Indium antimonide crystal growth method
By using a mixed atmosphere of ammonia and hydrogen during the growth of indium antimonide single crystals, the problem of oxide scum is solved, single crystal growth and performance improvement is achieved, and the scum removal process is simplified.
Patent Information
- Application Number
- CN202410959239.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-17
- Publication Date
- 2024-11-01
AI Technical Summary
During the growth of indium antimonide single crystals, the presence of oxide scum makes it difficult to control crystal growth, affecting heat dissipation efficiency and material performance. The prior art scum removal methods are complex and have limited effects.
By using a mixed atmosphere of ammonia and hydrogen at high temperature, ammonia reacts with oxide scum on the melt surface to generate indium nitride and water vapor, avoiding the generation of scum and dissolving in indium antimonide melt, simplifying floating Slag removal process.
It effectively avoids the generation of oxide scum, ensures the single crystal growth of indium antimonide crystals, improves the mechanical, chemical and electrical properties of the material, and simplifies the growth process.
Smart Images

Figure CN118880458A_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to the field of indium antimonide crystals, and more specifically to a method for growing indium antimonide crystals. Background Art
[0002] Indium antimonide (InSb) is a narrow-bandgap III-V semiconductor material with extremely high electron mobility in the 3-5μm band. It is one of the best materials for making medium-wave infrared detectors.
[0003] At present, the preparation of indium antimonide single crystals mainly adopts the direct pulling method. In the process of growing indium antimonide crystals by direct pulling method, no liquid sealant is required, but the oxide scum on the surface of the melt will have an adverse effect on the state of the melt surface: on the one hand, due to the presence of a large number of surface impurities, the crystal growth process will be difficult to control, and the impurities will adhere to the surface of the solidified crystal, affecting the heat dissipation efficiency of the crystal. This will cause changes in the local temperature gradient, thereby affecting the change in the shape of the solid-liquid interface. In addition, surface impurities enriched on the solid-liquid interface may become heterogeneous growth points, thereby producing twins or miscellaneous crystals. On the other hand, carbon and oxygen atoms can also enter the InSb melt, enter the InSb single crystal through segregation in the upper boundary layer of the growth interface, and even form secondary defects in subsequent device processes. These will affect the mechanical, chemical and electrical properties of materials or devices. Therefore, reducing the generation of oxide scum on the surface of the melt is conducive to the control of the growth process of indium antimonide single crystals, and is a practical factor that must be considered to obtain high-quality single crystals.
[0004] When pulling indium antimonide crystals, a reducing atmosphere containing hydrogen is usually used as a protective gas during growth to reduce the formation of scum on the surface of the solution. However, experiments have found that hydrogen cannot remove surface scum and has limited help in crystal growth. CN109778305A provides a scum impurity pretreatment device, but the device has a complex structure and affects practical use. Therefore, it is necessary to design a new indium antimonide crystal growth method. Summary of the invention
[0005] In view of the problems existing in the background technology, an object of the present disclosure is to provide a method for growing indium antimonide crystals, which can avoid the generation of oxide scum.
[0006] Another object of the present disclosure is to provide a method for growing indium antimonide crystals, which adopts a simple method to avoid the generation of oxide scum.
[0007] Another object of the present disclosure is to provide a method for growing an indium antimonide crystal, which can make the indium antimonide crystal grown by the Czochralski method a single crystal.
[0008] Thus, an indium antimonide crystal growth method includes the following steps: S1, loading, loading InSb polycrystalline material into a crucible, wherein the purity of the InSb polycrystalline material is above 7.5N; S2, evacuating, removing gas, and leak checking a Czochralski crystal growth device to achieve a vacuum in the Czochralski crystal growth device; S3, introducing hydrogen into the Czochralski crystal growth device to maintain a pressure of 0.1 MPa in the Czochralski crystal growth device; S4, heating the crucible by heating the material. , heating to melt the InSb polycrystalline material in the crucible; S5, after the InSb polycrystalline material is completely melted to form a melt, raising the temperature to 600-800°C, switching to introduce ammonia and hydrogen mixed gas, the volume ratio of ammonia in the mixed gas is 5-20%, the purity of ammonia and hydrogen is above 5N, and keeping warm for 10-20h, then introducing hydrogen to drive out the gas, and maintaining the hydrogen atmosphere, and lowering the temperature to 525°C; S6, after completing step S5, growing crystals by the Czochralski method.
[0009] The beneficial effects of the present disclosure are as follows.
[0010] In the indium antimonide crystal growth method according to the present disclosure, in step S5, after the InSb polycrystalline material is completely melted to form a melt, the temperature is raised and a mixture of ammonia and hydrogen is switched to be introduced and then kept warm. Ammonia reacts with indium oxide in the oxide scum on the surface of the melt at high temperature to generate indium nitride and water vapor. The water vapor is carried away from the melt surface by the air flow. Indium nitride can be well dissolved in the indium antimonide melt without generating scum, thereby avoiding the generation of scum. In addition, a small amount of nitrogen in indium antimonide will not affect the electrical properties and use of the crystal. In addition, the method of avoiding the generation of oxide scum by step S5 is simple.
[0011] In the InSb crystal growth method according to the present disclosure, through step S5, the InSb crystal grown by the Czochralski method is a single crystal (ie, without twin lines). BRIEF DESCRIPTION OF THE DRAWINGS
[0012] Figure 1 is a schematic diagram of an exemplary Czochralski crystal growth device used in the indium antimonide crystal growth method according to the present disclosure.
[0013] Figure 2 This is a photograph of the crystal rod of Example 1.
