High-strength steel sheet and method for producing same
By adjusting the microstructure of the steel plate, especially the proportion of tempered martensite and austenite and the heat treatment conditions, the deficiencies of high-strength steel plates in terms of tensile strength, yield ratio and flatness are solved, and efficient automotive applications are realized. Component materials.
Patent Information
- Application Number
- CN202380027218.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-25
- Filing Date
- 2023-01-30
- Publication Date
- 2024-10-18
AI Technical Summary
Existing high-strength steel plates have deficiencies in tensile strength, plate width flatness and processing embrittlement resistance, making it difficult to meet the excellent performance requirements of automotive parts.
By setting the amount of tempered martensite to more than 90%, the amount of retained austenite less than 3%, the total amount of ferrite and bainitic ferrite less than 10%, and controlling the original austenite grain size and maximum lath The occupancy rate of bundles is less than 70%. Combined with specific hot rolling and annealing treatments, high-strength steel plates with tensile strength of more than 1180MPa, yield ratio of more than 85%, excellent flatness in the plate width direction and resistance to processing embrittlement can be produced.
A high-strength steel plate with a TS of more than 1180MPa and a YR of more than 85% has been realized, which improves the flatness and processing embrittlement resistance in the width direction of the plate. It is suitable for automotive structural components and promotes the lightweight of the car body and the improvement of fuel efficiency.
Smart Images

Figure CN118804993A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a high-strength steel sheet having excellent tensile strength, flatness in the sheet width direction, and resistance to work embrittlement, and a method for producing the same. The high-strength steel sheet of the present invention can be suitably used as a structural member such as an automobile component. Background Art
[0002] In order to balance the reduction of CO2 emissions through vehicle weight reduction and the improvement of collision resistance through vehicle body weight reduction, the strength of thin steel sheets for automobiles is being increased, and new legal restrictions are also being introduced. Therefore, in order to increase the strength of the vehicle body, the use of high-strength steel sheets with a tensile strength (TS) of 1180MPa or above is increasing in the main structural parts of automobiles.
[0003] High-strength steel sheets used in automobiles require excellent resistance to work embrittlement and excellent yield ratio from the perspective of component performance. For example, in frame components such as automobile bumpers, it is preferred to use high-strength steel sheets that have excellent resistance to work embrittlement without embrittlement due to press forming and excellent impact absorption during YR-related collisions.
[0004] In addition, high-strength steel sheets used in automobiles are also required to have excellent flatness. Patent Document 1 states that the warping of steel sheets has an adverse effect on operational failures in forming lines and the dimensional accuracy of products. The present inventors have repeatedly conducted in-depth studies and found that the dimensional accuracy of products is not only affected by the warping of steel sheets, but also by the flatness in the width direction of the sheet evaluated by steepness. For example, in order to achieve excellent dimensional accuracy, the steepness in the width direction is preferably 0.02 or less.
[0005] In response to these requirements, for example, Patent Document 2 provides a high-strength steel sheet having a tensile strength of 1100 MPa or more and excellent in YR, surface properties and weldability, and a method for manufacturing the same. However, the technology described in Patent Document 2 does not take into account the flatness in the sheet width direction and the work embrittlement resistance characteristics.
[0006] Patent Document 3 provides a hot-dip galvanized steel sheet having excellent press formability and low-temperature toughness and having a tensile strength of 980 MPa or more and a method for manufacturing the same. However, the technology described in Patent Document 3 can improve the embrittlement of the steel sheet caused by temperature reduction, but does not consider the embrittlement of the steel sheet caused by processing. The flatness in the width direction of the sheet is also not considered.
[0007] Prior art literature
[0008] Patent Literature
[0009] Patent Document 1: Japanese Patent No. 4947176
[0010] Patent Document 2: Japanese Patent No. 6525114
[0011] Patent Document 3: Japanese Patent No. 6777272
[0012] Non-patent literature
[0013] Non-patent document 1: Intelligent Processing Magazine, 2013, Vol. 2, No. 3, p. 110-118 Summary of the invention
[0014] Problems to be solved by the invention
[0015] The present invention has been developed in view of the above circumstances, and an object of the present invention is to provide a high-strength steel sheet having a TS of 1180 MPa or more, a YR of 85% or more, and excellent flatness in the sheet width direction and resistance to work embrittlement, and a method for producing the same.
[0016] Methods used to solve problems
[0017] The present inventors have conducted intensive studies to achieve the above-mentioned objects and have found the following findings.
[0018] (1) By setting the tempered martensite content to 90% or more, a TS of 1180 MPa or more can be achieved.
[0019] (2) By setting the amount of retained austenite to less than 3% and the total amount of ferrite and bainitic ferrite to less than 10%, a YR of 85% or more can be achieved.
[0020] (3) By setting the occupancy rate of the largest lath bundle of tempered martensite in the prior austenite grains to 70% or less, it is possible to achieve excellent flatness in the sheet width direction.
[0021] (4) Excellent work embrittlement resistance can be achieved by setting the occupancy rate of the largest lath bundle of tempered martensite in the prior austenite grains to 70% or less and setting the average prior austenite grain size of the tempered martensite to 20 μm or less.
[0022] The present invention has been completed based on the above findings. That is, the gist of the present invention is as follows.
[0023] [1] A high-strength steel sheet comprising, in mass %, C: 0.030% to 0.500%, Si: 0.01% to 2.50%, Mn: 0.10% to 5.00%, P: 0.100% to 0.0200%, Al: 1.000% to 1.000%, N: 0.0100% to 0.0100%, and O: 0.0100% to 0.050%, with the remainder being Fe and inevitable impurities, wherein at a position of 1 / 4 of the sheet thickness, the amount of tempered martensite is 90% or more by area fraction, the amount of retained austenite is less than 3% by volume fraction, the total amount of ferrite and bainitic ferrite is less than 10% by area fraction, the average grain size of prior austenite is 20 μm or less, and the average value of the occupancy of lath bundles having the largest occupancy in prior austenite grains is 70% or less by area fraction.
[0024] [2] The high-strength steel sheet according to [1], wherein the above-mentioned chemical composition further contains, in mass %, at least one element selected from the group consisting of Ti: 0.200% or less, Nb: 0.200% or less, V: 0.200% or less, Ta: 0.10% or less, W: 0.10% or less, B: 0.0100% or less, Cr: 1.00% or less, Mo: 1.00% or less, Co: 0.010% or less, Ni: 1.00% or less, Cu: 1.00% or less, Sn: 0.200% or less, Sb: 0.200% or less, Ca: 0.0100% or less, Mg: 0.0100% or less, REM: 0.0100% or less, Zr: 0.100% or less, Te: 0.100% or less, Hf: 0.10% or less, and Bi: 0.200% or less.
