High-quality TC4 titanium alloy disc round wire blank for fastener as well as preparation and application of high-quality TC4 titanium alloy disc round wire blank

Through ingot preparation and multiple forging processes, the content of Fe and O elements and the amount of forging deformation are controlled to prepare a fine and uniform equiaxed α+β dual-phase structure, which solves the problem of poor quality of domestic TC4 titanium alloy fastener materials. , achieving high-quality microstructure and strength improvement.

CN118756079APending Publication Date: 2024-10-11INST OF METAL RESEARCH - CHINESE ACAD OF SCI
View PDF 0 Cites 6 Cited by

Patent Information

Application Number
CN202410792158.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-19
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

The material quality of domestically produced TC4 titanium alloy fasteners is poor. The traditional thermal processing process results in poor microstructure quality, making it difficult to achieve the A1 quality of the TC4 titanium alloy wire rod specifications for aerospace fasteners.

Method used

The steps of ingot preparation, billet forging, precision forging, continuous rolling and annealing are used to control the content of Fe and O elements and the amount of forging deformation. Through vacuum consumable arc melting, induction heating and air-cooling annealing, fine and uniform steel is produced. Axial α+β biphasic organization.

Benefits of technology

The high-quality microstructure of the TC4 titanium alloy wire blank has been achieved, reaching the A1 grade quality of the TC4 titanium alloy wire rod specification for aviation fasteners, meeting the requirements of TC4 titanium alloy material for fasteners, and improving the strength and plasticity of the material. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118756079A_ABST
    Figure CN118756079A_ABST
Patent Text Reader

Abstract

The invention relates to a preparation method of a high-quality microscopic structure TC4 titanium alloy large-piece-weight disc round wire billet for a fastener, which comprises the following steps: firstly, obtaining a TC4 titanium alloy cast ingot with the diameter of 500-700mm, then cogging and forging the TC4 titanium alloy cast ingot at the temperature of 1000-1200 DEG C to form a bar billet with the diameter of 170mm, then precisely forging the TC4 titanium alloy bar billet at the temperature of 930-960 DEG C to form a bar billet with the diameter of 100mm, and then continuously rolling the TC4 titanium alloy bar billet at the temperature of 880-940 DEG C to obtain the high-quality microscopic structure TC4 titanium alloy large-piece-weight disc round wire billet. The preparation method comprises the following steps of: rolling into a large-disc round wire with the diameter of 7.5-15mm, and then annealing at 760-800 DEG C, so that the annealed alloy structure is a fine, uniform and equiaxial alpha + beta double-phase structure, the A1-grade quality required by the microscopic structure of the TC4 titanium alloy wire bar specification for aviation fasteners is achieved, and the requirement of the TC4 titanium alloy material for fasteners is met.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of titanium alloy wire processing for fasteners, and in particular to a method for preparing a high-quality microstructure TC4 titanium alloy large single-weight disc round wire blank for fasteners. Background Art

[0002] TC4 titanium alloy is an α+β type titanium alloy with a nominal composition of Ti-6Al-4V. It has the characteristics of simple composition, low cost, excellent strength and fatigue resistance. More than 95% of titanium alloy fasteners in developed countries in Europe and America are made of TC4 titanium alloy. However, there is a gap between the quality of domestic titanium alloy fasteners and developed countries in Europe and America, and most of the materials for high-quality titanium alloy fasteners still rely on imports.

[0003] At present, most of the TC4 titanium alloy wires used for domestic fasteners are processed in small batches, with a weight of less than 30 kg, and the consistency of wire product quality is difficult to guarantee. In addition, in the traditional hot working process, the alloy needs to be heated multiple times, resulting in poor microstructure quality of the product, making it difficult to achieve the A1 grade quality required by the microstructure of the "TC4 Titanium Alloy Wire and Rod Specification for Aviation Fasteners".

[0004] Therefore, it is of great engineering significance to study the preparation process of large single weight disc TC4 titanium alloy wire billet and prepare large single weight disc TC4 titanium alloy wire billet with high quality microstructure. Summary of the invention

[0005] Based on this, it is necessary to provide a method for preparing large single-weight round wire blanks of TC4 titanium alloy with high-quality microstructure for fasteners in response to the above-mentioned technical problems. The prepared TC4 titanium alloy wire blanks have fine and uniform microstructure, reaching the A1 grade quality required by the microstructure of the "Specification for TC4 Titanium Alloy Wire Rods for Aerospace Fasteners", and meeting the requirements of TC4 titanium alloy materials for fasteners.

