crystallization treatment are both 10°C / min. The crystallized glass sample obtained above is treated according to a two-step chemical strengthening process to obtain a strengthened glass. The specific two-step chemical strengthening process conditions are described in Table 1.
[0188] The warpage of the test substrate glass produced during the heat treatment process is shown in Table 1.
[0189] The tempered glass sample obtained in Example 1 was tested as follows:
[0190] The crystal content, density and transmittance (under 550nm, 850nm and 1000nm wavelength light) of the exposed area and the non-exposed area of the strengthened glass sample were tested respectively, and the results are shown in Table 1.
[0191] Embodiment 2 to Embodiment 8
[0192] The above methods are respectively carried out with reference to Example 1, except that the raw material composition, different process parameters and corresponding test results of each example are shown in the table.
[0193] Among them, the XRD patterns of the exposed area and the non-exposed area of the tempered glass of Example 1 are as follows: Figure 7 As shown in the figure, it can be seen that the crystal phase structure of the strengthened glass contains lithium metasilicate.
[0194] The transmittance curves of the exposed area and the non-exposed area of the tempered glass of Example 7 are as follows: Figure 8 As shown in the figure, it can be seen that the exposed area of the tempered glass has a low transmittance in the infrared wavelength range, and the non-exposed area of the tempered glass has a high transmittance in the infrared wavelength range.
[0195] Table 1
[0196]
[0197]
[0198]
[0199] From the embodiment of Table 1 above, it can be seen that in each embodiment of the present application, the difference Δρ between the average density ρ1 of the exposed area of the tempered glass and the average density ρ2 of the non-exposed area is less than or equal to 0.01 g / cm 3range, so that the tempered glass has a lower warpage, below 80μm.
[0200] The above description is only a specific embodiment of the present application and is not intended to limit the present application. For those skilled in the art, the present application may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present application shall be included in the protection scope of the present application.
Claims
1. A tempered glass, characterized in that: The strengthened glass is obtained by processing a substrate glass; the substrate glass comprises a first region and a second region, the first region is subjected to masking treatment, and then the first region and the second region are subjected to processing treatment to obtain a non-exposed region and an exposed region, respectively, wherein the second region is a region that is not subjected to masking treatment, wherein the first region of the substrate glass corresponds to the first region of the strengthened glass, and the second region of the substrate glass corresponds to the second region of the strengthened glass; The processing includes radiation treatment, heat treatment and strengthening treatment; The tempered glass comprises the exposed area and the non-exposed area, the average density ρ1 of the exposed area is greater than the average density ρ2 of the non-exposed area, and the difference Δρ between the average density ρ1 of the exposed area and the average density ρ2 of the non-exposed area is ≤0.01 g / cm 3 , preferably the difference Δρ is ≤0.005g / cm 3 .
2. The tempered glass according to claim 1, wherein: The processing also includes one or more of cutting, CNC processing, grinding and polishing, cleaning, 3D hot bending and polishing before the chemical strengthening.
3. The tempered glass according to any one of claims 1 to 2, characterized in that: The masking process includes masking using masking ink and / or a reticle.
4. The tempered glass according to any one of claims 1 to 3, characterized in that: The radiation treatment method includes ultraviolet irradiation treatment.
5. The tempered glass according to claim 4, wherein: The wavelength of the ultraviolet irradiation treatment is 300nm-320nm; and / or the intensity of the ultraviolet irradiation treatment is 240mw / cm 2 ~260mw / cm 2 .
6. The tempered glass according to any one of claims 1 to 5, characterized in that: The heat treatment includes a nucleation treatment and a crystallization treatment.
7. The tempered glass according to claim 6, wherein: The heating rate of the nucleation treatment is 1°C / min to 10°C / min; and / or, The temperature of the nucleation treatment is 450°C to 600°C; and / or, The time of the nucleation treatment is 180 min to 300 min; and / or, The heating rate of the crystallization treatment is 1°C / min to 10°C / min; and / or, The temperature of the crystallization treatment is 550° C. to 800° C.; and / or, The crystallization treatment time is 30 min to 180 min.
8. The tempered glass according to any one of claims 1 to 7, characterized in that: The difference Δρ between the average density ρ1 of the exposed area and the average density ρ2 of the non-exposed area is 0.0005 g / cm 3 , 0.005g / cm 3 , 0.007g / cm 3 , 0.0066g / cm 3 , 0.0025g / cm 3 , 0.0032g / cm 3 , 0.0049g / cm 3 or 0.0096 g / cm 3 .
