Low-permeability high-temperature-resistant well cementation material as well as preparation method and application thereof
By using aluminate cement and auxiliary materials, the high-temperature resistance of cement stone is improved, the problems of strength decline and permeability increase of existing cementing materials at high temperatures are solved, and the stability and efficiency of heavy oil thermal recovery wells are achieved. promote.
Patent Information
- Application Number
- CN202410854212.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-27
- Publication Date
- 2024-10-29
AI Technical Summary
The strength of existing cementing materials declines and the permeability increases in high-temperature environments, causing the cement stone to crack and lose its sealing effect, making it difficult to meet the high-temperature stability requirements of heavy oil thermal recovery wells.
Aluminate cement is used as a high-temperature resistant material, combined with coal gangue, waste glass powder, silica sol and toughening materials. The compressive strength and permeability of the cement stone are improved through calcination and mixing processes, and water loss reducing agents and dispersants are used. Optimize the rheological properties of cement slurries.
It extends the production life of oil wells, improves the high temperature resistance of cement stone, reduces permeability and strength decline rate, and ensures the stability and efficiency of heavy oil thermal recovery wells.
Smart Images

Figure BDA0004917767240000141 
Figure BDA0004917767240000151 
Figure BDA0004917767240000152
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of heavy oil thermal recovery, and in particular to a low-permeability, high-temperature resistant cementing material and a preparation method and application thereof. Background Art
[0002] Heavy oil has high viscosity and density, and has great flow resistance in the formation, making it difficult to exploit. In order to improve the recovery rate of heavy oil, people have adopted a series of special methods, among which thermal exploitation such as steam stimulation, steam drive, burning oil layer, and hot water drive are the main ones. Burning oil layer is a thermal oil recovery method that has developed rapidly in recent years. It is one of the key methods to improve the recovery rate of heavy oil. It has the characteristics of high oil recovery efficiency, low production cost, and wide range of reservoir adaptability. It has obvious technical advantages and potential. However, in the combustion well, the heat generated by the flame combustion will greatly increase the temperature in the well, and the highest point can be above 500℃, so the cement stone is required to have the properties of low strength decay ability, no decrease in permeability, and no volume shrinkage under high temperature conditions greater than 500℃. Therefore, one of the key factors limiting the thermal recovery method of heavy oil in burning oil layer is high temperature resistant cementing material. However, the volume stability of commonly used silicate cement will seriously decrease when the ambient temperature exceeds 110°C, accompanied by a decrease in strength and an increase in permeability, which will eventually cause the cement stone to crack and completely lose the function of sealing the casing and dividing the oil layer. Even reducing the calcium / silicon ratio by adding sand cannot solve the above problems well. Summary of the invention
[0003] The purpose of the present invention is to provide a low permeability high temperature resistant cementing material and a preparation method and application thereof, so as to solve the problem that the existing cementing materials have strength reduction and permeability increase in a high temperature environment of ≥500°C.
[0004] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0005] The present invention provides a low-permeability and high-temperature resistant cementing material, which comprises the following raw materials in parts by weight: 100 parts of aluminate cement; 20 to 35 parts of coal gangue; 3 to 5 parts of waste glass powder; 4 to 8 parts of lime powder; 3 to 8 parts of silica sol; 0.1 to 0.8 parts of toughening material; 1 to 3 parts of fluid loss reducer; 0.2 to 1 part of retarder; 0.4 to 0.8 parts of dispersant; and 40 to 50 parts of water.
[0006] Preferably, in the low permeability and high temperature resistant cementing material, the content of Al2O3 in the aluminate cement is ω1 50≤ω1<60wt%; the specific surface area of the aluminate cement is 350-430m 2 / kg, particle size distribution is D 10 ≤2.0μm, D 50 ≤20μm, D 90 ≤65μm.
[0007] Preferably, in the low-permeability and high-temperature resistant cementing material, the content of Al2O3 in the coal gangue is 15-40wt%, and the content of SiO2 is 30-60wt%.
[0008] Preferably, in the low-permeability and high-temperature resistant cementing material, the content of SiO2 in the waste glass powder is ≥65wt%; and the content of CaO in the lime powder is ≥95wt%.
[0009] Preferably, in the low permeability and high temperature resistant cementing material, the content of SiO2 in the silica sol is 10-50wt%; the particle size of the SiO2 is 5-100nm, and the specific surface area is 50-400m 2 / g.
[0010] Preferably, in the low permeability and high temperature resistant cementing material, the toughening material is carbon fiber, polyester fiber or whisker; the average length of the toughening material is 0.01-80 μm, the tensile strength is ≥500 MPa, and the specific gravity is 1.3-2.8 g / cm 3 .
[0011] Preferably, in the low permeability and high temperature resistant cementing material, the fluid loss reducer comprises one or more of G301A, G302 and G33S; the retarder is a polymer retarder and / or a boric acid retarder; and the dispersant is a naphthalene-based dispersant and / or a lignin-based dispersant.
[0012] The present invention also provides a method for preparing the low-permeability and high-temperature resistant cementing material, comprising the following steps:
[0013] (1) mixing and grinding coal gangue, waste glass powder and lime powder to obtain a powder; calcining the powder to obtain an auxiliary cementitious material; mixing the auxiliary cementitious material with aluminate cement to obtain a cement-based material; mixing the cement-based material, a fluid loss reducer, a retarder and a dispersant to obtain a premixed dry mix;
[0014] mixing silica sol with water to obtain a mixed solution;
[0015] (2) Mixing the premixed dry mixture and toughening material described in step (1) with the mixed liquid described in step (1) to obtain a low-permeability and high-temperature resistant cementing material.