[0006] The present invention provides a method for preparing a high-quality microstructure TC4 titanium alloy large single-weight round wire blank for fasteners, comprising the following steps:

[0007] Step 1, ingot preparation, sponge titanium, aluminum beans, aluminum-vanadium master alloy, reduced iron powder and carbon powder are mixed and pressed into electrodes, and subjected to three vacuum consumable arc melting to obtain a TC4 titanium alloy ingot with a diameter of 500-700 mm, wherein the TC4 titanium alloy ingot is composed of the following elements in weight percentage: Al 5.50-6.75%, V 3.50-4.50%, Fe≤0.30%, O≤0.20%, C≤0.08%, N≤0.05%, H≤0.015%, other single impurity elements (including Cu, Mg, Ca, Si, etc.) ≤0.10%, the sum of other impurity elements ≤0.40%, and the balance is Ti;

[0008] Step 2: Forging the blank, heating to 900℃ and loading into the furnace, raising the temperature to 1000-1200℃, keeping the temperature for 2-3 hours, taking it out of the furnace and stretching it on the free forging machine. After stretching, the diameter of the blank is 165-175mm, and the surface defects are repaired;

[0009] Step 3: Finish forging: heat to 750℃ and put into furnace, raise the temperature to 930~960℃, keep warm for 2~3 hours, take out of furnace and stretch on finish forging machine, the diameter of the rod after stretching is 95~105mm, cut into pieces with a length of about 5000mm and a weight of 150~200KG, and grind the surface defects;

[0010] Step 4: continuous rolling: the bar billet after fine forging is heated to 880-940°C by induction heating, kept at this temperature for 5 minutes, and then rolled in a continuous rolling mill. The weight of the rolled round wire billet is 150-200KG and the diameter is 7-15mm.

[0011] Step 5: Annealing at 760-800° C. for 1-3 hours.

[0012] The present invention is also characterized in that:

[0013] In step 1, the TC4 composition is calculated by weight percentage, the Fe element content is controlled to be 0.15-0.30, and the O element content is controlled to be 0.10-0.20.

[0014] In step 2, the blank forging is free forging, the holding temperature is 1000-1200° C., and the total deformation is 80-95%.

[0015] In step 3, the precision forging temperature is 930-960° C., and the total deformation is 50-90%.

[0016] In step 4, the continuous rolling temperature is 880-940° C., and the total deformation is greater than or equal to 97%.

[0017] In step 5, the annealing temperature is 760-800° C., the annealing time is 1-3 hours, and the cooling method after annealing is air cooling.

[0018] The cross-sectional structure of the alloy of the present invention is a fine, uniform, equiaxed α+β dual-phase structure, reaching the A1 grade quality required by the microstructure of the "TC4 Titanium Alloy Wire and Rod Specification for Aviation Fasteners", and meeting the requirements of titanium alloy materials for fasteners.

[0019] The beneficial effects of the present invention are:

[0020] (1) In the composition design of the present invention, the Fe content is controlled in the range of 0.15 to 0.30 by weight, and the O content is controlled in the range of 0.10 to 0.20 by weight, which can effectively improve the strength of TC4 titanium alloy while having good plasticity.

[0021] (2) The blank forging temperature of the present invention is 1000-1200°C, the total deformation is 80-95%, and the microstructure after forging is a lamellar structure. The fine forging temperature is 930-960°C, the total deformation is 50-90%, and the microstructure after fine forging is a deformed lamellar structure. The continuous rolling temperature is 880-940°C, and the total deformation is greater than 97%. By controlling the rolled bar blank (i.e., the bar after fine forging) to be a deformed lamellar structure, controlling the continuous rolling temperature, and the continuous rolling large deformation mode, the microstructure of the TC4 titanium alloy after rolling is a fine, uniform, equiaxed dual-phase structure.

