Method for purifying micro-fine-particle crystalline flake graphite ore through combination of nanobubble and synchronous ultrasonic flotation

Through the combined synchronous ultrasonic flotation method of nanobubble, the problem of difficulty and low separation efficiency of traditional graphite flotation methods when dealing with fine-grained scale graphite is solved, and efficient fixed carbon enrichment and resource utilization is achieved, which is suitable for high-end application fields. .

CN118874701AActive Publication Date: 2024-11-01KUNMING UNIV OF SCI & TECH

Patent Information

Application Number
CN202411274205.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-12
Publication Date
2024-11-01
Estimated Expiration
2044-09-12

AI Technical Summary

Technical Problem

The traditional graphite flotation method is difficult to separate and has low efficiency when treating fine-grained scale graphite, and the fixed carbon enrichment is insufficient, so it is impossible to effectively utilize fine-grained graphite resources.

Method used

Using nanobubble combined with synchronous ultrasonic flotation method, nanobubble is used to mix fine-grained scale graphite with water and then add an ultrasonic probe for synchronous ultrasonic treatment, and supersaturated aqueous solution with air is introduced under ultrasonic conditions to form nanobubble, combined with stirring and agents To improve flotation efficiency and fixed carbon content of concentrate.

Benefits of technology

It significantly improves the fixed carbon content and recovery rate of graphite concentrate, solves the problem of separation between fine scale graphite and gangle minerals, is suitable for high-end application fields, and reduces the dosage of agents and environmental pollution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118874701A_ABST
    Figure CN118874701A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of mineral processing, and particularly relates to a method for purifying micro-fine-particle crystalline flake graphite ore through combination of nanobubbles and synchronous ultrasonic flotation. The method for purifying the micro-fine crystalline flake graphite ore through combination of nano bubbles and synchronous ultrasonic flotation comprises the steps that micro-fine crystalline flake graphite and water are mixed to prepare ore pulp, an ultrasonic probe is inserted into the ore pulp, an ultrasonic generator is turned on, then a pH regulator is added, the pH of the ore pulp is regulated to be 7-10, then an inhibitor, a collecting agent and a foaming agent are sequentially added, and the mixture is stirred to be uniform; the method comprises the following steps: firstly, generating nano bubbles by adopting a pressure air dissolving method, introducing water and compressed air into an air dissolving tank, dissolving air under the pressure of 0.3-0.5 MPa, then releasing the water dissolved with the air into a flotation tank through a pressure reducing valve to form the nano bubbles, and finally, carrying out air inflation and bubble scraping to obtain flotation concentrate. According to the method, the fixed carbon content of the micro-fine-particle flake graphite ore can be increased to 73% through one-time roughing, and the recovery rate is increased to 90% or above.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of mineral processing, and in particular relates to a method for purifying micro-grained flake graphite ore by combining nanobubbles with synchronous ultrasonic flotation. Background Art

[0002] As a resource of great strategic value, graphite has been widely used in many fields such as new energy, electronics, medical treatment, metallurgy, and aerospace due to its unique structure and outstanding characteristics such as thermal conductivity, electrical conductivity, lubrication, high temperature resistance and stable chemical properties. It has become an indispensable non-metallic material in the development of modern industry and high-tech industry, and occupies an increasingly important position in the development of global economy.

[0003] With the rapid development of the economy, the demand for graphite continues to increase, and the traditional coarse-grained graphite resources are gradually decreasing. Fine-grained graphite has become an important supplement to graphite resources. Making full use of fine-grained graphite resources can alleviate the contradiction between supply and demand of graphite resources and ensure the sustainable development of the industry. Moreover, with the continuous mining of graphite, the graphite mines in many places show the characteristics of fine and poor, resulting in insufficient dissociation. Therefore, multi-stage grinding is often used to promote dissociation, resulting in a large amount of fine-grained graphite, which is difficult to purify, resulting in serious waste of resources.

[0004] The prior art, such as a patented method for efficiently purifying coal-based graphite (publication number: CN115043399A), comprises the following steps: (1) electrochemically oxidizing and microwave heating the coal-based graphite in sequence to obtain expanded microcrystalline graphite; (2) mixing the expanded microcrystalline graphite obtained in step (1) with water and subjecting it to ultrasonic treatment to obtain graphite slurry; (3) subjecting the graphite slurry obtained in step (2) to nanobubble flotation to obtain graphite concentrate. The flotation conditions of nanobubble flotation in step (3) are: aeration volume 0.5-2.0 L / min, feed rate 0.5-2.0 L / min, foam layer thickness 200-500 mm, flushing water flow rate 0.5-2.0 L / min, and graphite slurry pH 9-10. This technology can process raw materials with a fixed carbon content of about 80% and obtain products with a fixed carbon content of about 90-97%. Compared with the raw materials, the fixed carbon content in the product is only 1.12-1.25 times that of the raw materials. Summary of the invention

[0005] Traditional graphite flotation methods often face some challenges when processing fine-grained flake graphite. On the one hand, due to its small particle size and large specific surface area, fine-grained flake graphite is easily mixed with gangue minerals during the flotation process, making it difficult to separate; on the other hand, the efficiency and selectivity of conventional flotation methods are limited, the flotation process is inefficient, and the fixed carbon enrichment is low. The present invention provides a method for purifying fine-grained flake graphite ore by nanobubble combined with synchronous ultrasonic flotation, which aims to effectively separate fine-grained flake graphite from gangue minerals, enhance flotation efficiency, and at the same time improve the fixed carbon recovery rate of the concentrate and significantly increase the fixed carbon content of the concentrate.

[0006] In order to achieve the above-mentioned object of the present invention, the present invention proposes for the first time a method for purifying fine-grained flake graphite ore by nanobubble combined with synchronous ultrasonic flotation, which comprises the following steps:

[0007] (1) adding fine flake graphite with a fixed carbon content of 30% or less into a flotation tank and mixing with water at a ratio of 8wt.% to 20wt.% of the ore pulp concentration, turning on a stirring switch to mix the ore pulp evenly, and preparing ore pulp;

[0008] (2) inserting an ultrasonic probe into the slurry of step (1), turning on an ultrasonic generator for synchronous ultrasonic treatment, and stirring for 3 to 5 minutes;

[0009] (3) adding a pH adjuster to the above slurry to adjust the pH of the slurry to 7-10, and stirring for 2-5 minutes;

[0010] (4) adding an inhibitor in an amount of 700 to 1200 g / t, preferably 800 to 1000 g / t, to the pH-adjusted slurry and stirring for 2 to 5 minutes;

[0011] (5) adding a collector to the slurry to which the inhibitor has been added at a dosage of 260 to 420 g / t, preferably 280 to 380 g / t, and more preferably 340 to 360 g / t, and stirring for 2 to 5 minutes;

[0012] (6) Adding a foaming agent in an amount of 150-320 g / t or 150-180 g / t to the slurry to which the collector has been added, and stirring for 1-3 minutes;

[0013] (7) introducing a supersaturated aqueous solution containing air formed by a pressure gas solution method into the slurry to which a foaming agent is added, and forming nanobubbles in the slurry; when the supersaturated aqueous solution containing air is formed, the pressure of the gas passing through is 0.3 to 0.5 MPa, preferably 0.35 to 0.45 MPa, and more preferably 0.38 to 0.42 MPa;

[0014] (8) Under ultrasonic conditions, a supersaturated aqueous solution containing air is introduced while air is filled to scrape and foam for 4 to 7 minutes. The foam scraped out is filtered and dried to obtain flake graphite concentrate, and the rest is tailings; the amount of air filled is 40 to 80 L / h.

