Preparation method of blood perfusion adsorbent with good blood compatibility
By combining argon plasma treatment with heparin sodium and ultrasonic cleaning, the problem of insufficient surface treatment of macroporous resin is solved, high biocompatibility and low coagulation risk of the adsorbent for hemoperfusion are achieved, and the safety of treatment is improved. and effect.
Patent Information
- Application Number
- CN202410878833.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-02
- Publication Date
- 2024-10-22
AI Technical Summary
There are few methods for treating the surface of macroporous resins in the prior art, which leads to problems with biocompatibility and coagulation reaction in hemoperfusion applications, affecting the therapeutic effect and safety.
The polystyrene divinylbenzene resin is pretreated with argon plasma, and active groups are introduced and then combined with heparin sodium. It is processed again by plasma equipment and ultrasonic cleaned to form an adsorbent with good blood compatibility.
By fixing heparin through chemical grafting, the hydrophilicity and biocompatibility of the resin are improved, the coagulation reaction is reduced, and the safety and effectiveness of hemoperfusion and dialysis treatments are improved.
Smart Images

Figure CN118807707A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of preparation of an adsorbent for blood perfusion, and in particular to a method for preparing an adsorbent for blood perfusion with good blood compatibility. Background Art
[0002] Plasma material surface modification can cause a series of physical and chemical changes on the material surface, thereby improving the surface properties of the material, while the material matrix properties are almost unaffected. Through plasma surface treatment, the material surface undergoes a variety of physical and chemical changes, or becomes rough due to etching, or forms a dense cross-linked layer, or introduces oxygen-containing polar groups, thereby improving the hydrophilicity, adhesion, dyeability, biocompatibility and electrical properties.
[0003] Argon treatment is a non-reactive gas that does not participate in the chemical reaction on the resin surface. Its ions, free radicals, excited molecules and other chemical collisions with the polymer surface produce chemically active free radicals.
[0004] The surface of polystyrene divinyl benzene resin pretreated by argon plasma contains polar groups such as one COOH or one OH. After being exposed to air, a highly cross-linked cross-linking layer is formed. On this basis, after passing through Ar plasma again, polystyrene divinyl benzene resin can be combined with heparin in the form of covalent bonds through the cross-linking layer. In particular, the literature shows that plasma treatment technology is widely used in the surface treatment of rubber, plastics, fibers and fabrics, metals, PP, PS, PC, etc., but there are few reports on the surface treatment of macroporous resins. Summary of the invention
[0005] The invention provides a method for preparing a blood perfusion adsorbent with good blood compatibility, which realizes surface treatment of a macroporous resin by utilizing argon gas.
[0006] The present invention provides a method for preparing a blood perfusion adsorbent with good blood compatibility, comprising the following steps:
[0007] placing polystyrene divinyl benzene resin in a plasma device and introducing argon gas for treatment to obtain treated polystyrene divinyl benzene resin;
[0008] immersing the treated polystyrene divinyl benzene resin in sodium heparin to obtain a polystyrene divinyl benzene resin after a first treatment;
[0009] After drying the polystyrene divinyl benzene resin after the first treatment at room temperature, the polystyrene divinyl benzene resin is treated by introducing argon gas using a plasma device to obtain a polystyrene divinyl benzene resin after the second treatment;
[0010] Immersing the re-treated polystyrene divinyl benzene resin in sodium heparin to obtain a second-treated polystyrene divinyl benzene resin;
[0011] The polystyrene divinyl benzene resin after the second treatment is cleaned by ultrasonic wave to obtain an adsorbent for blood perfusion with good blood compatibility.
[0012] In the method for preparing the adsorbent for blood perfusion with good blood compatibility, preferably, the conditions for introducing the argon gas are: the pressure in the plasma equipment is 1.0Pa-2.5Pa, and the argon gas flow rate is 50-150m / min.
[0013] In the method for preparing the adsorbent for blood perfusion with good blood compatibility, preferably, the discharge power is 60-200W and the processing time is 5-20min.
[0014] In the method for preparing the adsorbent for blood perfusion with good blood compatibility, preferably, the concentration of the heparin sodium is 0.25-5 mg / ml, and the reaction time of the heparin sodium is 4-10 h.