[0022] (3) The present invention can obtain a large single-weight TC4 titanium alloy wire billet for fasteners with excellent surface quality and excellent dimensional tolerance through a continuous rolling process. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 This is a microstructure photograph of the TC4 titanium alloy φ15mm diameter disc wire blank obtained in Example 1.

[0024] Figure 2 This is a microstructure photograph of the TC4 titanium alloy φ8.0mm diameter disc wire blank obtained in Example 2.

[0025] Figure 3 This is a microstructure photograph of the TC4 titanium alloy φ8.0mm diameter disc wire blank obtained in Example 1.

[0026] Figure 4 This is a microstructure photograph of the TC4 titanium alloy rod with a diameter of φ35 mm obtained in Example 2. DETAILED DESCRIPTION

[0027] In order to make the purpose, technical solutions and advantages of the present invention more clear, the present invention is further described in detail below with reference to the accompanying drawings and embodiments.

[0028] The present invention provides a method for preparing a large single-weight round wire blank of TC4 titanium alloy with high-quality microstructure for fasteners, which is specifically implemented in the following steps:

[0029] Step 1, ingot preparation, sponge titanium, aluminum beans, aluminum-vanadium master alloy, reduced iron powder and carbon powder are mixed and pressed into 20 electrodes of 100 kg, and 2000 kg TC4 titanium alloy ingots are obtained after three vacuum consumable arc melting. The ingot size is about φ600mm×1700mm, and the TC4 titanium alloy ingot is composed of the following elements in weight percentage: Al 6.00%, V4.00%, Fe 0.18%, O 0.14%, C 0.01%, N 0.002%, H≤0.001%, other single impurity elements (including Cu, Mg, Ca, Si, etc.) ≤0.10%, the sum of other impurity elements ≤0.40%, and the balance is Ti;

[0030] Step 2: Forging the blank. Heat the box-type industrial resistance furnace to 900℃ and heat it to 1150℃. Keep it warm for 3 hours. Take it out of the furnace and stretch it on a free forging machine (such as a 10MN fast hydraulic forging machine). After stretching, the diameter of the blank is φ170mm, the forging deformation is 92%, and the surface defects are ground until the surface is bright (without cracks and oxide scale).

[0031] Step 3, fine forging, heat the box-type industrial resistance furnace to 750℃, heat it to 945℃, keep it warm for 2.5 hours, take it out of the furnace and stretch it on the fine forging machine. The diameter of the rod billet after stretching is 100mm, the fine forging deformation is 65%, and the length is about 5000mm, the weight is 150-200KG, and the surface defects are repaired until the surface is bright (without cracks and oxide scale);

[0032] Step 4: continuous rolling: the bar billet after fine forging is heated to 880-940°C by induction heating, kept at this temperature for 5 minutes, and then rolled in a continuous rolling mill. The weight of the rolled round wire billet is 150-200KG and the diameter is 7.5-15mm.

[0033] Step 5: Annealing: 780°C for 2 hours, and air cooling.

[0034] Example 1

[0035] Step 1, ingot preparation, sponge titanium, aluminum beans, aluminum-vanadium master alloy, reduced iron powder and carbon powder are mixed and pressed into 20 electrodes of 100 kg, and after three vacuum consumable arc melting, 2000 kg TC4 titanium alloy ingots are obtained, and the ingot size is φ600mm×1700mm. The TC4 titanium alloy ingot is composed of the following elements in weight percentage: Al 6.00%, V4.00%, Fe 0.18%, O0.14%, C 0.01%, N 0.002%, H≤0.001%, other single impurity elements (including Cu, Mg, Ca, Si, etc.) ≤0.10%, the sum of other impurity elements ≤0.40%, and the balance is Ti;

[0036] Step 2: Forging the blank. Heat the box-type industrial resistance furnace to 900℃, charge the ingot, raise the temperature to 1150℃, keep it warm for 3 hours, and stretch it on a free forging machine (such as 10MN fast hydraulic forging machine). After stretching, the diameter of the blank is φ170mm, the forging deformation is 92%, and the surface defects are ground until the surface is bright (without cracks and oxide scale).