[0025] [3] The high-strength steel sheet according to [1] or [2], wherein the steel sheet has a plating layer on the surface.
[0026] [4] A method for producing a high-strength steel sheet according to [1] or [2], wherein a cold-rolled sheet produced by hot-rolling, pickling and cold-rolling a steel having the above composition is heated under conditions where an annealing temperature T1 is 750°C or higher and 950°C or lower, and a holding time t1 at the annealing temperature T1 is 10 seconds or higher and 1000 seconds or lower, and an average cooling rate at 750°C to 600°C is 20°C / s or higher and a cooling time between (Ms+50°C) and a rapid cooling start temperature is 100°C or higher. Cooling is performed under the conditions that the average cooling rate of T2 is 5°C / s or more and 30°C / s or less, the rapid cooling start temperature T2 is (Ms-80°C) or more and less than Ms, and the average cooling rate of the rapid cooling start temperature T2 to 80°C is 300°C / s or more, wherein Ms is the martensitic transformation start temperature (°C) specified by the formula (1), and heating is performed under the conditions that the tempering temperature T3 is 100°C or more and 400°C or less and the holding time t3 at the tempering temperature T3 is 10 seconds or more and 10000 seconds or less.
[0027] Ms=519-474×[%C]-30.4×[%Mn]-12.1×[%Cr]-7.5×[%Mo]-17.7×[%Ni]…(1)
[0028] Here, [%C], [%Mn], [%Cr], [%Mo], and [%Ni] represent the content (mass %) of C, Mn, Cr, Mo, and Ni, respectively, and when not contained, it is set to 0.
[0029] [5] The method for producing a high-strength steel sheet according to [4], wherein a plating treatment is performed.
[0030] Effects of the Invention
[0031] According to the present invention, a high-strength steel sheet having a TS of 1180 MPa or more, a YR of 85% or more, and excellent flatness in the width direction and resistance to work embrittlement can be obtained. In addition, by applying the high-strength steel sheet of the present invention to, for example, automotive structural members, it is possible to improve fuel efficiency by reducing the weight of the vehicle body. Therefore, the industrial utilization value is extremely high. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 This is a diagram showing the structure of lath bundles having the maximum occupancy in prior austenite grains according to the present invention and a calculation method thereof.
[0033] Figure 2 This is a diagram showing the concept of the steepness θ of the steel plate according to the present invention and a method for calculating the steepness θ. DETAILED DESCRIPTION
[0034] Hereinafter, embodiments of the present invention will be described.
[0035] First, the appropriate range of the chemical composition of the high-strength steel sheet and the reasons for its limitation are described. It should be noted that in the following description, "%" indicating the content of the component elements of the steel means "mass %" unless otherwise specified.
[0036] [C: 0.030% or more and 0.500% or less]
[0037] C is one of the important basic components of steel, and is an important element that affects the fraction of tempered martensite and the resistance to work embrittlement in the present invention. When the content of C is less than 0.030%, the fraction of tempered martensite decreases, and it is difficult to achieve a TS of more than 1180MPa. On the other hand, when the content of C is greater than 0.500%, the tempered martensite becomes brittle, and the resistance to work embrittlement decreases. Therefore, the content of C is set to be greater than 0.030% and less than 0.500%. The content of C is preferably set to be greater than 0.050%. The content of C is preferably set to be less than 0.400%. The content of C is more preferably set to be greater than 0.100%. The content of C is more preferably set to be less than 0.350%.
[0038] [Si: 0.01% or more and 2.50% or less]
[0039] Si is one of the important basic components of steel. In particular, in the present invention, Si is an important element that affects TS and the amount of retained austenite because it inhibits the formation of carbides during continuous annealing and promotes the formation of retained austenite. When the content of Si is less than 0.01%, it is difficult to achieve a TS of more than 1180MPa. On the other hand, when the content of Si is greater than 2.50%, the retained austenite increases excessively, making it difficult to achieve a YR of more than 85%. Therefore, the content of Si is set to be greater than 0.01% and less than 2.50%. The content of Si is preferably set to be greater than 0.05%. The content of Si is preferably set to be less than 2.00%. The content of Si is more preferably set to be greater than 0.10%. The content of Si is more preferably set to be less than 1.20%.
[0040] [Mn: 0.10% or more and 5.00% or less]
[0041] Mn is one of the important basic components of steel, and in particular, in the present invention, it is an important element that affects the fraction of tempered martensite and the resistance to work embrittlement. When the content of Mn is less than 0.10%, the fraction of tempered martensite decreases, and it is difficult to achieve a TS of more than 1180MPa. On the other hand, when the content of Mn is greater than 5.00%, the tempered martensite becomes brittle, and the resistance to work embrittlement decreases. Therefore, the content of Mn is set to be greater than 0.10% and less than 5.00%. The content of Mn is preferably set to be greater than 0.50%. The content of Mn is preferably set to be less than 4.50%. The content of Mn is more preferably set to be greater than 0.80%. The content of Mn is more preferably set to be less than 4.00%.
[0042] [P: 0.100% or less]
[0043] P segregates at the original austenite grain boundary and makes the grain boundary embrittled, thereby reducing the ultimate deformation capacity of the steel plate, and thus reducing the processing embrittlement resistance. Therefore, the P content needs to be set to 0.100% or less. It should be noted that the lower limit of the P content is not particularly specified, but since P is a solid solution strengthening element, it can increase the strength of the steel plate, so it is preferably set to 0.001% or more. Therefore, the P content is set to 0.100% or less. The P content is preferably set to 0.001% or more. The P content is preferably set to 0.070% or less.
[0044] [S: 0.0200% or less]
[0045] S exists in the form of sulfide, which reduces the ultimate deformation capacity of the steel plate, thereby reducing the resistance to processing embrittlement. Therefore, the S content needs to be set to 0.0200% or less. It should be noted that the lower limit of the S content is not particularly specified, but considering the limitations of production technology, it is preferably set to 0.0001% or more. Therefore, the S content is set to 0.0200% or less. The S content is preferably set to 0.0001% or more. The S content is preferably set to 0.0050% or less.
