Carbon fiber epoxy resin composite material based on cobalt-based metal organic framework synergistic flame retardant and preparation method

By using polyurethane to coat ammonium polyphosphate and ZIF-67 in carbon fiber epoxy resin composites to form flame-retardant microcapsules, the problems of poor flame retardancy and interface compatibility of epoxy resin composites are solved, significantly improving It has excellent flame retardant properties and is suitable for electronic products and other fields.

CN118772451APending Publication Date: 2024-10-15SHAANXI UNIV OF SCI & TECH

Patent Information

Application Number
CN202411034055.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Existing carbon fiber epoxy resin composite materials have poor flame retardancy and poor interface compatibility between ammonium polyphosphate and epoxy resin, which limits their application in electronic products and other fields.

Method used

Ammonium polyphosphate is coated with a polyurethane shell to prepare PUAPP, and ZIF-67 is coated on its surface to form ZIF-67@PUAPP, which is evenly dispersed into epoxy resin, and a flame-retardant type is prepared through co-precipitation and in-situ growth methods. Microcapsules improve interface compatibility and flame retardant properties.

Benefits of technology

The Co3O4 generated by the combustion of ZIF-67 promotes the formation of char layer and inhibits the release of combustion gases. The steam and gas generated during the combustion process are diluted and cooled, which significantly improves the flame retardant performance of the composite material and reduces the fire risk.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118772451A_ABST
    Figure CN118772451A_ABST
Patent Text Reader

Abstract

The invention discloses a carbon fiber epoxy resin composite material based on a cobalt-based metal organic framework synergistic flame retardant and a preparation method, and belongs to the technical field of flame-retardant modification of carbon fiber epoxy resin composites.The flame-retardant microcapsule PUAPP is prepared through an in-situ polymerization method, ZIF-67-coated PUAPP is prepared on ammonium polyphosphate coated with polyurethane through a coprecipitation method, and the ZIF-67-coated PUAPP is prepared through a coprecipitation method. The preparation method is simple in process and high in reaction speed, Co3O4 generated in the combustion process of ZIF-67 can promote generation of a carbon layer, attenuate oxygen on the surface of the composite material and further enable the carbon layer to be more compact, and therefore release of combustion gas generated in the decomposition process of the composite material is inhibited; steam, N2 and NH3 generated in the combustion process are beneficial to dilution of oxygen and inflammable gas on the surface of the composite material, heat absorption water vapor can be generated in the combustion process, dilution and cooling are facilitated, and therefore a better flame-retardant effect is achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of flame retardant modification of carbon fiber epoxy resin composite materials, and relates to a carbon fiber epoxy resin composite material based on a cobalt-based metal organic framework synergistic flame retardant and a preparation method thereof. Background Art

[0002] Carbon fiber reinforced resin-based composites have become the preferred material for aerospace equipment due to their overall integrated design, structure and manufacturing material performance, which can easily achieve the overall performance of large and complex components. Among them, CF is used as a reinforcing material in carbon fiber reinforced resin-based composites, thereby improving the mechanical properties of the composites, using resin polymers as a matrix to bond the fibers and protect them from environmental influences. An important problem currently faced in the study of CFRP interface modification: EP is flammable due to the limitations of its elemental composition, and its limiting oxygen index (LOI) is only 20%. The flammability of EP has seriously restricted the development of CFRP in certain specific fields (especially electronic products), so the study of its flame retardant properties is crucial.

[0003] Ammonium polyphosphate (APP) is widely used in the field of polymer flame retardancy due to its low cost, low toxicity and good flame retardant effect. Ammonium polyphosphate (APP) is an environmentally friendly flame retardant widely used to improve the flame retardancy of polymers. During the combustion process, APP releases NH3, water and inorganic acid. Inorganic acid can react with hydroxyl groups to form phosphate esters. Coking occurs when the phosphate ester is dehydrated, and then an expanded carbonaceous structure is formed during the release of NH3 and water. The expanded carbonaceous structure is used as a barrier to reduce thermal radiation and isolate pyrolysis products. However, APP has weak water resistance, is easy to absorb moisture, and has poor compatibility with polymers, which limits its application. In addition, during the preparation of the polymer, APP produces a separation layer in the prepolymer, resulting in the destruction of mechanical properties, changes in glass transition temperature and a decrease in flame retardant efficiency. However, the flame retardant efficiency of PUAPP after polyurethane monolayer coating ammonium polyphosphate is not significant when added to carbon fiber epoxy resin. Therefore, there are technical problems in the prior art that epoxy resin has poor flame retardancy and ammonium polyphosphate has poor interface compatibility with epoxy resin. Summary of the invention

[0004] The purpose of the present invention is to provide a carbon fiber epoxy resin composite material based on a cobalt-based metal organic framework synergistic flame retardant and a preparation method thereof, so as to solve the technical problems in the prior art of poor flame retardancy of epoxy resin and poor interface compatibility between ammonium polyphosphate and epoxy resin.

[0005] In order to achieve the above object, the present invention adopts the following technical solutions:

[0006] A method for preparing a carbon fiber epoxy resin composite material based on a cobalt-based metal organic framework and a synergistic flame retardant, comprising:

[0007] S1: Use polyurethane shell to coat ammonium polyphosphate to prepare PUAPP.