[0016] Preferably, in the method for preparing a low-permeability, high-temperature resistant cementing material, the specific surface area of the powder in step (1) is 300 to 350 m 2 / kg; the calcination temperature in step (1) is 700-800°C and the time is 2-3h; the mixing time of the auxiliary cementitious material and the aluminate cement in step (1) is 3-5min; the mixing time of the cement-based material, the fluid loss reducer, the retarder and the dispersant in step (1) is 5-8min; the mixing speed in step (2) is 4000-12000r / min and the time is 3-5min.
[0017] The present invention also provides an application of the low-permeability and high-temperature resistant cementing material or the low-permeability and high-temperature resistant cementing material prepared by the preparation method in thermal production of heavy oil.
[0018] It can be seen from the above technical solution that compared with the prior art, the present invention has the following beneficial effects:
[0019] (1) The present invention selects aluminate cement as high temperature resistant cement. Since aluminate cement has the characteristics of high temperature resistance and corrosion resistance, and has excellent mechanical properties, it helps to improve the cementing quality, thereby extending the production life of the oil well. Based on the above advantages of aluminate cement, it can solve the problem that the strength of existing quartz sand modified silicate cement in high temperature environment cannot meet the requirements of heavy oil thermal recovery cementing.
[0020] (2) The present invention introduces silica sol into cement paste, which can reduce the addition of free water, lower its water-to-solid ratio, and further reduce the shrinkage stress of cement paste; at the same time, because silica sol has high reactivity, it is easy to adsorb on the surface of Al2O3 particles during the reaction process to form a silica gel film, which penetrates and fills the pores of cement paste, thereby improving the anti-permeability of cement paste. After high-temperature curing at 700°C, the permeability of cement paste is less than 0.50mD.
[0021] (3) The toughening material (carbon fiber, polyester fiber or whisker) of the present invention can effectively improve the toughness of cement paste. Since the carbon fiber forms a fine rib structure with a supporting effect that is randomly scattered in the cement paste, it can reduce the number and size of cracks caused by stress, and mainly consumes the fracture energy in the form of "fiber pull-out", playing a toughening role; polyester fiber exhibits a "bridging effect" and "fiber pull-out" effect, but as a low-modulus soft fiber, it has little effect on improving the compressive strength of cement paste; calcium carbonate whiskers mainly play a role in strengthening and toughening cement paste at the micron scale, and have a bridging effect on microcracks, "fiber pull-out", crack deflection and other effects, so that the energy of cement destruction can be consumed. In summary, carbon fiber, polyester fiber or whisker can achieve high and low scale matching to enhance the mechanical properties of cement paste and improve the structure of cement paste. Therefore, the addition of toughening materials reduces the elastic modulus of cement stone by 3 to 5 GPa. Combined with the aforementioned characteristic of reduced permeability, it effectively prevents the oil, gas and water channeling problems caused by the substantial decline in cement sheath strength and interlayer isolation failure in the late stage of heavy oil thermal recovery wells. It has extremely important on-site guiding significance for improving the cementing quality of heavy oil thermal recovery wells, improving the exploitation of heavy oil resources, and extending the life of oil wells, and meets the needs of market development.
[0022] (4) The waste glass and coal gangue in the present invention are ground and calcined to increase their potential activity, and then lime powder is added to play the role of alkaline excitation active substances, so that the coal gangue and glass powder do not exist in the form of fillers, but participate in the volcanic ash reaction, effectively filling the capillaries in the cement stone and the tiny gaps between the particles, so that the formed cement stone structure becomes tighter, thereby improving the compressive strength of the cement stone; the early compressive strength of the cement stone at a low temperature of 50°C is high and long-term stable (24h ≥ 30MPa, 168h ≥ 35MPa), and it also has excellent high temperature resistance, especially after 700°C × 7d, the strength decay rate of the cement stone is ≤5%.
[0023] (5) The cement stone mineral solidified by using the low-permeability and high-temperature resistant cementing material of the present invention has no Ca(OH)2 generated in its components, and does not have structural defects caused by crystal transformation due to the volume expansion decomposition destructive effect, and can maintain the integrity of the cement stone under low and high temperature environmental conditions.
[0024] (6) The use of a retarder in the present invention can significantly prolong the thickening time of the modified aluminate cement slurry, and make the modified aluminate cement slurry free of flash setting and "core wrapping" phenomena during the thickening process, with a short transition time, an adjustable thickening time, and little effect on the compressive strength of mudstone.
[0025] (7) The fluid loss reducer of the present invention can effectively reduce the water loss of aluminate cement slurry and meet the requirements of engineering applications. The fluid loss reducer of the present invention mainly controls the water loss of cement slurry through adsorption and aggregation, so that polymer molecules are adsorbed on the surface of cement particles, and the network structure formed between polymers forms a close connection between cement particles through cross-linking and bridging, so that the cement filter cake has good density and small porosity.
[0026] (8) The dispersant used in the present invention is multi-molecule adsorbed on the surface of cement particles. The inner layer is chemically adsorbed through anionic groups, hydrogen bonds or complexes, and the outer layer is mostly physically adsorbed. The adsorption of the dispersant reduces the solid-liquid free energy between cement and water, thereby improving the rheological properties of the cement slurry. It can also improve the microstructure of the cement paste, reduce large pores, generate more micropores, and improve the density of the cement paste.
