Preparation method of hydrogel evaporator for light-driven interface seawater desalination
Through physical cross-linking of graphene oxide/hydrated calcium silicate nanosheets and polyvinyl alcohol and other materials, a hydrogel evaporator with efficient evaporation rate and excellent salt resistance is prepared, which solves the problem of salt resistance of existing hydrogels. Limitations in performance and cycle stability enable application prospects in seawater desalination and sewage purification.
Patent Information
- Application Number
- CN202411107489.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-13
- Publication Date
- 2024-10-22
AI Technical Summary
Existing hydrogels have limitations in salt resistance, circulation, and seawater evaporation rate, making it difficult to develop hydrogel evaporators with high evaporation rates and excellent salt resistance.
The hydrogel evaporator is prepared by physical cross-linking method using graphene oxide/hydrated calcium silicate nanosheets, polyvinyl alcohol, polyethyleneimine/diglyphosate polymer, and through specific mass ratios and preparation steps, a hydrogel evaporator is formed. Hydrogel with excellent photothermal properties and high evaporation efficiency.
The hydrogel evaporator achieves good performance in light and heat absorption, seawater evaporation and circulation stability, and has broad application prospects in seawater desalination and sewage purification.
Smart Images

Figure CN118807626A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the research field of light-driven interface seawater desalination technology and relates to a hydrogel evaporator used for light-driven interface seawater desalination and a preparation method thereof. Background Art
[0002] Although the ocean accounts for 96.2% of the world's total water, it contains a large amount of salt, electrolytes and high osmotic pressure, making it impossible to drink directly. Faced with these challenges, there is an urgent need to develop materials that can be used for efficient seawater desalination and water purification.
[0003] Hydrogels have a three-dimensional cross-linked polymer grid structure and are considered to be one of the most commonly used materials in light-driven interfacial desalination. In particular, they have an adjustable pore structure and morphology, which can further regulate the saturated water content and the state of water molecules to achieve rapid water supply and continuous evaporation of water. However, the hydrogels reported so far are still subject to various limitations in terms of salt resistance, cyclability, and seawater evaporation rate. The development of hydrogel evaporators with high evaporation rates and excellent salt resistance still faces great challenges. Summary of the invention
[0004] In view of the above problems, the purpose of the present invention is to propose a hydrogel evaporator for light-driven interfacial seawater desalination, which has good performance in light-heat absorption and conversion, seawater evaporation and cycle stability.
[0005] Another object of the present invention is to provide a method for preparing a hydrogel evaporator that can be used for light-driven interfacial seawater desalination.
[0006] The technical solution of the present invention is: a hydrogel evaporator for light-driven interfacial seawater desalination according to the present invention is prepared by a physical cross-linking method using graphene oxide / calcium silicate hydrate nanosheets, polyvinyl alcohol, polyethyleneimine / bis(glycyrrhizic acid) polymer;
[0007] Wherein, the mass percentage of the polyvinyl alcohol (total weight of water) is 3.5-10.5%;
[0008] The mass ratio (total mass ratio) of the graphene oxide / hydrated calcium silicate nanosheets and polyethyleneimine / bis(glycolylphosphine) polymer is 5-15:1.5-3.5.
[0009] Furthermore, the mass percentage of the polyvinyl alcohol (total weight of water) is 5.5-8.5%;
[0010] The mass ratio (total volume ratio) of the graphene oxide / hydrated calcium silicate nanosheets and polyethyleneimine / bis(glycophosphine) polymer is 5-8:1.5-2.5.
[0011] Furthermore, the mass percentage of the polyvinyl alcohol (total weight of water) is 7-8%;
[0012] The mass ratio (total volume ratio) of the graphene oxide / hydrated calcium silicate nanosheets and polyethyleneimine / bis(glycophosphine) polymer is 6-7:2-2.5.
