A 1000MPa low-density steel bar and a preparation method thereof

Through vacuum smelting and multi-stage heat treatment process, the tensile strength and plasticity of Fe-12Mn-8.5Al-0.3C low-density steel are improved, which solves the problem of insufficient mechanical properties of existing low-density steel and realizes 1000MPa-level low-density steel. The preparation is suitable for automotive lightweight applications.

CN116065081BActive Publication Date: 2024-10-25CHENGDU ADVANCED METAL MATERIALS IND TECH RES INST CO LTD
View PDF 0 Cites 4 Cited by

Patent Information

Application Number
CN202211622589.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-16
Publication Date
2024-10-25
Estimated Expiration
2042-12-16

AI Technical Summary

Technical Problem

The existing low-density steel has low mechanical properties and a tensile strength of less than 1000MPa, which limits its widespread use in automotive lightweight applications.

Method used

Fe-12Mn-8.5Al-0.3C low-density steel ingots are prepared through vacuum smelting, and the processes of high-temperature homogenization treatment, forging, solid solution, quenching and aging treatment are used to improve the tensile strength and plasticity of the material.

Benefits of technology

The tensile strength exceeds 1000MPa, the yield strength reaches 900MPa, the elongation after break is ≥30%, and the density is ≤7g/cm3. It significantly improves the comprehensive mechanical properties of the material and is suitable for manufacturing high-strength automotive parts.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116065081B_ABST
    Figure CN116065081B_ABST
Patent Text Reader

Abstract

The present invention discloses a 1000MPa-grade low-density steel bar and a preparation method thereof, and relates to the field of iron and steel metallurgy and metal material processing technology. The method comprises: step S1, vacuum smelting and casting the alloy raw materials according to the component ratio to obtain an ingot; step S2, finishing the ingot after high-temperature homogenization treatment to obtain a finished ingot; step S3, preheating and forging the finished ingot to obtain a forged rod; step S4, solutionizing, quenching and aging the forged rod to obtain a 1000MPa-grade low-density steel bar. The Fe‑12Mn‑8.5Al‑0.3C low-density steel prepared by the present invention is an austenitic low-density steel with good strength and plasticity, and a density of 6.98g / cm 3 Compared with ordinary steel, it can reduce weight by 10.5%. It has high strength and can maintain a certain plastic toughness. It is suitable for manufacturing automotive parts, which can effectively reduce the weight of the car and achieve the effect of lightweighting the car, making its application range more extensive.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of iron and steel metallurgy and metal material processing, and in particular to a 1000MPa-grade low-density steel bar and a preparation method thereof. Background Art

[0002] In recent years, with the progress of my country's economy and technology, cars have become one of the necessities of modern life and have been integrated into all aspects of our lives. The number of cars in my country has increased year by year, which has led to the rapid development of the automobile industry. At the same time, pollutants such as carbon monoxide, nitrogen monoxide, and hydrocarbons emitted by automobile exhaust have caused PM2.5 in the atmosphere to exceed the standard, seriously affecting the quality of the air environment. Studies have shown that for every 10% reduction in the weight of a car, its fuel consumption can be reduced by 6% to 8%, and exhaust emissions can be reduced by 5% to 6%; and for every 1L reduction in fuel consumption, 2.45Kg of carbon dioxide will be emitted less. Due to the need for energy conservation and environmental protection, lightweighting of cars has become a trend in the development of the world's automobiles. Studies have shown that the density of steel only needs to be reduced by 10% to maintain or even significantly improve the superiority and competitiveness of steel in the automotive industry.