9. The tempered glass according to any one of claims 1 to 8, characterized in that: The average density ρ1 of the exposure area satisfies 2.0000 g / cm 3 ≤ρ1≤3.0000g / cm 3 , preferably, 2.3000 g / cm 3 ≤ρ1≤2.7000g / cm 3 , more preferably, 2.3000 g / cm 3 ≤ρ1≤2.5000g / cm 3 and / or, The average density ρ2 of the non-exposed area satisfies 2.0000 g / cm 3 ≤ρ2≤3.0000g / cm 3 , preferably, 2.3000 g / cm 3 ≤ρ2≤2.7000g / cm 3 , more preferably, 2.4000 g / cm 3 ≤ρ2≤2.5000g / cm 3 .
10. The tempered glass according to any one of claims 1 to 9, characterized in that: The average density ρ1 of the exposure area is 2.4714 g / cm 3 , 2.4846g / cm 3 , 2.4896g / cm 3 , 2.4872g / cm 3 , 2.4918g / cm 3 , 2.4964g / cm 3 , 2.4753g / cm 3 or 2.4832 g / cm 3 ; and / or The average density ρ2 of the non-exposed area is 2.4709 g / cm 3 , 2.4796g / cm 3 , 2.4826g / cm 3 , 2.4806g / cm 3 , 2.4893g / cm 3 , 2.4932g / cm 3 , 2.4704g / cm 3 or 2.4736 g / cm 3 .
11. The tempered glass according to any one of claims 1 to 10, characterized in that: The average crystal content X in the exposure area C1 Greater than the average crystal content X in the non-exposed area C2 and / or, In terms of mass percentage, the average crystal content X in the exposure area is C1 Satisfy 3.00%≤X C1 ≤25.00%, preferably, 4.00%≤X C1 ≤20.00%, more preferably, 4.00%≤X C1 ≤15.00%; and / or, In terms of mass percentage, the average crystal content X in the non-exposed area is C2 Satisfy 0.50%≤X C2 ≤20.00%, preferably, 1.00%≤X C2 ≤18.00%, more preferably, 1.40%≤X C2 ≤13.00%.
12. The tempered glass according to any one of claims 1 to 11, characterized in that: In terms of mass percentage, the average crystal content X in the exposure area is C1 is 4.27%, 7.12%, 8.31%, 7.53%, 10.23%, 14.42%, 5.42% or 6.32%; and / or, In terms of mass percentage, the average crystal content X in the non-exposed area is C2 It is 1.49%, 5.14%, 6.35%, 5.65%, 8.54%, 12.53%, 3.56% or 4.45%.
13. The tempered glass according to any one of claims 1 to 12, characterized in that: The composition of the tempered glass, in terms of percentage by mass of oxides, comprises: SiO2: 65.00% to 75.00%, Al2O3: 5.00% to 10.00%, Li2O: 7.00% to 13.00%, Na2O: 2.00% to 4.00%, K2O: 2.00% to 4.00%, ZrO2: 5.00% to 7.00%, X: 0.05% to 0.80%, CeO2: 0.05% to 0.13% and Sb2O3: 0% to 0.50%; wherein X is Ag, Cu, Au, Bi and / or their respective oxides.
14. The tempered glass according to any one of claims 1 to 13, characterized in that: The composition of the tempered glass, measured in percentage by mass of oxides, comprises: The mass percentage of SiO2 is 66.00% to 74.50%, preferably, the mass percentage of SiO2 is 66.50% to 74.00%; and / or, The mass percentage of Al2O3 is 5.10% to 9.70%, preferably, the mass percentage of Al2O3 is 5.20% to 9.40%; and / or, The mass percentage of Li2O is 7.10% to 12.80%, preferably, the mass percentage of Li2O is 7.20% to 12.60%; and / or, The mass percentage of Na2O is 2.10% to 3.80%, preferably, the mass percentage of Na2O is 2.10% to 3.60%; and / or, The mass percentage of K2O is 2.10% to 3.95%, preferably, the mass percentage of K2O is 2.10% to 3.90%; and / or, The mass percentage of ZrO2 is 5.10% to 6.90%, preferably, the mass percentage of ZrO2 is 5.10% to 6.80%; and / or, The mass percentage of Ag2O is 0.05% to 0.80%, preferably, the mass percentage of Ag2O is 0.22% to 0.48%; and / or, The mass percentage of CeO2 is 0.05% to 0.12%, preferably, the mass percentage of CeO2 is 0.06% to 0.12%; and / or, The mass percentage of Sb2O3 is 0.06% to 0.48%, and preferably, the mass percentage of Sb2O3 is 0.07% to 0.46%.