[0046] [Al: 1.000% or less]
[0047] Al increases the A3 transformation point, resulting in a large amount of ferrite in the microstructure, so the fraction of tempered martensite is reduced, and it is difficult to achieve a TS of more than 1180MPa. Therefore, the content of Al needs to be set to 1.000% or less. It should be noted that the lower limit of the content of Al is not particularly specified, but from the perspective of suppressing the formation of carbides in continuous annealing and promoting the formation of retained austenite, the content of Al is preferably set to 0.001% or more. Therefore, the content of Al is set to 1.000% or less. The content of Al is preferably set to 0.001% or more. The content of Al is preferably 0.500% or less.
[0048] [N: 0.0100% or less]
[0049] N exists in the form of nitrides, which reduces the ultimate deformation capacity of the steel sheet, and thus reduces the resistance to processing embrittlement. Therefore, the N content needs to be set to 0.0100% or less. It should be noted that there is no special lower limit for the N content, but considering the limitations of production technology, the N content is preferably set to 0.0001% or more. Therefore, the N content is set to 0.0100% or less. It is preferably set to 0.0001% or more. It is preferably set to 0.0050% or less.
[0050] [O: 0.0100% or less]
[0051] O exists in the form of oxides, which reduces the ultimate deformation capacity of the steel plate, thereby reducing the resistance to processing embrittlement. Therefore, the content of O needs to be set to 0.0100% or less. It should be noted that there is no special lower limit for the content of O, but considering the limitations of production technology, the content of O is preferably set to 0.0001% or more. Therefore, the content of O is set to 0.0100% or less. The content of O is preferably set to 0.0001% or more. The content of O is preferably set to 0.0050% or less.
[0052] The high-strength steel sheet according to one embodiment of the present invention has a composition containing the above-mentioned components and the balance containing Fe and inevitable impurities. Here, as inevitable impurities, Zn, Pb, As, Ge, Sr and Cs can be listed. The total amount of these impurities is allowed to be 0.100% or less.
[0053] The high-strength steel sheet of the present invention may contain, in addition to the above-mentioned component composition, at least one element selected from the group consisting of Ti: 0.200% or less, Nb: 0.200% or less, V: 0.200% or less, Ta: 0.10% or less, W: 0.10% or less, B: 0.0100% or less, Cr: 1.00% or less, Mo: 1.00% or less, Ni: 1.00% or less, Co: 0.010% or less, Cu: 1.00% or less, Sn: 0.200% or less, Sb: 0.200% or less, Ca: 0.0100% or less, Mg: 0.0100% or less, REM: 0.0100% or less, Zr: 0.100% or less, Te: 0.100% or less, Hf: 0.10% or less, and Bi: 0.200% or less, alone or in combination.
[0054] When Ti, Nb and V are respectively less than 0.200%, coarse precipitates and inclusions will not be generated in large quantities, and the ultimate deformation capacity of the steel sheet will not be reduced, so the processing embrittlement resistance will not be reduced. Therefore, the contents of Ti, Nb and V are preferably set to less than 0.200%. It should be noted that the lower limits of the contents of Ti, Nb and V are not particularly specified. During hot rolling or continuous annealing, the strength of the steel sheet is increased by forming fine carbides, nitrides or carbonitrides. Therefore, the contents of Ti, Nb and V are more preferably set to more than 0.001%. Therefore, in the case of containing Ti, Nb and V, their contents are set to less than 0.200%. The contents of Ti, Nb and V are more preferably set to more than 0.001%. The contents of Ti, Nb and V are further preferably set to less than 0.100%.
[0055] When Ta and W are respectively less than 0.10%, coarse precipitates and inclusions will not be generated in large quantities, and the ultimate deformation capacity of the steel plate will not be reduced, so the resistance to processing embrittlement will not be reduced. Therefore, the contents of Ta and W are preferably set to less than 0.10%, respectively. It should be noted that the lower limits of the contents of Ta and W are not particularly specified. During hot rolling or continuous annealing, the strength of the steel plate is increased by forming fine carbides, nitrides or carbonitrides, so the contents of Ta and W are more preferably set to more than 0.01%, respectively. Therefore, in the case of containing Ta and W, their contents are set to less than 0.10%, respectively. The contents of Ta and W are more preferably set to more than 0.01%. The contents of Ta and W are further preferably set to less than 0.08%.
[0056] When B is below 0.0100%, cracks will not be generated inside the steel plate during casting or hot rolling, and the ultimate deformation capacity of the steel plate will not be reduced, so the processing embrittlement resistance characteristic will not be reduced. Therefore, the content of B is preferably set to below 0.0100%. It should be noted that the lower limit of the content of B is not particularly specified, but since it is an element that segregates at the austenite grain boundary and improves hardenability during annealing, the content of B is more preferably set to more than 0.0003%. Therefore, in the case of containing B, its content is set to less than 0.0100%. The content of B is more preferably set to more than 0.0003%. The content of B is further preferably set to less than 0.0080%.
[0057] When Cr, Mo and Ni are respectively less than 1.00%, coarse precipitates and inclusions do not increase, and the ultimate deformation capacity of the steel plate will not be reduced, so the processing embrittlement resistance characteristics will not be reduced. Therefore, the contents of Cr, Mo and Ni are preferably set to less than 1.00%, respectively. It should be noted that the lower limits of the contents of Cr, Mo and Ni are not particularly specified, but since they are elements that improve hardenability, the contents of Cr, Mo and Ni are more preferably set to more than 0.01%, respectively. Therefore, in the case of containing Cr, Mo and Ni, their contents are respectively set to less than 1.00%. The contents of Cr, Mo and Ni are more preferably set to more than 0.01%. The contents of Cr, Mo and Ni are further preferably set to less than 0.80%.
[0058] When Co is below 0.010%, coarse precipitates and inclusions do not increase, and the ultimate deformation capacity of the steel plate will not be reduced, so the processing embrittlement resistance characteristic will not be reduced. Therefore, the content of Co is preferably set to below 0.010%. It should be noted that the lower limit of the content of Co is not particularly specified, but since it is an element that improves hardenability, the content of Co is more preferably set to more than 0.001%. Therefore, in the case of containing Co, its content is set to less than 0.010%. The content of Co is more preferably set to more than 0.001%. The content of Co is further preferably set to less than 0.008%.