[0003] From the perspective of material selection, there are currently two main ways to reduce the weight of automobiles: one is to use lightweight materials, such as low-density aluminum and aluminum alloys, magnesium and magnesium alloys, engineering plastics, etc., but such lightweight materials have very low strength, which seriously limits their application in stress-bearing and load-bearing parts of automobiles. The second is to use ultra-high-strength steel to replace traditional steel, reduce the thickness of steel plates to reduce the weight of the vehicle body, but high-strength steel plates are prone to rebound after forming, and the rebound amount is much greater than that of traditional low-carbon steel plates, and the material properties are more complex and difficult to control. In the 1930s, Ton and Korter first proposed the concept of low-density steel. They added manganese and aluminum elements with low relative molecular mass to iron to form Fe-Mn-Al low-density steel, and made a phase diagram after quenching. In 1958, Ham and Cairns developed a low-cost Fe-34Mn-10Al-0.76C austenitic low-density steel with a tensile strength of 750MPa. Cr-Ni stainless steel requires the addition of a large amount of metals such as chromium and nickel. At that time, 95.1% of the world's chromium was in South Africa and Zimbabwe. Chromium became an extremely scarce element. The addition of chromium and nickel caused the production cost of stainless steel to be very high. The newly developed austenitic low-density steel has excellent corrosion resistance and oxidation resistance. Low-density steel not only has cost advantages, but also has the development potential of low density. Ham et al. proposed to use cheap Fe-Mn-Al low-density steel to replace expensive Cr-Ni stainless steel, which became a hot topic in the automotive and steel industries in the 1950s. Since the 1990s, environmental pollution has attracted much attention, and the requirements for energy saving and lightweight in various fields have become increasingly higher. A research and development idea with development potential for lightweight is to develop a steel grade that combines low density and high strength and toughness - low-density steel (low-density steel), so low-density steel has become a hot research topic in various countries. Some scholars pointed out that by adding a certain amount of lightweight elements such as aluminum, manganese, silicon and carbon to steel, a new type of steel with low density and high strength and toughness can be obtained on the basis of optimizing the alloy composition and heat treatment process. In this way, the weight of the car itself can be effectively reduced without sacrificing the strength and rigidity of the car structure. According to relevant research, in Fe-Mn-Al-C low-density steel, when the Al content is 2.5%-6.0%, the density of the steel is less than 7.5g / cm 3 , the weight reduction is 4.5%; when the Al content is 6.0%-10.0%, the density of the steel can be less than 7.2g / cm 3 , the weight reduction can be greater than 8.3%; when the Al content is 10.0%-15.0%, the density of the steel can be less than 6.5g / cm 3 , weight loss can reach 17.2%.

[0004] Patent CN104928569A discloses "a low-density steel with high ductility of 800MPa and a method for manufacturing the same". The method prepares a steel plate with a tensile strength of >800MPa and an elongation after fracture of >25% by adopting smelting, casting, hot rolling, pickling, cold rolling and continuous annealing processes. The method improves the comprehensive mechanical properties of low-density steel by means of rolling deformation, but its tensile strength does not exceed 1000MPa, and its mechanical properties are relatively low, which affects the application of low-density steel in lightweighting.

[0005] Patent CN110592487A discloses "700MPa grade austenitic ferrite dual-phase low-density cast steel and preparation method thereof". The chemical composition mass percentage of the low-density cast steel prepared by this method is: C: 0.01-1.0%, Si: 0.1-0.2%, Mn: 10.0-25.0%, Al: 10.0-15.0%, V: 0.01-1.0%, Nb: 0.01-1.0%, Ti: 0.01-1.0%, S≤0.01%, P≤0.02%, and the rest is Fe and unavoidable impurities; at the same time, the weight percentage of Mn and Al satisfies 25%≤Mn+Al≤35%; the weight percentage of Nb, V and Ti satisfies 0.05%≤Nb+V+Ti≤0.5%. This method uses medium frequency induction furnace smelting and solid solution and aging treatment to obtain 700MPa grade austenite-ferrite dual-phase low-density cast steel. The preparation process is simple, but the mechanical properties of the obtained low-density steel are low, and its tensile strength is less than 1000MPa. It is not suitable for manufacturing components with higher requirements for mechanical properties and will be severely restricted in lightweight applications.

[0006] Fe-12Mn-8.5Al-0.3C low-density steel is an austenitic low-density steel with a density of 6.98g / cm3. Compared with ordinary steel, it has a weight reduction effect of 10.5%. It has high strength and can maintain a certain degree of plasticity and toughness. It is suitable for manufacturing automotive parts and can effectively reduce the weight of the car and achieve the effect of lightweighting the car. However, the mechanical properties of existing low-density steel are low, generally lower than 1000MPa, which seriously affects the application of this material in lightweighting of automobiles. Summary of the invention

[0007] The present invention aims to provide a 1000MPa grade low-density steel bar and a preparation method thereof. A Fe-12Mn-8.5Al-0.3C low-density steel ingot is obtained by vacuum smelting, the density of the material is effectively reduced by adding Al element, and the comprehensive mechanical properties of the material are improved by forging processing, so that the tensile strength is greater than 1000MPa; the Fe-12Mn-8.5Al-0.3C low-density steel prepared by the present invention is an austenitic low-density steel with good strength and plasticity, and a density of 6.98g / cm 3Compared with ordinary steel, it can reduce weight by 10.5%. It has high strength and can maintain a certain plastic toughness. It is suitable for manufacturing automotive parts, which can effectively reduce the weight of the car and achieve the effect of lightweighting the car, making its application range more extensive.