[0015] The present invention can process micro-fine flake graphite ores with ultra-low fixed carbon content, such as micro-fine flake graphite ores with a fixed carbon content of 20% or less, and of course also micro-fine flake graphite ores with a fixed carbon content of 5% to 18%.

[0016] Preferably, the present invention provides a method for purifying fine-grained flake graphite ore by nanobubble combined with synchronous ultrasonic flotation.

[0017] The particle size of the micro-grained flake graphite is -300 mesh, accounting for more than 80%.

[0018] Preferably, the present invention provides a method for purifying fine-grained flake graphite ore by nanobubble combined with synchronous ultrasonic flotation.

[0019] The stirring process is stirred by the impeller of the flotation machine, and the speed is 1200-1900r / min, preferably 1500-1700r / min. The present invention controls the stirring speed to be 1200-1900r / min. In the stage of adding the flotation agent, it mainly plays the role of uniform agent. When the supersaturated aqueous solution containing dissolved air is introduced, it is conducive to the formation of more and finer nanobubbles. In conjunction with the subsequent ultrasound, the number of nanobubbles is further increased, thereby significantly improving the flotation effect, especially improving the enrichment effect of fixed carbon. If the speed is too low, the nanobubbles may not be fully dispersed into the pulp, affecting its contact with the mineral particles, and at the same time, the solid particles in the pulp may be easily precipitated, affecting the flotation process; if the speed is too high, the stability of the nanobubbles may be destroyed, causing them to break or merge prematurely, thereby reducing the role of the nanobubbles in flotation. At the same time, too high a speed will cause impurities to be entrained in the bubbles, thereby reducing the fixed carbon content of the concentrate.

[0020] Preferably, in the method of purifying fine-grained flake graphite ore by nanobubble combined with synchronous ultrasonic flotation of the present invention, the frequency of the ultrasound used is 18-25KHz, preferably 20KHz, and the power is set to 80-200W, preferably 135-165W.

[0021] Preferably, the present invention provides a method for purifying fine-grained flake graphite ore by nanobubble combined with synchronous ultrasonic flotation.

[0022] The pH adjusters used are HCl and NaOH. The pH of the slurry is controlled to be 7 to 10, preferably 7.5 to 8.5.

[0023] Preferably, the present invention provides a method for purifying fine-grained flake graphite ore by nanobubble combined with synchronous ultrasonic flotation.

[0024] The inhibitor used is one of water glass, sodium hexametaphosphate and sodium carboxymethyl cellulose. Preferably, it is water glass or a mixture of water glass and at least one of sodium hexametaphosphate and sodium carboxymethyl cellulose;

[0025] In the present invention, water glass is used as an inhibitor mainly because silicate ions can be adsorbed on the surface of gangue minerals under certain conditions to form a hydrophilic film to prevent it from interacting with the collector, and the range of action of silicate ions is generally around 8 to 11. If the pH is too low, the degree of hydrolysis of water glass is insufficient, the concentration of silicate ions is low, and the inhibitory effect is not obvious; when the pH is too high, it may cause changes in the surface charge of the mineral, affecting the adsorption of silicate ions. Due to the different properties of the ore, different pH values ​​will have different flotation effects. This specific pH is generally determined by experiments in actual situations. It is found in the experiment that the effect is better in the range of pH 7 to 10, so the pH range is limited to 7 to 10, and more preferably 7.5 to 8.5.

[0026] Preferably, the present invention provides a method for purifying fine-grained flake graphite ore by nanobubble combined with synchronous ultrasonic flotation.

[0027] The collector used is one of kerosene, diesel and liquid paraffin.

[0028] Preferably, the present invention provides a method for purifying fine-grained flake graphite ore by nanobubble combined with synchronous ultrasonic flotation.

[0029] The foaming agent used is one of pine oil, sec-octanol and methyl isobutyl carbinol.

[0030] Preferably, the present invention provides a method for purifying fine-grained flake graphite ore by nanobubble combined with synchronous ultrasonic flotation.

[0031] The preparation method of the supersaturated aqueous solution containing air formed by the pressure gas dissolution method is as follows: first, water and compressed air are passed into the gas dissolution tank, and the pressure is increased to 0.3-0.5MPa, preferably 0.35-0.45MPa, and more preferably 0.38-0.42MPa by a booster pump. Under this pressure, the air gradually dissolves in the water to form a supersaturated solution. In practical applications, the water containing air is slowly released into the flotation tank through a pressure reducing valve. When the pressure is reduced, the air dissolved in the water will quickly form nanobubbles. The size and number of nanobubbles can be controlled by adjusting the opening and release speed of the pressure reducing valve, thereby achieving the purpose of introducing nanobubbles in the flotation process.

[0032] In step 8 of the present invention, there is no strict requirement for the pressure of the air filled. In practical application, after turning on the inflation switch, the air in the nature is introduced through the flotation machine. During flotation, when the water level in the flotation tank is too high, the pulp will overflow, and when the water level is too low, the automatic scraping plate cannot scrape the foam. Therefore, there is a range of the height of the pulp during the flotation process. During the continuous flotation process, the liquid level drops due to the scraping of bubbles. At this time, it is necessary to add water slowly and continuously. The present invention uses a supersaturated aqueous solution containing dissolved air instead of the supplemented water. Therefore, the amount of water added here depends on the specific situation in the flotation. It is added slowly and will not exceed the mouth of the flotation tank. It is also within the scraping range of the scraping plate. In general, it is to add slowly to keep the pulp level within a water level line range.

[0033] The present invention can achieve a fixed carbon content of 70-73% in the graphite concentrate obtained by roughing, and a recovery rate of 88% or more. After at least two rounds of fine cleaning, the fixed carbon content of the graphite concentrate obtained by roughing is 93% or more.

[0034] The reagent system for selecting the graphite concentrate obtained by roughing is: 440-560g / t of inhibitor, 175-205g / t of collector, and 70-95g / t of frother. More preferably:

[0035] The reagent system for selecting the graphite concentrate obtained by roughing is: inhibitor water glass 450g / t, collector kerosene 175g / t, foaming agent pine alcohol 80g / t; or inhibitor sodium carboxymethyl cellulose 500g / t, collector diesel 180g / t, foaming agent methyl isobutyl carbinol 75g / t; or

[0036] Inhibitor water glass 550g / t, collector kerosene 200g / t, foaming agent 2-octanol 90g / t.

[0037] Compared with the prior art, the present invention has the following beneficial effects:

[0038] The present invention uses the synergistic effect of nanobubbles and ultrasound to effectively separate fine-grained flake graphite from gangue minerals, significantly improve the fixed carbon content of graphite concentrate, and meet the needs of high-end application fields; at the same time, nanobubbles increase the probability of attachment of mineral particles to bubbles, and ultrasound promotes the action of reagents and minerals and the dispersion of particles. The combined action of the two greatly improves the flotation efficiency and reduces the flotation time and the amount of reagents used; and the method is particularly suitable for the purification of fine-grained flake graphite, which solves the problem of traditional flotation methods in processing fine-grained minerals and provides a feasible technical solution for the efficient utilization of fine-grained mineral resources; compared with traditional methods, this method reduces the amount of reagents used to a certain extent and reduces pollution to the environment. At the same time, the energy required for ultrasonic treatment is relatively low, which has the advantage of energy saving. In addition to the above advantages, the present invention can process raw materials with low fixed carbon content and achieve efficient enrichment. BRIEF DESCRIPTION OF THE DRAWINGS

[0039] Figure 1 The figure is a flow chart of a specific implementation mode of the present invention.