[0059] When Cu is below 1.00%, coarse precipitates and inclusions do not increase, and the ultimate deformation capacity of the steel plate will not be reduced, so the processing embrittlement resistance characteristic will not be reduced. Therefore, the content of Cu is preferably set to below 1.00%. It should be noted that the lower limit of the content of Cu is not particularly specified, but since it is an element that improves hardenability, the content of Cu is preferably set to more than 0.01%. Therefore, in the case of containing Cu, its content is set to less than 1.00%. The content of Cu is more preferably set to more than 0.01%. The content of Cu is further preferably set to less than 0.80%.
[0060] When Sn is below 0.200%, cracks will not be generated inside the steel plate during casting or hot rolling, and the ultimate deformation capacity of the steel plate will not be reduced, so the processing embrittlement resistance characteristic will not be reduced. Therefore, the content of Sn is preferably set to below 0.200%. It should be noted that the lower limit of the content of Sn is not particularly specified, but since Sn is an element that improves hardenability (generally an element that improves corrosion resistance), the content of Sn is more preferably set to more than 0.001%. Therefore, in the case of containing Sn, its content is set to less than 0.200%. The content of Sn is more preferably set to more than 0.001%. The content of Sn is further preferably set to less than 0.100%.
[0061] When Sb is less than 0.200%, coarse precipitates and inclusions do not increase, and the ultimate deformation capacity of the steel plate will not be reduced, so the processing embrittlement resistance will not be reduced. Therefore, the Sb content is preferably set to less than 0.200%. It should be noted that the lower limit of the Sb content is not particularly specified, but since it is an element that can control the softening thickness of the surface layer and can adjust the strength, the Sb content is more preferably set to more than 0.001%. Therefore, in the case of containing Sb, its content is set to less than 0.200%. The Sb content is more preferably set to more than 0.001%. The Sb content is further preferably set to less than 0.100%.
[0062] When Ca, Mg and REM are respectively less than 0.0100%, coarse precipitates and inclusions do not increase, and the ultimate deformation capacity of the steel sheet will not be reduced, so the processing embrittlement resistance characteristics will not be reduced. Therefore, the content of Ca, Mg and REM is preferably set to 0.0100% or less. It should be noted that the lower limit of the content of Ca, Mg and REM is not particularly specified, but since they are elements that make the shape of nitrides and sulfides spherical and improve the ultimate deformation capacity of the steel sheet, the content of Ca, Mg and REM is more preferably set to 0.0005% or more. Therefore, in the case of containing Ca, Mg and REM, their contents are respectively set to 0.0100% or less. The content of Ca, Mg and REM is more preferably set to 0.0005% or more. The content of Ca, Mg and REM is further preferably set to 0.0050% or less.
[0063] When Zr and Te are respectively less than 0.100%, coarse precipitates and inclusions do not increase, and the ultimate deformation capacity of the steel plate will not be reduced, so the processing embrittlement resistance characteristics will not be reduced. Therefore, the content of Zr and Te is preferably set to 0.100% or less. It should be noted that the lower limit of the content of Zr and Te is not particularly specified, but since it is an element that makes the shape of nitrides and sulfides spherical and improves the ultimate deformation capacity of the steel plate, the content of Zr and Te is more preferably set to 0.001% or more. Therefore, in the case of containing Zr and Te, their contents are respectively set to 0.100% or less. The content of Zr and Te is more preferably set to 0.001% or more. The content of Zr and Te is further preferably set to 0.080% or less.
[0064] When Hf is less than 0.10%, coarse precipitates and inclusions do not increase, and the ultimate deformation capacity of the steel plate will not be reduced, so the processing embrittlement resistance characteristics will not be reduced. Therefore, the content of Hf is preferably set to 0.10% or less. It should be noted that the lower limit of the content of Hf is not particularly specified, but since it is an element that makes the shape of nitrides and sulfides spherical and improves the ultimate deformation capacity of the steel plate, the content of Hf is more preferably set to 0.01% or more. Therefore, in the case of containing Hf, its content is set to 0.10% or less. The content of Hf is more preferably set to 0.01% or more. The content of Hf is further preferably set to 0.08% or less.
[0065] When Bi is less than 0.200%, coarse precipitates and inclusions do not increase, and the ultimate deformation capacity of the steel plate will not be reduced, so the resistance to processing embrittlement will not be reduced. Therefore, the content of Bi is preferably set to 0.200% or less. It should be noted that the lower limit of the content of Bi is not particularly specified, but since it is an element that reduces segregation, the content of Bi is more preferably set to 0.001% or more. Therefore, in the case of containing Bi, its content is set to 0.200% or less. The content of Bi is more preferably set to 0.001% or more. The content of Bi is further preferably set to 0.100% or less.
[0066] It should be noted that, with respect to the above-mentioned Ti, Nb, V, Ta, W, B, Cr, Mo, Ni, Co, Cu, Sn, Sb, Ca, Mg, REM, Zr, Te, Hf and Bi, when the content of each is less than the preferred lower limit, the effect of the present invention will not be impaired, and therefore they are contained as unavoidable impurities.
[0067] Next, the steel structure of the high-strength steel sheet of the present invention will be described.
[0068] [Tempered martensite: 90% or more by area fraction]
[0069] It is an extremely important inventive constituent element in the present invention. By using tempered martensite as the main phase, a TS of 1180 MPa or more can be achieved. In order to obtain such an effect, it is necessary to make the tempered martensite more than 90% in terms of area fraction. Therefore, the tempered martensite is set to more than 90% in terms of area fraction. Preferably, it is more than 94%. More preferably, it is more than 96%.
[0070] Here, the method for measuring tempered martensite is as follows. After grinding the L section of the steel plate, it is corroded with a 3 volume % nitric acid ethanol solution, and 10 fields of view are observed at a magnification of 2000 times for 1 / 4 of the plate thickness (a position equivalent to 1 / 4 of the plate thickness in the depth direction from the surface of the steel plate). It should be noted that in the above-mentioned organizational image, tempered martensite is a structure with fine concavo-convex inside the structure, and a structure with carbides inside. The tempered martensite can be obtained from the average value of these values.
[0071] [Retained austenite content less than 3%]
[0072] It is an extremely important inventive constituent element in the present invention. When the volume fraction of retained austenite is 3% or more, it is difficult to achieve a YR of 85% or more. The reason for the reduction of YR is the reduction of YS caused by the processing-induced phase transformation of retained austenite due to the increase of retained austenite. Therefore, the retained austenite is set to less than 3%. It is preferably set to less than 1%. It should be noted that the lower limit of retained austenite is not particularly limited. The retained austenite can be 0%.