[0013] Furthermore, the polyvinyl alcohol is polyvinyl alcohol 1799, and the polyethyleneimine is polyethyleneimine 600;
[0014] Furthermore, the preparation method thereof comprises the following steps:
[0015] (1) Dissolve polyvinyl alcohol in deionized water, heat and stir until it is completely dissolved and transparent, then add polyethyleneimine / bis(glyphosate) polymer and graphene oxide / calcium silicate hydrate nanosheets in sequence, and continue stirring until uniformly dispersed;
[0016] (2) Pour the above dispersion evenly into a mold, and prepare a hydrogel evaporator by repeated thawing-freezing-freeze drying.
[0017] Furthermore, in step (1), the heating and stirring conditions are: 60-90° C., 6-10 h;
[0018] Furthermore, in step (1), the preparation method of the polyethyleneimine / bis(glycophosphine) polymer is as follows: PMIDA (0.1 g) is dissolved in deionized water (20 mL), DMTMM (0.19 g) is added, and then polyethyleneimine (0.3 mL) is added dropwise, stirred at room temperature for 10 to 18 hours, dialyzed with deionized water, and vacuum dried.
[0019] Furthermore, in step (1), the preparation method of the graphene oxide / hydrated calcium silicate nanosheets is as follows: dispersing the graphene oxide in an ethanol solution, ultrasonicating; adding an ammonia solution; then, dropping TEOS, centrifuging after ultrasonicating, and washing with water; dispersing the centrifuged sample in an aqueous solution, and then adding Ca(NO3)2·4H2O and Na2SiO3 solutions, stirring; adjusting the pH by adding NaOH, ultrasonicating, centrifuging, washing with water, and vacuum drying.
[0020] Furthermore, in step (2), the conditions of repeated thawing and freeze-drying are: -80°C for 8 to 12 hours and 25°C for 10 to 30 minutes.
[0021] The beneficial effects of the present invention are: 1. The hydrogel evaporator of the present invention has excellent photothermal performance and high evaporation efficiency, and also has good cycle stability; 2. The preparation method of the present invention is simple and the structure is novel; 3. The hydrogel evaporator of the present invention has broad application prospects in light-driven interface seawater desalination, sewage purification and the like. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 It is a schematic diagram of the preparation process of the present invention. DETAILED DESCRIPTION
[0023] The specific technical scheme of the present invention is further described in detail below with reference to specific examples.
[0024] Example 1
[0025] (1) Preparation of graphene oxide / calcium silicate hydrate nanosheets: Graphene oxide was dispersed in 120 ml of ethanol solution (4 mg mL -1 ) and placed in a bath at 25°C; add 2ml of 28% ammonia solution to the dispersion and sonicate for 1 to 3h; then, drop 0.3ml of LTEOS into the dispersion, sonicate for 2 to 4h, centrifuge and wash with water; disperse the centrifuged sample in an aqueous solution, then add 3ml of Ca(NO3)2·4H2O (60mM) and 3ml of Na2SiO3 (60mM) solution and stir; adjust the pH to ~13.0 by adding NaOH, sonicate for 2h, centrifuge, wash with water, and vacuum dry to obtain a powder;
[0026] (2) Preparation of polyethyleneimine / bis(ethylene glycol)phosphine polymer: PMIDA (0.1 g) was dissolved in deionized water (20 mL), and DMTMM (0.19 g) was added at the same time; PEI (0.3 mL) was then added dropwise, and the mixture was stirred at room temperature for 10 to 18 h, and then dialyzed with deionized water, and repeated three times; and a powder was obtained after vacuum drying;
[0027] (3) Preparation of hydrogel evaporator: Weigh polyvinyl alcohol and dissolve it in deionized water, heat and stir at 60°C for 10 hours to obtain a 7.5% solution; then, add polyethyleneimine / bis(glycyrrhizic acid) powder and continue stirring; finally, add graphene oxide / calcium silicate hydrate powder and stir until evenly dispersed; pour the mixed solution into a polytetrafluoroethylene mold, and repeatedly thaw and freeze three times (8 hours at -80°C, 10 minutes at 25°C) to obtain a composite hydrogel.