[0008] S2: ZIF-67 was coated on PUAPP to prepare ZIF-67@PUAPP;

[0009] S3: The successfully prepared ZIF-67@PUAPP is evenly dispersed into the epoxy resin E-51 system to obtain a mixture, and the mixture is evenly applied on the carbon fiber cloth and post-cured to obtain a ZIF-67@PUAPP / CF / EP composite material.

[0010] Preferably, it is characterized in that said S1 specifically includes:

[0011] S101: Dissolve PEG2000 in polyvinyl alcohol solution to obtain solution A

[0012] S102: HDI trimer, emulsifier OP-10, ammonium polyphosphate, catalyst dibutyltin dilaurate, and solvent dimethyl sulfoxide are mixed, and stirred until the mixture is uniform to obtain solution B;

[0013] S103: adding solution B dropwise into solution A to mix and disperse, and after dispersion, taking out the emulsion and letting it stand to obtain a mixed solution C;

[0014] S104: The mixed solution C is slowly heated in a water bath for reaction, and a chain extender 1,4-butanediol is added, and the temperature is raised for reaction. After the reaction is completed, the solution is cooled to room temperature and centrifuged to obtain PUAPP.

[0015] Preferably, the mass fraction of polyvinyl alcohol in solution A in S101 is 1.5%; the molar ratio of HDI trimer in S102 to PEG2000 in S101 is 1.2:1, and the mass ratio of polyurethane to ammonium polyphosphate is 1:0.5 when HDI trimer and PEG2000 are used to prepare synthetic polyurethane.

[0016] Preferably, the addition of the chain extender BDO in S104 complies with a chain extension coefficient of 0.90.

[0017] Preferably, the S2 specifically includes:

[0018] S201: Dissolve 2-methylimidazole in methanol to obtain a mixed solution D.

[0019] S202: Dissolve cobalt nitrate hexahydrate (Co(NO3)2·6H2O) in methanol to obtain a mixed solution E.

[0020] S203: dispersing PUAPP in methanol to obtain a mixed solution F;

[0021] S204: adding the mixed solution F dropwise into the mixed solution D to obtain a mixed solution G, and then quickly pouring the mixed solution E into the mixed solution G, recorded as a mixed solution H;

[0022] S205: The mixed solution H is stirred at room temperature, allowed to stand, and then filtered, and washed with methanol to obtain ZIF-67@PUAPP.

[0023] Preferably, the usage ratio of 2-methylimidazole to methanol in S201 is (2-5) mmol: (12.5-31.25) mL.

[0024] Preferably, the usage ratio of cobalt nitrate hexahydrate and methanol in S202 is (0.5-1.5) mmol: (12.5-37.5) mL.

[0025] Preferably, the S3 specifically includes:

[0026] S301: Disperse ZIF-67@PUAPP evenly into the epoxy resin system, stir evenly in a water bath, add curing agent H256, ensure that the mass ratio of resin to curing agent reaches 100:32, then heat it to make it flowable, and evenly apply it on the carbon fiber cloth;

[0027] S302: Place the coated carbon fiber cloth into a preheated mold, and perform three-stage temperature rise curing to obtain a ZIF-67@PUAPP / CF / EP composite material.

[0028] Preferably, the three-stage temperature-raising curing is specifically to keep the temperature at 90°C and normal pressure for 2 hours, then pressurize to 5MPa, then heat to 120°C and keep the temperature for 2 hours, and in the third stage keep the temperature at 150°C for 3 hours.

[0029] The present application also discloses a carbon fiber epoxy resin composite material based on a cobalt-based metal organic framework and a synergistic flame retardant, characterized in that it is prepared by any one of the preparation methods described above.

[0030] Compared with the prior art, the present invention has the following beneficial effects:

[0031] The present invention discloses a method for preparing a carbon fiber epoxy resin composite material based on a cobalt-based metal organic framework synergistic flame retardant. The flame-retardant microcapsule PUAPP is prepared by an in-situ polymerization method, and ZIF-67@PUAPP is prepared by a coprecipitation method on ammonium polyphosphate that has been coated with polyurethane. The process is relatively simple and the reaction speed is relatively fast. The Co3O4 generated during the combustion of ZIF-67 can promote the formation of a carbon layer, attenuate the oxygen on the surface of the composite material, and further make the carbon layer denser, thereby inhibiting the release of combustion gases generated during the decomposition of the composite material. In addition, the steam, N2 and NH3 generated during the combustion process help to dilute the oxygen and flammable gas on the surface of the composite material. During the combustion process, heat-absorbing water vapor will be generated, which is conducive to dilution and cooling, thereby achieving a better flame retardant effect. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.

[0033] Figure 1 is the infrared spectrum;

[0034] Figure 2 It is the XRD analysis spectrum;

[0035] Figure 3 Scanning SEM images, (a) shows ammonium polyphosphate; (b) shows polyurethane-coated ammonium polyphosphate; (c) shows ZIF-67-coated PUAPP;

[0036] Figure 4 The flame retardant performance test results of carbon fiber epoxy resin composites before and after adding cobalt-based metal organic framework synergistic flame retardant, where (a) is the maximum heat release rate (PHRR) graph; (b) is the maximum total heat release (THR) graph. DETAILED DESCRIPTION

[0037] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Generally, the components of the embodiments of the present invention described and shown in the drawings here can be arranged and designed in various different configurations.

