Wiring board and method for manufacturing same
By forming a cover film and a via conductor between the first conductive layer and the second insulating layer in the wiring substrate, the problem of low adhesion strength between the insulating layer and the conductive layer is solved, and higher adhesion strength and conductive stability are achieved. sex.
Patent Information
- Application Number
- CN202410292190.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-04-11
- Filing Date
- 2024-03-14
- Publication Date
- 2024-10-18
AI Technical Summary
In existing wiring substrates, the adhesion strength between the insulating layer and the conductive layer is low. Especially after the through-hole is formed in the covering film on the upper surface of the pad, the existence of the peeling portion causes the adhesion strength between the pad and the insulating layer to decrease.
By forming a cover film between the first conductive layer and the second insulating layer to improve the adhesion strength, and forming a via conductor on the upper surface of the pad, the peeling part is located within 15 μm around the outer edge of the through hole to enhance the connection between the pad and Insulating layer connection.
The adhesion strength between the liner and the insulating layer is improved, the resistance rise of the conductive layer is suppressed, and the conductive stability and adhesion strength are improved through uniform covering film and conductor filling.
Smart Images

Figure CN118804469A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a wiring substrate having a via-hole conductor and a method for manufacturing the same. Background Art
[0002] As such a conventional wiring substrate, there is known a wiring substrate in which a conductive layer is covered with a cover film in order to improve the adhesion strength between the conductive layer and the insulating layer thereon (for example, refer to Patent Document 1).
[0003] Patent Document 1: Japanese Patent Application Publication No. 2021-5646 ( Figure 1 )
[0004] However, in the above-mentioned conventional wiring substrate, in order to connect the via conductor penetrating the insulating layer to the pad included in the conductive layer, a through hole is formed in the cover film on the upper surface of the pad. Moreover, a peeling portion is formed between the insulating layer and the conductive layer starting from the through hole, and the peeling portion extends from the upper surface of the pad to the side surface, and the reduction of the adhesion strength between the pad and the insulating layer thereon becomes a problem. Therefore, the object of the present invention is to provide a wiring substrate in which the adhesion strength between the pad and the insulating layer thereon is higher than that in the past. Summary of the invention
[0005] A wiring substrate according to one embodiment of the present invention comprises: a first insulating layer; a first conductive layer formed in a manner that partially covers the upper surface of the first insulating layer; a second insulating layer stacked on the first insulating layer via the first conductive layer; a second conductive layer formed in a manner that partially covers the upper surface of the second insulating layer; a covering film that covers the first conductive layer in order to improve the adhesion strength between the first conductive layer and the second insulating layer; and a via conductor formed in a through hole that penetrates the upper surface of the pad and the covering film and the second insulating layer in order to connect a pad included in the first conductive layer to the second conductive layer, wherein the root mean square roughness of the upper surface of the pad is greater than 0.10 μm and less than 0.23 μm, and a peeling portion is formed between the pad and the second insulating layer, and the peeling portion is within a range of 15 μm around the outer edge of the through hole on the upper surface of the pad.
[0006] In a method for manufacturing a wiring substrate of one embodiment of the present invention, in the wiring substrate, a pad included in a first conductive layer under an insulating layer is connected to a second conductive layer on the insulating layer through a via conductor, wherein the method for manufacturing the wiring substrate includes the following steps: covering the first conductive layer with a covering film in order to improve the sealing strength between the first conductive layer and the insulating layer; forming a through hole for forming the via conductor in the covering film and the insulating layer on the upper surface of the pad; forming the via conductor and the second conductive layer; and forming a peeling portion between the pad and the insulating layer, the size of the peeling portion being within a range of 15 μm around the outer edge of the through hole on the upper surface of the pad. BRIEF DESCRIPTION OF THE DRAWINGS
[0007] Figure 1 This is a cross-sectional view of a wiring substrate according to one embodiment of the present invention.
[0008] Figure 2 It is a top cross-sectional view of a wiring substrate.
[0009] Figure 3 It is a cross-sectional view showing the manufacturing process of the wiring substrate.