[0027] (9) The preparation method of the present invention has reliable principle, simple operation and low production cost. DETAILED DESCRIPTION
[0028] The present invention provides a low-permeability and high-temperature resistant cementing material, which comprises the following raw materials in parts by weight: 100 parts of aluminate cement; 20 to 35 parts of coal gangue; 3 to 5 parts of waste glass powder; 4 to 8 parts of lime powder; 3 to 8 parts of silica sol; 0.1 to 0.8 parts of toughening material; 1 to 3 parts of fluid loss reducer; 0.2 to 1 part of retarder; 0.4 to 0.8 parts of dispersant; and 40 to 50 parts of water.
[0029] In the present invention, the content ω1 of Al2O3 in the aluminate cement is preferably 50≤ω1<60wt%, more preferably 50≤ω1<55wt%, and more preferably 50≤ω1<52wt%; the specific surface area of the aluminate cement is preferably 350-430m 2 / kg, more preferably 380 to 420 m 2 / kg, more preferably 400 to 420 m 2 / kg; the particle size distribution of the aluminate cement is preferably: D 10 ≤2.0μm, D 50 ≤20μm, D 90 ≤65μm, more preferably D 10 ≤1.8μm, D 50 ≤19.5μm, D 90 ≤60μm, preferably D 10 ≤1.7μm, D 50 ≤18.5μm, D 90 ≤55μm.
[0030] In the present invention, the aluminate cement is preferably aluminate cement CA50. Specifically in the embodiments of the present invention, the model of the aluminate cement CA50 is preferably A600, A700 or A900.
[0031] In the present invention, the Al2O3 content in the coal gangue is preferably 15-40wt%, more preferably 15-25wt%, and more preferably 15-20wt%; the SiO2 content is preferably 30-60wt%, more preferably 45-60wt%, and more preferably 55-60wt%.
[0032] In the present invention, the mass fraction of the coal gangue is 20 to 35 parts, preferably 25 to 35 parts, and more preferably 30 to 35 parts.
[0033] In the present invention, the waste glass powder is preferably obtained by grinding waste flat glass.
[0034] In the present invention, the content of SiO2 in the waste glass powder is preferably ≥65wt%, further preferably ≥70wt%, and more preferably ≥75wt%.
[0035] In the present invention, the mass fraction of the waste glass powder is 3 to 5 parts, preferably 4 to 5 parts, and more preferably 4 to 4.5 parts.
[0036] In the present invention, the content of CaO in the lime powder is preferably ≥95wt%, more preferably ≥96.5wt%, and even more preferably ≥97wt%.
[0037] In the present invention, the mass fraction of the lime powder is 4 to 8 parts, preferably 4 to 6 parts, and more preferably 5 to 6 parts.
[0038] In the present invention, the content of SiO2 in the silica sol is preferably 10 to 50 wt%, more preferably 15 to 45 wt%, and even more preferably 25 to 35 wt%.
[0039] In the present invention, the particle size of SiO2 is preferably 5 to 100 nm, more preferably 5 to 20 nm, and more preferably 8 to 15 nm; the specific surface area is preferably 50 to 400 m 2 / g, more preferably 100 to 300 m 2 / g, more preferably 250 to 300 m 2 / g.
[0040] In the present invention, specifically in the embodiments, the silica sol is preferably alkaline silica sol.
[0041] In the present invention, the mass fraction of the silica sol is 3 to 8 parts, preferably 4 to 8 parts, and more preferably 5 to 8 parts.
[0042] In the present invention, the toughening material is preferably carbon fiber, polyester fiber or whisker.
[0043] In the present invention, the type of the whisker is preferably magnesium oxide whisker, calcium carbonate whisker or silicon carbide whisker, more preferably magnesium oxide whisker or calcium carbonate whisker, and more preferably calcium carbonate whisker.
[0044] In the present invention, specifically in the embodiments, the type of the carbon fiber is preferably PAN-based short carbon fiber.
[0045] In the present invention, specifically in the embodiment, the type of the polyester fiber is preferably polyethylene terephthalate fiber (PET).
[0046] In the present invention, specifically in the embodiments, the model of the calcium carbonate whisker is preferably NP-CW2.
[0047] In the present invention, the average length of the toughening material is preferably 0.01 to 80 μm, more preferably 0.01 to 30 μm, and more preferably 25 to 40 μm; the tensile strength is preferably ≥500 MPa, more preferably ≥550 MPa, and more preferably ≥600 MPa; the specific gravity is preferably 1.3 to 2.8 g / cm 3 , more preferably 1.5 to 2.5 g / cm 3 , more preferably 1.7 to 2.0 g / cm 3 .
[0048] In the present invention, the mass fraction of the toughening material is 0.1 to 0.8 parts, preferably 0.3 to 0.6 parts, and more preferably 0.4 to 0.6 parts.
[0049] In the present invention, the fluid loss additive preferably comprises one or more of G301A, G302 and G33S, further preferably comprises one or both of G302 and G33S, and more preferably comprises G302 or G33S.
[0050] In the present invention, the mass fraction of the fluid loss agent is 1 to 3 parts, preferably 1 to 2 parts, and more preferably 1.2 to 2 parts.
[0051] In the present invention, the retarder is preferably a polymer retarder and / or a boric acid retarder, and more preferably a polymer retarder or a boric acid retarder.