[0038] Therefore, the following detailed description of the embodiments of the present invention provided in the accompanying drawings is not intended to limit the scope of the invention claimed for protection, but merely represents selected embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0039] It should be noted that similar reference numerals and letters denote similar items in the following drawings, and therefore, once an item is defined in one drawing, further definition and explanation thereof is not required in subsequent drawings.

[0040] In the description of the embodiments of the present invention, it should be noted that if the terms "upper", "lower", "horizontal", "inner", etc. indicate an orientation or positional relationship based on the orientation or positional relationship shown in the drawings, or the orientation or positional relationship in which the product of the invention is usually placed when in use, it is only for the convenience of describing the present invention and simplifying the description, and does not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present invention. In addition, the terms "first", "second", etc. are only used to distinguish the description, and cannot be understood as indicating or implying relative importance.

[0041] In addition, if the term "horizontal" appears, it does not mean that the component must be absolutely horizontal, but can be slightly tilted. For example, "horizontal" only means that its direction is more horizontal than "vertical", which does not mean that the structure must be completely horizontal, but can be slightly tilted.

[0042] In the description of the embodiments of the present invention, it is also necessary to explain that, unless otherwise clearly specified and limited, the terms "set", "install", "connect", and "connect" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be indirectly connected through an intermediate medium, or it can be the internal connection of two components. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.

[0043] The present invention is further described in detail below in conjunction with the accompanying drawings:

[0044] A method for preparing a carbon fiber epoxy resin composite material based on a cobalt-based metal organic framework and a synergistic flame retardant, comprising the following steps:

[0045] S1: Use polyurethane shell to coat ammonium polyphosphate to prepare PUAPP.

[0046] S2: ZIF-67 was coated on PUAPP to prepare ZIF-67@PUAPP;

[0047] S3: The successfully prepared ZIF-67@PUAPP is evenly dispersed into the epoxy resin E-51 system to obtain a mixture, and the mixture is evenly applied on the carbon fiber cloth and post-cured to obtain a ZIF-67@PUAPP / CF / EP composite material.

[0048] The flame-retardant microcapsule PUAPP was prepared by in-situ polymerization, and ZIF-67@PUAPP was prepared by co-precipitation on ammonium polyphosphate coated with polyurethane. The process is relatively simple and the reaction speed is fast. The Co3O4 produced during the combustion of ZIF-67 can promote the formation of a carbon layer, attenuate the oxygen on the surface of the composite material, and further make the carbon layer denser, thereby inhibiting the release of combustion gases produced during the decomposition of the composite material. In addition, the steam, N2 and NH3 produced during the combustion process help to dilute the oxygen and flammable gases on the surface of the composite material. During the combustion process, heat-absorbing water vapor will be generated, which is conducive to dilution and cooling, thereby achieving a better flame retardant effect.

[0049] In some embodiments, a method for preparing a carbon fiber epoxy resin composite material based on a cobalt-based metal organic framework and a synergistic flame retardant comprises the following steps:

[0050] (1) Using polyurethane shell to coat ammonium polyphosphate to prepare PUAPP

[0051] S101: Dissolve the measured amount of PEG2000 in 150 ml of polyvinyl alcohol solution to obtain solution A.

[0052] S102: adding measured HDI trimer, emulsifier OP-10, ammonium polyphosphate (APP), catalyst dibutyltin dilaurate, and solvent dimethyl sulfoxide (DMSO) into a 100 mL beaker, stirring with a magnetic stirrer for 30 min, and obtaining solution B after mixing evenly, in which HDI trimer and PEG2000 are used to prepare synthetic polyurethane;

[0053] S103: adding solution B dropwise into solution A and mixing them, dispersing them in a homogenizer at a speed of 10000 r / min for 20 min, taking out the emulsion and letting it stand for 20 min, and then adding it to a 250 mL three-necked flask to obtain a mixed solution C;

[0054] S104: The mixed solution C is slowly heated to 60° C. in a water bath and reacted for 0.5 h. A measured amount of chain extender 1,4-butanediol (BDO) is added and the temperature is raised to 80° C. and reacted for 4 h. After cooling to room temperature, PUAPP is obtained by centrifugation.

[0055] (2) Coating ZIF-67 on PUAPP to prepare ZIF-67@PUAPP

[0056] S201: Dissolve 2-methylimidazole in methanol to obtain a mixed solution D.

[0057] S202: Dissolve cobalt nitrate hexahydrate (Co(NO3)2·6H2O) in methanol to obtain a mixed solution E.

[0058] S203: dispersing PUAPP in methanol to obtain a mixed solution F;

[0059] S204: adding the mixed solution F dropwise into the mixed solution D, and performing ultrasonication for 30 minutes to obtain a mixed solution G, and then quickly pouring the mixed solution E into the mixed solution G, recorded as a mixed solution H;

[0060] S109: The mixed solution H is stirred at room temperature for 1 to 3 hours, allowed to stand for 24 hours, filtered, and washed three times with methanol to obtain ZIF-67@PUAPP.