[0008] According to one aspect of the present disclosure, a method for preparing a 1000 MPa grade low-density steel bar is provided, the preparation method comprising the following steps:

[0009] Step S1, vacuum smelting and casting the alloy raw materials according to the composition ratio to obtain an ingot;

[0010] Step S2, subjecting the ingot to high temperature homogenization treatment and then finishing it to obtain a finished ingot;

[0011] Step S3, preheating and forging the finished ingot to obtain a forged rod;

[0012] Step S4: subjecting the forged rod to solid solution treatment, quenching and aging treatment to obtain a 1000 MPa grade low-density steel rod.

[0013] In a possible implementation, in step S1,

[0014] The vacuum smelting condition is to evacuate to 1Pa-10Pa;

[0015] The casting temperature is 1500°C to 1650°C;

[0016] The ingot diameter is 200 mm to 250 mm.

[0017] In a possible implementation, in step S2,

[0018] The high temperature homogenization treatment includes: a temperature of 1200°C to 1300°C and a holding time of 10h to 15h;

[0019] The diameter of the finishing ingot is 200 mm to 230 mm.

[0020] In a possible implementation, in step S3, the preheating includes:

[0021] The heating temperature is 1100℃~1200℃, and the holding time is 3h~5h.

[0022] In a possible implementation, in step S3, the forging process includes:

[0023] After 10s to 120s, the preheated fine ingot is forged for the first time to obtain a square billet;

[0024] The square billet is forged for the second time after an interval of 1s to 15s to obtain a forged rod.

[0025] In a possible implementation, during the first forging process:

[0026] The feeding speed of the finishing ingot is 0.3m / s~0.5m / s;

[0027] The rotation feeding angle is 90° / hammer;

[0028] The forging hammer frequency is 80 times / min to 100 times / min;

[0029] The diameter of the square billet is 80mm~100mm.

[0030] In a possible implementation, during the second forging process:

[0031] The feeding speed of the billet is 0.3m / s to 0.5m / s;

[0032] The rotation feeding angle is 30° / hammer;

[0033] The forging hammer frequency is 80 times / min to 100 times / min;

[0034] The diameter of the forging rod is 50mm~60mm.

[0035] In a possible implementation, in step S4,

[0036] The solution treatment includes: the solution temperature is 900-1200°C and the holding time is 1h-3h;

[0037] The quenching treatment includes: the quenching medium is water, and the initial temperature of the medium is 25°C to 50°C;

[0038] The aging treatment includes: an aging temperature of 300° C. to 600° C. and a heat preservation time of 1 h to 10 h.

[0039] According to one aspect of the present disclosure, a 1000MPa grade Fe-12Mn-8.5Al-0.3C low-density steel bar is provided, and the components and mass percentages of the low-density steel bar are:

[0040] C: 0.31% ~ 0.34%; Mn: 12.1% ~ 12.5%; Al: 8.51% ~ 8.55%; Ni: 10.0% ~ 15.0%; P: 0.005% ~ 0.008; S: 0.001% ~ 0.002%; H: 0.0004% ~ 0.0005%; O: 0.001% ~ 0.008%; N: 0.003% ~ 0.005%, the rest is Fe and unavoidable impurity elements.

[0041] Technical effects and advantages of the present invention:

[0042] First, the present invention uses a vacuum induction furnace to melt and refine the raw materials. Under vacuum conditions, there is no air and slag pollution, the metal is not easy to volatilize and oxidize, and the chemical composition of the Fe-12Mn-8.5Al-0.3C low-density steel can be accurately controlled and adjusted. At the same time, vacuum smelting also creates good degassing conditions, and carbon can be used for deoxidation. The deoxidation product is gas. At the same time, there is a certain amount of electromagnetic stirring in the molten pool, which can promote the uniformity of the composition and temperature of the molten steel, so that the inclusions in the steel float up, thereby obtaining high-quality Fe-12Mn-8.5Al-0.3C low-density steel ingots.