[0073] Here, the method for measuring retained austenite is as follows. Retained austenite is obtained by grinding a steel plate from a 1 / 4 portion of the plate thickness to a surface of 0.1 mm, then further grinding 0.1 mm by chemical grinding, and measuring the integrated intensity ratios of the diffraction peaks of the {200}, {220}, and {311} planes of fcc iron and the {200}, {211}, and {220} planes of bcc iron using an X-ray diffractometer using CoKα rays, and averaging the obtained 9 integrated intensity ratios to obtain retained austenite.
[0074] [Total of ferrite and bainitic ferrite: less than 10% by area fraction]
[0075] It is an extremely important invention constituent element in the present invention. When the total of ferrite and bainitic ferrite is more than 10%, it is difficult to achieve a TS of more than 1180MPa, and it is difficult to achieve a YR of more than 85%. The reason for the reduction of YR is that ferrite and bainitic ferrite are soft structures, so they cause yielding at an early stage. Therefore, the total of ferrite and bainitic ferrite is set to less than 10%. It is preferably set to less than 8%. It is more preferably set to less than 5%. It should be noted that the lower limit of the total of ferrite and bainitic ferrite is not particularly limited. It can be 0%.
[0076] Here, the method for determining the total of ferrite and bainitic ferrite is as follows. After grinding the L section of the steel plate, it is corroded with a 3 volume % nitric acid ethanol solution, and 10 fields of view are observed at a magnification of 2000 times for 1 / 4 of the plate thickness (a position equivalent to 1 / 4 of the plate thickness in the depth direction from the surface of the steel plate). It should be noted that in the above-mentioned organizational image, ferrite and bainitic ferrite are organizations with concave parts and flat inside the organization, and are organizations without carbides inside. The total of ferrite and bainitic ferrite can be obtained from the average value of these values.
[0077] As structures other than all the above structures, pearlite, neomartensite, acicular ferrite, etc. are conceivable. These structures do not affect the properties as long as they are within a range of 5% or less, so they may be contained.
[0078] [Average grain size of prior austenite is 20 μm or less]
[0079] It is an extremely important inventive constituent element in the present invention. By reducing the average crystal grain size of the original austenite, the propagation of cracks can be suppressed, thereby improving the work embrittlement resistance of the steel plate. In order to obtain such an effect, it is necessary to set the average crystal grain size of the original austenite to less than 20μm. It should be noted that the lower limit of the average crystal grain size of the original austenite is not particularly limited. When the average crystal grain size of the original austenite is less than 2μm, the residual austenite sometimes increases, so it is preferably more than 2μm. Therefore, the average crystal grain size of the original austenite is set to less than 20μm. It is preferably set to more than 2μm. It is preferably set to less than 15μm. It is more preferably set to more than 3μm. It is more preferably set to less than 10μm.
[0080] Here, the method for measuring the average grain size of the original austenite is as follows. After grinding the L section of the steel plate, etching is performed with a mixed solution of picric acid and ferric chloride to make the original austenite grain boundary appear, and then 3 to 10 fields of view are photographed at a magnification of 400 times for 1 / 4 of the plate thickness (a position equivalent to 1 / 4 of the plate thickness in the depth direction from the surface of the steel plate). For the obtained image data, 20 straight lines of 10 vertical × 10 horizontal are drawn at equal intervals and obtained by the cutting method.
[0081] [The average occupancy of the lath bundle having the largest occupancy in the prior austenite grains is 70% or less in terms of area fraction]
[0082] It is an extremely important inventive element in the present invention. The occupancy rate of the lath bundle with the largest occupancy rate in the original austenite grains affects the flatness in the width direction of the plate and the work embrittlement resistance. The lath bundle with the largest occupancy rate in the original austenite grains refers to, for example Figure 1As shown, there are up to 4 regions with the same crystal habit plane during the phase transformation called lath bundles in the original austenite grain, which refers to the lath bundle with the largest occupancy. The occupancy of one lath bundle in the original austenite grain is calculated by dividing the area of the specified lath bundle by the overall area of the original austenite grain. The inventors have repeatedly conducted in-depth studies and found that by reducing the occupancy of the lath bundles with the largest occupancy in the original austenite grain, the strain between the lath bundles is relaxed and the flatness in the width direction of the plate is improved. It is also found that by reducing the occupancy of the lath bundles with the largest occupancy in the original austenite grain, the structure is refined, the propagation of cracks can be suppressed, and thus the work embrittlement resistance of the steel plate is improved. Therefore, the average value of the occupancy of the lath bundles with the largest occupancy in the original austenite grain is set to less than 70%. It is preferably set to less than 60%. It should be noted that the lower limit of the average value of the occupancy rate of the lath bundles with the maximum occupancy rate in the prior austenite grains is not particularly limited. The types of lath bundles are at most 4, and when 4 lath bundles are equally present, the occupancy rate of the lath bundles with the maximum occupancy rate in the prior austenite grains is 25%. Therefore, the lower limit of the average value of the occupancy rate of the lath bundles with the maximum occupancy rate in the prior austenite grains is set to 25% or more, but it is not limited thereto.
[0083] Here, the method for determining the average occupancy of the lath bundle with the maximum occupancy in the original austenite grain is as follows. First, a test piece for tissue observation is cut from a cold-rolled steel plate. Then, the cut test piece is polished by colloidal silica vibration polishing in a manner that the rolling direction section (L section) is used as the observation surface. Make the observation surface a mirror surface. Next, electron backscatter diffraction (EBSD) measurement is performed on 1 / 4 of the plate thickness (a position equivalent to 1 / 4 of the plate thickness in the depth direction from the surface of the steel plate) to obtain local crystal orientation data. At this time, the SEM magnification is set to 1000 times, the step size is set to 0.2μm, the measurement area is set to 80μm square, and the WD is set to 15mm. The obtained local orientation data is analyzed using OIMAnalysis7 (OIM), and a color-differentiated diagram (CP mapping) is prepared according to the method described in non-patent document 1 according to the close-packed plane group (Close-packed Planegroup, CP group). In the present invention, lath bundles are defined as areas belonging to the same CP group. The area of the lath bundle with the maximum occupancy is obtained from the obtained CP map, and divided by the entire area in the original austenite grain, thereby obtaining the occupancy of the lath bundle with the maximum occupancy in the original austenite grain. This analysis is performed on more than 10 adjacent original austenite grains, and the average value is taken as the average occupancy of the lath bundle with the maximum occupancy in the original austenite grain.
