Easily degradable corrugated paper additive and preparation method thereof
By using modified reinforcing agents on corrugated board, combined with oxidized starch and small molecular weight branched epoxy silicone oil, the folding resistance and wet tensile strength of corrugated board are improved, which solves the problem of insufficient performance of traditional corrugated board and achieves higher performance. Environmental protection and service life.
Patent Information
- Application Number
- CN202411107841.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-13
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2044-08-13
AI Technical Summary
Traditional corrugated cardboard has limited performance in terms of waterproofing, moisture-proofing, and pressure resistance. Existing sizing agents are difficult to degrade naturally and cannot meet the needs of environmentally friendly production. Starch sizing additives have limited strengthening effects and insufficient water resistance.
Using oxidized starch as the base material, through independently developed modified reinforcing agents, small molecular weight branched epoxy silicone oil and fluorine structure, combined with ethoxysilane structure, enhance the folding resistance and wet tensile strength of corrugated paper, and on the surface A fluorine-containing silicone water-resistant layer is introduced to form a rivet function to improve the bonding strength of paper fibers.
It significantly improves the folding resistance and wet tensile strength of corrugated paper, improves its biodegradability and environmental protection, extends its service life, and improves packaging stability.
Smart Images

Figure BDA0004991327100000081
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of packaging materials, and in particular relates to a degradable corrugated paper additive and a preparation method thereof. Background Art
[0002] With the rapid development of the packaging industry, the demand for corrugated cardboard as an important packaging material has increased year by year. The main function of corrugated cardboard is to provide packaging strength and protect the packaging contents, especially during transportation and storage. However, traditional corrugated cardboard has certain limitations in terms of waterproof, moisture-proof, and compression resistance, which limits its application in certain special environments.
[0003] At present, one of the main methods to improve the performance of corrugated paperboard is sizing treatment, that is, applying sizing agents on the surface or inside of corrugated paperboard. Existing sizing agents mainly include synthetic resin sizing agents and paraffin sizing agents. Although these sizing agents effectively improve the performance of corrugated paperboard, they are difficult to degrade naturally and do not meet the requirements of environmentally friendly production. Starch sizing agents are new biodegradable and environmentally friendly corrugated paper additives. They are made of natural starch converted into modified starch with the required properties through physical, chemical or enzymatic treatment as the base material. They can improve the performance of corrugated paper to a certain extent, but their strengthening effect is limited and their water resistance is insufficient, which greatly limits the application of starch sizing agents. Summary of the invention
[0004] In order to solve the technical problems mentioned in the background technology, the purpose of the present invention is to provide a degradable corrugated paper additive and a preparation method thereof.
[0005] The purpose of the present invention can be achieved through the following technical solutions:
[0006] A degradable corrugated paper additive, comprising, by weight:
[0007] 50 parts of oxidized starch, 6-8 parts of modified enhancer, 0.5-0.7 parts of thickener, 0.15-0.2 parts of dispersant, 0.1-0.13 parts of defoamer, 0.02-0.03 parts of mildewproof agent and 90-100 parts of water.
[0008] The modified reinforcing agent is prepared by the following method:
[0009] Step A1: epoxy silicone oil, triethylamine and acetone are mixed, nitrogen is introduced for protection, the temperature is raised to 45-55°C, stirring is applied at 120-180 rpm, 2,2-difluoroethylamine is slowly added, and the reaction is carried out for 2.5-3.5 hours. After the reaction is completed, the mixture is rotary evaporated, washed with water, and vacuum dried to obtain an intermediate;
[0010] Further, the epoxy silicone oil is selected from branched epoxy silicone oil;
[0011] Furthermore, epoxy silicone oil is a low molecular weight silicone oil with a room temperature viscosity of no more than 30 mm 2 / s;
[0012] Furthermore, the epoxy content of the epoxy silicone oil, the amount ratio of 2,2-difluoroethylamine, triethylamine and acetone is 0.1 mol: 0.102-0.105 mol: 15-20 mL: 55-70 mL, and the active amino group of 2,2-difluoroethylamine opens the ring with the epoxy silicone oil to introduce a fluorine structure into the silicone oil chain.
[0013] Step A2: The intermediate, 3-chloropropyltriethoxysilane and anhydrous dioxane are mixed, dry nitrogen is introduced for protection, sodium hydroxide is added and mixed, the temperature is raised to 80-100° C., stirring is applied at 90-120 rpm, the reaction is carried out for 5-7 hours, and after the reaction is completed, the modified enhancer is obtained by filtering and rotary evaporation;
[0014] Furthermore, the usage ratio of the intermediate, 3-chloropropyltriethoxysilane, sodium hydroxide and anhydrous dioxane is 50g:0.06-0.08mol:5-8g:120-160mL. Under the promotion of the strong alkalinity of sodium hydroxide, 3-chloropropyltriethoxysilane replaces the intermediate and introduces the ethoxysilane structure at the ring-opening site.