[0043] Second, high-temperature homogenization treatment is a heat treatment process that heats the Fe-12Mn-8.5Al-0.3C low-density steel ingot to a temperature below the solidus line for a long time, and then slowly cools it to eliminate dendrite segregation and chemical composition inhomogeneity. Due to the rapid cooling rate of the molten steel, the structure of the Fe-12Mn-8.5Al-0.3C low-density steel ingot after condensation is in a non-equilibrium state to varying degrees, which is mainly manifested in the generation of dendrite segregation. Due to the existence of segregation, the composition of each part of the ingot is quite different, which makes the phase change process different. It will lead to extremely uneven structure and performance of large ingots, and at the same time generate great organizational stress. The banded structure formed by segregation will cause serious deterioration of the mechanical properties of low-density steel. The purpose of homogenization treatment is to eliminate dendrite segregation and regional segregation generated in the ingot during solidification, and to dissolve the coarse primary phase into the matrix, so that the composition and structure of Fe-12Mn-8.5Al-0.3C low-density steel are homogenized, and the strength and toughness of the material are improved.

[0044] Third, through a large number of tests, the present invention strictly controls the process parameters of high temperature homogenization, forging, solid solution and aging of Fe-12Mn-8.5Al-0.3C low-density steel, and finally makes the tensile strength of Fe-12Mn-8.5Al-0.3C low-density steel ≥1000MPa, yield strength ≥900MPa, elongation after fracture ≥30%, density ≤7g / cm 3 Compared with ordinary steel, the weight reduction effect is up to 10%, making Fe-12Mn-8.5Al-0.3C low-density steel not only have a lower density, but also have good comprehensive mechanical properties.

[0045] Other features and advantages of the present invention will be described in the following description, and partly become apparent from the description, or understood by practicing the present invention. The purpose and other advantages of the present invention can be realized and obtained by the structures pointed out in the description, claims and drawings. BRIEF DESCRIPTION OF THE DRAWINGS

[0046] The accompanying drawings herein are incorporated into the specification and constitute a part of the specification, illustrate embodiments consistent with the present disclosure, and together with the specification are used to explain the principles of the present disclosure. Obviously, the accompanying drawings described below are only some embodiments of the present disclosure, and for ordinary technicians in this field, other accompanying drawings can be obtained based on these accompanying drawings without creative work.

[0047] Figure 1 A flow chart of a method for preparing a 1000MPa grade low-density steel bar according to an exemplary embodiment of the present invention;

[0048] Figure 2 A schematic diagram of a stress-strain curve of a Fe-12Mn-8.5Al-0.3C low-density steel bar according to an exemplary embodiment of the present invention;

[0049] Figure 3 This is a scanning electron microscope image of the tensile fracture of a Fe-12Mn-8.5Al-0.3C low-density steel bar according to an exemplary embodiment of the present invention. DETAILED DESCRIPTION

[0050] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0051] The flowcharts shown in the accompanying drawings are only exemplary and do not necessarily include all the steps. For example, some steps may be decomposed, while some steps may be combined or partially combined, so the actual execution order may change according to the actual situation.

[0052] The terms "first", "second", etc. in the specification and claims of the present application and the above-mentioned drawings are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the terms used in this way can be interchanged where appropriate, so that the embodiments of the present application described herein can be implemented in an order other than those illustrated or described herein, for example.

[0053] In addition, the terms "include" and "have" and any variations thereof are intended to cover non-exclusive inclusions. For example, a process, method, system, product, or apparatus comprising a series of steps or sub-modules is not necessarily limited to those steps or sub-modules explicitly listed, but may include other steps or sub-modules not explicitly listed or inherent to these processes, methods, products, or apparatuses.