15. The tempered glass according to any one of claims 1 to 14, characterized in that: The composition of the tempered glass, measured in percentage by mass of oxides, comprises: The mass percentage of SiO2 is 66.93%, 68.16%, 70.07%, 72.61%, 70.01%, 73.52%, 69.94% or 72.40%; and / or, The mass percentage of Al2O3 is 7.19%, 9.19%, 7.86%, 5.23%, 7.87%, 7.35%, 8.36% or 5.87%; and / or, The mass percentage of Li2O is 12.32%, 11.56%, 8.95%, 10.25%, 8.93%, 7.33%, 9.77% or 9.80%; and / or, The mass percentage of Na2O is 3.47%, 2.14%, 3.11%, 2.66%, 3.08%, 2.41%, 2.32% or 2.84%; and / or, The mass percentage of K2O is 3.83%, 3.02%, 3.72%, 2.42%, 3.74%, 2.15%, 3.34% or 2.34%; and / or, The mass percentage of ZrO2 is 5.62%, 5.12%, 5.74%, 6.25%, 5.71%, 6.78%, 5.54% or 5.77%; and / or, The mass percentage of Ag2O is 0.25%, 0.41%, 0.37%, 0.35%, 0.39%, 0.33%, 0.28% or 0.43%; and / or, The mass percentage of CeO2 is 0.12%, 0.08%, 0.09%, 0.11%, 0.06%, 0.10% or 0.12%; and / or, The mass percentage of Sb2O3 is 0.27%, 0.32%, 0.09%, 0.12%, 0.16%, 0.07%, 0.35% or 0.43%.
16. The tempered glass according to any one of claims 1 to 15, characterized in that: The surface CS of the tempered glass is greater than or equal to 300 MPa, and preferably greater than or equal to 350 MPa.
17. The tempered glass according to any one of claims 1 to 16, characterized in that: The CS_50 of the tempered glass is 50 MPa to 100 MPa, preferably 55 MPa to 95 MPa.
18. The tempered glass according to any one of claims 1 to 17, characterized in that: The exposed area has a low transmittance in the infrared wavelength range, and the non-exposed area has a high transmittance in the infrared wavelength range; and / or, At a thickness of 0.70 mm, for light of 550 nm wavelength, the transmittance T1 of the exposed area is less than 20%, preferably the transmittance T1 is less than 10%, preferably the transmittance T1 is less than 5%, and preferably the transmittance T1 is 0; the transmittance T2 of the non-exposed area is above 90%; and / or, At a thickness of 0.70 mm, for light with a wavelength of 850 nm, the transmittance T3 of the exposed area is 0% to 10%, preferably less than 5%, and the transmittance T4 of the non-exposed area is above 90%. At a thickness of 0.70 mm, for light with a wavelength of 1000 nm, the transmittance T5 of the exposed area is 0% to 5%, and the transmittance T6 of the non-exposed area is above 90%.
19. The tempered glass according to any one of claims 1 to 18, characterized in that: The crystalline phase of the exposure area includes one or more of lithium metasilicate, lithium disilicate, petalite, quartz, spodumene, eucryptite, zinc oxide, Ag nanocrystals, Cu nanocrystals, Au nanocrystals, and Bi nanocrystals; and / or, The crystalline phase of the non-exposed area includes one or more of lithium metasilicate, lithium disilicate, petalite, quartz, spodumene, eucryptite, zinc oxide, Ag nanocrystals, Cu nanocrystals, Au nanocrystals, and Bi nanocrystals.
20. A method for preparing a tempered glass according to any one of claims 1 to 19, characterized in that: The method comprises: Obtaining substrate glass; performing masking treatment on a first region of the substrate glass, and not performing masking treatment on a second region of the substrate glass, and then performing processing on the first region and the second region to obtain a non-exposed region and an exposed region, respectively, wherein the processing includes radiation treatment, heat treatment, and strengthening treatment; wherein the first region of the substrate glass corresponds to the first region of the strengthened glass, and the second region of the substrate glass corresponds to the second region of the strengthened glass; The average density ρ1 of the exposed area is greater than the average density ρ2 of the non-exposed area, and the difference Δρ between the average density ρ1 of the exposed area and the average density ρ2 of the non-exposed area is ≤0.01 g / cm 3 , preferably the difference Δρ≤0.005g / cm 3 .