[0015] Preferably, the thickener is sodium carboxymethylcellulose.
[0016] Preferably, the dispersant is a polyether dispersant.
[0017] Preferably, the defoaming agent is a polyether defoaming agent.
[0018] Preferably, the mildewcide is a water-based mildewcide.
[0019] A preparation method for an easily degradable corrugated paper additive comprises the following specific operations: premixing a modifying enhancer, a dispersant, a defoaming agent, a mildew preventer and half of the water, then adding oxidized starch to mix, heating to 65±2°C and stirring for 25-30 minutes, then premixing a thickener and the remaining water and adding and mixing to obtain the easily degradable corrugated paper additive.
[0020] Beneficial effects of the present invention:
[0021] The corrugated paper additive disclosed in the present invention is mainly used for gluing corrugated paper. It uses oxidized starch as a base material, has good biodegradability, and is more environmentally friendly than traditional synthetic resin sizing, paraffin sizing, etc.
[0022] The invention greatly improves the folding resistance and wet tensile strength of corrugated paper by adding a self-developed modifying and reinforcing agent to an oxidized starch sizing aid. The modifying and reinforcing agent uses a small molecular weight branched epoxy silicone oil as a raw material, and the active amino group of 2,2-difluoroethylamine and the epoxy silicone oil are open-ringed to introduce a fluorine structure into the silicone oil chain, and then 3-chloropropyltriethoxysilane and an intermediate are substituted to introduce an ethoxysilane structure at the open-ring site. During the sizing and curing process, the ethoxysilane of the side chain of the modifying and reinforcing agent molecule is coupled and condensed with the hydroxyl group of the paper fiber, and the main chain thereof is engaged in the macromolecular chain of the starch to generate a rivet effect, thereby increasing the bonding strength between the paper fibers and preventing the paper from cracking during the bending process. In addition, during the coupling and condensation process, a fluorine-containing organic silicon water-resistant layer is uniformly introduced into the surface of the paperboard substrate, thereby effectively improving the water resistance stability of the paperboard. DETAILED DESCRIPTION
[0023] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0024] Example 1: This example prepares a degradable corrugated paper additive, and the specific implementation process is as follows:
[0025] (1) Preparation of Modifying Enhancer
[0026] Step A1: Mix epoxy silicone oil, triethylamine and acetone, introduce nitrogen protection, heat to 55°C, stir at 180rpm, slowly add 2,2-difluoroethylamine, the addition time is 1h, continue to stir at constant temperature after complete addition, and control the total reaction time of 2,2-difluoroethylamine to be 2.5h. Among them, the epoxy silicone oil uses X-22-343 type small molecular weight branched epoxy silicone oil, and the room temperature viscosity is about 25mm 2 / s, the epoxy content of epoxy silicone oil, 2,2-difluoroethylamine, triethylamine and acetone are used in a ratio of 0.1 mol: 0.105 mol: 20 mL: 70 mL. After the reaction, acetone is removed by rotary evaporation, water is added to the rotary evaporation substrate for washing, the aqueous phase is removed and the product is dried in vacuo to obtain an intermediate.
[0027] Step A2: Take the intermediate, 3-chloropropyltriethoxysilane and anhydrous dioxane, mix them, pass dry nitrogen protection, then add sodium hydroxide and mix, heat to 100°C, stir at 120rpm, and react for 5h, wherein the amount ratio of the intermediate, 3-chloropropyltriethoxysilane, sodium hydroxide and anhydrous dioxane is 50g:0.08mol:8g:160mL. After the reaction is completed, filter to remove insoluble matter, and remove dioxane by rotary evaporation to obtain a modified enhancer.
[0028] (2) Preparation of biodegradable corrugated paper additives
[0029] Ingredients: The raw materials are measured by weight: 50 parts of oxidized starch, and the oxidized starch for sizing produced by Tai'an Jinshan Modified Starch Co., Ltd. is used in the implementation process; 6 parts of modified enhancer, which is homemade in this embodiment; 0.7 parts of thickener, and the FVH6-A type raw material produced by Weifang Lite Composite Materials Co., Ltd. is used in the implementation process; 0.15 parts of dispersant, and the polyether dispersant AEO-9 produced by Guangzhou Gongxin Chemical Co., Ltd. is used in the implementation process; 0.1 parts of defoamer, and the polyether defoamer CL-368 produced by Guangdong Nanhui New Materials Co., Ltd. is used in the implementation process; 0.02 parts of mildewcide, and the water-based mildewcide KEPUYIN-M002 produced by Guangdong Kepuyin Biotechnology Co., Ltd. is used in the implementation process; 90 parts of water.