[0037] Step 3, fine forging, heat the box-type industrial resistance furnace to 750℃, load the bar billet into the furnace, heat it to 945℃, keep it warm for 2.5 hours, take it out of the furnace and stretch it on the fine forging machine. After stretching, the diameter of the bar billet is 100mm, the fine forging deformation is 65%, cut into a length of about 5000mm, weigh 175KG, and grind the surface defects until its surface is bright (without cracks and oxide scale);

[0038] Step 4: continuous rolling: the bar billet after fine forging is heated to 920°C by electromagnetic induction heating, kept at this temperature for 5 minutes, and then rolled in a continuous rolling mill. The weight of the rolled round wire billet is 170KG and the diameter is 15mm.

[0039] Step 5: Annealing: 780°C for 2 hours, and air cooling.

[0040] like Figure 1 The figure shows the microstructure of a TC4 titanium alloy φ15mm diameter round wire blank. The microstructure is a fine and uniform equiaxed α+β two-phase structure, in which the α grain size is about 8μm.

[0041] Example 2

[0042] Step 1, ingot preparation, sponge titanium, aluminum beans, aluminum-vanadium master alloy, reduced iron powder and carbon powder are mixed and pressed into 20 electrodes of 100 kg, and after three vacuum consumable arc melting, 2000 kg TC4 titanium alloy ingots are obtained, and the ingot size is φ600mm×1700mm. The TC4 titanium alloy ingot is composed of the following elements in weight percentage: Al 6.00%, V4.00%, Fe 0.18%, O0.14%, C 0.01%, N 0.002%, H≤0.001%, other single impurity elements (including Cu, Mg, Ca, Si, etc.) ≤0.10%, the sum of other impurity elements ≤0.40%, and the balance is Ti;

[0043] Step 2: Forging the blank. Heat the box-type industrial resistance furnace to 900℃, charge the ingot, raise the temperature to 1150℃, keep it warm for 3 hours, and stretch it on a free forging machine (such as 10MN fast hydraulic forging machine). After stretching, the diameter of the blank is φ170mm, the forging deformation is 92%, and the surface defects are ground until the surface is bright (without cracks and oxide scale).

[0044] Step 3, fine forging, heat the box-type industrial resistance furnace to 750℃, load the bar billet into the furnace, heat it to 945℃, keep it warm for 2.5 hours, take it out of the furnace and stretch it on the fine forging machine. After stretching, the diameter of the bar billet is 100mm, the fine forging deformation is 65%, cut into a length of about 5000mm, weigh 175KG, and grind the surface defects until its surface is bright (without cracks and oxide scale);

[0045] Step 4: continuous rolling: the bar billet after fine forging is heated to 920°C by electromagnetic induction heating, kept at this temperature for 5 minutes, and then rolled in a continuous rolling mill. The weight of the rolled round wire billet is 170KG and the diameter is 8mm.

[0046] Step 5: Annealing: 780°C for 2 hours, and air cooling.

[0047] like Figure 2 The figure shows the microstructure of a TC4 titanium alloy φ8mm diameter round wire blank. The microstructure is a fine and uniform equiaxed α+β two-phase structure, in which the α grain size is about 6μm.

[0048] Comparative Example 1

[0049] Step 1, ingot preparation, sponge titanium, aluminum beans, aluminum-vanadium master alloy, reduced iron powder and carbon powder are mixed and pressed into 20 electrodes of 100 kg, and after three vacuum consumable arc melting, 2000 kg TC4 titanium alloy ingots are obtained, and the ingot size is φ600mm×1700mm. The TC4 titanium alloy ingot is composed of the following elements in weight percentage: Al 6.00%, V4.00%, Fe 0.18%, O0.14%, C 0.01%, N 0.002%, H≤0.001%, other single impurity elements (including Cu, Mg, Ca, Si, etc.) ≤0.10%, the sum of other impurity elements ≤0.40%, and the balance is Ti;

[0050] Step 2: Forging the blank. Heat the box-type industrial resistance furnace to 900℃, charge the ingot, raise the temperature to 1150℃, keep it warm for 3 hours, take it out of the furnace and upset it on a free forging machine (such as 10MN fast hydraulic forging machine). After upsetting, the diameter of the bar blank is φ170mm, the forging deformation is 92%, and the surface defects are ground until the surface is bright (without cracks and oxide scale);

[0051] Step 3, fine forging, heat the box-type industrial resistance furnace to 750℃, load the bar billet into the furnace, heat it to 945℃, keep it warm for 2.5 hours, take it out of the furnace and stretch it on the fine forging machine. After stretching, the diameter of the bar billet is 100mm, the fine forging deformation is 65%, cut into a length of about 5000mm, weigh 175KG, and grind the surface defects until its surface is bright (without cracks and oxide scale);

[0052] Step 4: continuous rolling: the bar billet after fine forging is heated to 920°C by electromagnetic induction heating, kept at this temperature for 5 minutes, and then rolled in a continuous rolling mill. The weight of the rolled round wire billet is 170KG and the diameter is 8mm.

