Electrolyte and lithium metal battery
By using an electrolyte containing a nitroxyl radical catalyst in a lithium metal battery to activate dead lithium and achieve reversible reduction, the problems of dead lithium accumulation and SEI structural complexity in lithium metal batteries are solved, extending battery life and improving Energy density and Coulombic efficiency.
Patent Information
- Application Number
- CN202410806511.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-21
- Publication Date
- 2024-10-29
AI Technical Summary
During the cycle process of lithium metal batteries, dead lithium accumulates due to uneven lithium ion flux, which affects battery capacity and life, and the traditional SEI structure is difficult to meet high energy density requirements.
An electrolyte containing lithium salt, anion regulator, soluble salt solvent, diluent and nitroxyl radical catalyst is used. The nitroxyl radical catalyst shuttles between the positive and negative electrodes, oxidizes on the surface of the positive electrode, and activates the negative electrode. Dead lithium realizes its own reversible reduction reaction and inhibits the accumulation of dead lithium.
It improves the utilization rate of lithium, slows down dendrite formation, promotes smooth and stable SEI growth, extends the cycle life of lithium metal batteries, and improves the energy density and Coulombic efficiency of the battery.
Smart Images

Figure BDA0004904893660000021 
Figure BDA0004904893660000031 
Figure BDA0004904893660000061
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of lithium batteries, and in particular to an electrolyte and a lithium metal battery. Background Art
[0002] Lithium (Li) is the charge carrier of traditional lithium-ion batteries and emerging lithium metal batteries, and is an indispensable medium to ensure the operation of batteries. In various applications such as electric vehicles and grid energy storage, there is an urgent need to improve the energy, life and safety of lithium batteries. It is currently believed that inactive lithium in the form of solid electrolyte interface phase (SEI) and metallic inert lithium that loses contact with the electrode and loses its conductive path (commonly known as dead lithium) are the main reasons for capacity decay and insufficient life. At the same time, dead lithium may be the cause of thermal runaway of the battery before lithium dendrites. These adverse obstacles are critically dependent on the properties of SEI on the anode surface.
[0003] It is generally believed that the SEI components in typical lithium-ion batteries with typical graphite anodes mainly include lithium fluoride, and a certain degree of Li2CO3, alkyl carbonates, etc., which are produced by the reduction of organic electrolytes in the first charge and discharge cycle. However, traditional lithium-ion batteries based on graphite anode intercalation chemistry can no longer meet the energy density requirements of lithium batteries in various emerging markets. To meet the urgent need for higher energy density battery systems, lithium metal batteries (LMBs) are considered to be an ideal choice due to their high theoretical capacity and lowest potential. During charging, lithium ions are precipitated from the cathode and deposited on the surface of the current collector, while during subsequent discharge, lithium ions are stripped from the lithium anode and returned to the cathode. Replacing the graphite anode in lithium batteries with lithium metal anodes can increase the energy density by about 50%.
[0004] However, the further development of LMB is hindered by poor lithium plating / stripping performance and irreversible lithium loss. On the one hand, due to the uneven lithium ion flux, the deposited lithium easily forms dendrites on the anode. The lithium stripping behavior occurring at the tip of the dendrite will seriously lead to the accumulation of dead lithium, which is electronically isolated from the lithium metal anode. On the other hand, the transition from graphite to higher energy lithium metal anode greatly complicates the formation of SEI, because the chemical composition of SEI is highly dependent not only on the type of electrolyte but also on the reactivity of the anode. At present, some advanced artificial SEI structures and electrolyte additives for regulating SEI, such as cesium hexafluorophosphate, ethylene fluoride carbonate, lithium nitrate, lithium fluoride, and lithium iodide, have been proposed to improve the performance of lithium metal. However, due to the change in the volume of Li plating, SEI breaks, and fresh metal lithium is exposed to the electrolyte again to form a new SEI. This repeated destruction and repair of SEI makes the protection not durable in long-term cycles. In order to achieve long life, while forming stable protection on the anode, it is necessary to reduce the irreversible loss of lithium, inhibit the degradation of battery capacity and cycle life decay, and maintain high coulombic efficiency. Summary of the invention
[0005] The purpose of the present invention is to provide an electrolyte and a lithium metal battery, in which a circulatory redox catalyst in the electrolyte shuttles between the positive and negative electrodes, is oxidized on the surface of the positive electrode, activates dead lithium into active lithium at the negative electrode, and completes its own reversible reduction reaction, thereby inhibiting the accumulation of dead lithium and improving the long-cycle performance of the battery.