[0040] Figure 2 These are electron microscope images of the raw material and the selected product in Example 1, where (a) is a backscattered image of the raw material at 3000 times magnification, and (b) is a backscattered image of the selected concentrate at 3000 times magnification.

[0041] from Figure 1 The basic process of the present invention can be seen in FIG.

[0042] Figure 2 In the graphite, the black part is graphite, and the bright white part is impurity elements such as aluminum and silicon. Figure 2 (a) It can be seen that the raw material particle size is mostly 5-20um, which is fine-grained flake graphite, and the white part accounts for the majority, indicating that the raw material has a low fixed carbon content and a high impurity content. Figure 2 (b) It can be seen that there are only a few bright white particles in the graphite concentrate after concentration. Figure 2 (a) In contrast, the impurity content is greatly reduced, indicating that the method provided by the present invention can effectively purify fine-grained graphite. DETAILED DESCRIPTION

[0043] The embodiments of the present invention will be described in detail below in conjunction with the examples, but those skilled in the art will understand that the following examples are only used to illustrate the present invention and should not be considered to limit the scope of the present invention. If no specific conditions are specified in the examples, the conventional conditions or the conditions recommended by the manufacturer are followed. The reagents or instruments used without indicating the manufacturer are all conventional products that can be obtained commercially.

[0044] In this embodiment, the fixed carbon content of the graphite concentrate obtained in step (8) can reach 72.93%, and the recovery rate can reach 90.26%.

[0045] The specific implementation modes of the present invention are further described below in conjunction with embodiments, but the present invention is not limited to the scope of the embodiments.

[0046] Example 1

[0047] The XRD test results of the fine-grained natural flake graphite ore produced in the Xinjiang mining area show that the impurities are mainly mica, quartz and feldspar, and its composition is shown in Table 1.

[0048] Table 1 Composition of natural flake graphite in a mining area in Xinjiang

[0049]

[0050] First, water and compressed air are introduced into the air dissolving tank, and the pressure is increased to 0.4MPa by a booster pump, so that the air is gradually dissolved in the water to form a supersaturated solution containing air;

[0051] The fine-grained natural flake graphite produced in Xinjiang is mixed with water at a ratio of 15% of the slurry concentration, and the stirring switch is turned on at a speed of 1600 r / min to mix the slurry evenly to obtain slurry;

[0052] Then, an ultrasonic probe was inserted into the slurry, and the ultrasonic generator was turned on for synchronous ultrasonic treatment. The ultrasonic power was set to 150 W. After stirring at a speed of 1600 rpm for 4 minutes, a pH adjuster was added to adjust the pH of the slurry to 8. After stirring for 3 minutes, an inhibitor, water glass, was added at a dosage of 900 g / t. After stirring for 3 minutes, a collector, kerosene, was added at a dosage of 350 g / t. After stirring for 3 minutes, a foaming agent, pine alcohol, was added at a dosage of 160 g / t. The mixture was stirred at a speed of 1600 rpm for 2 minutes.

[0053] Then, the supersaturated solution containing air prepared above is slowly released into the flotation tank through the pressure reducing valve. Then, the pressure is reduced to allow the air dissolved in the water to quickly form nanobubbles, thereby introducing nanobubbles, and stirring at a speed of 1600 rpm for 1 min, then the aeration switch is turned on (at this time, ultrasound is continuously applied and a supersaturated solution containing air is introduced), the air intake rate is controlled to be 60 L / h, and then the frothing is scraped for 5 min, and the frothing is continuously introduced during the frothing process until no foam is scraped, and then the flotation and aeration are terminated. During the frothing process, the supersaturated solution containing air is continuously and slowly introduced to keep the height of the pulp within a range within which the pulp will not overflow, and the frothing scraper can also scrape the foam well, and the scraped foam is filtered and dried at 105°C to obtain flake graphite concentrate.

[0054] During the flotation process, natural flake graphite ore was flotated at room temperature. The indicators of the flotation products obtained through continuous expansion tests were: fixed carbon content of 72.93% and recovery rate of 89.71%.

[0055] The graphite concentrate obtained by rough selection was refined in the presence of 450g / t of water glass as an inhibitor, 175g / t of kerosene as a collector and 80g / t of pine alcohol as a foaming agent. After three rounds of refinement, the fixed carbon content in the graphite concentrate increased to 95.13%.

[0056] Example 1-1

[0057] The other conditions are the same as those in Example 1, except that when nanobubbles are generated, the booster pump pressure is 0.3 MPa, that is:

[0058] First, water and compressed air are introduced into the air dissolving tank, and the pressure is increased to 0.3MPa by a booster pump, so that the air is gradually dissolved in the water to form a supersaturated solution containing air;

[0059] The fine-grained natural flake graphite produced in Xinjiang is mixed with water at a ratio of 15% of the slurry concentration, and the stirring switch is turned on at a speed of 1600 r / min to mix the slurry evenly to obtain slurry;

[0060] Then, an ultrasonic probe was inserted into the slurry, and the ultrasonic generator was turned on for synchronous ultrasonic treatment. The ultrasonic power was set to 150 W. After stirring at a speed of 1600 rpm for 4 minutes, a pH adjuster was added to adjust the pH of the slurry to 8. After stirring for 3 minutes, an inhibitor, water glass, was added at a dosage of 900 g / t. After stirring for 3 minutes, a collector, kerosene, was added at a dosage of 350 g / t. After stirring for 3 minutes, a foaming agent, pine alcohol, was added at a dosage of 160 g / t. The mixture was stirred at a speed of 1600 rpm for 2 minutes.

[0061] Then, the supersaturated solution containing air prepared above is slowly released into the flotation tank through the pressure reducing valve. Then, the pressure is reduced to allow the air dissolved in the water to quickly form nanobubbles, thereby introducing nanobubbles, and stirring at a speed of 1600 rpm for 1 min, then the aeration switch is turned on (at this time, ultrasound is continuously applied and a supersaturated solution containing air is introduced), the air intake rate is controlled to be 60 L / h, and then the frothing is scraped for 5 min, and the frothing is continuously introduced during the frothing process until no foam is scraped, and then the flotation and aeration are terminated. During the frothing process, the supersaturated solution containing air is continuously and slowly introduced to keep the height of the pulp within a range within which the pulp will not overflow, and the frothing scraper can also scrape the foam well, and the scraped foam is filtered and dried at 105°C to obtain flake graphite concentrate.

[0062] During the flotation process, natural flake graphite ore was flotated at room temperature. The indicators of the flotation products obtained through continuous expansion tests were: fixed carbon content of 71.80% and recovery rate of 85.36%.

[0063] The graphite concentrate obtained by rough selection was refined in the presence of 450g / t of water glass as an inhibitor, 175g / t of kerosene as a collector and 80g / t of pine alcohol as a foaming agent. After three rounds of refinement, the fixed carbon content in the graphite concentrate increased to 94.74%.