[0052] In the present invention, the type of the polymer retarder is preferably AMPS copolymer. Specifically in the embodiment of the present invention, the model of the polymer retarder is preferably GH-9.
[0053] In the present invention, when the number of the retarders is preferably two, the ratio between the two retarders is not limited and can be adjusted as required.
[0054] In the present invention, the mass fraction of the retarder is preferably 0.2 to 1 part, more preferably 0.25 to 0.5 part, and even more preferably 0.25 to 0.4 part.
[0055] In the present invention, the dispersant is preferably a nylon-based dispersant and / or a lignin-based dispersant, and more preferably a nylon-based dispersant or a lignin-based dispersant.
[0056] In the present invention, the type of the naphthalene-based dispersant is preferably a high-efficiency naphthalene-based dispersant.
[0057] In the present invention, specifically in the embodiments, the model of the naphthalene series dispersant is preferably FDN.
[0058] In the present invention, the type of the lignin-based dispersant is preferably lignin sulfonate.
[0059] In the present invention, specifically in the embodiments, the model of the lignin-based dispersant is preferably HD1.
[0060] In the present invention, when the dispersants are preferably two, the ratio between the two dispersants is not limited and can be adjusted as needed.
[0061] In the present invention, the mass fraction of the dispersant is 0.4 to 0.8 parts, preferably 0.5 to 0.8 parts, and more preferably 0.6 to 0.8 parts.
[0062] In the present invention, the mass fraction of water is 40 to 50 parts, preferably 42 to 48 parts, and more preferably 44 to 46 parts.
[0063] The present invention also provides a method for preparing the low-permeability and high-temperature resistant cementing material, comprising the following steps:
[0064] (1) mixing and grinding coal gangue, waste glass powder and lime powder to obtain a powder; calcining the powder to obtain an auxiliary cementitious material; mixing the auxiliary cementitious material with aluminate cement to obtain a cement-based material; mixing the cement-based material, a fluid loss reducer, a retarder and a dispersant to obtain a premixed dry mix;
[0065] mixing silica sol with water to obtain a mixed solution;
[0066] (2) Mixing the premixed dry mixture and toughening material described in step (1) with the mixed liquid described in step (1) to obtain a low-permeability and high-temperature resistant cementing material.
[0067] In the present invention, the equipment for mixed grinding in step (1) is preferably a ball mill.
[0068] In the present invention, the specific surface area of the powder in step (1) is preferably 300 to 350 m 2 / kg, more preferably 320 to 350m 2 / kg, more preferably 340 to 350m 2 / kg.
[0069] In the present invention, the calcination equipment in step (1) is preferably a high temperature furnace.
[0070] In the present invention, the calcination temperature in step (1) is preferably 700-800°C, more preferably 750-800°C, and more preferably 750-780°C; the calcination time is preferably 2-3h, more preferably 2.5-3h, and more preferably 3h.
[0071] In the present invention, the time for mixing the auxiliary cementitious material and the aluminate cement in step (1) is preferably 3 to 5 minutes, more preferably 3.5 to 5 minutes, and more preferably 4.5 minutes.
[0072] In the present invention, the time for mixing the cement-based material, fluid loss reducer, retarder and dispersant in step (1) is preferably 5 to 8 minutes, more preferably 6 to 7 minutes, and more preferably 6.5 minutes.
[0073] In the present invention, the mixing speed in step (2) is preferably 4000-12000 r / min, more preferably 4500-10000 r / min, more preferably 6000-8000 r / min; the mixing time is preferably 3-5 min, more preferably 3.5-4.8 min, more preferably 4.5 min.
[0074] In the present invention, for other parameters in the above preparation method, schemes well known to those skilled in the art can be adopted.
[0075] The present invention also provides an application of the low-permeability and high-temperature resistant cementing material or the low-permeability and high-temperature resistant cementing material prepared by the preparation method in thermal production of heavy oil.
[0076] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0077] Example 1
[0078] The present embodiment provides a low permeability and high temperature resistant cementing material, comprising the following raw materials in parts by weight: 100 parts of aluminate cement CA50-A900, 35 parts of coal gangue, 4 parts of waste glass powder, 5 parts of lime powder, 4 parts of silica sol, 0.3 parts of carbon fiber, 1 part of fluid loss reducer G33S, 0.4 parts of polymer retarder, 0.6 parts of naphthalene dispersant, and 44 parts of water;
[0079] The Al2O3 content of aluminate cement is 53.84% and the specific surface area is 430m 2 / kg, particle size distribution: D 10 =1.5μm, D 50 =12.5μm, D 90 =47.6μm;
[0080] The Al2O3 content in coal gangue is 16.31wt%, and the SiO2 content is 56.18wt%;
[0081] The SiO2 content in waste glass powder is 70.42wt%;
[0082] The CaO content in lime powder is 95.01wt%;
[0083] The silica sol model is alkaline silica sol, the SiO2 content in the silica sol is 30wt%, the SiO2 particle size is 8nm, and the SiO2 specific surface area is 280m 2 / g;
[0084] The carbon fiber model is PAN-based short carbon fiber with an average length of 0.05μm, a tensile strength of 550MPa, and a specific gravity of 1.7g / cm 3 ;
[0085] The type of polymer retarder is AMPS copolymer, model GH-9;
[0086] The type of nylon series dispersant is high-efficiency nylon series dispersant, model FDN.