[0006] In a first aspect, the present invention provides an electrolyte solution, comprising a lithium salt, an anion regulator, a soluble salt solvent, a diluent, and a nitroxyl free radical catalyst;
[0007] The nitroxyl free radical catalyst is at least one of the following:
[0008]
[0009] Based on the above technical scheme, the electrolyte of the present invention comprises a lithium salt, an anion regulator, a soluble salt solvent, a diluent and a nitroxyl radical catalyst. The addition of the nitroxyl radical catalyst in the electrolyte can effectively improve the utilization rate of lithium, slow down the formation of dendrites, promote the growth of a smooth and stable SEI, and extend the cycle life of LMB.
[0010] In the above electrolyte, the mass percentage of the nitroxyl free radical catalyst in the electrolyte may be 0.1% to 1%, specifically 0.1%, 0.2%, 0.9%, or 1%.
[0011] In the above electrolyte, the anion regulator may be any one of lithium bis(trifluoromethanesulfonyl)imide (LiTFSI) and lithium difluorobis(oxalato)phosphate (LiDFBOP).
[0012] In the above electrolyte, the mass percentage of the anion regulator in the electrolyte may be 0.1% to 20%, specifically 0.1%, 1%, 10%, or 20%.
[0013] In the above-mentioned electrolyte, the lithium salt may be any one of lithium hexafluorophosphate (LiPF6) and lithium bis(fluorosulfonyl)imide (LiFSI).
[0014] In the above electrolyte, the concentration of the lithium salt in the electrolyte may be 1-3 M, specifically 1.0 M, 1.2 M, 2.0 M, 3.0 M. The LMB electrolyte of the present invention is a local high-concentration electrolyte.
[0015] In the above electrolyte, the soluble salt solvent is one or more of ethylene glycol dimethyl ether (DME), diethylene glycol dimethyl ether (DEGME), and triethylene glycol dimethyl ether (TEGDME).
[0016] In the above-mentioned electrolyte, the diluent may be one or more of 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether (TTE), bis(2,2,2-trifluoroethyl) ether (BTFE), 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether (HFE), and tris(trifluoroethoxy)methane (TFEO).
[0017] In the above-mentioned electrolyte, the volume ratio of the soluble salt solvent to the diluent may be 1:(0.5-7), specifically 1:0.5, 1:2, 1:5, 1:7.
[0018] In a second aspect, the present invention provides a lithium metal battery, comprising a lithium negative electrode plate, a positive electrode plate, an electrolyte and a separator, wherein the electrolyte is the electrolyte described in any one of the above items.
[0019] In the above-mentioned lithium metal battery, the positive electrode plate is a NCM ternary positive electrode plate.
[0020] The present invention has the following beneficial effects:
[0021] (1) Regulating the solvation structure through double anions to reduce Li + The desolvation energy is improved, the kinetics of the lithium deposition / dissolution process is improved, and a high ionic conductivity and sustainable solid electrolyte interface film are induced at the lithium metal anode interface.
[0022] (2) The NO bond conjugation of the nitroxyl radical leads to the formation of unpaired electrons, which is a stable free radical. The redox reaction between the nitroxyl radical and the corresponding cation is highly reversible. The present invention introduces a recyclable redox catalyst into the electrolyte for lithium metal batteries through a simple and inexpensive method. The nitroxyl radical is oxidized into a cation on the cathode surface, which can serve as an electron acceptor to consume the inactive dead lithium on the negative electrode surface, change the original lithium deposition behavior, improve the reversibility of lithium deposition / dissolution, reduce the nucleation potential, and achieve more uniform lithium deposition. Due to the activation of dead lithium, the formation of lithium dendrites is suppressed to a certain extent, the lithium metal negative electrode is stabilized, and it is conducive to higher coulombic efficiency and battery life. This activation behavior is continuously reversible with the reduction of the corresponding cation of the nitroxyl radical, providing the electrolyte with continuously oxidized lithium ions, thereby improving the battery cycle performance.