[0028] In this embodiment, the mass ratio of polyethyleneimine / bis(ethylene glycol)phosphine polymer to graphene oxide / calcium silicate hydrate nanosheets is 5:3.5.
[0029] Example 2
[0030] (1) Preparation of graphene oxide / calcium silicate hydrate nanosheets: same as in Example 1.
[0031] (2) Preparation of polyethyleneimine / bis(ethylene glycol)phosphine polymer: same as in Example 1.
[0032] (3) Preparation of hydrogel evaporator: Weigh polyvinyl alcohol and dissolve it in deionized water, heat and stir at 80°C for 8 hours to obtain a 3.5% solution; then, add polyethyleneimine / bis(glycyrrhizic acid) powder and stir until it is evenly dispersed; finally, add graphene oxide / calcium silicate hydrate powder and continue stirring; pour the mixed solution into a polytetrafluoroethylene mold and repeatedly thaw and freeze three times (10 hours at -80°C and 20 minutes at 25°C) to obtain a composite hydrogel.
[0033] In this embodiment, the mass ratio of polyethyleneimine / bis(ethylene glycol)phosphine polymer to graphene oxide / calcium silicate hydrate nanosheets is 10:2.5.
[0034] Example 3
[0035] (1) Preparation of graphene oxide / calcium silicate hydrate nanosheets: same as in Example 1.
[0036] (2) Preparation of polyethyleneimine / bis(ethylene glycol)phosphine polymer: same as in Example 1.
[0037] (3) Preparation of hydrogel evaporator: Weigh polyvinyl alcohol and dissolve it in deionized water, heat and stir at 90°C for 6 hours to obtain a 10.5% solution; then, add polyethyleneimine / bis(glycyrrhizic acid) powder and stir; finally, add graphene oxide / calcium silicate hydrate powder and continue stirring; pour the mixed solution into a polytetrafluoroethylene mold, and repeatedly thaw and freeze three times (12 hours at -80°C and 30 minutes at 25°C) to obtain a composite hydrogel.
[0038] In this embodiment, the mass ratio of polyethyleneimine / bis(ethylene glycol)phosphine polymer to graphene oxide / calcium silicate hydrate nanosheets is 15:3.5.
[0039] Comparative Example 1
[0040] (1) Preparation of polyethyleneimine / bis(ethylene glycol)phosphine polymer: same as in Example 1.
[0041] (2) Preparation of hydrogel evaporator: Weigh polyvinyl alcohol and dissolve it in deionized water, heat and stir at 60°C for 10 hours to obtain a 7.5% solution; then, add polyethyleneimine / bis(glycyrrhizin) powder and stir; finally, add graphene oxide powder and continue stirring; pour the mixed solution into a polytetrafluoroethylene mold, and repeatedly thaw and freeze three times (8 hours at -80°C, 10 minutes at 25°C) to obtain a composite hydrogel.
[0042] In this embodiment, the mass ratio of polyethyleneimine / bis(glycophosphine) polymer to graphene oxide is 5:1.5. The results of Comparative 1 show that the evaporation rate and evaporation efficiency of the hydrogel evaporator doped with graphene oxide are relatively low.
[0043] Comparative Example 2
[0044] Preparation of hydrogel evaporator: Weigh polyvinyl alcohol and dissolve it in deionized water, heat and stir at 60°C for 10 hours to obtain a 7.5% solution, pour the mixed solution into a polytetrafluoroethylene mold, and repeatedly thaw and freeze three times (8 hours at -80°C, 10 minutes at 25°C) to obtain a composite hydrogel; The results of Comparative Example 1 show that the single polystyrene hydrogel evaporator does not have photothermal performance, and the evaporation rate and evaporation efficiency are too low.