[0061] Specifically, ZIF-67 is a material containing transition metal Co and a large amount of nitrogen. The metal oxides generated by the reaction can be used as polymer flame retardant enhancers and smoke suppressants. After PUAPP is coated with ZIF-67, the incompatibility between ammonium polyphosphate and epoxy resin interfaces can be further improved, thereby promoting the improvement of interface performance and overall material performance.

[0062] (3) The successfully prepared ZIF-67@PUAPP was evenly dispersed into the epoxy resin E-51 system to obtain a mixture, and the mixture was evenly applied on the carbon fiber cloth and post-cured to obtain the ZIF-67@PUAPP / CF / EP composite material.

[0063] S301: Weigh a certain amount of ZIF-67@PUAPP and evenly disperse it into the epoxy resin system. Stir the mixture in a water bath at 60°C for 2h, then add curing agent H256 to ensure that the mass ratio of resin to curing agent reaches 100:32. Then heat it in a water bath to make it flowable and evenly apply it on a 10cm×10cm carbon fiber cloth.

[0064] S302: placing the coated carbon cloth into a mold preheated at 90° C., and placing the mold in a hot press for curing, to obtain a composite material which is a CF / ZIF-67@PUAPP / EP composite material.

[0065] Preferably, the three-stage temperature-raising curing is performed, i.e., keeping the temperature at 90°C and normal pressure for 2 hours, then pressurizing to 5MPa, then heating to 120°C and keeping the temperature for 2 hours, and in the third stage, keeping the temperature at 150°C for 3 hours. The mass ratio of resin to curing agent in the epoxy resin system is 100:32.

[0066] In some embodiments, the mass fraction of polyvinyl alcohol in the polyvinyl alcohol solution in S101 is 1.5%;

[0067] Polyurethane was first successfully prepared from the HDI trimer in S102 and PEG2000 in S101, with a molar ratio of 1.2:1 and a mass ratio of polyurethane wall material to ammonium polyphosphate core material of 1:0.5;

[0068] The addition of chain extender BDO in S104 complies with the chain extension coefficient of 0.90.

[0069] In some embodiments, the usage ratio of 2-methylimidazole and methanol in S201 is (2-5) mmol: (12.5-31.25) mL;

[0070] The dosage ratio of cobalt nitrate hexahydrate and methanol in S202 is (0.5~1.5) mmol: (12.5~37.5) mL.

[0071] In some embodiments, a method for preparing a carbon fiber epoxy resin composite material based on a cobalt-based metal organic framework and a synergistic flame retardant comprises the following steps:

[0072] (1) Since carbon fibers need to be sizing before leaving the factory, and the sizing agent usually affects the fiber surface modification and bulk characterization results, the carbon fibers need to be cleaned before use to remove impurities such as the sizing agent. The specific operation is as follows: 6 pieces of carbon fibers are placed in a Soxhlet extractor filled with acetone, refluxed for 48 hours, and vacuum dried at 80°C for 24 hours.

[0073] (2) PUAPP was prepared by in situ polymerization.

[0074] First, 6.6 g of PEG2000 was dissolved in 150 ml of polyvinyl alcohol solution (mass fraction of 1.5%) to obtain solution A; secondly, 2 g of HDI trimer, 0.69 g of emulsifier OP-10, 4.25 g of ammonium polyphosphate (APP), 1 to 2 drops of dibutyltin dilaurate, and solvent dimethyl sulfoxide (DMSO) were added to a 100 mL beaker, and magnetic stirring was performed for 30 minutes to obtain solution B after mixing evenly; then solution B was added dropwise to solution A and mixed, and dispersed in a homogenizer at a speed of 10000 r / min for 15 minutes, and the emulsion was taken out and allowed to stand for 20 minutes and then added to a 250 mL three-necked flask to obtain a mixed solution C;

[0075] Finally, the mixed solution C was slowly heated to 60°C in a water bath, reacted for 0.5h, 112μL of 1,4-butanediol (BDO) was added, the temperature was raised to 80°C and maintained for 4h, cooled to room temperature, centrifuged to obtain PUAPP, and dried in a vacuum oven at 60°C for 24-48h.

[0076] (3) ZIF-67@PUAPP was prepared by co-precipitation and in situ growth methods

[0077] First, 2-methylimidazole was dissolved in methanol to obtain a mixed solution D, cobalt nitrate hexahydrate (Co(NO3)2·6H2O) was dissolved in methanol to obtain a mixed solution E, and PUAPP was dispersed in methanol to obtain a mixed solution F; then the mixed solution F was added dropwise to the mixed solution D, and ultrasonicated for 30 minutes to obtain a mixed solution G, and then the mixed solution E was quickly poured into the mixed solution G, recorded as mixed solution H; finally, the mixed solution H was stirred at room temperature for 1 to 3 hours, allowed to stand for 24 hours, then filtered, and washed three times with methanol to obtain ZIF-67@PUAPP.