[0023] (3) The strategy of the present invention can reduce the amount of negative electrode lithium used and improve the energy density of lithium batteries. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1The charge and discharge cycle curves of the soft-pack batteries assembled with the electrolytes in Comparative Example 1 (A), Comparative Example 2 (B), Example 1 (C), Example 2 (D), Example 3 (E), and Example 4 (F); wherein blue is the coulomb efficiency, red is the discharge capacity, and gray is the charge capacity.
[0025] Figure 2 The charge and discharge cycle performance of lithium symmetrical batteries assembled with the electrolytes in Comparative Example 1 (left), Comparative Example 2 (middle), and Example 3 (right). DETAILED DESCRIPTION
[0026] As described in the background art, the existing advanced artificial SEI structure and SEI-adjusting electrolyte additives can no longer meet people's demand for long cycle life of lithium metal batteries. The electrolyte provided by the present invention includes a lithium salt, an anion regulator, a soluble salt solvent, a diluent and a nitroxyl free radical catalyst; the nitroxyl free radical catalyst is at least one of the following:
[0027]
[0028] According to the present invention, the mass percentage of the nitroxyl free radical catalyst in the electrolyte is 0.1% to 1%, including but not limited to 0.1%, 0.2%, 0.9%, and 1%.
[0029] In a preferred embodiment of the present invention, the anion regulator is lithium bis(trifluoromethanesulfonyl)imide (LiTFSI); the present invention adopts a dual anion electrolyte, uses LiTFSI, a lithium salt in LiDFBOP as an anion regulator of the LMB electrolyte, regulates the solvation structure of LMB, and reduces the binding of Li in the solvation sheath. + The desolvation of the electrodes promotes the formation of highly ionic conductive and sustainable inorganic-rich interfaces.
[0030] According to the present invention, the mass percentage of the anion regulator in the electrolyte may be 0.1% to 20%, including but not limited to 0.1%, 1%, 10%, and 20%.
[0031] The present invention optimizes the electrolyte formula, adds an anion regulator and a nitroxyl radical catalyst to the electrolyte, uses LiTFSI, a lithium salt in LiDFBOP as an anion regulator of the LMB electrolyte, regulates the solvation structure through double anions, reduces the desolvation energy of Li+, improves the kinetics of the lithium deposition / dissolution process, and induces high ionic conductivity and sustainable solid electrolyte interface film (SEI) at the lithium metal negative electrode interface; on the other hand, by adding a shuttle redox agent-nitroxyl radical catalyst, the reversibility of lithium deposition / dissolution is improved, and high coulomb efficiency and stable circulation are achieved. This type of catalyst is a stable free radical, and the conjugation of the NO bond leads to the formation of unpaired electrons. During the charging process, the free radical is first oxidized to the corresponding cation on the cathode surface and then diffuses into the electrolyte body. The cation formed by the oxidation of the free radical can serve as an electron acceptor, oxidize the dead lithium in the electrolyte, reactivate it into active lithium ions, and then be reduced and reset to be oxidized into active cations in the next charging process, thereby completing the entire cyclic reversible process. In this cycle, dead lithium and lithium dendrites are continuously converted into active lithium ions, which fully and effectively improves the utilization rate of lithium, slows down the formation of dendrites, promotes the growth of smooth and stable SEI, and prolongs the cycle life of LMB.
[0032] The lithium metal battery provided by the present invention comprises a lithium negative electrode plate, a positive electrode plate, an electrolyte and a separator, wherein the electrolyte is any of the electrolytes described above. In a test example of the present invention, the lithium metal battery is a lithium metal soft pack battery, the positive electrode plate is an NCM ternary positive electrode plate, and the separator is a PE or PP separator.
[0033] The present invention is further described in detail below in conjunction with specific embodiments, and the examples provided are only for illustrating the present invention, rather than for limiting the scope of the present invention. The examples provided below can be used as a guide for further improvements by those of ordinary skill in the art, and do not constitute a limitation of the present invention in any way.
[0034] The methods used in the following examples, unless otherwise specified, are all conventional methods, carried out according to the techniques or conditions described in the literature in the art or according to the product instructions. The materials, reagents, etc. used in the following examples, unless otherwise specified, can all be obtained from commercial sources.