[0054] Figure 1 FIG. 1 is a flow chart of a method for preparing a 1000 MPa grade low-density steel bar according to an exemplary embodiment of the present invention, as shown in FIG. Figure 1 As shown, the present invention discloses a method for preparing a 1000MPa grade Fe-12Mn-8.5Al-0.3C low-density steel bar, comprising:

[0055] Step S1, vacuum smelting and casting the alloy raw materials according to the composition ratio to obtain an ingot;

[0056] Step S2, subjecting the ingot to high temperature homogenization treatment and then finishing it to obtain a finished ingot;

[0057] Step S3, preheating and forging the finished ingot to obtain a forged rod;

[0058] Step S4: subjecting the forged rod to solid solution treatment, quenching and aging treatment to obtain a 1000 MPa grade low-density steel rod.

[0059] In step S1 of the present invention, the vacuum induction furnace is evacuated to 1Pa-10Pa, preferably 1Pa; the steel casting temperature is 1500°C-1650°C, preferably 1500°C; and the ingot is cast into a diameter of 200mm-250mm, preferably 230mm.

[0060] In step S2 of the present invention, the homogenization treatment temperature is 1200°C to 1300°C, preferably 1250°C; the holding time is 10h to 15h, preferably 15h; the ingot treated with high temperature homogenization is air-cooled to room temperature and then peeled, and then refined into an ingot with a diameter of 200mm to 230mm, preferably 200mm.

[0061] In step S3 of the present invention, the finished ingot is preheated in a muffle furnace before forging, and the preheating temperature is set to 1100°C to 1200°C, preferably 1150°C; the surface temperature and core temperature of the ingot are both controlled within ±10°C, and the insulation time is 3h to 5h, preferably 5h.

[0062] Further, the time interval from the finishing ingot being discharged from the furnace to the first forging is 10s to 120s, preferably 60s; the feed speed of the first forging process is controlled at 0.3m / s to 0.5m / s, preferably 0.5m / s; the rotation feed angle is 90° / hammer; the forging hammer frequency is controlled at 80 times / min to 100 times / min, preferably 100 times / min, and by controlling the hammer frequency, the surface temperature rise of the ingot is controlled at 0°C to 20°C, and the core temperature rise is controlled below 20°C; the first forging finally forges the ingot into a square billet of 80mm to 100mm, preferably a square billet of 90mm;

[0063] After the first forging is completed, the second forging is performed, and the time interval from the end of the first forging to the start of the second forging is 1s to 15s; the feed speed of the second forging process is controlled at 0.3m / s to 0.5m / s, preferably 0.5m / s; the rotation feed angle is 30° / hammer; the forging hammer frequency is controlled at 80 times / min to 100 times / min, preferably 100 times / min, and by controlling the hammer frequency, the surface temperature rise of the ingot is controlled at 0℃ to 20℃, and the core temperature rise is controlled below 15℃; the final forging size obtained after the second forging is a forged rod with a diameter of 50mm to 60mm, preferably 50mm.

[0064] In step S4 of the present invention, the solution treatment and aging treatment of the forged rod are carried out in a muffle furnace, firstly the solution treatment is carried out, the solution temperature is 900-1200°C, preferably 1000°C; the heat preservation is carried out for 1h-3h, preferably 2h; water is used as the quenching medium, and the initial temperature of the quenching medium is 25°C-50°C; the aging treatment is carried out within 5h after quenching, the aging temperature is 300°C-600°C, preferably 450°C; the heat preservation is carried out for 1h-10h, preferably 5h; then the forged rod is taken out of the furnace and air-cooled, and finally a 1000MPa grade Fe-12Mn-8.5Al-0.3C low-density steel bar is obtained.

[0065] Based on the above method, the present invention also provides a 1000MPa grade Fe-12Mn-8.5Al-0.3C low-density steel bar, the components and mass percentages of the low-density steel bar are:

[0066] C: 0.31% ~ 0.34%; Mn: 12.1% ~ 12.5%; Al: 8.51% ~ 8.55%; Ni: 10.0% ~ 15.0%; P: 0.005% ~ 0.008; S: 0.001% ~ 0.002%; H: 0.0004% ~ 0.0005%; O: 0.001% ~ 0.008%; N: 0.003% ~ 0.005%, the rest is Fe and unavoidable impurity elements.