[0087] This embodiment also provides a method for preparing a low-permeability, high-temperature resistant cementing material, comprising the following steps:
[0088] (1) Mix coal gangue, waste glass powder and lime powder and grind them in a ball mill to obtain a Blaine surface area of 350m 2 / kg of powder; fully calcining the powder in a high-temperature furnace at 700°C for 3h to obtain an auxiliary cementitious material; manually mixing and stirring the auxiliary cementitious material with aluminate cement for 3.5min to obtain a cement-based material; manually mixing and premixing the cement-based material, a fluid loss reducer, a retarder and a dispersant for 6min, mixing them evenly to obtain a premixed dry mix;
[0089] Adding silica sol into pure water and mixing evenly to obtain a mixed solution;
[0090] (2) The premixed dry mixture and carbon fiber of step (1) are slowly and evenly added to the mixed solution of step (1), and the mixture is fully mixed at a speed of 4000 r / min for 5 minutes to uniformly disperse the carbon fiber in the slurry, thereby obtaining a low-permeability and high-temperature resistant cementing material.
[0091] Example 2
[0092] The present embodiment provides a low permeability and high temperature resistant cementing material, comprising the following raw materials in parts by weight: 100 parts of aluminate cement CA50-A900, 30 parts of coal gangue, 5 parts of waste glass powder, 5 parts of lime powder, 5 parts of silica sol, 0.6 parts of magnesium oxide whisker, 1.2 parts of fluid loss reducer G302, 0.25 parts of boric acid retarder, 0.8 parts of lignin dispersant, and 48 parts of water;
[0093] The Al2O3 content of aluminate cement is 54.29wt% and the specific surface area is 420m 2 / kg, particle size distribution: D 10 =1.4μm, D 50 =11.8μm, D 90 =45.2μm;
[0094] The Al2O3 content in coal gangue is 16.31wt%, and the SiO2 content is 56.18wt%;
[0095] The SiO2 content in waste glass powder is 70.42wt%;
[0096] The CaO content in lime powder is 95.01wt%;
[0097] The silica sol model is alkaline silica sol, the SiO2 content in the silica sol is 30wt%, the SiO2 particle size is 8nm, and the SiO2 specific surface area is 280m 2 / g;
[0098] The model of calcium carbonate whisker is NP-CW2, with an average length of 30μm, a tensile strength of 800MPa, and a specific gravity of 2.8g / cm 3 ;
[0099] The type of lignin-based dispersant is lignin sulfonate, model HD1.
[0100] This embodiment also provides a method for preparing a low-permeability, high-temperature resistant cementing material, comprising the following steps:
[0101] (1) Mix coal gangue, waste glass powder and lime powder and grind them in a ball mill to obtain a Blaine surface area of 350m 2 / kg of powder; fully calcining the powder in a high-temperature furnace at 750°C for 3h to obtain an auxiliary cementitious material; fully mixing the auxiliary cementitious material with aluminate cement by manual stirring for 4.5min to obtain a cement-based material; manually premixing the cement-based material, fluid loss reducer, retarder and dispersant for 7min, mixing them uniformly to obtain a premixed dry mix;
[0102] Adding silica sol into pure water and mixing evenly to obtain a mixed solution;
[0103] (2) slowly and evenly adding the premixed dry mixture and magnesium oxide whiskers described in step (1) into the mixed solution described in step (1), and mixing them thoroughly at a speed of 8000 r / min for 3.5 min to uniformly disperse the calcium carbonate whiskers in the slurry, thereby obtaining a low-permeability and high-temperature resistant cementing material.
[0104] Example 3
[0105] The present embodiment provides a low permeability and high temperature resistant cementing material, comprising the following raw materials in parts by weight: 100 parts of aluminate cement CA50-A700, 25 parts of coal gangue, 4 parts of waste glass powder, 6 parts of lime powder, 8 parts of silica sol, 0.4 parts of polyester fiber, 2 parts of fluid loss reducer G33S, 0.5 parts of polymer retarder, 0.6 parts of naphthalene dispersant, and 48 parts of water;
[0106] The Al2O3 content of aluminate cement is 51.58wt% and the specific surface area is 380m 2 / kg, particle size distribution: D 10 =1.88μm, D 50 =17.4μm, D 90 =59.0μm;
[0107] The Al2O3 content in coal gangue is 16.31wt% and the SiO2 content is 56.18wt%
[0108] The SiO2 content in waste glass powder is 70.42wt%;
[0109] The CaO content in lime powder is 95.01wt%;
[0110] The silica sol model is alkaline silica sol, the SiO2 content in the silica sol is 30wt%, the SiO2 particle size is 8nm, and the SiO2 specific surface area is 280m 2 / g;
[0111] The type of polyester fiber is polyethylene terephthalate fiber (PET), with an average length of 25 μm, a tensile strength of 500 MPa, and a specific gravity of 1.36 g / cm 3 ;
[0112] The type of polymer retarder is AMPS copolymer, model GH-9;
[0113] The type of nylon series dispersant is high-efficiency nylon series dispersant, model FDN.