[0053] Step 5: Annealing: 780°C for 2 hours, and air cooling.

[0054] like Figure 3The figure shows the microstructure of a TC4 titanium alloy φ8mm diameter round wire blank. The microstructure is a coarse dual-phase structure, in which the α grain size is about 15μm.

[0055] Comparative Example 2

[0056] Step 1, ingot preparation, sponge titanium, aluminum beans, aluminum-vanadium master alloy, reduced iron powder and carbon powder are mixed and pressed into 20 electrodes of 100 kg, and after three vacuum consumable arc melting, 2000 kg TC4 titanium alloy ingots are obtained, and the ingot size is φ600mm×1700mm. The TC4 titanium alloy ingot is composed of the following elements in weight percentage: Al 6.00%, V4.00%, Fe 0.18%, O0.14%, C 0.01%, N 0.002%, H≤0.001%, other single impurity elements (including Cu, Mg, Ca, Si, etc.) ≤0.10%, the sum of other impurity elements ≤0.40%, and the balance is Ti;

[0057] Step 2: Forging the blank. Heat the box-type industrial resistance furnace to 900℃, charge the ingot, raise the temperature to 1150℃, keep it warm for 3 hours, take it out of the furnace and upset it on a free forging machine (such as 10MN fast hydraulic forging machine). After upsetting, the diameter of the bar blank is φ170mm, the forging deformation is 92%, and the surface defects are ground until the surface is bright (without cracks and oxide scale);

[0058] Step 3, fine forging, heat the box-type industrial resistance furnace to 750℃, load the bar billet into the furnace, heat it to 945℃, keep it warm for 2.5 hours, take it out of the furnace and stretch it on the fine forging machine. After stretching, the diameter of the bar billet is 100mm, the fine forging deformation is 65%, cut into a length of about 5000mm, weigh 175KG, and grind the surface defects until its surface is bright (without cracks and oxide scale);

[0059] Step 4: continuous rolling: the bar billet after fine forging is heated to 920°C by electromagnetic induction heating, kept at this temperature for 5 minutes, and then rolled in a continuous rolling mill. The weight of the rolled round wire billet is 170KG and the diameter is 35mm.

[0060] like Figure 4 The figure shows the microstructure of TC4 titanium alloy rod with a diameter of φ35mm. The microstructure is a deformed lamellar structure, in which the length of the α grain lamellar is about 10μm.

[0061] With reference to the enterprise standard ZZQB903-003 “Specifications for TC4 titanium alloy wire and rod for aviation fasteners” of Chengdu Aircraft Design Institute, the microstructures of the TC4 titanium alloys obtained in Examples 1 to 2 and Comparative Examples 1 to 2 were evaluated respectively. The evaluation results are shown in Table 1.

[0062] Microstructure classification Example 1 A1 Example 2 A1 Comparative Example 1 A3 Comparative Example 2 A4

[0063] From the results of Examples 1 to 2 in Table 1 and Figure 1 , Figure 2 It can be seen that the microstructures of Examples 1 and 2 are of grade A1, which is the optimal microstructure specified in ZZQB903-003 "Specifications for TC4 Titanium Alloy Wire and Rod for Aerospace Fasteners".

[0064] The above description is only an implementation method of the present application, and does not limit the patent scope of the present application. Any equivalent structure or equivalent process transformation made using the contents of the present application specification and drawings, or directly or indirectly used in other related technical fields, are also included in the patent protection scope of the present application.