[0010] Figure 4 It is a cross-sectional view showing the manufacturing process of the wiring substrate.
[0011] Figure 5 It is a cross-sectional view showing the manufacturing process of the wiring substrate.
[0012] Description of symbols
[0013] 10: wiring substrate; 21: first insulating layer; 22: second insulating layer; 31: first conductive layer; 32: second conductive layer; 31P, 32P: pads; 33: via conductor; 33H: via (through hole); 40: cover film; 40H: through hole; 50: peeling portion. DETAILED DESCRIPTION
[0014] Below, refer to Figure 1 to Figure 5 The wiring substrate 10 of the present embodiment is a multilayer laminated substrate in which a plurality of conductive layers 30 and a plurality of insulating layers 20 are alternately laminated on both sides of a core substrate and a solder resist layer (not shown) is laminated on the outermost surface. Figure 1 Only two insulating layers 20 and two conductive layers 30 are shown in (A). Figure 1 The lower insulating layer 20 in (A) is referred to as a first insulating layer 21, and the upper insulating layer 20 is referred to as a second insulating layer 22. In addition, the conductive layer 30 is also referred to as a first conductive layer 31 and a second conductive layer 32 in the same manner.
[0015] The first conductive layer 31 and the second conductive layer 32 are, for example, copper-plated, and the conductor is composed of a chemically plated layer 30A and an electroplated layer 30B. The first conductive layer 31 and the second conductive layer 32 include a plurality of pads 31P and 32P. A via hole 33H equivalent to the "through hole" in the claims is formed between the pads 31P and 32P that overlap in the stacking direction in the second insulating layer 22, and a via conductor 33 that connects the pads 31P and 32P to each other is formed in the via hole 33H. In addition, the plurality of pads 31P and 32P are formed, for example, in a circular shape when viewed from above, and are arranged in such a manner that the central axis of the via conductor 33, whose diameter decreases downward, passes through the center of each pad 31P and 32P (see Figure 2 ).
[0016] The wiring substrate 10 of the present embodiment is a high-speed transmission substrate. In order to suppress the increase in impedance caused by the skin effect, the surface roughness of the surface of the conductive layer 30 including the first conductive layer 31 and the second conductive layer 32 is, for example, about 0.05 μm to 0.2 μm. In addition, in order to improve the adhesion strength between the conductive layer 30 including these first conductive layer 31 and the second conductive layer 32 and the insulating layer 20 including the second insulating layer 22 stacked thereon, the conductive layer 30 is covered with a cover film 40.
[0017] The cover film 40 is formed of a material that can be bonded to both the insulating layer 20 and the conductive layer 30, for example, a silane coupling agent containing a silane compound is used. In addition, the cover film 40 covers the portion of the insulating layer 20 exposed from the conductive layer 30 in addition to the upper surface and side surfaces of the conductive layer 30. Furthermore, the thickness of the cover film 40 is substantially uniform, for example, 0.02 μm to 0.5 μm.
[0018] Furthermore, the cover film 40 is provided on all the conductive layers 30, but may be provided on only a part of the conductive layers 30 (for example, provided only on the first conductive layer 31). Figure 1 In (A), in addition to the conductive layer 30, the portion of the insulating layer 20 exposed from the conductive layer 30 is also covered by the covering film 40, but for example, only the surface (i.e., the upper surface and the side surface) of the conductive layer 30 may be covered by the covering film 40. Furthermore, the thickness of the covering film 40 may be different between the surface of the conductive layer 30 and the surface of the insulating layer 20.
[0019] In addition, a through hole 40H (see FIG. 40H ) for connecting to the via conductor 33 is formed in the cover film 40 on the upper surface 31A of the pad 31P. Figure 4 (A)). Furthermore, a peeling portion 50 is formed with the through hole 40H as a starting point.