[0078] (4) Preparation of ZIF-67@PUAPP / CF / EP composites

[0079] Weigh ZIF-67@PUAPP and evenly disperse it in the epoxy resin system. Stir the mixture in a water bath at 60℃ for 2h, then add curing agent H256 to ensure that the mass ratio of resin and curing agent reaches 100:32, then heat it in a water bath to make it flow, and evenly apply it on a 10cm×10cm carbon fiber cloth, then put the sample into a mold preheated at 90℃, and place the mold in a hot press. The preparation process of the composite material adopts a three-stage heating process, that is, 90℃ normal pressure insulation for 2h, then pressurized to 5MPa, then heated to 120℃ and kept warm for 2h, and the third stage keeps the temperature at 150℃ for 3h. After the mold is cooled to room temperature, demoulding is performed, and the obtained composite material is CF / ZIF-67@PUAPP / EP composite material. According to the test requirements, the obtained samples are cut to appropriate sizes for testing.

[0080] This application starts from the perspective of flame retardant modification of carbon fiber epoxy resin composites. First, polyurethane is used to coat ammonium polyphosphate to form PUAPP, and then ZIF-67 is prepared by coprecipitation and in-situ growth method to coat the surface of PUAPP, so as to improve the morphology and flame retardant properties of PUAPP, thereby introducing ZIF-67@PUAPP into the carbon fiber epoxy resin composite material to study the change law of the flame retardant properties of the composite material. At the same time, SEM, FTIR, XRD, cone calorimetry and other performance tests are used to test the surface microstructure and surface chemical properties of ZIF-67@PUAPP. The effect of the addition of ZIF-67@PUAPP on the flame retardant properties of carbon fiber epoxy resin composites is systematically studied, and the details are shown in the following examples:

[0081] Example 1

[0082] (1) Since carbon fibers need to be sizing before leaving the factory, and the sizing agent usually affects the fiber surface modification and bulk characterization results, the carbon fibers need to be cleaned before use to remove impurities such as the sizing agent. The specific operation is as follows: 6 pieces of carbon fibers are placed in a Soxhlet extractor filled with acetone, refluxed for 48 hours, and vacuum dried at 80°C for 24 hours.

[0083] (2) PUAPP was prepared by in situ polymerization.

[0084] First, 6.6 g of PEG2000 was dissolved in 150 ml of polyvinyl alcohol solution (mass fraction of 1.5%) to obtain solution A; secondly, 2 g of HDI trimer, 0.69 g of emulsifier OP-10, 4.25 g of ammonium polyphosphate (APP), 1 to 2 drops of dibutyltin dilaurate, and solvent dimethyl sulfoxide (DMSO) were added to a 100 mL beaker, and magnetic stirring was performed for 30 minutes to obtain solution B after mixing evenly; then solution B was added dropwise to solution A and mixed, and dispersed in a homogenizer at a speed of 10000 r / min for 15 minutes, and the emulsion was taken out and allowed to stand for 20 minutes and then added to a 250 mL three-necked flask to obtain a mixed solution C;

[0085] Finally, the mixed solution C was slowly heated to 60°C in a water bath, reacted for 0.5h, 112μL of 1,4-butanediol (BDO) was added, the temperature was raised to 80°C and maintained for 4h, cooled to room temperature, centrifuged to obtain PUAPP, and dried in a vacuum oven at 60°C for 24-48h.

[0086] (3) ZIF-67@PUAPP was prepared by co-precipitation and in situ growth methods

[0087] First, 164.2 mg of 2-methylimidazole was dissolved in 12.5 mL of methanol to obtain a mixed solution D, 145.5 mg of cobalt nitrate hexahydrate (Co(NO3)2·6H2O) was dissolved in 12.5 mL of methanol to obtain a mixed solution E, and 250 mg of PUAPP was dispersed in 25 mL of methanol to obtain a mixed solution F; then, the mixed solution F was added dropwise to the mixed solution D, and then ultrasonicated for 30 min to obtain a mixed solution G, and then the mixed solution E was quickly poured into the mixed solution G, recorded as a mixed solution H; finally, the mixed solution H was stirred at room temperature for 1 h, allowed to stand for 24 h, then filtered, and washed three times with methanol to obtain ZIF-67@PUAPP.

[0088] (4) Preparation of ZIF-67@PUAPP / CF / EP composites

[0089] Weigh ZIF-67@PUAPP and evenly disperse it in the epoxy resin system. Stir the mixture in a water bath at 60℃ for 2h, then add curing agent H256 to ensure that the mass ratio of resin and curing agent reaches 100:32, then heat it in a water bath to make it flow, and evenly apply it on a 10cm×10cm carbon fiber cloth, then put the sample into a mold preheated at 90℃, and place the mold in a hot press. The preparation process of the composite material adopts a three-stage heating process, that is, 90℃ normal pressure insulation for 2h, then pressurized to 5MPa, then heated to 120℃ and kept warm for 2h, and the third stage keeps the temperature at 150℃ for 3h. After the mold is cooled to room temperature, demoulding is performed, and the obtained composite material is CF / ZIF-67@PUAPP / EP composite material. According to the test requirements, the obtained samples are cut to appropriate sizes for testing.