[0030] Preparation of additives: premix the modified enhancer, dispersant, defoamer, mildew preventer and half of the water, then add oxidized starch and mix, heat to 65±2°C and stir for 25 minutes, then premix the thickener and the remaining water and add and mix to obtain a degradable corrugated paper additive.
[0031] Example 2: This example prepares a degradable corrugated paper additive, and the specific implementation process is as follows:
[0032] (1) Preparation of Modifying Enhancer
[0033] Step A1: Take epoxy silicone oil, triethylamine and acetone and mix them, introduce nitrogen protection, heat to 45°C, apply stirring at 120rpm, slowly add 2,2-difluoroethylamine, the addition time is 1.5h, continue to stir at constant temperature after complete addition, and control the total reaction time of 2,2-difluoroethylamine to be 3.5h. Among them, the epoxy silicone oil uses X-22-343 type small molecular weight branched epoxy silicone oil, and the room temperature viscosity is about 25mm 2 / s, the epoxy content of epoxy silicone oil, 2,2-difluoroethylamine, triethylamine and acetone are used in a ratio of 0.1 mol: 0.102 mol: 15 mL: 55 mL. After the reaction is completed, acetone is removed by rotary evaporation, water is added to the rotary evaporation substrate for washing, the aqueous phase is removed and the product is dried in vacuo to obtain an intermediate.
[0034] Step A2: Take the intermediate, 3-chloropropyltriethoxysilane and anhydrous dioxane, mix them, pass dry nitrogen protection, then add sodium hydroxide and mix, heat to 80°C, stir at 90rpm, and react for 7h, wherein the amount ratio of the intermediate, 3-chloropropyltriethoxysilane, sodium hydroxide and anhydrous dioxane is 50g:0.06mol:5g:120mL. After the reaction is completed, filter to remove insoluble matter, and remove dioxane by rotary evaporation to obtain a modified enhancer.
[0035] (2) Preparation of biodegradable corrugated paper additives
[0036] Ingredients: The raw materials are taken according to weight parts, 50 parts of oxidized starch, and the oxidized starch for sizing produced by Tai'an Jinshan Modified Starch Co., Ltd. is used in the implementation process; 8 parts of modified enhancer, which is self-made in this embodiment; 0.5 parts of thickener, and the FVH6-A type raw material of Weifang Lite Composite Materials Co., Ltd. is used in the implementation process; 0.2 parts of dispersant, and the polyether dispersant AEO-9 of Guangzhou Gongxin Chemical Co., Ltd. is used in the implementation process; 0.13 parts of defoamer, and the polyether defoamer CL-368 of Guangdong Nanhui New Materials Co., Ltd. is used in the implementation process; 0.03 parts of mildewcide, and the water-based mildewcide KEPUYIN-M002 of Guangdong Kepuyin Biotechnology Co., Ltd. is used in the implementation process; 100 parts of water.
[0037] Preparation of additives: premix the modified enhancer, dispersant, defoamer, mildew preventer and half of the water, then add oxidized starch and mix, heat to 65±2°C and stir for 30 minutes, then premix the thickener and the remaining water and add and mix to obtain a degradable corrugated paper additive.
[0038] Example 3: This example prepares an easily degradable corrugated paper additive, and the specific implementation process is as follows:
[0039] (1) Preparation of Modifying Enhancer
[0040] Step A1: Mix epoxy silicone oil, triethylamine and acetone, introduce nitrogen protection, heat to 50°C, stir at 120rpm, slowly add 2,2-difluoroethylamine, the addition time is 1.2h, continue to stir at constant temperature after complete addition, and control the total reaction time of 2,2-difluoroethylamine to be 3h. Among them, the epoxy silicone oil uses X-22-343 type small molecular weight branched epoxy silicone oil, and the room temperature viscosity is about 25mm 2 / s, the epoxy content of epoxy silicone oil, 2,2-difluoroethylamine, triethylamine and acetone are used in a ratio of 0.1 mol: 0.103 mol: 18 mL: 65 mL. After the reaction is completed, acetone is removed by rotary evaporation, water is added to the rotary evaporation substrate for washing, the aqueous phase is removed and the product is dried in vacuo to obtain an intermediate.