[0035] Example 1
[0036] Prepare the electrolyte as follows:
[0037] Lithium salt LiPF6, anion regulator LiTFSI, soluble salt solvent ethylene glycol dimethyl ether DME and diluent 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether (TTE) are mixed, and nitroxyl free radical catalyst nor-AZADO is added to the mixed solution, and mixed evenly by magnetic stirring for 1 hour to obtain an electrolyte, wherein the concentration of lithium salt in the electrolyte is 1.0M, the mass percentage of the anion regulator in the electrolyte is 0.1wt%, the volume ratio of the soluble salt solvent and the diluent is 1:0.5, and the mass percentage of the nitroxyl free radical catalyst in the electrolyte is 0.1wt%.
[0038] Example 2
[0039] Prepare the electrolyte as follows:
[0040] Lithium salt LiFSI, anion regulator LiDFBOP, soluble salt solvent diethylene glycol dimethyl ether DEGME and diluent 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether (TTE) are mixed, and nitroxyl free radical catalyst AZADOL is added to the mixed solution, and mixed evenly for 3 hours by magnetic stirring to obtain an electrolyte, wherein the concentration of lithium salt in the electrolyte is 1.2M, the mass percentage of the anion regulator in the electrolyte is 1wt%, the volume ratio of the soluble salt solvent and the diluent is 1:2, and the mass percentage of the nitroxyl free radical in the electrolyte is 0.2wt%.
[0041] Example 3
[0042] Prepare the electrolyte as follows:
[0043] Lithium salt LiFSI, anion regulator LiTFSI, soluble salt solvent ethylene glycol dimethyl ether DME and diluent tris(trifluoroethoxy)methane (TFEO) are mixed, and then the nitroxyl radical catalyst TEMPO is added to the mixed solution, and the mixture is mixed evenly by magnetic stirring for 8 hours to obtain an electrolyte, wherein the concentration of lithium salt in the electrolyte is 2.0M, the mass percentage of the anion regulator in the electrolyte is 10wt%, the volume ratio of the soluble salt solvent and the diluent is 1:5, and the mass percentage of the nitroxyl radical in the electrolyte is 0.9wt%.
[0044] Example 4
[0045] Prepare the electrolyte as follows:
[0046] Lithium salt LiPF6, anion regulator LiDFBOP, soluble salt solvent diethylene glycol dimethyl ether DEGME and diluent 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether (HFE) are mixed, and nitroxyl free radical catalyst 1-ME-AZADO is added to the mixed solution, and mixed evenly by magnetic stirring for 12 hours to obtain an electrolyte, wherein the concentration of lithium salt in the electrolyte is 3.0M, the mass percentage of the anion regulator in the electrolyte is 20wt%, the volume ratio of the soluble salt solvent and the diluent is 1:7, and the mass percentage of the nitroxyl free radical in the electrolyte is 1wt%.
[0047] Comparative Example 1
[0048] The lithium salt LiFSI, the soluble salt solvent ethylene glycol dimethyl ether DME and the diluent tris(trifluoroethoxy)methane (TFEO) were mixed and mixed evenly by magnetic stirring for 8 hours to obtain an electrolyte, wherein the concentration of the lithium salt in the electrolyte was 2.0 M, and the volume ratio of the soluble salt solvent to the diluent was 1:5.
[0049] Comparative Example 2
[0050] The lithium salt LiFSI, the anion regulator LiTFSI, the soluble salt solvent ethylene glycol dimethyl ether DME and the diluent tris(trifluoroethoxy)methane (TFEO) are mixed, and the mixture is evenly mixed by magnetic stirring for 8 hours to obtain an electrolyte, wherein the concentration of the lithium salt in the electrolyte is 2.0M, the mass percentage of the anion regulator in the electrolyte is 10wt%, and the volume ratio of the soluble salt solvent to the diluent is 1:5.