[0064] Example 1-2

[0065] The other conditions are the same as those in Example 1, except that when nanobubbles are generated, the booster pump pressure is 0.5 MPa, that is:

[0066] First, water and compressed air are introduced into the air dissolving tank, and the pressure is increased to 0.5MPa by a booster pump, so that the air is gradually dissolved in the water to form a supersaturated solution containing air;

[0067] The fine-grained natural flake graphite produced in Xinjiang is mixed with water at a ratio of 15% of the slurry concentration, and the stirring switch is turned on at a speed of 1600 r / min to mix the slurry evenly to obtain slurry;

[0068] Then, an ultrasonic probe was inserted into the slurry, and the ultrasonic generator was turned on for synchronous ultrasonic treatment. The ultrasonic power was set to 150 W. After stirring at a speed of 1600 rpm for 4 minutes, a pH adjuster was added to adjust the pH of the slurry to 8. After stirring for 3 minutes, an inhibitor, water glass, was added at a dosage of 900 g / t. After stirring for 3 minutes, a collector, kerosene, was added at a dosage of 350 g / t. After stirring for 3 minutes, a foaming agent, pine alcohol, was added at a dosage of 160 g / t. The mixture was stirred at a speed of 1600 rpm for 2 minutes.

[0069] Then, the supersaturated solution containing air prepared above is slowly released into the flotation tank through the pressure reducing valve. Then, the pressure is reduced to allow the air dissolved in the water to quickly form nanobubbles, thereby introducing nanobubbles, and stirring at a speed of 1600 rpm for 1 min, then the aeration switch is turned on (at this time, ultrasound is continuously applied and a supersaturated solution containing air is introduced), the air intake rate is controlled to be 60 L / h, and then the frothing is scraped for 5 min, and the frothing is continuously introduced during the frothing process until no foam is scraped, and then the flotation and aeration are terminated. During the frothing process, the supersaturated solution containing air is continuously and slowly introduced to keep the height of the pulp within a range within which the pulp will not overflow, and the frothing scraper can also scrape the foam well, and the scraped foam is filtered and dried at 105°C to obtain flake graphite concentrate.

[0070] During the flotation process, natural flake graphite ore was flotated at room temperature. The indicators of the flotation products obtained through continuous expansion tests were: fixed carbon content of 68.89% and recovery rate of 88.01%.

[0071] The graphite concentrate obtained by rough selection was refined in the presence of 450g / t of water glass as an inhibitor, 175g / t of kerosene as a collector and 80g / t of pine alcohol as a foaming agent. After three rounds of refinement, the fixed carbon content in the graphite concentrate increased to 94.15%.

[0072] Examples 1-3

[0073] The other conditions are the same as those in Example 1, except that the amount of inhibitor is 1200 g / t, that is:

[0074] First, water and compressed air are introduced into the air dissolving tank, and the pressure is increased to 0.4MPa by a booster pump, so that the air is gradually dissolved in the water to form a supersaturated solution containing air;

[0075] The fine-grained natural flake graphite produced in Xinjiang is mixed with water at a ratio of 15% of the slurry concentration, and the stirring switch is turned on at a speed of 1600 r / min to mix the slurry evenly to obtain slurry;

[0076] Then, an ultrasonic probe was inserted into the slurry, and the ultrasonic generator was turned on for synchronous ultrasonic treatment. The ultrasonic power was set to 150 W. After stirring at a speed of 1600 rpm for 4 minutes, a pH adjuster was added to adjust the pH of the slurry to 8. After stirring for 3 minutes, an inhibitor, water glass, was added at a dosage of 1200 g / t. After stirring for 3 minutes, a collector, kerosene, was added at a dosage of 350 g / t. After stirring for 3 minutes, a foaming agent, pine alcohol, was added at a dosage of 160 g / t. The mixture was stirred at a speed of 1600 rpm for 2 minutes.

[0077] Then, the supersaturated solution containing air prepared above is slowly released into the flotation tank through the pressure reducing valve. Then, the pressure is reduced to allow the air dissolved in the water to quickly form nanobubbles, thereby introducing nanobubbles, and stirring at a speed of 1600 rpm for 1 min, then the aeration switch is turned on (at this time, ultrasound is continuously applied and a supersaturated solution containing air is introduced), the air intake rate is controlled to be 60 L / h, and then the frothing is scraped for 5 min, and the frothing is continuously introduced during the frothing process until no foam is scraped, and then the flotation and aeration are terminated. During the frothing process, the supersaturated solution containing air is continuously and slowly introduced to keep the height of the pulp within a range within which the pulp will not overflow, and the frothing scraper can also scrape the foam well, and the scraped foam is filtered and dried at 105°C to obtain flake graphite concentrate.

[0078] During the flotation process, natural flake graphite ore was flotated at room temperature. The indicators of the flotation products obtained through continuous expansion tests were: fixed carbon content of 70.66% and recovery rate of 87.95%.

[0079] The graphite concentrate obtained by rough selection was refined in the presence of 450g / t of water glass as an inhibitor, 175g / t of kerosene as a collector and 80g / t of pine alcohol as a foaming agent. After three rounds of refinement, the fixed carbon content in the graphite concentrate increased to 94.90%.

[0080] Examples 1-4

[0081] The other conditions are the same as those in Example 1, except that the amount of collector is 280 g / t, that is:

[0082] First, water and compressed air are introduced into the air dissolving tank, and the pressure is increased to 0.4MPa by a booster pump, so that the air is gradually dissolved in the water to form a supersaturated solution containing air;

[0083] The fine-grained natural flake graphite produced in Xinjiang is mixed with water at a ratio of 15% of the slurry concentration, and the stirring switch is turned on at a speed of 1600 r / min to mix the slurry evenly to obtain slurry;

[0084] Then, an ultrasonic probe was inserted into the slurry, and the ultrasonic generator was turned on for synchronous ultrasonic treatment. The ultrasonic power was set to 150 W. After stirring at a speed of 1600 rpm for 4 minutes, a pH adjuster was added to adjust the pH of the slurry to 8. After stirring for 3 minutes, an inhibitor, water glass, was added at a dosage of 900 g / t. After stirring for 3 minutes, a collector, kerosene, was added at a dosage of 280 g / t. After stirring for 3 minutes, a foaming agent, pine alcohol, was added at a dosage of 160 g / t. The mixture was stirred at a speed of 1600 rpm for 2 minutes.

[0085] Then, the supersaturated solution containing air prepared above is slowly released into the flotation tank through the pressure reducing valve. Then, the pressure is reduced to allow the air dissolved in the water to quickly form nanobubbles, thereby introducing nanobubbles, and stirring at a speed of 1600 rpm for 1 min, then the aeration switch is turned on (at this time, ultrasound is continuously applied and a supersaturated solution containing air is introduced), the air intake rate is controlled to be 60 L / h, and then the frothing is scraped for 5 min, and the frothing is continuously introduced during the frothing process until no foam is scraped, and then the flotation and aeration are terminated. During the frothing process, the supersaturated solution containing air is continuously and slowly introduced to keep the height of the pulp within a range within which the pulp will not overflow, and the frothing scraper can also scrape the foam well, and the scraped foam is filtered and dried at 105°C to obtain flake graphite concentrate.

[0086] During the flotation process, natural flake graphite ore was flotated at room temperature. The indicators of the flotation products obtained through continuous expansion tests were: fixed carbon content of 72.01% and recovery rate of 82.16%.

[0087] The graphite concentrate obtained by rough selection was refined in the presence of 450g / t of water glass as an inhibitor, 175g / t of kerosene as a collector and 80g / t of pine alcohol as a foaming agent. After three rounds of refinement, the fixed carbon content in the graphite concentrate increased to 94.93%.