[0015] In the method for preparing the adsorbent for blood perfusion with good blood compatibility, preferably, the ultrasonic cleaning specifically comprises the following steps:
[0016] Ultrasonic cleaning with distilled water to remove surface impurities and ungrafted heparin sodium from the polystyrene divinyl benzene resin after the second treatment, and drying at room temperature to obtain the washed polystyrene divinyl benzene resin;
[0017] The polystyrene divinyl benzene resin is cleaned with ethanol ultrasonic wave to remove other compounds after cleaning, and then dried at room temperature to obtain an adsorbent for blood perfusion with good blood compatibility.
[0018] The beneficial effects are:
[0019] Heparin sodium is mostly used to prevent thrombosis and embolism, and to treat disseminated intravascular coagulation and other coagulation inside and outside the body caused by various reasons.
[0020] The resin prepared in the present application grafts and fixes heparin on the resin, and introduces hydrophilic groups hydroxyl and carboxyl: on the one hand, the compatibility and biocompatibility of the resin in the blood are improved, which can reduce various types of adverse reactions during the treatment process; on the other hand, the heparin firmly bonded by chemical grafting can reduce the coagulation reaction of the perfusion device and the dialyzer during the treatment process, so that the perfusion and dialysis treatment can be carried out smoothly, achieve the clinical use effect, and reduce the patient's coagulation risk and blood loss caused by coagulation. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1is the result after the first treatment;
[0022] Figure 2 This is the result after the second processing. DETAILED DESCRIPTION
[0023] In order to make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention will be clearly and completely described below in conjunction with the accompanying drawings. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0024] A method for preparing a blood perfusion adsorbent with good blood compatibility comprises the following steps:
[0025] S1: placing polystyrene divinyl benzene resin into a plasma device and introducing argon gas for treatment to obtain treated polystyrene divinyl benzene resin.
[0026] The treatment in step S1 causes the surface of the polystyrene divinyl benzene resin to collide with the active plasma to break the covalent bonds, and introduce various active chemical functional groups, such as carboxyl, carbonyl, hydroxyl, etc., on the surface of the polystyrene divinyl benzene resin.
[0027] The conditions for introducing the argon gas are as follows: the pressure in the plasma equipment is 1.0Pa-2.5Pa, the argon gas flow rate is 50-150m / min, the discharge power is 60-200W, and the processing time is 5-20min.
[0028] S2: Immersing the treated polystyrene divinyl benzene resin in sodium heparin to obtain polystyrene divinyl benzene resin after the first treatment.
[0029] After the polystyrene divinyl benzene resin treated in step S2 enters the sodium heparin, the active functional groups on the surface of the polystyrene divinyl benzene resin will form covalent bonds with the sodium heparin, thereby fixing the sodium heparin on the resin surface.
[0030] Wherein, the concentration of the heparin sodium is 0.25-5 mg / ml, and the reaction time of the heparin sodium is 4-10 h.
[0031] S3: After drying the polystyrene divinyl benzene resin after the first treatment at room temperature, the polystyrene divinyl benzene resin is treated by introducing argon gas using a plasma device to obtain a polystyrene divinyl benzene resin after a second treatment.
[0032] The step S3 specifically includes the following steps:
[0033] S31: After the plasma equipment is vacuumed to 1.0Pa-2.5Pa, argon gas is introduced with an argon flow rate of 50-150m / min and a discharge power of 60-200W to perform plasma glow discharge treatment. After 5-20 minutes, the polystyrene divinyl benzene resin is taken out.
[0034] S32: The polystyrene divinyl benzene resin is immersed in 0.2 g-1.0 g heparin sodium / 200-800 mL solution, and taken out after 4-10 hours to obtain the polystyrene divinyl benzene resin after being treated again.
[0035] S4: immersing the re-treated polystyrene divinyl benzene resin in sodium heparin to obtain a second-treated polystyrene divinyl benzene resin.
[0036] S5: ultrasonically cleaning the polystyrene divinyl benzene resin after the second treatment to obtain a blood perfusion adsorbent with good blood compatibility.