[0041] Step A2: Take the intermediate, 3-chloropropyltriethoxysilane and anhydrous dioxane and mix them, pass dry nitrogen protection, then add sodium hydroxide and mix, heat to 90°C, apply stirring at 120rpm, and react for 5.5h, wherein the amount ratio of the intermediate, 3-chloropropyltriethoxysilane, sodium hydroxide and anhydrous dioxane is 50g:0.07mol:7g:150mL. After the reaction is completed, filter to remove insoluble matter, and remove dioxane by rotary evaporation to obtain a modified enhancer.
[0042] (2) Preparation of biodegradable corrugated paper additives
[0043] Ingredients: The raw materials are taken according to weight parts, 50 parts of oxidized starch, and the oxidized starch for sizing produced by Tai'an Jinshan Modified Starch Co., Ltd. is used in the implementation process; 6.5 parts of modified enhancer, which is self-made in this embodiment; 0.6 parts of thickener, and the FVH6-A type raw material of Weifang Lite Composite Materials Co., Ltd. is used in the implementation process; 0.18 parts of dispersant, and the polyether dispersant AEO-9 of Guangzhou Gongxin Chemical Co., Ltd. is used in the implementation process; 0.12 parts of defoamer, and the polyether defoamer CL-368 of Guangdong Nanhui New Materials Co., Ltd. is used in the implementation process; 0.02 parts of mildewcide, and the water-based mildewcide KEPUYIN-M002 of Guangdong Kepuyin Biotechnology Co., Ltd. is used in the implementation process; 95 parts of water.
[0044] Preparation of additives: premix the modified enhancer, dispersant, defoamer, mildew preventer and half of the water, then add oxidized starch and mix, heat to 65±2°C and stir for 30 minutes, then premix the thickener and the remaining water and add and mix to obtain a degradable corrugated paper additive.
[0045] Example 4: This example prepares a degradable corrugated paper additive, and the specific implementation process is as follows:
[0046] (1) Preparation of Modifying Enhancer
[0047] Step A1: Mix epoxy silicone oil, triethylamine and acetone, introduce nitrogen protection, heat to 55°C, stir at 180rpm, slowly add 2,2-difluoroethylamine, the addition time is 1.2h, continue to stir at constant temperature after complete addition, and control the total reaction time of 2,2-difluoroethylamine to be 2.8h. Among them, the epoxy silicone oil uses X-22-343 type small molecular weight branched epoxy silicone oil, and the room temperature viscosity is about 25mm 2 / s, the epoxy content of epoxy silicone oil, 2,2-difluoroethylamine, triethylamine and acetone are used in a ratio of 0.1 mol: 0.103 mol: 20 mL: 65 mL. After the reaction, acetone is removed by rotary evaporation, water is added to the rotary evaporation substrate for washing, the aqueous phase is removed and the product is dried in vacuo to obtain an intermediate.
[0048] Step A2: Take the intermediate, 3-chloropropyltriethoxysilane and anhydrous dioxane and mix them evenly, pass dry nitrogen protection, then add sodium hydroxide and mix, heat to 85°C, apply stirring at 120rpm, and react for 6.5h, wherein the amount ratio of the intermediate, 3-chloropropyltriethoxysilane, sodium hydroxide and anhydrous dioxane is 50g:0.07mol:6g:140mL. After the reaction is completed, filter to remove insoluble matter, and remove dioxane by rotary evaporation to obtain a modified enhancer.
[0049] (2) Preparation of biodegradable corrugated paper additives
[0050] Ingredients: The raw materials are measured by weight: 50 parts of oxidized starch, and the oxidized starch for sizing produced by Tai'an Jinshan Modified Starch Co., Ltd. is used in the implementation process; 7.2 parts of modified enhancer, which is homemade in this embodiment; 0.55 parts of thickener, and the FVH6-A type raw material produced by Weifang Lite Composite Materials Co., Ltd. is used in the implementation process; 0.16 parts of dispersant, and the polyether dispersant AEO-9 produced by Guangzhou Gongxin Chemical Co., Ltd. is used in the implementation process; 0.12 parts of defoamer, and the polyether defoamer CL-368 produced by Guangdong Nanhui New Materials Co., Ltd. is used in the implementation process; 0.02 parts of mildewcide, and the water-based mildewcide KEPUYIN-M002 produced by Guangdong Kepuyin Biotechnology Co., Ltd. is used in the implementation process; 95 parts of water.
[0051] Preparation of additives: premix the modified enhancer, dispersant, defoamer, mildew preventer and half of the water, then add oxidized starch and mix, heat to 65±2°C and stir for 30 minutes, then premix the thickener and the remaining water and add and mix to obtain a degradable corrugated paper additive.