[0088] Examples 1-5

[0089] The other conditions are the same as those in Example 1, except that the amount of foaming agent is 320 g / t, that is:

[0090] First, water and compressed air are introduced into the air dissolving tank, and the pressure is increased to 0.4MPa by a booster pump, so that the air is gradually dissolved in the water to form a supersaturated solution containing air;

[0091] The fine-grained natural flake graphite produced in Xinjiang is mixed with water at a ratio of 15% of the slurry concentration, and the stirring switch is turned on at a speed of 1600 r / min to mix the slurry evenly to obtain slurry;

[0092] Then, an ultrasonic probe was inserted into the slurry, and the ultrasonic generator was turned on for synchronous ultrasonic treatment. The ultrasonic power was set to 150 W. After stirring at a speed of 1600 rpm for 4 minutes, a pH adjuster was added to adjust the pH of the slurry to 8. After stirring for 3 minutes, an inhibitor, water glass, was added at a dosage of 900 g / t. After stirring for 3 minutes, a collector, kerosene, was added at a dosage of 350 g / t. After stirring for 3 minutes, a foaming agent, pine alcohol, was added at a dosage of 320 g / t. The mixture was stirred at a speed of 1600 rpm for 2 minutes.

[0093] Then, the supersaturated solution containing air prepared above is slowly released into the flotation tank through the pressure reducing valve. Then, the pressure is reduced to allow the air dissolved in the water to quickly form nanobubbles, thereby introducing nanobubbles, and stirring at a speed of 1600 rpm for 1 min, then the aeration switch is turned on (at this time, ultrasound is continuously applied and a supersaturated solution containing air is introduced), the air intake rate is controlled to be 60 L / h, and then the frothing is scraped for 5 min, and the frothing is continuously introduced during the frothing process until no foam is scraped, and then the flotation and aeration are terminated. During the frothing process, the supersaturated solution containing air is continuously and slowly introduced to keep the height of the pulp within a range within which the pulp will not overflow, and the frothing scraper can also scrape the foam well, and the scraped foam is filtered and dried at 105°C to obtain flake graphite concentrate.

[0094] During the flotation process, natural flake graphite ore was flotated at room temperature. The indicators of the flotation products obtained through continuous expansion tests were: fixed carbon content of 65.17% and recovery rate of 87.64%.

[0095] The graphite concentrate obtained by rough selection was refined in the presence of 450g / t of water glass as an inhibitor, 175g / t of kerosene as a collector and 80g / t of pine alcohol as a foaming agent. After three rounds of refinement, the fixed carbon content in the graphite concentrate increased to 93.99%.

[0096] Examples 1-6

[0097] The other conditions are the same as those in Example 1, except that the speed is adjusted to 1200 r / min and the air intake volume is controlled to 40 L / h, that is:

[0098] First, water and compressed air are introduced into the air dissolving tank, and the pressure is increased to 0.4MPa by a booster pump, so that the air is gradually dissolved in the water to form a supersaturated solution containing air;

[0099] The fine-grained natural flake graphite produced in Xinjiang is mixed with water at a ratio of 15% of the slurry concentration, and the stirring switch is turned on at a speed of 1200 r / min to mix the slurry evenly to obtain slurry;

[0100] Then, an ultrasonic probe was inserted into the slurry, and the ultrasonic generator was turned on for synchronous ultrasonic treatment. The ultrasonic power was set to 150 W. After stirring at a speed of 1200 rpm for 4 minutes, a pH adjuster was added to adjust the pH of the slurry to 8. After stirring for 3 minutes, an inhibitor, water glass, was added at a dosage of 900 g / t. After stirring for 3 minutes, a collector, kerosene, was added at a dosage of 350 g / t. After stirring for 3 minutes, a foaming agent, pine alcohol, was added at a dosage of 160 g / t. The mixture was stirred at a speed of 1200 rpm for 2 minutes.

[0101] Then, the supersaturated solution containing air prepared above is slowly released into the flotation tank through the pressure reducing valve. Then, the pressure is reduced to allow the air dissolved in the water to quickly form nanobubbles, thereby introducing nanobubbles, and stirring at a speed of 1200 rpm for 1 min, then the aeration switch is turned on (at this time, ultrasound is continuously applied and a supersaturated solution containing air is introduced), the air intake rate is controlled to be 40 L / h, and then the frothing is scraped for 5 min, and the frothing is continuously introduced during the frothing process until no foam is scraped, and then the flotation and aeration are terminated. During the frothing process, the supersaturated solution containing air is continuously and slowly introduced to keep the height of the pulp within a range within which the pulp will not overflow, and the frothing scraper can also scrape the foam well, and the scraped foam is filtered and dried at 105°C to obtain flake graphite concentrate.

[0102] During the flotation process, natural flake graphite ore was flotated at room temperature. The indicators of the flotation products obtained through continuous expansion tests were: fixed carbon content of 68.51% and recovery rate of 88.04%.

[0103] The graphite concentrate obtained by rough selection was refined in the presence of 450g / t of water glass as an inhibitor, 175g / t of kerosene as a collector and 80g / t of pine alcohol as a foaming agent. After three rounds of refinement, the fixed carbon content in the graphite concentrate increased to 93.42%.

[0104] Examples 1-7

[0105] The other conditions are the same as those in Example 1, except that the speed is adjusted to 1900 r / min and the air intake volume is controlled to 80 L / h, that is:

[0106] First, water and compressed air are introduced into the air dissolving tank, and the pressure is increased to 0.4MPa by a booster pump, so that the air is gradually dissolved in the water to form a supersaturated solution containing air;

[0107] The fine-grained natural flake graphite produced in Xinjiang is mixed with water at a ratio of 15% of the slurry concentration, and the stirring switch is turned on at a speed of 1900 r / min to mix the slurry evenly to obtain slurry;

[0108] Then, an ultrasonic probe was inserted into the slurry, and the ultrasonic generator was turned on for synchronous ultrasonic treatment. The ultrasonic power was set to 150 W. After stirring at a speed of 1900 rpm for 4 minutes, a pH adjuster was added to adjust the pH of the slurry to 8. After stirring for 3 minutes, an inhibitor, water glass, was added at a dosage of 900 g / t. After stirring for 3 minutes, a collector, kerosene, was added at a dosage of 350 g / t. After stirring for 3 minutes, a foaming agent, pine alcohol, was added at a dosage of 160 g / t. The mixture was stirred at a speed of 1900 rpm for 2 minutes.

[0109] Then, the supersaturated solution containing air prepared above is slowly released into the flotation tank through the pressure reducing valve. Then, the pressure is reduced to allow the air dissolved in the water to quickly form nanobubbles, thereby introducing nanobubbles, and stirring at a speed of 1900 rpm for 1 min, then the aeration switch is turned on (at this time, ultrasound is continuously applied and a supersaturated solution containing air is introduced), the air intake rate is controlled to be 80 L / h, and then the frothing is scraped for 5 min, and the frothing is continuously introduced during the frothing process until no foam is scraped, and then the flotation and aeration are terminated. During the frothing process, the supersaturated solution containing air is continuously and slowly introduced to keep the height of the pulp within a range within which the pulp will not overflow, and the frothing scraper can also scrape the foam well, and the scraped foam is filtered and dried at 105°C to obtain flake graphite concentrate.

[0110] During the flotation process, natural flake graphite ore was flotated at room temperature. The indicators of the flotation products obtained through continuous expansion tests were: fixed carbon content of 66.82% and recovery rate of 90.03%.