[0114] This embodiment also provides a method for preparing a low-permeability, high-temperature resistant cementing material, comprising the following steps:
[0115] (1) Mix coal gangue, waste glass powder and lime powder and grind them in a ball mill to obtain a Blaine surface area of 300m 2 / kg of powder; fully calcining the powder in a high-temperature furnace at 780°C for 3h to obtain an auxiliary cementitious material; manually stirring and fully mixing the auxiliary cementitious material with aluminate cement for 5min to obtain a cement-based material; manually stirring and premixing the cement-based material, a fluid loss reducer, a retarder and a dispersant for 6min to obtain a premixed dry mix;
[0116] Adding silica sol into pure water and mixing evenly to obtain a mixed solution;
[0117] (2) The premixed dry blend and polyester fiber of step (1) are slowly and evenly added to the mixed solution of step (1), and the mixture is fully mixed at a speed of 12000 r / min for 3 min to uniformly disperse the polyester fiber in the slurry, thereby obtaining a low-permeability and high-temperature resistant cementing material.
[0118] Example 4
[0119] The present embodiment provides a low permeability and high temperature resistant cementing material, comprising the following raw materials in parts by weight: 100 parts of aluminate cement CA50-A600, 30 parts of coal gangue, 3 parts of waste glass powder, 5 parts of lime powder, 5 parts of silica sol, 0.6 parts of calcium carbonate whiskers, 1.5 parts of fluid loss reducer G33S, 0.25 parts of boric acid retarder, 0.5 parts of lignin dispersant, and 50 parts of water;
[0120] The Al2O3 content of aluminate cement is 50.89wt% and the specific surface area is 360m 2 / kg, particle size distribution: D 10 =1.88μm, D 50 =17.1μm, D 90 =57.6μm;
[0121] The Al2O3 content in coal gangue is 16.31wt% and the SiO2 content is 56.18wt%
[0122] The SiO2 content in waste glass powder is 70.42wt%;
[0123] The CaO content in lime powder is 95.01wt%;
[0124] The silica sol model is alkaline silica sol, the SiO2 content in the silica sol is 30wt%, the SiO2 particle size is 8nm, and the SiO2 specific surface area is 280m 2 / g;
[0125] The model of calcium carbonate whisker is NP-CW2, with an average length of 30μm, a tensile strength of 800MPa, and a specific gravity of 2.8g / cm 3 ;
[0126] The type of lignin-based dispersant is lignin sulfonate, model HD1.
[0127] This embodiment also provides a method for preparing a low-permeability, high-temperature resistant cementing material, comprising the following steps:
[0128] (1) Mix coal gangue, waste glass powder and lime powder and grind them in a ball mill to obtain a Blaine surface area of 300m 2 / kg of powder; fully calcining the powder in a high-temperature furnace at 780°C for 3h to obtain an auxiliary cementitious material; manually mixing and stirring the auxiliary cementitious material with aluminate cement for 5min to obtain a cement-based material; manually mixing and premixing the cement-based material, a fluid loss reducer, a retarder and a dispersant for 8min, mixing them uniformly to obtain a premixed dry mix;
[0129] Adding silica sol into pure water and mixing evenly to obtain a mixed solution;
[0130] (2) slowly and evenly adding the premixed dry mix and calcium carbonate whiskers described in step (1) into the mixed solution described in step (1), and mixing them thoroughly at a speed of 8000 r / min for 4.5 min to uniformly disperse the calcium carbonate whiskers in the slurry, thereby obtaining a low-permeability and high-temperature resistant cementing material.
[0131] Comparative Example 1
[0132] This comparative example provides a thermal well cementing material, comprising the following raw materials in parts by weight: 100 parts of aluminate cement CA50-A900, 0.3 parts of carbon fiber, 1 part of fluid loss reducer G33S, 0.6 parts of polymer retarder, 0.5 parts of lignin-based dispersant, and 50 parts of water;
[0133] The Al2O3 content of aluminate cement is 54.29wt% and the specific surface area is 420m 2 / kg, particle size distribution: D 10 =1.4μm, D 50 =11.8μm, D 90 =45.2μm;
[0134] The carbon fiber model is PAN-based short carbon fiber with an average length of 0.05μm, a tensile strength of 550MPa, and a specific gravity of 1.7g / cm 3 ;
[0135] The type of polymer retarder is AMPS copolymer, model GH-9;
[0136] The type of lignin-based dispersant is lignin sulfonate, model HD1.
[0137] This comparative example also provides a method for preparing a thermal recovery well cementing material, comprising the following steps:
[0138] (1) manually mixing aluminate cement, fluid loss additive, retarder and dispersant for 8 minutes, mixing them evenly to obtain a premixed dry mix;
[0139] (2) The premixed dry mixture and carbon fiber of step (1) are slowly and evenly added into water, and fully mixed at a speed of 12000 r / min for 3 min to make the carbon fiber evenly dispersed in the slurry, thereby obtaining a thermal well cementing material.
[0140] Comparative Example 2
[0141] This comparative example provides a thermal well cementing material, comprising the following raw materials in parts by weight: 100 parts of aluminate cement CA50-A900, 5 parts of silica sol, 0.3 parts of carbon fiber, 1 part of fluid loss reducer G33S, 0.6 parts of polymer retarder, 0.5 parts of lignin-based dispersant, and 50 parts of water;
[0142] The Al2O3 content of aluminate cement is 54.29wt% and the specific surface area is 420m 2 / kg, particle size distribution: D 10 =1.4μm, D 50 =11.8μm, D 90 =45.2μm;
[0143] The silica sol model is alkaline silica sol, the SiO2 content in the silica sol is 30wt%, the SiO2 particle size is 8nm, and the SiO2 specific surface area is 280m 2 / g;
[0144] The carbon fiber model is PAN-based short carbon fiber with an average length of 0.05μm, a tensile strength of 550MPa, and a specific gravity of 1.7g / cm 3 ;
[0145] The type of polymer retarder is AMPS copolymer, model GH-9;
[0146] The type of lignin-based dispersant is lignin sulfonate, model HD1.