[0067] Example:

[0068] A method for preparing a 1000MPa grade low-density steel bar comprises the following steps:

[0069] Step S1: The alloy raw materials are loaded into the crucible according to the composition ratio, the vacuum induction furnace is evacuated to 1 Pa, and then the alloy raw materials are completely melted by power. The composition is tested and fine-tuned before steelmaking. Steelmaking can be done after the composition test is qualified. The steelmaking casting temperature is 1550°C, and the ingot with a diameter of 230 mm is cast. The ingot is slowly cooled in the furnace to obtain the ingot. The main components of the ingot and their mass percentage are shown in Table 1.

[0070] Table 1 Composition and mass percentage of ingot

[0071] element Mn Al C Ni O N H P S Fe content 12.0 8.5 0.3 10.1 0.002 0.003 0.0005 0.005 0.002 margin

[0072] Step S2: using the ingot with a diameter of 230 mm obtained by smelting in a vacuum induction furnace as the base ingot for high-temperature homogenization treatment, the homogenization treatment temperature is 1250° C., and the holding time is 15 hours; the ingot treated with high-temperature homogenization is air-cooled to room temperature, peeled, and then refined into a refined ingot with a diameter of 200 mm;

[0073] Step S3: preheating the finished ingot in a muffle furnace before forging, the preheating temperature is set between 1150°C, the surface temperature and the core temperature of the ingot are controlled within ±10°C, and the holding time is 5h;

[0074] The preheated fine ingot is taken out of the furnace for forging. The forging process is one-time heating and two-pass forging. The final Fe-12Mn-8.5Al-0.3C low-density steel bar with a diameter of 50mm is obtained. The time interval from the ingot being taken out of the furnace to the first forging is 60s; the feeding speed of the first forging process is controlled at 0.5m / s; the rotating feeding angle is 90° / hammer; the forging hammer frequency is 100 times / min. By controlling the hammer frequency, the surface temperature rise of the ingot is controlled at 0℃~20℃, and the core temperature rise is controlled below 20℃. The first pass finally forges the ingot into a 90mm square billet;

[0075] After the first forging is completed, the second forging is performed, and the time interval from the end of the first forging to the start of the second forging is 5s; the feed speed of the second forging process is 0.5m / s; the rotation feed angle is 30° / hammer; the forging hammer frequency is 100 times / min, and the surface temperature rise of the ingot is controlled at 0℃~20℃ and the core temperature rise is controlled below 15℃ by controlling the hammer frequency; the final forging size obtained after the second forging is a Fe-12Mn-8.5Al-0.3C low-density steel bar with a diameter of 50mm;

[0076] Step S4: The forged rod is subjected to solution treatment and aging treatment in a muffle furnace. Solution treatment is first performed at a solution temperature of 1000°C for 2 hours, and water is used as a quenching medium with an initial temperature of 25°C to 50°C. Aging treatment is performed within 5 hours after quenching at a temperature of 450°C for 5 hours, and then the rod is taken out of the furnace and air-cooled. Finally, a 1000MPa grade Fe-12Mn-8.5Al-0.3C low-density steel bar is obtained, and its components and mass percentages are as follows:

[0077] C: 0.32%; Mn: 12.3%; Al: 8.52%; Ni: 10.1%; P: 0.005%; S: 0.002%; H: 0.0005%; O: 0.002%; N: 0.003%, and the rest are Fe and unavoidable impurity elements.

[0078] Figure 2 FIG. 1 is a schematic diagram of a stress-strain curve of a Fe-12Mn-8.5Al-0.3C low-density steel bar according to an exemplary embodiment of the present invention, Figure 2 It can be seen that the stress-strain curve has no obvious yield platform, showing continuous yield deformation and high plastic deformation capacity. Figure 3 The tensile fracture scanning electron microscope image of the Fe-12Mn-8.5Al-0.3C low-density steel of the embodiment of the present invention is shown in FIG. Figure 3 It can be seen that dimples appear on the fracture surfaces, indicating ductile fracture, which indicates that the Fe-12Mn-8.5Al-0.3C low-density steel bar of the present invention has good plasticity and toughness.

[0079] The mechanical properties of the sample prepared in this embodiment were measured by making a tensile test bar with a diameter of 5 mm using a universal tensile testing machine in accordance with the national standard GB / T228.1-2010; the hardness of the sample prepared in this embodiment was measured using a Rockwell hardness tester in accordance with the national standard GB / T230.2-2012; and the density of the sample prepared in this embodiment was measured using a precision balance. Its hardness, tensile strength, yield strength, elongation after fracture, and density are shown in Table 2.