[0084] Next, the production method of the present invention will be described.
[0085] In the present invention, the method for melting the steel material (steel slab) is not particularly specified, and any known melting method such as a converter or an electric furnace is suitable. In order to prevent macrosegregation, the steel slab is preferably produced by a continuous casting method.
[0086] In the present invention, there is no particular provision for the billet heating temperature, billet soaking holding time and coiling temperature in hot rolling. As a method for hot rolling a billet, there can be cited a method of rolling the billet after heating it, a method of directly rolling the billet without heating the billet after continuous casting, and a method of rolling the billet after a short heating treatment for a continuous casting. There is no particular provision for the billet heating temperature, billet soaking holding time, finish rolling temperature and coiling temperature in hot rolling, and the lower limit of the billet heating temperature is preferably above 1100°C. The upper limit of the billet heating temperature is preferably below 1300°C. The lower limit of the billet soaking holding time is preferably above 30 minutes. The upper limit of the billet soaking holding time is preferably below 250 minutes. The lower limit of the finish rolling temperature is preferably above the Ar3 transformation point. In addition, the lower limit of the coiling temperature is preferably above 350°C. In addition, the upper limit of the coiling temperature is preferably below 650°C.
[0087] The hot-rolled steel sheet manufactured in this way is pickled. Pickling can remove oxides on the surface of the steel sheet, so it is important for ensuring good chemical conversion treatment and plating quality of the high-strength steel sheet of the final product. In addition, pickling can be performed once or in multiple times. In addition, cold rolling can be performed while the pickled sheet is kept after hot rolling, or cold rolling can be performed after heat treatment.
[0088] The reduction ratio in cold rolling and the plate thickness after rolling are not particularly limited, but the lower limit of the reduction ratio is preferably 30% or more. In addition, the upper limit of the reduction ratio is preferably set to 80% or less. It should be noted that the number of rolling passes and the reduction ratio of each pass are not particularly limited, and the effect of the present invention can be obtained.
[0089] The cold rolled steel sheet obtained as above was annealed. The annealing conditions were as follows.
[0090] [Annealing temperature T1: 750°C or higher and 950°C or lower]
[0091] When the annealing temperature T1 is less than 750°C, the total area fraction of ferrite and bainitic ferrite is more than 10%, and it is difficult to achieve a TS of more than 1180 MPa, and it is difficult to achieve a YR of more than 85%. On the other hand, when the annealing temperature T1 is greater than 950°C, the original austenite grain size increases excessively, the original austenite grain size is greater than 20 μm, and the work embrittlement resistance is reduced. Therefore, the annealing temperature T1 is set to be greater than 750°C and less than 950°C. The annealing temperature T1 is preferably greater than 800°C. The annealing temperature T1 is preferably less than 900°C.
[0092] [Retention time t1 at annealing temperature T1: 10 seconds or more and 1000 seconds or less]
[0093] When the holding time t1 at the annealing temperature T1 is less than 10 seconds, austenitization becomes insufficient, and the total area fraction of ferrite and bainitic ferrite is more than 10%, and it is difficult to achieve a TS of more than 1180MPa, and it is difficult to achieve a YR of more than 85%. On the other hand, when the holding time at the annealing temperature T1 is more than 1000 seconds, the original austenite grain size increases excessively, and the resistance to work embrittlement decreases. Therefore, the holding time t1 at the annealing temperature T1 is set to more than 10 seconds and less than 1000 seconds. Preferably, it is more than 50 seconds. Preferably, it is less than 500 seconds.
[0094] [The average cooling rate from 750℃ to 600℃ is 20℃ / s or more]
[0095] When the average cooling rate at 750°C to 600°C is less than 20°C / s, the total area fraction of ferrite and bainitic ferrite is 10% or more, and it is difficult to achieve a TS of 1180 MPa or more, and it is difficult to achieve a YR of 85% or more. Therefore, the average cooling rate at 750°C to 600°C is set to 20°C / s or more. Preferably, it is 30°C / s or more. The upper limit does not need to be particularly limited, and is preferably 2000°C / s or less.
[0096] [The average cooling rate from (Ms+50°C) to the rapid cooling start temperature T2 is 5°C / s or more and 30°C / s or less]
[0097] It is an extremely important inventive constituent element in the present invention. The average cooling rate from (Ms+50°C) to the quenching start temperature T2 affects the total area fraction of ferrite and bainitic ferrite and the average occupancy of the lath bundle with the maximum occupancy in the original austenite grain. When the average cooling rate from (Ms+50°C) to the quenching start temperature T2 is less than 5°C / s, the total area fraction of ferrite and bainitic ferrite is more than 10%, and it is difficult to achieve a TS of more than 1180MPa, and it is difficult to achieve a YR of more than 85%. On the other hand, when the average cooling rate from (Ms+50°C) to the quenching start temperature T2 is greater than 30°C / s, the average occupancy of the lath bundle with the maximum occupancy in the original austenite grain is greater than 70%, the flatness in the plate width direction deteriorates, and the resistance to work embrittlement is reduced. Therefore, the average cooling rate from (Ms+50°C) to the quenching start temperature T2 is set to be greater than 5°C / s and less than 30°C / s. It is preferably 10°C / s or more and preferably 20°C / s or less.
[0098] [Quick cooling start temperature T2 is (Ms-80°C) or higher and lower than Ms]
[0099] It is an extremely important inventive constituent element in the present invention. The quenching start temperature T2 is set to be greater than (Ms-80°C) and less than Ms, and quenching is performed in a state where the martensitic transformation rate before the start of quenching is greater than 1% and less than 80%. As a result, a structure in which the average occupancy of the lath bundles with the maximum occupancy in the original austenite grains is less than 70% and the retained austenite is less than 3% by volume fraction can be obtained. When the quenching start temperature T2 is less than (Ms-80°C), the martensitic transformation rate before the start of quenching is greater than 80%, so the retained austenite is greater than 3% by volume fraction, and it is difficult to achieve a YR of more than 85%. On the other hand, when the quenching start temperature T2 is greater than Ms, the martensitic transformation rate before the start of quenching is less than 1%, the average occupancy of the lath bundles with the maximum occupancy in the original austenite grains is greater than 70%, the flatness in the plate width direction deteriorates, and the resistance to work embrittlement is reduced. Therefore, the rapid cooling start temperature T2 is set to be (Ms-80°C) or higher and lower than Ms. Preferably, it is (Ms-50°C) or higher. Preferably, it is (Ms-5°C) or lower. It should be noted that the martensitic transformation start temperature Ms (°C) is defined by the following formula (1).