Claims

1. A method for preparing high-quality TC4 titanium alloy disc wire blank for fasteners, characterized in that: The specific steps are as follows: Step 1, prepare an ingot: take a TC4 titanium alloy ingot with a diameter of 500-700 mm, the TC4 titanium alloy ingot is composed of the following elements by weight percentage: Al 5.50-6.75% (preferably 5.50-6.50%), V 3.50-4.50% (preferably 3.75-4.25%), Fe≤0.30% (preferably 0.15-0.30%), O≤0.20% (preferably 0.08-0.20%), C≤0.08%, N≤0.05%, H≤0.015%, other single impurity elements≤0.10%, the sum of other impurity elements≤0.40%, and the balance is Ti; Step 2, billet forging: heat the heating furnace to 850-950℃ to load the ingot, raise the temperature to 1000-1200℃, keep warm for 2-3 hours, take out of the furnace and stretch on the forging machine, the diameter of the billet after stretching is 165-175mm, and grind the surface defects; Step 3, precision forging: heat the heating furnace to 750-850℃ to load the billet into the furnace, raise the temperature to 930-960℃, keep it warm for 2-3 hours, take it out of the furnace and stretch it on the precision forging machine. After stretching, the diameter of the billet is 95-105mm, cut into a length of about 4500-5500mm, and weigh 150-200KG. After precision forging, the billet is ground to remove surface defects; Step 4, continuous rolling: the bar billet after fine forging is heated to 880-940°C by electromagnetic induction heating, kept warm for 5-10 minutes, and then rolled in a continuous rolling unit. The weight of the rolled round wire billet is 150-200KG and the diameter is 7.5-15mm; Step 5: Annealing at 760-800° C. for 1-3 hours.

2. The preparation method according to claim 1, characterized in that: In the step 1, the TC4 composition is calculated by weight percentage, the Fe element content is controlled to be 0.15-0.30%, and the O element content is controlled to be 0.10-0.20%; other impurity elements include one or more of Cu, Mg, Ca, Si, etc.; The process of preparing the ingot is: sponge titanium, aluminum beans, aluminum-vanadium master alloy, iron powder, titanium dioxide and carbon powder are mixed and pressed into electrodes, and after no less than 3 vacuum consumable arc melting, a cylindrical ingot of TC4 titanium alloy with a diameter of 500-700mm is obtained, and the alloy phase transition point is 995±10℃.

3. The preparation method according to claim 1, characterized in that: In the step 2, the blank forging is free forging, the holding temperature is 1000-1200° C. (preferably 1150-1180° C.), and the total deformation is 80-95% (preferably 92-94%).

4. The preparation method according to claim 1, characterized in that: In the step 3, the fine forging temperature is 930-960° C. (preferably 945-950° C.), the total deformation is 50-90% (preferably 65-70%), the cut length is 4500-5500 mm, and the weight is 150-200 KG.

5. The preparation method according to claim 1, characterized in that: In the step 4, the continuous rolling temperature is 880-940° C. (preferably 920-930° C.), the total deformation is greater than or equal to 97%, the diameter after rolling is 7.5-15 mm, and the weight is 150-200 kg.

6. The preparation method according to claim 1, characterized in that: In the step 5, the annealing temperature is 760-800° C. (preferably 780-790° C.), the annealing time is 1-3 hours (preferably 2-2.5 hours), and the cooling method after annealing is air cooling.

7. The preparation method according to claim 1, characterized in that: The ingot in step 1 is cylindrical, with a diameter ranging from 500 to 700 mm (preferably 550 to 600 mm); The obtained TC4 titanium alloy wire billet has a weight of 150-200 kg and a diameter of 7.5-15 mm.

8. A TC4 titanium alloy wire prepared by the preparation method according to any one of claims 1 to 7.

9. Use of the TC4 titanium alloy wire material according to claim 8 as a fastener.

Citation Information

Cited By

  • Preparation method of TC10 titanium alloy large-disc round wire for fastener

    CN119553113A

  • Preparation method of TC16 titanium alloy large-piece-weight disc round wire for fastener

    CN119685631A

  • Preparation method of TB9 titanium alloy large-disc round wire for self-plugging rivet

    CN119747540A

  • Preparation method of TA1G large-disc round wire for fastener

    CN119839090A

  • Preparation method of TC4 titanium alloy disc round wire for low-cost fastener

    CN119972846A