[0090] Example 2

[0091] (1) Since carbon fibers need to be sizing before leaving the factory, and the sizing agent usually affects the fiber surface modification and bulk characterization results, the carbon fibers need to be cleaned before use to remove impurities such as the sizing agent. The specific operation is as follows: 6 pieces of carbon fibers are placed in a Soxhlet extractor filled with acetone, refluxed for 48 hours, and vacuum dried at 80°C for 24 hours.

[0092] (2) PUAPP was prepared by in situ polymerization.

[0093] First, 6.6 g of PEG2000 was dissolved in 150 ml of polyvinyl alcohol solution (mass fraction of 1.5%) to obtain solution A; secondly, 2 g of HDI trimer, 0.69 g of emulsifier OP-10, 4.25 g of ammonium polyphosphate (APP), 1 to 2 drops of dibutyltin dilaurate, and solvent dimethyl sulfoxide (DMSO) were added to a 100 mL beaker, and magnetic stirring was performed for 30 minutes to obtain solution B after mixing evenly; then solution B was added dropwise to solution A and mixed, and dispersed in a homogenizer at a speed of 10000 r / min for 15 minutes, and the emulsion was taken out and allowed to stand for 20 minutes and then added to a 250 mL three-necked flask to obtain a mixed solution C;

[0094] Finally, the mixed solution C was slowly heated to 60°C in a water bath, reacted for 0.5h, 112μL of 1,4-butanediol (BDO) was added, the temperature was raised to 80°C and maintained for 4h, cooled to room temperature, centrifuged to obtain PUAPP, and dried in a vacuum oven at 60°C for 24-48h.

[0095] (3) ZIF-67@PUAPP was prepared by co-precipitation and in situ growth methods

[0096] First, 328.4 mg of 2-methylimidazole was dissolved in 25 mL of methanol to obtain a mixed solution D, 291 mg of cobalt nitrate hexahydrate (Co(NO3)2·6H2O) was dissolved in 25 mL of methanol to obtain a mixed solution E, and 500 mg of PUAPP was dispersed in 25 mL of methanol to obtain a mixed solution F; then, the mixed solution F was added dropwise to the mixed solution D, and then ultrasonicated for 30 min to obtain a mixed solution G, and then the mixed solution E was quickly poured into the mixed solution G, recorded as a mixed solution H; finally, the mixed solution H was stirred at room temperature for 2 h, allowed to stand for 24 h, then filtered, and washed three times with methanol to obtain ZIF-67@PUAPP.

[0097] (4) Preparation of ZIF-67@PUAPP / CF / EP composites

[0098] Weigh ZIF-67@PUAPP and evenly disperse it in the epoxy resin system. Stir the mixture in a water bath at 60℃ for 2h, then add curing agent H256 to ensure that the mass ratio of resin and curing agent reaches 100:32, then heat it in a water bath to make it flow, and evenly apply it on a 10cm×10cm carbon fiber cloth, then put the sample into a mold preheated at 90℃, and place the mold in a hot press. The preparation process of the composite material adopts a three-stage heating process, that is, 90℃ normal pressure insulation for 2h, then pressurized to 5MPa, then heated to 120℃ and kept warm for 2h, and the third stage keeps the temperature at 150℃ for 3h. After the mold is cooled to room temperature, demoulding is performed, and the obtained composite material is CF / ZIF-67@PUAPP / EP composite material. According to the test requirements, the obtained samples are cut to appropriate sizes for testing.

[0099] Example 3

[0100] (1) Since carbon fibers need to be sizing before leaving the factory, and the sizing agent usually affects the fiber surface modification and bulk characterization results, the carbon fibers need to be cleaned before use to remove impurities such as the sizing agent. The specific operation is as follows: 6 pieces of carbon fibers are placed in a Soxhlet extractor filled with acetone, refluxed for 48 hours, and vacuum dried at 80°C for 24 hours.

[0101] (2) PUAPP was prepared by in situ polymerization.

[0102] First, 6.6 g of PEG2000 was dissolved in 150 ml of polyvinyl alcohol solution (mass fraction of 1.5%) to obtain solution A; secondly, 2 g of HDI trimer, 0.69 g of emulsifier OP-10, 4.25 g of ammonium polyphosphate (APP), 1 to 2 drops of dibutyltin dilaurate, and solvent dimethyl sulfoxide (DMSO) were added to a 100 mL beaker, and magnetic stirring was performed for 30 minutes to obtain solution B after mixing evenly; then solution B was added dropwise to solution A and mixed, and dispersed in a homogenizer at a speed of 10000 r / min for 15 minutes, and the emulsion was taken out and allowed to stand for 20 minutes and then added to a 250 mL three-necked flask to obtain a mixed solution C;

[0103] Finally, the mixed solution C was slowly heated to 60°C in a water bath, reacted for 0.5h, 112μL of 1,4-butanediol (BDO) was added, the temperature was raised to 80°C and maintained for 4h, cooled to room temperature, centrifuged to obtain PUAPP, and dried in a vacuum oven at 60°C for 24-48h.