[0100] Ms=519-474×[%C]-30.4×[%Mn]-12.1×[%Cr]-7.5×[%Mo]-17.7×[%Ni]…(1)
[0101] Here, [%C], [%Mn], [%Cr], [%Mo], and [%Ni] represent the content (mass %) of C, Mn, Cr, Mo, and Ni, respectively, and when not contained, it is set to 0.
[0102] [The average cooling rate from the rapid cooling start temperature T2 to 80°C is 300°C / s or more]
[0103] When the average cooling rate of the quenching start temperature T2 to 80°C is less than 300°C / s, the retained austenite is 3% or more in volume fraction, and it is difficult to achieve a YR of 85% or more. Therefore, the average cooling rate of the quenching start temperature T2 to 80°C is set to 300°C / s or more. Preferably, it is 800°C / s or more. The upper limit does not need to be particularly limited, but is preferably 2000°C / s or less.
[0104] [Tempering temperature T3 is 100°C or higher and 400°C or lower]
[0105] In the present invention, tempered martensite refers to a structure in which martensite below 80°C is subjected to a heat treatment at a tempering temperature of 100°C or higher and a holding time of 10s or higher. Therefore, when the tempering temperature T3 is less than 100°C, the martensite cannot be fully tempered, and becomes a structure of martensite as a main body in the quenched state, and the martensite deteriorates the work embrittlement resistance in the quenched state. On the other hand, when the tempering temperature T3 is greater than 400°C, the tempered martensite decomposes and becomes ferrite, so the tempered martensite is less than 90% in terms of area fraction, and it is difficult to achieve a TS of more than 1180MPa. Therefore, the tempering temperature T3 is set to be greater than 100°C and less than 400°C. It is preferably set to be greater than 150°C. It is preferably set to be less than 350°C.
[0106] [The holding time t3 at the tempering temperature T3 is 10 seconds or more and 10000 seconds or less]
[0107] In the present invention, tempered martensite refers to a structure in which martensite below 80°C is subjected to a heat treatment at a tempering temperature of 100°C or above and a holding time of 10s or above. Therefore, when the holding time t3 at the tempering temperature T3 is less than 10 seconds, the martensite cannot be fully tempered, and becomes a structure of martensite main body in the quenched state, and the martensite deteriorates the work embrittlement resistance in the quenched state. On the other hand, when the tempering temperature T3 is greater than 10000 seconds, the tempered martensite decomposes and becomes ferrite, so the tempered martensite is less than 90% in terms of area fraction, and it is difficult to achieve a TS of more than 1180MPa. Therefore, the holding time t3 at the tempering temperature T3 is set to be greater than 10 seconds and less than 10000 seconds. It is preferably set to be greater than 50 seconds. It is preferably set to be less than 5000 seconds.
[0108] The cooling after tempering does not need to be particularly specified, and the material may be cooled to a desired temperature by any method. It should be noted that the desired temperature is preferably about room temperature.
[0109] The high-strength steel sheet may be processed under conditions to achieve an equivalent plastic strain of 0.10% to 5.00%, or reheated again at 100° C. to 400° C. after processing.
[0110] In addition, when a high-strength steel sheet is traded, it is usually traded after being cooled to room temperature.
[0111] The high-strength steel sheet may be plated during or after annealing.
[0112] As the plating treatment during annealing, for example, a hot-dip galvanizing treatment during or after cooling under the condition that the average cooling rate at 750°C to 600°C is 20°C / s or more, and an alloying treatment after hot-dip galvanizing can be exemplified. In addition, as the plating treatment after annealing, for example, a Zn-Ni electroplating alloy treatment or a pure Zn electroplating treatment after tempering can be exemplified. A plating layer can be formed by electroplating, and hot-dip galvanizing-aluminum-magnesium alloy can also be implemented. It should be noted that in the above-mentioned plating treatment, the case of galvanizing is mainly described, but the type of plating metal such as Zn plating and Al plating is not particularly specified. The conditions of other manufacturing methods are not particularly specified. From the perspective of productivity, the above-mentioned series of treatments such as annealing, hot-dip galvanizing, and alloying treatment of the galvanized layer are preferably performed by CGL (Continuous Galvanizing Line: Continuous Hot-dip Galvanizing Line) as a hot-dip galvanizing line. After hot-dip galvanizing, wiping can be performed to adjust the unit area weight of the plating layer. It should be noted that the plating and other conditions other than the above conditions can be carried out according to a conventional hot-dip galvanizing method.
[0113] After the annealing and plating treatment, the steel may be worked again under the condition that the equivalent plastic strain is 0.10% or more and 5.00 or less. Also, after the working, the steel may be reheated again under the condition of 100° C. or more and 400° C. or less.
[0114] Example
[0115] Steel having the composition shown in Tables 1 and 2, with the balance being Fe and inevitable impurities, was melted in a converter and made into a steel slab by a continuous casting method. Next, the obtained steel slab was heated, pickled after hot rolling, and then cold rolled, and annealed and tempered as shown in Tables 3 to 6 to obtain a high-strength cold-rolled steel sheet with a thickness of 0.6 to 2.2 mm. It should be noted that for some steel sheets, a plating treatment was performed during or after annealing to obtain a high-strength cold-rolled steel sheet.
[0116]
[0117]
[0118]
[0119]
[0120]
[0121]
[0122] The high-strength cold-rolled steel sheets obtained as described above were used as test steels, and the tensile properties, flatness in the sheet width direction, and work embrittlement resistance were evaluated according to the following test methods.
[0123] (Organization Observation)
[0124] The total amount of tempered martensite, retained austenite, ferrite, bainitic ferrite, and the prior austenite average grain size were determined by the above method.
[0125] (Occupancy of lath bundles with maximum occupancy in the original austenite grain)
[0126] According to the above method, the average value of the occupancy of the lath bundle having the maximum occupancy in the prior austenite grains is obtained.