Claims
1. A method for preparing a hydrogel evaporator for light-driven interfacial seawater desalination, characterized in that , the hydrogel evaporator is prepared by a physical cross-linking method of graphene oxide / hydrated calcium silicate nanosheets, polyvinyl alcohol, polyethyleneimine / bis(glycolylphosphine) polymer; The preparation steps are as follows: Step (1): dissolving the prepared polyvinyl alcohol in deionized water, heating and stirring until it is dissolved and becomes transparent, then sequentially adding polyethyleneimine / bis(glycyrrhizic acid) polymer and graphene oxide / calcium silicate hydrate nanosheets, and continuing to stir until uniformly dispersed; Step (2): Pour the above-mentioned uniformly stirred dispersion into a mold evenly, and finally obtain a hydrogel evaporator through a repeated thawing-freezing-freeze drying process.
2. The method for preparing a hydrogel evaporator for light-driven interfacial seawater desalination according to claim 1, characterized in that: In step (1), the mass percentage of the polyvinyl alcohol is 3.5 to 10.5%; The mass ratio of the graphene oxide / hydrated calcium silicate nanosheets to the polyethyleneimine / bis(glycophosphine) polymer is 5-15:1.5-3.
5.
3. The method for preparing a hydrogel evaporator for light-driven interfacial seawater desalination according to claim 2, characterized in that: The mass percentage of the polyvinyl alcohol is 5.5-8.5%; The mass ratio of the graphene oxide / hydrated calcium silicate nanosheets to the polyethyleneimine / bis(glycophosphine) polymer is 5-8:1.5-2.
5.
4. The method for preparing a hydrogel evaporator for light-driven interfacial seawater desalination according to claim 2, characterized in that: The mass percentage of the polyvinyl alcohol is 7-8%; The mass ratio of the graphene oxide / hydrated calcium silicate nanosheets to the polyethyleneimine / bis(glycophosphine) polymer is 6-7:2-2.
5.
5. The method for preparing a hydrogel evaporator for light-driven interfacial seawater desalination according to claim 1, characterized in that: In step (1), the heating and stirring conditions are: 60-90° C., 6-10 h.
6. The method for preparing a hydrogel evaporator for light-driven interfacial seawater desalination according to claim 1, characterized in that: In step (1), the polyvinyl alcohol is polyvinyl alcohol 1799; and the polyethyleneimine is polyethyleneimine 600.
7. The method for preparing a hydrogel evaporator for light-driven interfacial seawater desalination according to claim 1, characterized in that: In step (1), the preparation process of the polyethyleneimine / diglycol phosphine polymer is as follows: dissolve the prepared diglycol phosphine in deionized water, add 4-(4,6-dimethoxytriazine-2-yl)-4-methylmorpholine hydrochloride and then drop polyethyleneimine, stir at room temperature for 10 to 18 hours, dialyze with deionized water, and vacuum dry.
8. The method for preparing a hydrogel evaporator for light-driven interfacial seawater desalination according to claim 1, characterized in that: In step (1), the preparation process of the graphene oxide / hydrated calcium silicate nanosheets is as follows: dispersing the graphene oxide in an ethanol solution, ultrasonicating, adding an ammonia solution; then, dripping tetramethoxysilane, ultrasonicating, centrifuging, and washing with water; The centrifuged sample was dispersed in an aqueous solution, and then Ca(NO3)2·4H2O and Na2SiO3 solutions were added and stirred; the pH was adjusted by adding NaOH, ultrasonicated, centrifuged, washed with water, and vacuum dried.
9. The method for preparing a hydrogel evaporator for light-driven interfacial seawater desalination according to claim 1, characterized in that: In step (2), the conditions for repeated thawing and freeze-drying are: 8 to 12 hours at -80°C and 10 to 30 minutes at 25°C.
10. Use of the hydrogel evaporator prepared by the preparation method according to any one of claims 1 to 9 in light-driven interfacial seawater desalination.
Citation Information
Cited By
Graphene composite hydrogel interface evaporation material as well as preparation method and application thereof
CN121628265A
Graphene composite hydrogel interfacial evaporation material and preparation method and application thereof
CN121628265B
Sea water desalination hydrogel evaporator and preparation method thereof
CN122079278A