[0020] like Figure 1 (B) and Figure 2As shown, the stripping portion 50 extends between the upper surface 31A of the pad 31P and the second insulating layer 22, and becomes a roughly annular shape surrounding the via conductor 33. Specifically, with respect to the stripping portion 50, the width L1 between the lower end portion of the via conductor 33 (specifically, the lower end opening edge 22K of the through hole 22H of the second insulating layer 22 in the via hole 33H forming the via conductor 33, which is equivalent to the "outer edge of the through hole" in the claims) and the front end portion is within a range of 15 μm or less (specifically, within a range of 5 μm to 15 μm, preferably within a range of 5 μm to 10 μm). In addition, the shortest distance L2 from the lower end portion of the via conductor 33 (the lower end opening edge 22K) to the outer edge of the upper surface 31A of the pad 31P is greater than 15 μm. Thus, the stripping portion 50 is accommodated within the upper surface 31A of the pad 31P. More specifically, even in the portion where the width L1 of the peeling portion 50 is the widest, the width of the peeling portion 50 relative to the distance L2 is suppressed to, for example, 60% or less (preferably 50% or less).
[0021] The peeling portion 50 is filled with the conductor (chemical plating layer 30A and electroplating layer 30B) constituting the via conductor 33. Figure 2 As shown, the stripping portion 50 is filled with a conductor in a manner extending from the outer edge of the via-hole conductor 33 toward the outside. Figure 2 In the example shown, the conductor is filled up to the front end of the peeling portion 50 in a part in the circumferential direction.
[0022] In addition, the peeling portion 50 only needs to be formed between the upper surface 31A of the pad 31P and the second insulating layer 22. For example, the peeling portion 50 can be formed along the boundary between the upper surface 31A of the pad 31P and the covering film 40, or along the boundary between the covering film 40 and the second insulating layer 22, or multiple peeling portions 50 can be formed in the thickness direction of the covering film 40.
[0023] In addition, the peeling portion 50 may not be filled with a conductor, or may be filled with a conductor as a whole. In addition, the conductor filled in the peeling portion 50 may be continuous with the conductor constituting the via-hole conductor 33, or may be a plurality of conductors, such as granular ones, which are discontinuous with the conductor constituting the via-hole conductor 33. Furthermore, the portion of the peeling portion 50 not filled with a conductor may be a void, for example, a state where the residue of the cover film 40 is clogged.
[0024] The wiring substrate 10 of the present invention is manufactured as follows. (1) A core substrate (not shown) is prepared, a first insulating layer 21 is stacked on the conductive layers on both sides of the core substrate by a known method, and a first conductive layer 31 (including a plurality of pads 31P) is formed on the first insulating layer 21. Figure 3At this time, the surface of the first conductive layer 31 (specifically, the upper surface and the side surface) is not roughened, or is slightly roughened. Thus, the root mean square roughness (Rq) of the surface of the first conductive layer 31 is greater than or equal to 0.10 μm and less than or equal to 0.23 μm.
[0025] (2) Then, Figure 3 As shown in (B), the upper surface and side surfaces of the first conductive layer 31 and the portion of the first insulating layer 21 exposed from the first conductive layer 31 are covered with the cover film 40. At this time, the cover film 40 is formed substantially uniformly with a thickness of, for example, 0.02 μm to 0.5 μm or less.
[0026] (3) Figure 3 As shown in (C), the second insulating layer 22 is stacked on the cover film 40. This improves the adhesion strength between the first conductive layer 31 and the second insulating layer 22.
[0027] (4) Next, by laser irradiation, a via hole 33H is formed that penetrates the second insulating layer 22 and the cover film 40 on the upper surface 31A of the pad 31P (see Figure 4 (A)). Moreover, the lower end of the via hole 33H becomes the through hole 40H of the above-mentioned cover film 40, and the upper side thereof becomes the through hole 22H of the second insulating layer 22. Figure 4 In the Figure 1 The pad 31P portion to which the via conductor 33 is connected in the first conductive layer 31 shown in (A).
[0028] (5) The inside of the via hole 33H is cleaned (desmear treatment) to remove the residue of the cover film 40 adhering to the upper surface 31A of the pad 31P.