[0051] Test Example 1
[0052] The electrolytes in Comparative Examples 1-2 and Example 3 are assembled into lithium metal soft-pack batteries. The assembly of lithium metal soft-pack batteries is carried out in a glove box filled with argon. The negative electrode plate is a lithium strip, the positive electrode plate is an NCM ternary positive electrode plate, the diaphragm is a PE or PP diaphragm, and the electrolytes are the electrolytes prepared in the above-mentioned examples and comparative examples. Among them, the lithium strip is purchased from Tianjin Zhongneng, with a cutting size of 59*63mm, the current collector is copper foil, and the single-sided lithium coating thickness is 30μm, the PE diaphragm is purchased from Shanghai Enjie, with a width of 68mm and no coating, the NCM ternary positive electrode is purchased from Umicore, the electrode plate size is 53*60mm, the current collector is aluminum foil, and the positive electrode material (Umicore MZW8Tc) loading is 250g / m 2 The battery charge and discharge test system is used to test the battery charge and discharge cycle performance. The test conditions are as follows: at room temperature, 0.1C charge and discharge for 3 cycles, 0.2C charge, and 0.5C discharge for a long cycle.
[0053] The test results of the ionic conductivity of the electrolytes of the embodiments and comparative examples are shown in Table 1.
[0054] Table 1. Ionic conductivity
[0055]
[0056] As can be seen from Table 1, the conductivity of the electrolyte in Example 3 is 6.9 mS / cm, which is the best. It is higher than 5.2 mS / cm of the electrolyte in Comparative Example 1 and 5.5 mS / cm of the electrolyte in Comparative Example 2, indicating that the anion regulator can improve the ionic conductivity to a certain extent, which is attributed to the regulation of the solvation structure by the double anion, reducing the Li + The desolvation energy of nitroxyl free radical catalyst is further improved by adding nitroxyl free radical catalyst, which improves the kinetics of lithium deposition / dissolution process. The higher the ionic conductivity, the smaller the impedance inside the battery, the faster the battery charge and discharge rate, and the better the performance. In the process of battery operation, the free ions in the electrolyte will continuously react with the electrode to form a passivation layer, which hinders the transfer speed of ions and reduces the life of the battery. The high conductivity of the electrolyte can promote the transfer of free ions, thereby slowing down the speed of this reaction and extending the battery life.
[0057] The battery cycle data are shown in Table 2.
[0058] Table 2. Battery cycle performance test results
[0059]
[0060] The charge and discharge cycle curve of soft pack battery is as follows Figure 1 As shown, the charge and discharge cycle performance of each comparative example and embodiment is listed.
[0061] From Table 2 and Figure 1It can be seen that in Comparative Example 1, the electrolyte without adding anion regulator and nitroxyl free radical catalyst has an initial discharge capacity of 0.80Ah, in Comparative Example 2, the electrolyte with adding anion regulator but not adding nitroxyl free radical catalyst has an initial discharge capacity of 0.81Ah, and in Example 3, the electrolyte with adding both anion regulator and nitroxyl free radical catalyst has an initial discharge capacity of 0.89Ah. Under the same gram weight conditions, the energy density is greater, which is significantly higher than the discharge capacity in the comparative example, indicating that the electrolyte is conducive to the development of the positive electrode capacity and fully utilizes the capacity of the active material. At the same time, Example 3 has the highest initial efficiency of 91.49% and the lowest capacity loss. One reason for the initial efficiency is that the structure of the positive electrode ternary material changes after the first delithiation, resulting in the inability to 100% embedding of lithium ions; on the other hand, for the negative electrode, the initial efficiency is caused by the formation of SEI. The higher first effect preliminarily shows that the electrolyte in Example 3 has higher reversibility. Through further comparison of the long cycle performance of the battery, it can be seen that the lithium metal soft-pack battery assembled with the electrolyte in Example 3 has a higher coulombic efficiency of 100.55%@200cls and a capacity retention rate of 93.54%@200cls, and is significantly better than the electrolyte without anion regulator and nitroxyl radical catalyst in Comparative Example 1 and the electrolyte without nitroxyl radical catalyst in Comparative Example 2. The battery cycle performance of the embodiment is generally more stable than that of the comparative example, the capacity is higher, and the performance of Example 3 is the best among the embodiments with different proportions. It shows that the excellent and stable cycle performance depends largely on the addition of nitroxyl radical catalysts, which is attributed to the inherent stability of nitroxyl radicals, which can be used as electron acceptors to consume inactive dead lithium on the negative electrode surface, thereby changing the original lithium deposition behavior and improving the reversibility of lithium deposition / dissolution. The activation behavior is continuously reversible with the reduction of the corresponding cations of the nitroxyl radicals, providing the electrolyte with continuously oxidized lithium ions, improving the coulombic efficiency and battery life.