[0104] (3) ZIF-67@PUAPP was prepared by co-precipitation and in situ growth methods

[0105] First, 410.5 mg of 2-methylimidazole was dissolved in 31.25 mL of methanol to obtain a mixed solution D, and 436.5 mg of cobalt nitrate hexahydrate (Co(NO3)2·6H2O) was dissolved in 37.5 mL of methanol to obtain a mixed solution E. At the same time, 1 g of PUAPP was dispersed in 25 mL of methanol to obtain a mixed solution F. Then, the mixed solution F was added dropwise to the mixed solution D, and ultrasonicated for 30 min to obtain a mixed solution G. Then, the mixed solution E was quickly poured into the mixed solution G, recorded as a mixed solution H. Finally, the mixed solution E was stirred at room temperature for 3 h, allowed to stand for 24 h, then filtered, and washed three times with methanol to obtain ZIF-67@PUAPP.

[0106] (4) Preparation of ZIF-67@PUAPP / CF / EP composites

[0107] Weigh ZIF-67@PUAPP and evenly disperse it in the epoxy resin system. Stir the mixture in a water bath at 60℃ for 2h, then add curing agent H256 to ensure that the mass ratio of resin and curing agent reaches 100:32, then heat it in a water bath to make it flow, and evenly apply it on a 10cm×10cm carbon fiber cloth, then put the sample into a mold preheated at 90℃, and place the mold in a hot press. The preparation process of the composite material adopts a three-stage heating process, that is, 90℃ normal pressure insulation for 2h, then pressurized to 5MPa, then heated to 120℃ and kept warm for 2h, and the third stage keeps the temperature at 150℃ for 3h. After the mold is cooled to room temperature, demoulding is performed, and the obtained composite material is CF / ZIF-67@PUAPP / EP composite material. According to the test requirements, the obtained samples are cut to appropriate sizes for testing.

[0108] In order to characterize the morphological features, the target product was tested by Fourier transform infrared spectroscopy (FTIR), see Figure 1 In the infrared spectrum, it can be seen that the ZIF-67@PUAPP has a 3200-3400 cm -1 There is a cooperative stretching vibration peak of NH and OH at 700 cm -1 The stretching vibration peak of Co-O also appears nearby, at 430 cm -1 The stretching vibration peak of Co-N and the characteristic peak of ammonium polyphosphate also appeared, which preliminarily proved the successful synthesis of ZIF-67@PUAPP.

[0109] In order to verify the crystal structure characteristics of the material, the product was tested by X-ray powder diffraction (XRD). Figure 2 Figure 3 is the XRD spectra of ZIF-67@PUAPP, PUAPP and APP. The XRD of ZIF-67@PUAPP contains both the topological structure of ZIF-67 and the characteristic diffraction peaks of APP. It can also be seen from XRD that after coating with ZIF-67, the lattice plane growth of APP is inhibited, but the diffraction peak still appears, proving that coating with ZIF-67 will not affect the performance of ammonium polyphosphate itself.

[0110] Figure 3 Scanning diagram of ZIF-67@PUAPP before and after coating. Figure a shows ammonium polyphosphate, Figure b shows PUAPP, and Figure c shows ZIF-67@PUAPP. It can be seen that a lot of ZIF-67 nanoparticles are loaded on the surface of PUAPP, and the nanomorphology of ZIF-67 has not been deformed, proving that the coating is successful.

[0111] Figure 4The flame retardant performance test. (a) is the maximum heat release rate (PHRR) diagram; (b) is the maximum total heat release (THR) diagram. It can be observed from the figure that the carbon fiber epoxy composite material without any flame retardant has the highest maximum heat release rate (PHRR) and maximum total heat release (THR). After adding ZIF-67@PUAPP, its PHRR decreased by 43.33% and THR decreased by 22.52%. It shows that the fire hazard is greatly reduced and the flame retardant performance is improved.

[0112] In summary, the present invention enhances the interfacial compatibility between epoxy resin and ammonium polyphosphate without sacrificing the original performance of ammonium polyphosphate, and improves the flame retardant properties of carbon fiber epoxy composites. First, a flame retardant microcapsule with polyurethane as shell material and ammonium polyphosphate as core material is prepared, and then ZIF-67 is used to coat the surface of PUAPP and add the carbon fiber epoxy resin composite material. At the same time, the changes in the morphology, thermal stability and flame retardant properties of ZIF-67@PUAPP when it acts on the carbon fiber epoxy matrix are studied. After PUAPP is coated with ZIF-67, the poor water resistance of APP is changed, and the compatibility with the epoxy resin matrix is ​​improved. Among them, the Co3O4 generated during the combustion of ZIF-67 can promote the formation of the carbon layer, attenuate the oxygen on the surface of the composite material, and further make the carbon layer denser, thereby inhibiting the release of the combustion gas generated during the decomposition of the composite material. In addition, the steam, N2 and NH3 generated during the combustion process help dilute the oxygen and flammable gas on the surface of the composite material, and absorb hot water vapor will be generated during the combustion process, which is conducive to dilution and cooling, thereby achieving a better flame retardant effect. A bridge is built between APP and the epoxy resin matrix, which greatly improves the flame retardancy of carbon fiber epoxy resin composites.