[0029] (6) Soft etching is performed as a pre-treatment for chemical plating. Figure 4 As shown in (B), the covering film 40 is dissolved from the surface of the through hole 40H of the covering film 40, and the peeling portion 50 is formed between the second insulating layer 22 and the pad 31P. In addition, the plating layer 30B is dissolved from the upper surface 31A of the exposed pad 31P, and the center portion of the upper surface 31A is slightly concave. Here, in this embodiment, the time, number of times or concentration of the immersion in the liquid medicine is adjusted so that the width L1 of the peeling portion 50 between the lower end opening edge 22K of the through hole 22H of the second insulating layer 22 and the front end is within the range of 15μm (specifically, the range of 5μm to 15μm or less, preferably the range of 5μm to 10μm or less).
[0030] (7) Next, chemical plating is performed. Specifically, the substrate is immersed in a chemical plating solution such as Figure 1 (B) and Figure 5 As shown in (A), the chemical plating layer 30A is formed on the inner surface of the via hole 33H and the portion of the pad 31P exposed from the cover film 40. In addition, at this time, the chemical plating liquid enters the stripping portion 50, and the chemical plating layer 30A is also formed in the stripping portion 50 (refer to Figure 1 (B) and Figure 2 ).
[0031] It should be noted that, in order to facilitate the formation of the chemical plating layer 30A in the release portion 50 , for example, other pretreatment may be performed after the soft etching, or the concentration of the chemical solution, the immersion time or the number of times may be adjusted during the chemical plating treatment.
[0032] (8) The plating resist 11 is stacked in a predetermined pattern on the chemical plating layer 30A.
[0033] (9) Then, electroplating treatment is performed, such as Figure 5 As shown in (B), the via hole 33H is filled with electroplating to form the via conductor 33, and the electroplating layer 30B is formed on the portion of the chemical plating layer 30A exposed from the plating resist 11. In addition, at this time, the electroplating layer 30B is formed on the chemical plating layer 30A in the peeling portion 50, and the peeling portion 50 is filled with a conductor continuous with the conductor constituting the via conductor 33 (see Figure 1 (B) and Figure 2 ).
[0034] Furthermore, in order to facilitate the formation of the electroplated layer 30B on the chemically plated layer 30A of the peeling portion 50 , for example, the concentration of the chemical solution, the immersion time, or the number of times may be adjusted during the electroplating process.
[0035] (10) Next, the plating resist 11 is peeled off, and the chemical plating layer 30A on the lower side of the plating resist 11 is removed. Then, the second conductive layer 32 is formed by using the remaining chemical plating layer 30A and the electroplating layer 30B (see Figure 1 Here, similarly to the first conductive layer 31, the surface of the second conductive layer 32 is not subjected to roughening treatment, or is subjected to roughening treatment to a slightly roughened degree, and the root mean square roughness (Rq) of the surface is 0.10 μm or more and 0.23 μm or less.
[0036] (11) The above steps (2) to (10) are repeated to stack a solder resist layer on the outermost insulating layer 20. Thus, the wiring board 10 is completed.
[0037] The above is a description of the structure of the wiring substrate 10 of the present embodiment and its manufacturing method. Thus, in the wiring substrate 10 of the present embodiment, the peeling portion 50 between the pad 31P included in the first conductive layer 31 and the second insulating layer 22 thereon is contained within the upper surface 31A of the pad 31P, so that the adhesion strength between the pad 31P and the second insulating layer 22 thereon is higher than that of the conventional wiring substrate in which the peeling portion 50 reaches the side surface 31B of the pad 31P.
[0038] Furthermore, in the present embodiment, not only is the peeling portion 50 confined within the upper surface 31A of the pad 31P, but the width L1 of the peeling portion 50 is suppressed to, for example, a range of less than 60% (preferably less than 50%) relative to the shortest distance L2 from the lower end portion of the via conductor 33 (lower end opening edge 22K) to the outer edge portion of the upper surface 31A of the pad 31P, thereby further improving the adhesion strength between the pad 31P and the second insulating layer 22 thereon.