[0062] Test Example 2
[0063] In order to study the stability of the electrolyte to lithium metal, the electrolytes in Comparative Examples 1-2 and Example 3 were assembled into lithium symmetric button cells. The assembly of the lithium symmetric button cells was carried out in a glove box filled with argon. The H2O and O2 contents in the glove box were both less than 0.1ppm. The specific battery composition was lithium sheets (lithium sheets, 8mm in diameter, 0.2mm in thickness) for the positive and negative electrodes, PE diaphragm (9mm in diameter), and the above-prepared electrolyte. The battery charge and discharge test system was used to test the charge and discharge cycle performance of the battery. The test conditions are as follows: at room temperature, 0.2mA / cm 2 Charge and discharge 5 cycles, 0.5mA / cm 2 Charge and discharge 5 cycles, 2mA / cm 2 Long loop.
[0064] Lithium-Lithium Symmetric Battery Cycle Results Visible Figure 2 ,Depend on Figure 2 It can be seen that the lithium symmetric button cell assembled with the electrolyte in Example 3 has the highest stability, no leakage current and short circuit occur during the cycle, and the polarization overpotential is the smallest, close to 0.2 V. This indicates that in Example 3, the nitroxyl radical electrolyte can act as an electron acceptor to consume inactive dead lithium on the negative electrode surface, change the original lithium deposition behavior, improve the reversibility of lithium deposition / dissolution, reduce the nucleation potential, achieve more uniform lithium deposition, inhibit and mitigate the formation of lithium dendrites to a certain extent, and show stability to lithium and better cycle performance.
[0065] The present invention has been described in detail above. For those skilled in the art, without departing from the purpose and scope of the present invention, can implement the present invention in a wider range under equivalent parameters, concentrations and conditions. Although the present invention provides specific embodiments, it should be understood that the present invention can be further improved. In a word, according to the principle of the present invention, the application is intended to include any changes, uses or improvements to the present invention, including departing from the disclosed scope in the application and the changes made with conventional techniques known in the art.
Claims
1. An electrolyte, characterized in that: It includes a lithium salt, an anion regulator, a soluble salt solvent, a diluent and a nitroxyl free radical catalyst; The nitroxyl free radical catalyst is at least one of the following:
2. The electrolyte according to claim 1, characterized in that: The mass percentage of the nitroxyl free radical catalyst in the electrolyte is 0.1% to 1%.
3. The electrolyte according to claim 1, characterized in that: The anion regulator is any one of lithium bis(trifluoromethanesulfonyl)imide and lithium difluorobis(oxalato)phosphate.
4. The electrolyte according to claim 1, characterized in that: The mass percentage of the anion regulator in the electrolyte is 0.1% to 20%.
5. The electrolyte according to claim 1, characterized in that: The lithium salt is any one of lithium hexafluorophosphate and lithium bis(fluorosulfonyl)imide.
6. The electrolyte according to claim 1, characterized in that: The concentration of the lithium salt in the electrolyte is 1-3M.
7. The electrolyte according to claim 1, characterized in that: The soluble salt solvent is one or more of ethylene glycol dimethyl ether, diethylene glycol dimethyl ether, and triethylene glycol dimethyl ether.
8. The electrolyte according to claim 1, characterized in that: The diluent is one or more of 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether, bis(2,2,2-trifluoroethyl) ether, 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether, and tris(trifluoroethoxy)methane.
9. The electrolyte according to claim 1, characterized in that: The volume ratio of the soluble salt solvent to the diluent is 1:(0.5-7).
10. A lithium metal battery, comprising a lithium negative electrode sheet, a positive electrode sheet, an electrolyte and a separator, characterized in that: The electrolyte is the electrolyte according to any one of claims 1 to 9.
Citation Information
Patent Citations
Electrolyte additive, electrolyte, lithium ion secondary battery containing electrolyte additive and application
CN113921902A
Lithium metal secondary battery electrolyte
CN114421000A
Metal lithium-based secondary battery electrolyte and application thereof
CN114512722A
Lithium metal secondary electrolyte and lithium metal secondary battery
CN114792806A
Lithium ion battery electrolyte, preparation method thereof and lithium ion battery
CN117117311A