[0111] The graphite concentrate obtained by rough selection was refined in the presence of 450g / t of water glass as an inhibitor, 175g / t of kerosene as a collector and 80g / t of pine alcohol as a foaming agent. After three rounds of refinement, the fixed carbon content in the graphite concentrate increased to 93.77%.

[0112] Examples 1-8

[0113] Other conditions were the same as those in Example 1, except that the ultrasonic power was 200 W, the rotation speed was 1500 r / min, and the pH was adjusted to 9, that is:

[0114] First, water and compressed air are introduced into the air dissolving tank, and the pressure is increased to 0.4MPa by a booster pump, so that the air is gradually dissolved in the water to form a supersaturated solution containing air;

[0115] The fine-grained natural flake graphite produced in Xinjiang is mixed with water at a ratio of 15% of the slurry concentration, and the stirring switch is turned on at a speed of 1500 r / min to mix the slurry evenly to obtain slurry;

[0116] Then, an ultrasonic probe was inserted into the slurry, and the ultrasonic generator was turned on for synchronous ultrasonic treatment. The ultrasonic power was set to 200 W. After stirring at a speed of 1500 rpm for 4 minutes, a pH adjuster was added to adjust the pH of the slurry to 9. After stirring for 3 minutes, an inhibitor, water glass, was added at a dosage of 900 g / t. After stirring for 3 minutes, a collector, kerosene, was added at a dosage of 350 g / t. After stirring for 3 minutes, a foaming agent, pine alcohol, was added at a dosage of 160 g / t, and stirred at a speed of 1500 rpm for 2 minutes.

[0117] Then, the supersaturated solution containing air prepared above is slowly released into the flotation tank through the pressure reducing valve. Then, the pressure is reduced to allow the air dissolved in the water to quickly form nanobubbles, thereby introducing nanobubbles, and stirring at a speed of 1500 rpm for 1 min, then the aeration switch is turned on (at this time, ultrasound is continuously applied and a supersaturated solution containing air is introduced), the air intake rate is controlled to be 60 L / h, and then the frothing is scraped for 5 min, and the frothing is continuously introduced during the frothing process until no foam is scraped, and then the flotation and aeration are terminated. During the frothing process, the supersaturated solution containing air is continuously and slowly introduced to keep the height of the pulp within a range within which the pulp will not overflow, and the frothing scraper can also scrape the foam well, and the scraped foam is filtered and dried at 105°C to obtain flake graphite concentrate.

[0118] During the flotation process, natural flake graphite ore was flotated at room temperature. The indicators of the flotation products obtained through continuous expansion tests were: fixed carbon content of 64.27% and recovery rate of 87.14%.

[0119] The graphite concentrate obtained by rough selection was refined in the presence of 450g / t of water glass as an inhibitor, 175g / t of kerosene as a collector and 80g / t of pine alcohol as a foaming agent. After three rounds of refinement, the fixed carbon content in the graphite concentrate increased to 94.67%.

[0120] Examples 1-9

[0121] The other conditions were the same as those in Example 1, except that the ultrasonic power was 80 W, the rotation speed was 1500 r / min, and the pH was adjusted to 10, that is:

[0122] First, water and compressed air are introduced into the air dissolving tank, and the pressure is increased to 0.4MPa by a booster pump, so that the air is gradually dissolved in the water to form a supersaturated solution containing air;

[0123] The fine-grained natural flake graphite produced in Xinjiang is mixed with water at a ratio of 15% of the slurry concentration, and the stirring switch is turned on at a speed of 1500 r / min to mix the slurry evenly to obtain slurry;

[0124] Then, an ultrasonic probe was inserted into the slurry, and the ultrasonic generator was turned on for synchronous ultrasonic treatment. The ultrasonic power was set to 80W. After stirring at a speed of 1500 rpm for 4 minutes, a pH adjuster was added to adjust the pH of the slurry to 10. After stirring for 3 minutes, an inhibitor, water glass, was added at a dosage of 900 g / t. After stirring for 3 minutes, a collector, kerosene, was added at a dosage of 350 g / t. After stirring for 3 minutes, a foaming agent, pine alcohol, was added at a dosage of 160 g / t, and the mixture was stirred at a speed of 1500 rpm for 2 minutes.

[0125] Then, the supersaturated solution containing air prepared above is slowly released into the flotation tank through the pressure reducing valve. Then, the pressure is reduced to allow the air dissolved in the water to quickly form nanobubbles, thereby introducing nanobubbles, and stirring at a speed of 1500 rpm for 1 min, then the aeration switch is turned on (at this time, ultrasound is continuously applied and a supersaturated solution containing air is introduced), the air intake rate is controlled to be 60 L / h, and then the frothing is scraped for 5 min, and the frothing is continuously introduced during the frothing process until no foam is scraped, and then the flotation and aeration are terminated. During the frothing process, the supersaturated solution containing air is continuously and slowly introduced to keep the height of the pulp within a range within which the pulp will not overflow, and the frothing scraper can also scrape the foam well, and the scraped foam is filtered and dried at 105°C to obtain flake graphite concentrate.

[0126] During the flotation process, natural flake graphite ore was flotated at room temperature. The indicators of the flotation products obtained through continuous expansion tests were: fixed carbon content of 65.21% and recovery rate of 51.37%.

[0127] The graphite concentrate obtained by rough selection was refined in the presence of 450 g / t of water glass as an inhibitor, 175 g / t of kerosene as a collector and 80 g / t of pine alcohol as a foaming agent. After three rounds of refinement, the fixed carbon content in the graphite concentrate increased to 87.92%.

[0128] Example 2

[0129] The XRD test results of fine-grained natural flake graphite produced in a mining area in Henan Province show that the impurities are mainly mica, quartz, feldspar and pyrite. The composition is shown in Table 2.

[0130] Table 2 Composition of natural flake graphite in a mining area in Henan

[0131]

[0132] First, water and compressed air are introduced into the air dissolving tank, and the pressure is increased to 0.3MPa by a booster pump, so that the air is gradually dissolved in the water to form a supersaturated solution containing air;

[0133] The fine-grained natural flake graphite produced in Henan Province is mixed with water at a ratio of 20% of the slurry concentration, and the stirring switch is turned on at a speed of 1400 r / min to mix the slurry evenly to obtain slurry;

[0134] Then, an ultrasonic probe was inserted into the slurry, and the ultrasonic generator was turned on for synchronous ultrasonic treatment. The ultrasonic power was set to 160 W. After stirring at a speed of 1400 rpm for 4 minutes, a pH adjuster was added to adjust the pH of the slurry to 8. After stirring for 3 minutes, an inhibitor, sodium carboxymethyl cellulose, was added at a dosage of 1000 g / t. After stirring for 3 minutes, a collector, diesel, was added at a dosage of 360 g / t. After stirring for 3 minutes, a foaming agent, methyl isobutyl carbinol, was added at a dosage of 150 g / t. The mixture was stirred at a speed of 1400 rpm for 2 minutes.

[0135] Then, the supersaturated solution containing air prepared above is slowly released into the flotation tank through the pressure reducing valve. Then, the pressure is reduced to allow the air dissolved in the water to quickly form nanobubbles, thereby introducing nanobubbles, and stirring at a speed of 1400 rpm for 1 min, then the aeration switch is turned on (at this time, ultrasound is continuously applied and a supersaturated solution containing air is introduced), the air intake rate is controlled to be 40 L / h, and then the frothing is scraped for 6 min, and the frothing is continuously introduced during the frothing process until no foam is scraped, and then the flotation and aeration are terminated. During the frothing process, the supersaturated solution containing air is continuously and slowly introduced to keep the height of the slurry within a range within which the slurry will not overflow, and the frothing scraper can also scrape the foam well, and the scraped foam is filtered and dried at 105°C to obtain flake graphite concentrate.