[0037] Wherein, the ultrasonic cleaning specifically comprises the following steps:
[0038] Step 1: ultrasonically clean the polystyrene divinyl benzene resin with distilled water for 5-15 minutes to remove surface impurities and ungrafted heparin sodium of the polystyrene divinyl benzene resin after the second treatment, and dry at room temperature to obtain the cleaned polystyrene divinyl benzene resin;
[0039] Step 2: Use 95% ethanol to perform ultrasonic cleaning for 5-15 minutes to remove other compounds of the polystyrene divinyl benzene resin after the cleaning, and dry at room temperature to obtain a blood perfusion adsorbent with good blood compatibility.
[0040] like Figure 1 and Figure 2 As shown, polar groups hydroxyl and carbonyl were introduced, and the modified polystyrene divinyl benzene resin showed good hydrophilicity and anticoagulant properties.
[0041] 1. Qualitative analysis
[0042] 1 # After one treatment, the resin and 2 # The structure of the resin after secondary treatment was qualitatively analyzed and blood compatibility analyzed, as shown in Table 1 and Table 2, respectively.
[0043] Among them, 1 # The resin after the first treatment is the resin obtained after the treatment in step S1 and step S2. # The resin after the secondary treatment is processed through step S3 and step S4 to obtain the resin.
[0044] Table 1 Summary of qualitative analysis results
[0045]
[0046] Table 2 Blood compatibility results
[0047]
[0048] The results showed that the PTT and PT values of the samples treated with plasma were significantly prolonged, which can reduce the risk of coagulation during clinical use. However, the PTT / PT value of the samples treated twice was higher than that of the samples treated once.
[0049] 2. Controlled trials
[0050] The test is based on the national standard GB / T16886.4-2022 "Biological Evaluation of Medical Devices Part 4: Selection of Tests for Interactions with Blood". The partial thromboplastin time (PTT) test and prothrombin time (PT) test methods are used to conduct in vitro blood compatibility tests on the test samples to evaluate the effect of the samples on the coagulation time of human plasma.
[0051] Test medium: Collect human blood in a vacuum blood collection tube containing sodium citrate anticoagulant (3.2%, 0.109M), centrifuge at 3500r / min for 10min, take the upper plasma and place it in a polypropylene test tube (with a cap), and store it on ice.
[0052] Sample preparation: The test sample was steam sterilized at 115℃ for 30min, and 0.2g of the test sample was prepared in 1.0ml of the test medium based on the ratio of 0.2g / ml. The test sample was immersed in the test medium and incubated at (37±1)℃ and 60r / min shaking for (1±0.1)h, and 6 tubes were prepared in parallel.
[0053] The sample is: raw material resin (polystyrene divinyl benzene resin), 1 # After one treatment, the resin and 2 # Resin after secondary treatment.
[0054] Negative control: based on 6cm 2 / ml ratio, 6.0cm 2 Prepare high-density polyethylene in 1.0 ml of test medium. Cut the negative control into small pieces and immerse them in the test medium at (37±1)℃, shake at 60r / min for (1±0.1)h. Prepare 6 tubes in parallel.
[0055] Blank control: Sodium citrate anticoagulated human plasma was used as blank control. 1.0 ml human plasma was incubated at (37±1)℃ and 60r / min for (1±0.1)h. Six tubes were prepared in parallel.
[0056] Positive control: based on 6cm2 / ml ratio, 6.0cm 2 Glass beads were prepared in 1.0 ml of test medium. The positive control was immersed in the test medium and incubated at (37±1)°C with shaking at 60 r / min for (1±0.1) h. Six tubes were prepared in parallel.
[0057] Experimental steps: Place the test sample, negative control and positive control in polypropylene test tubes, 6 parallel tubes each. Add an appropriate volume of plasma to each tube and incubate at (37±1)℃ for (1±0.1)h. Prepare the blank control in the same way. After the incubation, place the plasma in a new test tube and store it in ice water before analysis. Measure the partial thromboplastin time (PTT) and prothrombin time (PT) of each tube.
[0058] Calculation results:
[0059] The mean coagulation time and standard deviation of the test sample, negative control, positive control and blank control were calculated respectively.