[0039] Furthermore, in the present embodiment, the peeling portion 50 is filled with the conductor (chemical plating layer 30A and electroplating layer 30B) constituting the via-hole conductor 33 , and the conduction between the pad 31P and the via-hole conductor 33 is stable.
[0040] In the present embodiment, by setting the thickness of the cover film 40 to 0.02 μm to 0.5 μm, the peeling portion 50 between the pad 31P and the second insulating layer 22 can be easily contained within 15 μm around the via conductor 33 (the through hole 40H or the lower opening edge 22K of the cover film 40 ).
[0041] [Other embodiments]
[0042] (1) In the above embodiment, the laminated conductive layer is described as an example, but the present invention is not limited to this. For example, the structure of the present invention may be applied to a conductive layer of a core substrate.
[0043] (2) In the above embodiment, an example is given in which the portion of the peeling portion 50 with the largest width L1 is 60% or less relative to the distance L2, but the present invention is not limited thereto. For example, the area of the largest portion of the peeling portion 50 may be 60% or less (preferably 50% or less) relative to the area of the upper surface 31A of the pad 31P excluding the lower end of the via conductor 33 in the stacking direction. In addition, the area of the largest portion of the peeling portion 50 in the stacking direction may be replaced by, for example, the area of the boundary portion between the pad 31P and the cover film 40 or the area of the boundary portion between the cover film 40 and the second insulating layer 22.
[0044] In addition, in this specification and the drawings, specific examples of the technology included in the claims are disclosed, but the technology described in the claims is not limited to these specific examples, and also includes examples obtained by making various modifications and changes to the specific examples, and also includes examples obtained by taking out a part from the specific examples separately.
Claims
1. A wiring substrate, comprising: a first insulating layer; a first conductive layer formed in a manner of partially covering an upper surface of the first insulating layer; a second insulating layer stacked on the first insulating layer via the first conductive layer; a second conductive layer formed in a manner of partially covering an upper surface of the second insulating layer; a covering film covering the first conductive layer in order to improve the adhesion strength between the first conductive layer and the second insulating layer; as well as a via conductor formed in a through hole penetrating the cover film and the second insulating layer on the upper surface of the pad in order to connect the pad included in the first conductive layer to the second conductive layer, in, The root mean square roughness of the upper surface of the liner is not less than 0.10 μm and not more than 0.23 μm, A peeling portion is formed between the liner and the second insulating layer, The peeling portion is located within a range of 15 μm around the outer edge of the through hole on the upper surface of the liner.
2. The wiring substrate according to claim 1, wherein: The thickness of the covering film is 0.02 μm to 0.5 μm.
3. The wiring substrate according to claim 1 or 2, wherein: The release portion is located within 60% of a distance from an outer edge of the through hole to an outer edge of the liner on the upper surface of the liner.
4. The wiring substrate according to claim 1 or 2, wherein: The peeling portion is filled with a conductor constituting the via-hole conductor.
5. A method for manufacturing a wiring substrate, in which a pad included in a first conductive layer below an insulating layer is connected to a second conductive layer on the insulating layer through a via conductor, in, The manufacturing method of the wiring substrate comprises the following steps: In order to improve the adhesion strength between the first conductive layer and the insulating layer, the first conductive layer is covered with a cover film; forming a through hole for forming the via conductor in the cover film and the insulating layer on the upper surface of the pad; forming the via conductor and the second conductive layer; as well as A peeling portion is formed between the liner and the insulating layer, and the size of the peeling portion is within a range of 15 μm around the outer edge of the through hole on the upper surface of the liner.
6. The method for manufacturing a wiring substrate according to claim 5, wherein: The root mean square roughness of the upper surface of the pad included in the first conductive layer is greater than or equal to 0.10 μm and less than or equal to 0.23 μm.
7. The method for manufacturing a wiring substrate according to claim 5 or 6, wherein: The step of forming the cover film includes the step of forming the cover film to have a thickness of 0.02 μm to 0.5 μm.
8. The method for manufacturing a wiring substrate according to claim 5 or 6, wherein: The manufacturing method of the wiring board includes the step of filling the peeling portion with a conductor constituting the via-hole conductor.