[0136] During the flotation process, natural flake graphite ore was flotated at room temperature. The indicators of the flotation products obtained through continuous expansion tests were: fixed carbon content of 70.64% and recovery rate of 88.71%.

[0137] The graphite concentrate obtained by rough selection is refined in the presence of 500 g / t of sodium carboxymethyl cellulose, an inhibitor, 180 g / t of diesel, and 75 g / t of methyl isobutyl carbinol, a foaming agent. After four refinements, the fixed carbon content in the graphite concentrate is increased to 94.98%.

[0138] Example 3

[0139] The XRD test results of natural flake graphite produced in a mining area in Heilongjiang show that the impurities are mainly mica and quartz. Its composition is shown in Table 3.

[0140] Table 3 Composition of natural flake graphite in a mining area in Heilongjiang

[0141]

[0142] First, water and compressed air are introduced into the air dissolving tank, and the pressure is increased to 0.5MPa by a booster pump, so that the air is gradually dissolved in the water to form a supersaturated solution containing air;

[0143] The fine-grained natural flake graphite produced in Heilongjiang is mixed with water at a ratio of 12% of the slurry concentration, and a stirring switch is turned on at a speed of 1500 r / min to mix the slurry evenly to obtain slurry;

[0144] Then, an ultrasonic probe was inserted into the slurry, and the ultrasonic generator was turned on for synchronous ultrasonic treatment. The ultrasonic power was set to 150W. After stirring for 4 minutes, a pH adjuster was added to adjust the pH of the slurry to 9. After stirring for 3 minutes, an inhibitor, water glass, was added at a dosage of 1100 g / t. After stirring for 3 minutes, a collector, kerosene, was added at a dosage of 400 g / t. After stirring for 3 minutes, a foaming agent, octanol, was added at a dosage of 180 g / t, and stirred for 2 minutes.

[0145] Then, the supersaturated solution containing air prepared above is slowly released into the flotation tank through the pressure reducing valve. Then, the pressure is reduced to allow the air dissolved in the water to quickly form nanobubbles, thereby introducing nanobubbles. After continuing to stir for 1 minute, the aeration switch is turned on (at this time, ultrasound is continuously applied and a supersaturated solution containing air is introduced), the air intake rate is controlled to be 80L / h, and then the frothing is scraped for 6 minutes. During the frothing process, the frothing is continuously introduced until no foam is scraped, and the flotation and aeration are terminated. During the frothing process, the supersaturated solution containing air is continuously and slowly introduced to keep the height of the pulp within a range within which the pulp will not overflow, and the frothing scraper can also scrape the foam well. The scraped foam is filtered and dried at 105°C to obtain flake graphite concentrate.

[0146] During the flotation process, natural flake graphite ore was flotated at room temperature. The indicators of the flotation products obtained through continuous expansion tests were: fixed carbon content of 70.98% and recovery rate of 90.26%.

[0147] The graphite concentrate obtained by rough selection was refined in the presence of 550 g / t of water glass as an inhibitor, 200 g / t of kerosene as a collector and 90 g / t of octanol as a foaming agent. After three rounds of refinement, the fixed carbon content in the graphite concentrate increased to 93.72%.

[0148] Comparative Example 1

[0149] The other conditions are the same as those in the roughing process of Example 1, except that no ultrasonic treatment is performed; that is:

[0150] First, water and compressed air are introduced into the air dissolving tank, and the pressure is increased to 0.4MPa by a booster pump, so that the air is gradually dissolved in the water to form a supersaturated solution containing air;

[0151] The fine-grained natural flake graphite produced in Xinjiang is mixed with water at a ratio of 15% of the slurry concentration, and the stirring switch is turned on, and the speed is 1600r / min (the stirring speed is 1600r / min below) to mix the slurry evenly to obtain slurry;

[0152] After stirring for 4 minutes, add pH adjuster to adjust the pH of the pulp to 8, stir for 3 minutes, add inhibitor water glass at a dosage of 900g / t, stir for 3 minutes, add collector kerosene at a dosage of 350g / t, stir for 3 minutes, add foaming agent pine oil at a dosage of 160g / t, and stir for 2 minutes;

[0153] Then, the prepared water containing air is slowly released into the flotation tank through a pressure reducing valve. Then, the pressure is reduced to allow the air dissolved in the water to quickly form nanobubbles, thereby introducing nanobubbles. After stirring for 1 minute, the aeration switch is turned on, and then the foam is scraped for 5 minutes. The scraped foam is filtered and dried at 105°C to obtain flake graphite concentrate.

[0154] During the flotation process, natural flake graphite ore was flotated at room temperature. The indicators of the flotation products obtained through continuous expansion tests were: fixed carbon content of 57.04% and recovery rate of 43.27%.

[0155] Comparative Example 2

[0156] The other conditions are the same as those in the roughing process of Example 1, except that nanobubbles are not introduced; that is:

[0157] The fine-grained natural flake graphite produced in Xinjiang is mixed with water at a ratio of 15% of the slurry concentration, and the stirring switch is turned on, and the speed is 1600r / min (the stirring speed is 1600r / min below) to mix the slurry evenly to obtain slurry;

[0158] Then, an ultrasonic probe was inserted into the slurry, and the ultrasonic generator was turned on for synchronous ultrasonic treatment. The ultrasonic power was set to 150 W. After stirring for 4 minutes, a pH adjuster was added to adjust the pH of the slurry to 8. After stirring for 3 minutes, an inhibitor, water glass, was added in an amount of 900 g / t. After stirring for 3 minutes, a collector, kerosene, was added in an amount of 350 g / t. After stirring for 3 minutes, a foaming agent, pine alcohol oil, was added in an amount of 160 g / t. After stirring for 3 minutes, the aeration switch was turned on, and then the foam was scraped for 5 minutes. The scraped foam was filtered and dried at 105° C. to obtain flake graphite concentrate.

[0159] During the flotation process, natural flake graphite ore was flotated at room temperature. The indicators of the flotation products obtained through continuous expansion tests were: fixed carbon content of 60.29% and recovery rate of 62.83%.

[0160] Comparative Example 3

[0161] The other conditions are the same as those in the roughing process of Example 1, except that no synchronous ultrasonic treatment is performed and no nanobubbles are introduced; that is:

[0162] The fine-grained natural flake graphite produced in Xinjiang is mixed with water at a ratio of 15% of the slurry concentration, and the stirring switch is turned on, and the speed is 1600r / min (the stirring speed is 1600r / min below) to mix the slurry evenly to obtain slurry;

[0163] After stirring for 4 minutes, a pH adjuster was added to adjust the pH of the slurry to 8. After stirring for 3 minutes, 900 g / t of water glass as an inhibitor was added. After stirring for 3 minutes, 350 g / t of kerosene as a collector was added. After stirring for 3 minutes, 160 g / t of pine oil as a foaming agent was added. After stirring for 3 minutes, the aeration switch was turned on, and then the foam was scraped for 5 minutes. The scraped foam was filtered and dried at 105°C to obtain flake graphite concentrate.

[0164] During the flotation process, natural flake graphite ore was flotated at room temperature. The indicators of the flotation products obtained through continuous expansion tests were: fixed carbon content of 49.77% and recovery rate of 29.96%.