[0127] (Tensile test)
[0128] In the tensile test, a JIS No. 5 test piece (point distance 50 mm, parallel part width 25 mm) was cut so that the long side of the test piece was perpendicular to the rolling direction, and the test was carried out according to JIS Z 2241. -1 The tensile test was carried out under the condition of 10000 rpm and 20000 rpm, and YS and TS were measured. It should be noted that in the present invention, TS of 1180 MPa or more was judged as qualified. Yield ratio (YR) of 85% or more was judged as qualified. It should be noted that YR was calculated by the following formula (2).
[0129] YR=100×YS / TS…(2)
[0130] (Flatness in the board width direction)
[0131] For various cold-rolled steel sheets obtained through the above operations, Figure 2Specifically, a plate with a length of 500 mm (coil width × 500 mmL × plate thickness) is cut from the coil along the rolling direction, and placed on a platform with the warped end face facing upward. A contact displacement meter with a stylus moving on the measured object is used to continuously measure the height of the steel plate in the entire width direction. According to the results, Figure 2 The method shown in the figure measures the steepness θ, which is an index indicating the flatness of the shape of the steel plate. A steel plate with a steepness greater than 0.02 is evaluated as "×", a steel plate with a steepness greater than 0.01 and less than 0.02 is evaluated as "○", a steel plate with a steepness of less than 0.01 is evaluated as "◎", and a steel plate with a steepness of less than 0.02 is judged as "excellent flatness in the plate width direction".
[0132] (Machining brittleness resistance)
[0133] The resistance to working brittleness is evaluated by the Charpy test. For the Charpy test piece, multiple steel plates are overlapped and fastened with bolts. After confirming that there is no gap between the steel plates, a test piece with a V-shaped notch with a depth of 2 mm is made. The number of overlapping steel plates is set so that the thickness of the test piece after stacking is closest to 10 mm. For example, in the case of a plate thickness of 1.2 mm, 8 plates are stacked and the test piece thickness is 9.6 mm. The stacked Charpy test piece is cut with the plate width direction as the long side. As an indicator of the resistance to working brittleness, the ratio of the impact absorption energy at room temperature between the steel plate in the manufactured state (unprocessed) and the steel plate subjected to 10% rolling, vE, is measured. 0% / vE 10% . 0% / vE 10% The steel plates with a value less than 0.6 were evaluated as “×” and vE 0% / vE 10% The steel plates with vE of 0.6 or more and less than 0.7 were evaluated as "○", and vE 0% / vE 10% The steel plates with a vE of 0.7 or more were rated as “◎”. 0% / vE 10% A steel plate with a value of 0.6 or more is judged to be “excellent in resistance to work brittleness.” It should be noted that the conditions other than the above are in accordance with JIS Z2242:2018.
[0134] The results are shown in Tables 7 to 10. As shown in these tables, in the examples of the present invention, TS is 1180 MPa or more, YR is 85% or more, and the flatness in the plate width direction and the work embrittlement resistance are excellent. On the other hand, in the comparative examples, one or more of TS, YR, flatness in the plate width direction, or work embrittlement resistance is poor.
[0135]
[0136]
[0137]
[0138]
Claims
1. A high-strength steel plate, The composition is as follows: in mass %, it contains C: 0.030% to 0.500%, Si: 0.01% to 2.50%, Mn: 0.10% to 5.00%, P: 0.100% to 0.0200% to 0.0200%, Al: 1.000% to 1.000%, N: 0.0100% to 0.0100% and O: 0.0100% to 0.0100%, with the balance being Fe and unavoidable impurities. At the 1 / 4 position of the plate thickness, the amount of tempered martensite is more than 90% by area fraction, the amount of retained austenite is less than 3% by volume fraction, the total amount of ferrite and bainitic ferrite is less than 10% by area fraction, the average grain size of the original austenite is less than 20μm, and the average occupancy of the lath bundle with the maximum occupancy in the original austenite grains is less than 70% by area fraction.
2. The high-strength steel plate according to claim 1, wherein: The component composition further contains, in mass %, at least one element selected from the group consisting of Ti: 0.200% or less, Nb: 0.200% or less, V: 0.200% or less, Ta: 0.10% or less, W: 0.10% or less, B: 0.0100% or less, Cr: 1.00% or less, Mo: 1.00% or less, Co: 0.010% or less, Ni: 1.00% or less, Cu: 1.00% or less, Sn: 0.200% or less, Sb: 0.200% or less, Ca: 0.0100% or less, Mg: 0.0100% or less, REM: 0.0100% or less, Zr: 0.100% or less, Te: 0.100% or less, Hf: 0.10% or less, and Bi: 0.200% or less.
3. The high-strength steel sheet according to claim 1 or 2, wherein: The steel plate has a coating on its surface.
4. A method for producing a high-strength steel sheet, which is the method for producing a high-strength steel sheet according to claim 1 or 2, wherein: For a cold-rolled sheet produced by hot-rolling, pickling and cold-rolling the steel having the above-mentioned chemical composition, The heating is performed under the conditions that the annealing temperature T1 is 750° C. or higher and 950° C. or lower, and the holding time t1 at the annealing temperature T1 is 10 seconds or higher and 1000 seconds or lower, Cooling is performed under the conditions that the average cooling rate from 750°C to 600°C is 20°C / s or more, the average cooling rate from (Ms+50°C) to the quenching start temperature T2 is 5°C / s or more and 30°C / s or less, the quenching start temperature T2 is (Ms-80°C) or more and less than Ms, and the average cooling rate from the quenching start temperature T2 to 80°C is 300°C / s or more, wherein Ms is the martensitic transformation start temperature (°C) specified by the formula (1), The heating is performed under the conditions that the tempering temperature T3 is 100° C. or higher and 400° C. or lower and the holding time t3 at the tempering temperature T3 is 10 seconds or higher and 10000 seconds or lower. Ms=519-474×[%C]-30.4×[%Mn]-12.1×[%Cr]-7.5×[%Mo]-17.7×[%Ni]…(1) Here, [%C], [%Mn], [%Cr], [%Mo], and [%Ni] represent the content (mass %) of C, Mn, Cr, Mo, and Ni, respectively, and when not contained, it is set to 0.
5. The method for producing a high-strength steel sheet according to claim 4, wherein: A plating treatment is performed.
Citation Information
Cited By
Steel plate for automobile chassis part and preparation process of steel plate
CN119956223A