[0060] Calculate the percentage of PPT of the test sample, negative control and positive control relative to the blank control using the following formula:
[0061]
[0062] Results Validity:
[0063] (1) PTT test: The percentage of negative control relative to blank control should be >80%. The percentage of positive control relative to blank control should usually be <50%.
[0064] (2) PT test: The normal range of PT time is 10.0-14.0 seconds. If the average PT value of the blank control exceeds this range by ±1 second, the test is considered invalid and needs to be retested.
[0065] The statistical analysis was performed using analysis of variance (Tukey method). The positive control should have significant differences compared with the blank control and the negative control (P < 0.05), and the negative control should have no significant difference compared with the blank control (P ≥ 0.05).
[0066] The comparative test results percentages of table 3 raw material resin (polystyrene divinyl benzene resin) are shown in the following table:
[0067]
[0068] Table 41 # The percentage of comparative test results of the resin after one treatment is shown in the following table:
[0069]
[0070] Table 52 # The percentage of comparative test results of the resin after secondary treatment is shown in the following table:
[0071]
[0072] As shown in Tables 3 to 5, the percentage of PTT value of the untreated resin in the test samples relative to the blank control was 70%, while the percentages of the resin #1 after one treatment and the resin #2 after two treatments were 93% and 149%, respectively.
[0073] The average PT values of the untreated resin, 1# resin after one treatment and 2# resin after two treatments in the test samples were 13.5 seconds, 31.9 seconds and 41.0 seconds respectively. The average PT value of the negative control was 11.8 seconds, and the average PT value of the blank control was 11.8 seconds. The test samples were significantly different from the negative control and the blank control, but not lower than the negative control and the blank control.
[0074] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for preparing an adsorbent for blood perfusion with good blood compatibility, characterized in that: The steps include: The polystyrene divinyl benzene resin is placed in a plasma device and treated by passing argon gas to obtain a polystyrene divinyl benzene resin with active chemical functional groups introduced on the surface; The polystyrene divinyl benzene resin with active chemical functional groups introduced on the surface is immersed in sodium heparin to obtain a resin after a single treatment; After drying the resin after the primary treatment at room temperature, the resin is treated by introducing argon gas using a plasma device to obtain a resin with active chemical functional groups introduced on the surface; The resin with active chemical functional groups introduced on the surface is immersed in sodium heparin to obtain a resin after secondary treatment; The resin after the secondary treatment is cleaned by ultrasonic wave to obtain an adsorbent for blood perfusion with good blood compatibility.
2. The method for preparing a blood perfusion adsorbent with good blood compatibility according to claim 1, characterized in that: The conditions for introducing the argon gas are: the pressure in the plasma equipment is 1.0Pa-2.5Pa, and the flow rate of the argon gas is 50-150m / min.
3. The method for preparing a blood perfusion adsorbent with good blood compatibility according to claim 2, characterized in that: The discharge power is 60-200W, and the treatment time is 5-20min.
4. The method for preparing a blood perfusion adsorbent with good blood compatibility according to claim 3, characterized in that: The concentration of the sodium heparin is 0.25-5 mg / ml, and the reaction time of the sodium heparin is 4-10 h.
5. The method for preparing a blood perfusion adsorbent with good blood compatibility according to claim 4, characterized in that: The ultrasonic cleaning specifically comprises the following steps: Ultrasonic cleaning with distilled water to remove surface impurities and ungrafted heparin sodium from the polystyrene divinyl benzene resin after the second treatment, and drying at room temperature to obtain the washed polystyrene divinyl benzene resin; The polystyrene divinyl benzene resin is cleaned with ethanol ultrasonic wave to remove other compounds after cleaning, and then dried at room temperature to obtain an adsorbent for blood perfusion with good blood compatibility.
Citation Information
Patent Citations
Bilirubin adsorbent for blood perfusion
CN104174385A
High molecular material surface modification method and its product and application
CN107189096A
Adsorbent material for removing LDL during hemoperfusion and preparation method thereof
CN110117379A
Heparinization of plasma treated substrates
EP0124200A2
Cited By
Kit for testing partial thromboplastin time of medical instrument and application
CN119044513A