[0165] Comparative Example 4

[0166] The other conditions are consistent with the roughing process in Example 2, except that when nanobubbles are generated, the booster pump pressure is not within the protection range of 0.3-0.5 MPa of the present invention, that is:

[0167] First, water and compressed air are introduced into the air dissolving tank, and the pressure is increased to 0.7MPa by a booster pump, so that the air is gradually dissolved in the water to form a supersaturated solution;

[0168] The fine-grained natural flake graphite produced in Xinjiang is mixed with water at a ratio of 15% of the slurry concentration, and the stirring switch is turned on, and the speed is 1600r / min (the stirring speed is 1600r / min below) to mix the slurry evenly to obtain slurry;

[0169] Then, an ultrasonic probe was inserted into the slurry, and the ultrasonic generator was turned on for synchronous ultrasonic treatment. The ultrasonic power was set to 150W. After stirring for 4 minutes, a pH adjuster was added to adjust the pH of the slurry to 8. After stirring for 3 minutes, an inhibitor, water glass, was added at a dosage of 900 g / t. After stirring for 3 minutes, a collector, kerosene, was added at a dosage of 350 g / t. After stirring for 3 minutes, a foaming agent, pine alcohol, was added at a dosage of 160 g / t, and stirred for 2 minutes.

[0170] Then, the prepared water containing air is slowly released into the flotation tank through a pressure reducing valve. Then, the pressure is reduced to allow the air dissolved in the water to quickly form nanobubbles, thereby introducing nanobubbles. After stirring for 1 minute, the aeration switch is turned on, and then the foam is scraped for 5 minutes. The scraped foam is filtered and dried at 105°C to obtain flake graphite concentrate.

[0171] During the flotation process, natural flake graphite ore was flotated at room temperature. The indicators of the flotation products obtained through continuous expansion tests were: fixed carbon content of 65.09% and recovery rate of 83.71%.

Claims

1. A method for purifying fine-grained flake graphite ore by nanobubble combined with synchronous ultrasonic flotation, characterized in that: The following steps are involved: (1) adding fine flake graphite with a fixed carbon content of 30% or less into a flotation tank and mixing with water at a ratio of 8wt.% to 20wt.% of the ore pulp concentration, turning on a stirring switch to mix the ore pulp evenly, and preparing ore pulp; (2) inserting an ultrasonic probe into the slurry of step (1), turning on an ultrasonic generator for synchronous ultrasonic treatment, and stirring for 3 to 5 minutes; (3) adding a pH adjuster to the above slurry to adjust the pH of the slurry to 7-10, and stirring for 2-5 minutes; (4) adding an inhibitor in an amount of 700 to 1200 g / t, preferably 800 to 1000 g / t, to the pH-adjusted slurry and stirring for 2 to 5 minutes; (5) adding a collector to the slurry to which the inhibitor has been added at a dosage of 260 to 420 g / t, preferably 280 to 380 g / t, and more preferably 340 to 360 g / t, and stirring for 2 to 5 minutes; (6) Adding a foaming agent in an amount of 150-320 g / t or 150-180 g / t to the slurry to which the collector has been added, and stirring for 1-3 minutes; (7) introducing a supersaturated aqueous solution containing air formed by a pressure gas solution method into the slurry to which a foaming agent is added, and forming nanobubbles in the slurry; when the supersaturated aqueous solution containing air is formed, the pressure of the gas passing through is 0.3 to 0.5 MPa, preferably 0.35 to 0.45 MPa, and more preferably 0.38 to 0.42 MPa; (8) Under ultrasonic conditions, a supersaturated aqueous solution containing air is introduced while air is filled to scrape and foam for 4 to 7 minutes. The foam scraped out is filtered and dried to obtain flake graphite concentrate, and the rest is tailings; the amount of air filled is 40 to 80 L / h.

2. The method for purifying fine-grained flake graphite ore by nanobubble combined with synchronous ultrasonic flotation according to claim 1, characterized in that: The fixed carbon content in the micro-grained flake graphite is less than or equal to 20%.

3. The method for purifying fine-grained flake graphite ore by nanobubble combined with synchronous ultrasonic flotation according to claim 1, characterized in that: The particle size of the micro-grained flake graphite is -300 mesh, accounting for more than 80%.

4. The method for purifying fine-grained flake graphite ore by nanobubble combined with synchronous ultrasonic flotation according to claim 1, characterized in that: The stirring process is carried out by using a flotation machine impeller, and the rotation speed is 1200-1900 r / min, preferably 1500-1700 r / min.

5. The method for purifying fine-grained flake graphite ore by nanobubble combined with synchronous ultrasonic flotation according to claim 1, characterized in that: The frequency of the ultrasound used is 18-25 KHz, preferably 20 KHz, and the power is set to 80-200 W, preferably 135-165 W.

6. The method for purifying fine-grained flake graphite ore by nanobubble combined with synchronous ultrasonic flotation according to claim 1, characterized in that: The pH adjusters used are HCl and NaOH. The pH of the slurry is controlled to be 7 to 10, preferably 7.5 to 8.

5.

7. The method for purifying fine-grained flake graphite ore by nanobubble combined with synchronous ultrasonic flotation according to claim 1, characterized in that: The inhibitor used is one of water glass, sodium hexametaphosphate and sodium carboxymethyl cellulose, preferably water glass or a mixture of water glass and at least one of sodium hexametaphosphate and sodium carboxymethyl cellulose.

8. The method for purifying fine-grained flake graphite ore by nanobubble combined with synchronous ultrasonic flotation according to claim 1, characterized in that: The collector used is one of kerosene, diesel and liquid paraffin; The foaming agent used is one of pine oil, sec-octanol and methyl isobutyl carbinol.

9. The method for purifying fine-grained flake graphite ore by nanobubble combined with synchronous ultrasonic flotation according to claim 1, characterized in that: The preparation method of the supersaturated aqueous solution containing air formed by the pressure gas dissolution method is as follows: first, water and compressed air are introduced into a gas dissolution tank, and the pressure is increased to 0.3-0.5 MPa, preferably 0.35-0.45 MPa, and more preferably 0.38-0.42 MPa by a booster pump.

10. The method for purifying fine-grained flake graphite ore by nanobubble combined with synchronous ultrasonic flotation according to claim 1, characterized in that: The fixed carbon content of the graphite concentrate obtained by roughing can reach 70-73%, and the recovery rate is greater than or equal to 88%. After at least 2 times of fine cleaning, the fixed carbon content of the graphite concentrate obtained by roughing is greater than or equal to 93%; The reagent system for selecting the graphite concentrate obtained from roughing is: inhibitor 440-560g / t, collector 175-205g / t, frother 70-95g / t.

Citation Information

Patent Citations

  • Short process purification method of graphite

    CN109647630A

  • Micro-fine particle nano-bubble flotation method and system

    CN110479501A

  • Method for recovering graphite from waste cathode through ultrasonic-assisted flotation

    CN117259021A

  • AU2020104144A4

Cited By

  • Pressure reduction-ultrasonic annular industrial flotation column and flotation method

    CN120001534A

  • A reduced pressure-ultrasonic annular industrial flotation column and a flotation method

    CN120001534B

  • Laboratory dissolved gas-ultrasonic flotation column device and method

    CN120023027A

  • A laboratory dissolved air-ultrasonic flotation column apparatus and method

    CN120023027B

  • Flotation machine foam layer parameter detection method and system and flotation machine