21. The method for preparing tempered glass according to claim 20, characterized in that: The average density ρ1 of the exposure area satisfies 2.0000 g / cm 3 ≤ρ1≤3.0000g / cm 3 , preferably, 2.3000 g / cm 3 ≤ρ1≤2.7000g / cm 3 , more preferably, 2.3000 g / cm 3 ≤ρ1≤2.5000g / cm 3 and / or, The average density ρ2 of the non-exposed area satisfies 2.0000 g / cm 3 ≤ρ2≤3.0000g / cm 3 , preferably, 2.3000 g / cm 3 ≤ρ2≤2.7000g / cm 3 , more preferably, 2.4000 g / cm 3 ≤ρ2≤2.5000g / cm 3 .
22. The method for preparing a tempered glass according to any one of claims 20 to 21, characterized in that: The average crystal content X in the exposure area C1 Greater than the average crystal content X in the non-exposed area C2 and / or, In terms of mass percentage, the average crystal content X in the exposure area is C1 Satisfy 3.00%≤X C1 ≤25.00%, preferably, 4.00%≤X C1 ≤20.00%, more preferably, 4.00%≤X C1 ≤15.00%; and / or, In terms of mass percentage, the average crystal content X in the non-exposed area is C2 Satisfy 0.50%≤X C2 ≤20.00%, preferably, 1.00%≤X C2 ≤18.00%, more preferably, 1.40%≤X C2 ≤13.00%.
23. The method for preparing a tempered glass according to any one of claims 20 to 22, characterized in that: The composition of the substrate glass, in terms of percentage by mass of oxides, comprises: SiO2: 65.00% to 75.00%, Al2O3: 5.00% to 10.00%, Li2O: 7.00% to 13.00%, Na2O: 2.00% to 4.00%, K2O: 2.00% to 4.00%, ZrO2: 5.00% to 7.00%, X: 0.05% to 0.80%, CeO2: 0.05% to 0.13% and Sb2O3: 0% to 0.50%; wherein X is Ag, Cu, Au, Bi and / or their respective oxides.
24. A cover glass, characterized in that: The cover glass is made of the tempered glass according to any one of claims 1 to 19 or the tempered glass prepared by the preparation method according to any one of claims 20 to 23.
25. An electronic device, characterized in that: The electronic device comprises the tempered glass according to any one of claims 1 to 19 or the tempered glass prepared by the preparation method according to any one of claims 20 to 23.
26. The electronic device according to claim 25, characterized in that: The electronic device comprises a housing, wherein the housing comprises the tempered glass according to any one of claims 1 to 19 or the tempered glass prepared by the preparation method according to any one of claims 20 to 23.
27. The electronic device according to claim 26, characterized in that: The electronic device also includes a camera assembly, the housing includes a camera protection cover, the camera protection cover is covered on the camera assembly, and the camera protection cover includes the tempered glass described in any one of claims 1-19 or the tempered glass prepared by the preparation method described in any one of claims 20-23.
28. Use of the tempered glass according to any one of claims 1 to 19 or the tempered glass prepared by the preparation method according to any one of claims 20 to 23 in components for mobile phones, smart watches, wearable devices, camera modules or vehicles.
Citation Information
Patent Citations
Shell structure, shell, electronic equipment and preparation method of shell structure
CN116406106A
Glass for optical construction elements consists of lithium-aluminum silicate glass with density of at least 2.4 grams per cubic centimeter
DE102008007871A1
Variably translucent glass-ceramic article and method for making
US5173453A
Cited By
Photosensitive microcrystalline glass, preparation method thereof and chemically strengthened photosensitive microcrystalline glass
CN122212483A
Photosensitive glass-ceramics and method for preparing the same, chemically strengthened photosensitive glass-ceramics
CN122212483B
Photosensitive glass, preparation method thereof, reinforced photosensitive glass and application
CN122380651A
A photosensitive glass, its preparation method, a strengthened photosensitive glass, and its applications.
CN122380651B
Photosensitive glass, preparation method thereof, reinforced photosensitive glass and application
CN122464609A