[0052] Comparative Example 1
[0053] This comparative example refers to Example 4, except that the modified reinforcing agent is replaced with the same weight portion of oxidized starch, and the rest of the implementation process is exactly the same.
[0054] Comparative Example 2
[0055] This comparative example refers to the prior art, and adopts a fluorine-containing silane coupling agent to prepare the auxiliary agent. The implementation process refers to Example 4. According to production experience, 2.2 parts of tridecafluorooctyltrimethoxysilane are used to replace the modified reinforcing agent, and the rest of the implementation process is exactly the same.
[0056] In order to test the strengthening effect of the additives prepared above on corrugated paper, the paperboard after papermaking and drying was taken as the substrate, and the additives were coated on the surface of the substrate, and the coating amount was controlled to be 3.5g / m 2 , and then placed in an oven and dried at 60°C for 2h to obtain a paper sheet;
[0057] Samples were taken from the paper sheets prepared as above, and the folding endurance test was performed according to GB / T457-2008 standard; the tensile strength test was performed according to GB / T12914-2018 standard, including dry / wet state test, the dry state was the direct sampling of the paper sheets, and the wet state was the sampling after the paper sheets were soaked in room temperature water for 10 minutes; the tear strength test was performed according to GB / T455-2002; the stiffness test was performed according to GB / T2679.3-1996 standard; the bursting resistance test was performed according to GB / T454-2020 standard; the specific test results are shown in the following table:
[0058]
[0059] It can be seen from the test results in the above table that the additives of the examples give the corrugated paper excellent comprehensive properties, especially significantly improve the folding resistance and wet tensile strength, which can effectively extend the service life of the corrugated paper and improve the packaging stability of the corrugated paper.
[0060] In the description of the specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.
[0061] The above contents are merely examples and explanations of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the invention or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.
Claims
1. A degradable corrugated paper additive, characterized in that: The composition comprises, by weight: 50 parts of oxidized starch, 6-8 parts of modified enhancer, 0.5-0.7 parts of thickener, 0.15-0.2 parts of dispersant, 0.1-0.13 parts of defoamer, 0.02-0.03 parts of mildewproofing agent and 90-100 parts of water; The modified reinforcing agent is prepared by the following method: Step A1: Mix epoxy silicone oil, triethylamine and acetone, introduce nitrogen protection, heat to 45-55°C, stir and slowly add 2,2-difluoroethylamine to react for 2.5-3.5h, and after the reaction is completed, rotary evaporate, wash with water, and vacuum dry to obtain an intermediate; Step A2: The intermediate, 3-chloropropyltriethoxysilane and anhydrous dioxane are mixed, dry nitrogen is introduced for protection, sodium hydroxide is added and mixed, the temperature is raised to 80-100° C., and the reaction is stirred for 5-7 hours. After the reaction is completed, the mixture is filtered and rotary evaporated to obtain a modified enhancer.
2. The easily degradable corrugated paper additive according to claim 1, characterized in that: The epoxy content of epoxy silicone oil, 2,2-difluoroethylamine, triethylamine and acetone are used in a ratio of 0.1 mol: 0.102-0.105 mol: 15-20 mL: 55-70 mL.
3. The easily degradable corrugated paper additive according to claim 2, characterized in that: Epoxy silicone oil is a branched epoxy silicone oil with a room temperature viscosity of no more than 30 mm 2 / s.
4. The easily degradable corrugated paper additive according to claim 3, characterized in that: The usage ratio of the intermediate, 3-chloropropyltriethoxysilane, sodium hydroxide and anhydrous dioxane is 50g: 0.06-0.08mol: 5-8g: 120-160mL.
5. The easily degradable corrugated paper additive according to claim 1, characterized in that: The thickener is sodium carboxymethyl cellulose.
6. The easily degradable corrugated paper additive according to claim 1, characterized in that: The dispersant is a polyether dispersant.
7. The easily degradable corrugated paper additive according to claim 1, characterized in that: The defoamer is a polyether defoamer.
8. The easily degradable corrugated paper additive according to claim 1, characterized in that: The mildew preventer is a water-based mildew preventer.
9. The method for preparing a degradable corrugated paper additive according to any one of claims 1 to 8, characterized in that: The specific operation is: premix the modified enhancer, dispersant, defoamer, mildew preventer and half of the water, then add oxidized starch and mix, heat to 65±2℃ and stir for 25-30min, then premix the thickener and the remaining water and add and mix to obtain the easily degradable corrugated paper additive.
Citation Information
Patent Citations
Glue for corrugated paper
CN108531111A
Moisture-proof corrugated paper and preparation method thereof
CN118461367A
GREASE AND MOISTURE RESISTANT CORRUGATED CARDBOARD
RU154469U1