[0080] Table 2 Various properties of the samples prepared in this example

[0081]

[0082] As can be seen from Table 2, the Fe-12Mn-8.5Al-0.3C low-density steel bar prepared by the method of the present invention has higher strength and plasticity and lower density, can better replace the structural parts of the automobile, reduce the weight of the whole vehicle, and achieve a good lightweight effect.

[0083] Finally, it should be noted that the above is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, it is still possible for those skilled in the art to modify the technical solutions described in the aforementioned embodiments or to make equivalent substitutions for some of the technical features therein. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing a 1000MPa grade low-density steel bar, characterized in that: The preparation method comprises the following steps: Step S1, vacuum smelting and casting the alloy raw materials according to the composition ratio to obtain an ingot; the vacuum smelting condition is to evacuate to 1 Pa; the casting temperature is 1500° C.; Step S2, subjecting the ingot to high temperature homogenization treatment and then finishing to obtain a finished ingot; the high temperature homogenization treatment includes: the temperature is 1250°C, the surface temperature and the core temperature of the ingot are controlled within ±10°C, and the holding time is 15h; Step S3, preheating and forging the finished ingot to obtain a forged rod; the preheating includes: a heating temperature of 1150° C. and a holding time of 5 hours; The forging process comprises: After 60s interval, the preheated fine ingot is forged for the first time to obtain a square billet; during the first forging process: the feeding speed of the fine ingot is 0.5m / s; the rotation feeding angle is 90° / hammer; the forging hammer frequency is 100 times / min; by controlling the hammer frequency, the surface temperature rise of the ingot is controlled at 0℃~20℃, and the core temperature rise is controlled below 20℃; The square billet is forged for the second time after an interval of 5 seconds to obtain a forged rod; during the second forging process: the billet feeding speed is 0.5 m / s; the rotation feeding angle is 30° / hammer; the forging hammer frequency is 100 times / min; by controlling the hammer frequency, the surface temperature rise of the ingot is controlled at 0°C to 20°C, and the core temperature rise is controlled below 15°C; Step S4, subjecting the forged rod to solid solution treatment, quenching and aging treatment to obtain a 1000MPa grade low-density steel rod; the solid solution treatment includes: the solid solution temperature is 1000°C and the holding time is 2h; the quenching treatment includes: the quenching medium is water, the initial temperature of the medium is 25°C to 50°C, and the aging treatment is performed within 5h after quenching; the aging treatment includes: the aging temperature is 450°C and the holding time is 5h; The components and mass percentages of the low-density steel bar are: C: 0.31%~0.34%; Mn: 12.1%~12.5%; Al: 8.51%~8.55%; Ni: 10.0%~15.0%; P: 0.005%~0.008%; S: 0.001%~0.002%; H: 0.0004%~0.0005%; O: 0.001%~0.008%; N: 0.003%~0.005%, and the rest are Fe and unavoidable impurity elements.

2. The method for preparing a 1000MPa grade low-density steel bar according to claim 1, characterized in that: In step S1, The ingot diameter is 200 mm to 250 mm.

3. The method for preparing a 1000MPa grade low-density steel bar according to claim 1, characterized in that: In step S2, The diameter of the finishing ingot is 200 mm to 230 mm.

4. The method for preparing a 1000MPa grade low-density steel bar according to claim 1, characterized in that: The diameter of the square billet is 80mm~100mm.

5. The method for preparing a 1000MPa grade low-density steel bar according to claim 1, characterized in that: The diameter of the forging rod is 50mm~60mm.

6. The method for preparing a 1000MPa grade low-density steel bar according to claim 1, characterized in that: The mechanical properties of the low-density steel bar include: Tensile strength ≥1000MPa, yield strength ≥900MPa, elongation after fracture ≥30%, density ≤7g / cm 3 .

Citation Information

Cited By

  • 1000MPa-grade low-density medium manganese steel and preparation method thereof

    CN120758805A

  • A 1000mpa grade low density medium manganese steel and a method of making the same

    CN120758805B

  • Nb-Mo-V-Si-B gold high-strength plastic hot-rolled low-density steel and preparation method thereof

    CN120924879A

  • Nb-mo-v-si-b alloyed high strength-to-plasticity hot-rolled low-density steel and method for manufacturing the same