[0147] This comparative example also provides a method for preparing a thermal recovery well cementing material, comprising the following steps:
[0148] (1) manually mixing aluminate cement, fluid loss additive, retarder and dispersant for 8 minutes, mixing them evenly to obtain a premixed dry mix;
[0149] Adding silica sol into pure water and mixing evenly to obtain a mixed solution;
[0150] (2) Slowly and evenly adding the premixed dry blend and carbon fiber described in step (1) into the mixed solution described in step (1), and mixing them thoroughly for 3 minutes at a rotation speed of 12000 r / min to uniformly disperse the carbon fiber in the slurry, thereby obtaining a thermal well cementing material.
[0151] Comparative Example 3
[0152] This comparative example provides a thermal well cementing material, comprising the following raw materials in parts by weight: 100 parts of aluminate cement CA50-A900, 35 parts of coal gangue, 0.3 parts of carbon fiber, 1 part of fluid loss reducer G33S, 0.6 parts of polymer retarder, 0.5 parts of lignin-based dispersant, and 49 parts of water;
[0153] The Al2O3 content of aluminate cement is 54.29wt% and the specific surface area is 420m 2 / kg, particle size distribution: D 10 =1.4μm, D 50 =11.8μm, D 90 =45.2μm;
[0154] The Al2O3 content in coal gangue is 16.31wt% and the SiO2 content is 56.18wt%
[0155] The carbon fiber model is PAN-based short carbon fiber with an average length of 0.05μm, a tensile strength of 550MPa, and a specific gravity of 1.7g / cm 3 ;
[0156] The type of polymer retarder is AMPS copolymer, model GH-9;
[0157] The type of lignin-based dispersant is lignin sulfonate, model HD1.
[0158] This comparative example also provides a method for preparing a thermal recovery well cementing material, comprising the following steps:
[0159] (1) Grind the coal gangue in a ball mill to obtain a Brinell surface area of 300 m 2 / kg of powder; fully calcining the powder in a high-temperature furnace at 780°C for 3h to obtain an auxiliary cementitious material; manually stirring and fully mixing the auxiliary cementitious material with aluminate cement for 5min to obtain a cement-based material; manually premixing the cement-based material, a fluid loss reducer, a retarder and a dispersant for 8min, mixing them uniformly to obtain a premixed dry mix;
[0160] (2) The premixed dry mixture and carbon fiber of step (1) are slowly and evenly added into water, and fully mixed at a speed of 8000 r / min for 4.5 min to make the carbon fiber evenly dispersed in the slurry, thereby obtaining a thermal well cementing material.
[0161] The engineering performance tests were conducted on the cementing materials prepared in Examples 1 to 4 and Comparative Examples 1 to 3, and the results are shown in Tables 1 to 4.
[0162] Table 1. Test results of conventional properties of cementing materials
[0163]
[0164] Note: In Table 1, cement slurry density, fluidity, sedimentation stability, filtration loss, thickening time and compressive strength tests were carried out according to the operating methods and steps in GB / T 19139-2012 "Test methods for oil well cement".
[0165] The elastic modulus is determined by using a triaxial rock mechanics test system in accordance with GB / T 50266-2013 “Standard for Engineering Rock Test Methods” to measure the stress and strain of cement paste, thereby obtaining its elastic modulus.
[0166] As can be seen from Table 1, Examples 1 to 4 are low permeability and high temperature resistant cementing materials prepared by the present invention, and the cement slurry density is 1.86 to 1.88 g / cm 3 When the slurry is slurried, it has good slurry stability and thickening time adjustability, and the filtration loss is <50mL, which is beneficial to the cementing site construction of heavy oil thermal recovery wells; at the same time, the early compressive strength of cement paste (50℃ / 24h) is ≥30MPa, which can meet the strength requirements of on-site cementing, and the elastic modulus is <5.0GPa, showing that the cement paste has the characteristics of low toughness. Comparative Examples 1 to 3 respectively show the characteristics of low early strength of cement paste, high elastic modulus, poor settlement stability, and poor flow performance.
[0167] Table 2. Test results of low temperature early strength performance of cementing materials
[0168]
[0169] Note: The compressive strength in Table 2 is tested according to GB / T 19139-2012 “Test methods for oil well cement”.
[0170] It can be seen from Table 2 that, compared with comparative examples 1 to 3, the early strength of the cement paste of embodiments 1 to 4 of the present invention after curing at 50° C. for different ages is stable and is about 5 to 10 MPa higher than that of the comparative examples.
[0171] Table 3. High temperature performance test results of cementing materials
[0172]
[0173] Note: The compressive strength in Table 3 was evaluated and tested with reference to SY / T 6466-2016 “Evaluation Method for High Temperature Resistance of Oil Well Cement Stone”.
[0174] As can be seen from Table 3, the cement paste formed by the cementing material prepared by the present invention can maintain a compressive strength of more than 35MPa after being cured at high temperatures of 300°C, 500°C, and 700°C for 7 days, respectively, and has excellent high temperature resistance, with a high temperature strength decay rate of ≤5%. However, after high temperature curing, the compressive strength of the cement paste of Comparative Examples 1 to 3 shrinks to varying degrees, especially in Comparative Examples 1 and 2, where no admixture is added, and the mechanical properties of the cement paste decrease significantly.