[0113] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing a carbon fiber epoxy resin composite material based on a cobalt-based metal organic framework and a synergistic flame retardant, characterized in that: include: S1: using polyurethane shell to coat ammonium polyphosphate to prepare PUAPP; S2: Coating ZIF-67 on PUAPP to prepare ZIF-67@PUAPP; S3: The successfully prepared ZIF-67@PUAPP is evenly dispersed into the epoxy resin E-51 system to obtain a mixture, and the mixture is evenly applied on the carbon fiber cloth and post-cured to obtain a ZIF-67@PUAPP / CF / EP composite material.

2. The method for preparing a carbon fiber epoxy resin composite material based on a cobalt-based metal organic framework synergistic flame retardant according to claim 1, characterized in that: The S1 specifically includes: S101: Dissolve PEG2000 in polyvinyl alcohol solution to obtain solution A S102: mixing HDI trimer, emulsifier OP-10, ammonium polyphosphate, catalyst dibutyltin dilaurate, and solvent dimethyl sulfoxide, and stirring until the mixture is uniform to obtain solution B; S103: adding solution B dropwise into solution A to mix and disperse, and after dispersion, taking out the emulsion and letting it stand to obtain a mixed solution C; S104: The mixed solution C is slowly heated in a water bath for reaction, and a chain extender 1,4-butanediol is added, and the temperature is raised for reaction. After the reaction is completed, the solution is cooled to room temperature and centrifuged to obtain PUAPP.

3. The method for preparing a carbon fiber epoxy resin composite material based on a cobalt-based metal organic framework synergistic flame retardant according to claim 2, characterized in that: The mass fraction of polyvinyl alcohol in solution A in S101 is 1.5%; the molar ratio of HDI trimer in S102 and PEG2000 in S101 is 1.2:1, and the HDI trimer and PEG2000 are used to prepare synthetic polyurethane, and the mass ratio of polyurethane to ammonium polyphosphate is 1:0.

5.

4. The method for preparing a carbon fiber epoxy resin composite material based on a cobalt-based metal organic framework synergistic flame retardant according to claim 2, characterized in that: The addition of chain extender BDO in S104 complies with the chain extension coefficient of 0.

90.

5. The method for preparing a carbon fiber epoxy resin composite material based on a cobalt-based metal organic framework synergistic flame retardant according to claim 1, characterized in that: The S2 specifically includes: S201: Dissolve 2-methylimidazole in methanol to obtain a mixed solution D. S202: Dissolve cobalt nitrate hexahydrate (Co(NO3)2·6H2O) in methanol to obtain a mixed solution E. S203: dispersing PUAPP in methanol to obtain a mixed solution F; S204: adding the mixed solution F dropwise into the mixed solution D to obtain a mixed solution G, and then quickly pouring the mixed solution E into the mixed solution G, recorded as a mixed solution H; S205: The mixed solution H is stirred at room temperature, allowed to stand, and then filtered, and washed with methanol to obtain ZIF-67@PUAPP.

6. The method for preparing a carbon fiber epoxy resin composite material based on a cobalt-based metal organic framework synergistic flame retardant according to claim 5, characterized in that: The usage ratio of 2-methylimidazole and methanol in the S201 is (2-5) mmol: (12.5-31.25) mL.

7. The method for preparing a carbon fiber epoxy resin composite material based on a cobalt-based metal organic framework and a synergistic flame retardant according to claim 5, characterized in that: The usage ratio of cobalt nitrate hexahydrate and methanol in the S202 is (0.5-1.5) mmol: (12.5-37.5) mL.

8. The method for preparing a carbon fiber epoxy resin composite material based on a cobalt-based metal organic framework and a synergistic flame retardant according to claim 1, characterized in that: The S3 specifically includes: S301: Disperse ZIF-67@PUAPP evenly into the epoxy resin system, stir evenly in a water bath, add curing agent H256, ensure that the mass ratio of resin to curing agent reaches 100:32, then heat it to make it flowable, and evenly apply it on the carbon fiber cloth; S302: Place the coated carbon fiber cloth into a preheated mold, and perform three-stage temperature rise curing to obtain a ZIF-67@PUAPP / CF / EP composite material.

9. The method for preparing a carbon fiber epoxy resin composite material based on a cobalt-based metal organic framework and a synergistic flame retardant according to claim 8, characterized in that: The three-stage temperature rise curing is specifically to keep the temperature at 90°C and normal pressure for 2 hours, then pressurize to 5MPa, then heat to 120°C and keep the temperature for 2 hours, and in the third stage, keep the temperature at 150°C for 3 hours.

10. A carbon fiber epoxy resin composite material based on a cobalt-based metal organic framework and a synergistic flame retardant, characterized in that: The method is prepared by any one of claims 1 to 9.

Citation Information

Patent Citations

  • Method for preparing microcapsule coated ammonium polyphosphate

    CN101972620A

  • Preparation method for metal organic framework structure wrapped ammonium polyphosphate fire retardant and application

    CN109320910A

  • Functional heat-insulation fireproof waterproof anticorrosive paint

    CN114517036A

  • Preparation method and application of layer-by-layer self-assembled flame-retardant material

    CN116515161A

  • Bio-based microencapsulated mfapp flame retardant, and preparation method therefor and use thereof

    WO2023050316A1

Cited By

  • Composite flame retardant for epoxy resin and preparation method thereof

    CN119463298A

  • Impact-resistant ceramic polymer composite material and preparation method thereof

    CN120399403A