[0175] Table 4. Permeability performance test results of cementing materials under low and high temperature environmental conditions
[0176]
[0177] Note: In Table 4, the cement paste permeability and porosity are tested using the DKS-Ⅲ core-pore permeability tester. Before the test, the samples cured to the specified age need to be dried in an oven at a constant temperature, with nitrogen as the medium, at a displacement pressure of 7.0 MPa and a confining pressure of 10 MPa.
[0178] As can be seen from Table 4, when the temperature of the cementing material obtained by the present invention is continuously raised to 700°C, most of the hydration products of the cement stone are dehydrated and decomposed, and the remaining phase is relatively stable. At this time, the permeability and porosity are basically stable, meeting the requirements of heavy oil production. The cement stone of Comparative Examples 1 to 3 has a larger permeability under low and high temperature conditions.
[0179] In summary, the present invention uses aluminate cement as a high temperature resistant cementing material, uses volcanic ash active substances (lime powder, coal gangue and glass powder) as auxiliary cementing materials, and uses the coagulation effect of silica sol and the filling and sintering effect of SiO2 nanoparticles to prepare a low permeability high temperature resistant cementing material. The low permeability high temperature resistant cementing material system obtained by the present invention has good engineering performance and can meet the requirements of cementing field operations of heavy oil thermal recovery wells; at the same time, because industrial active waste slag, waste glass powder, silica sol and toughening materials are added to the system to act on aluminate cement, the permeability resistance of cement stone is improved, and the compressive strength decay rate of cement stone at high temperature is ≤5%, thus showing excellent mechanical properties and low permeability, which can meet the performance requirements of thermal recovery well conditions for high temperature long-term stability of cement stone.
[0180] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A low permeability and high temperature resistant cementing material, characterized in that: The preparation material comprises the following raw materials in parts by weight: 100 parts of aluminate cement; 20-35 parts of coal gangue; 3-5 parts of waste glass powder; 4-8 parts of lime powder; 3-8 parts of silica sol; 0.1-0.8 parts of toughening material; 1-3 parts of fluid loss reducer; 0.2-1 parts of retarder; 0.4-0.8 parts of dispersant; and 40-50 parts of water.
2. A low permeability and high temperature resistant cementing material as claimed in claim 1, characterized in that: The content of Al2O3 in the aluminate cement is ω1 50≤ω1<60wt%; the specific surface area of the aluminate cement is 350-430m 2 / kg, particle size distribution is D 10 ≤2.0μm, D 50 ≤20μm, D 90 ≤65μm.
3. The low permeability and high temperature resistant cementing material according to claim 1, characterized in that: In the coal gangue, the content of Al2O3 is 15-40wt%, and the content of SiO2 is 30-60wt%.
4. A low permeability and high temperature resistant cementing material as claimed in claim 1 or 3, characterized in that: The content of SiO2 in the waste glass powder is ≥65wt%; the content of CaO in the lime powder is ≥95wt%.
5. The low permeability and high temperature resistant cementing material according to claim 1, characterized in that: The content of SiO2 in the silica sol is 10-50wt%; the particle size of the SiO2 is 5-100nm, and the specific surface area is 50-400m 2 / g.
6. A low permeability and high temperature resistant cementing material according to any one of claims 1 to 3 or 5, characterized in that: The toughening material is carbon fiber, polyester fiber or whisker; the average length of the toughening material is 0.01-80 μm, the tensile strength is ≥500 MPa, and the specific gravity is 1.3-2.8 g / cm 3 .
7. The low permeability and high temperature resistant cementing material according to claim 1, characterized in that: The fluid loss additive comprises one or more of G301A, G302 and G33S; the retarder is a polymer retarder and / or a boric acid retarder; and the dispersant is a naphthalene-based dispersant and / or a lignin-based dispersant.
8. The method for preparing a low permeability and high temperature resistant cementing material according to any one of claims 1 to 7, characterized in that: The following steps are involved: (1) mixing and grinding coal gangue, waste glass powder and lime powder to obtain a powder; The powder is calcined to obtain an auxiliary cementitious material; the auxiliary cementitious material is mixed with aluminate cement to obtain a cement-based material; the cement-based material, a fluid loss reducer, a retarder and a dispersant are mixed to obtain a premixed dry mix; mixing silica sol with water to obtain a mixed solution; (2) Mixing the premixed dry mixture and toughening material described in step (1) with the mixed liquid described in step (1) to obtain a low-permeability and high-temperature resistant cementing material.
9. The method for preparing a low-permeability, high-temperature resistant cementing material according to claim 8, characterized in that: The specific surface area of the powder in step (1) is 300 to 350 m 2 / kg; the calcination temperature in step (1) is 700-800°C and the time is 2-3h; the mixing time of the auxiliary cementitious material and the aluminate cement in step (1) is 3-5min; the mixing time of the cement-based material, the fluid loss reducer, the retarder and the dispersant in step (1) is 5-8min; the mixing speed in step (2) is 4000-12000r / min and the time is 3-5min.
10. Use of the low permeability and high temperature resistant cementing material according to any one of claims 1 to 7 or the low permeability and high temperature resistant cementing material prepared by the preparation method according to claim 8 or 9 in heavy oil thermal recovery.
Citation Information
Cited By
Slope ecological restoration base material based on multistage synergistic solidification and layered spray-seeding method
CN120240275A
Slope ecological restoration substrate based on multi-stage collaborative curing and layered spray seeding method
CN120240275B