[0014] Figure 3 This is a photograph of the crystal rod of Comparative Example 1.
[0015] Figure 4 This is a photograph of the crystal rod of Comparative Example 2. DETAILED DESCRIPTION
[0016] It will be understood that the disclosed embodiments are merely examples of the present disclosure, which may be implemented in various forms, and therefore, the specific details disclosed herein should not be interpreted as limiting, but merely as a basis for the claims and as a representative basis for teaching one of ordinary skill in the art to implement the present disclosure in various ways.
[0017] [Indium Antimonide Crystal Growth Method]
[0018] Reference Figure 1 According to the present disclosure, the indium antimonide crystal growth method comprises the steps of:
[0019] S1, loading, loading InSb polycrystalline material into a crucible, the purity of the InSb polycrystalline material being above 7.5N;
[0020] S2, evacuating the CZC crystal growth device, removing air, and checking for leaks, so that the CZC crystal growth device reaches a vacuum;
[0021] S3, introducing hydrogen into the CZC crystal growth device to maintain the pressure in the CZC crystal growth device at 0.1 MPa;
[0022] S4, melting the material, turning on the heating of the crucible to increase the temperature and melt the InSb polycrystalline material in the crucible;
[0023] S5, after the InSb polycrystalline material is completely melted to form a melt, the temperature is raised to 600-800°C, and a mixture of ammonia and hydrogen is introduced, wherein the volume ratio of ammonia in the mixture is 5-20%, and the purity of ammonia and hydrogen is above 5N, and the mixture is kept warm for 10-20 hours, and then hydrogen is introduced to drive out the gas, and the hydrogen atmosphere is maintained, and the temperature is lowered to 525°C;
[0024] S6, after step S5 is completed, growing crystals by the Czochralski method.
[0025] In the indium antimonide crystal growth method according to the present disclosure, in step S5, after the InSb polycrystalline material is completely melted to form a melt, the temperature is raised and a mixture of ammonia and hydrogen is switched to be introduced and then kept warm. Ammonia reacts with indium oxide in the oxide scum on the surface of the melt at high temperature to generate indium nitride and water vapor. The water vapor is carried away from the melt surface by the air flow. Indium nitride can be well dissolved in the indium antimonide melt without generating scum, thereby avoiding the generation of scum. In addition, a small amount of nitrogen in indium antimonide will not affect the electrical properties and use of the crystal. In addition, the method of avoiding the generation of oxide scum by step S5 is simple.
[0026] In the InSb crystal growth method according to the present disclosure, through step S5, the InSb crystal grown by the Czochralski method is a single crystal (ie, without twin lines).
[0027] In one example, in step S1 , the crucible is a quartz crucible.
[0028] In one example, in step S1, the InSb polycrystalline material is a zone melting polycrystalline material, which is cleaned with aqua regia, rinsed with deionized water for more than 3 times, and dried in a vacuum oven for later use.
[0029] In one example, in step S2 , the vacuum pressure achieved is 10 Pa.
[0030] In one example, in step S2, the flushing gas is 7N nitrogen.
[0031] In one example, in step S3, after the pressure in the Czochralski crystal growth apparatus reaches 0.1 MPa, the gas inlet in the Czochralski crystal growth apparatus is closed.
[0032] In one example, in step S4, the heater used for heating includes a graphite heater, a graphite double-layer insulation cover and carbon felt. The graphite heater is arranged around the crucible, the graphite double-layer insulation cover is arranged around the graphite heater, and the carbon felt is filled between the inner layer and the outer layer of the graphite double-layer insulation cover. The heater for heating the quartz crucible is the only heating device in the Czochralski crystal growth equipment.
[0033] In one example, in step S5, switching to introduce ammonia and hydrogen mixed gas is: opening the gas inlet in the Czochralski crystal growth equipment, maintaining the vacuum interface to evacuate, the flow rate of the mixed gas is 1-3L / min, the introduction time is 1-2h, and after the introduction time is over, the gas inlet and the vacuum interface are closed, and then insulation is performed.
[0034] In one example, in step S5, hydrogen is introduced to drive out gas while opening the gas inlet in the Czochralski crystal growth equipment and maintaining the vacuum interface closed. The drive out time is 5-7 hours, and the hydrogen atmosphere is maintained in a state where both the gas inlet and the vacuum interface are closed.
[0035] In one example, in step S6, the pulling rod drives the seed crystal to move downward into the crucible and immerse into the melt from the surface, and then the pulling rod pulls the crystal upward to grow the crystal to form a crystal rod. During the crystal growth process, the quartz crucible and the pulling rod maintain opposite rotation speeds, the rotation speed of the crucible is 0.5-1.5 rpm, the rotation speed of the pulling rod is 2-4 rpm, the seed crystal is an indium antimonide single crystal with a purity of 7.5N, and the pulling speed is constant at 5-15 mm / h;
[0036] In one example, in step S7, after the crystal growth is completed, the heating is stopped, the temperature is lowered, and the gas in the Czochralski crystal growth device is replaced with nitrogen. Then, the Czochralski crystal growth device is opened and the crystal rod is cut off from the pulling rod.
[0037] [test]
[0038] Example 1
[0039] Example 1 adopts the following steps:
[0040] S1, loading, loading the dried InSb polycrystalline material into a crucible, the purity of the InSb polycrystalline material is 7.5N, wherein the crucible is a quartz crucible, and the InSb polycrystalline material is a zone melting polycrystalline material, after being cleaned with aqua regia, rinsed with deionized water for more than 3 times, and dried in a vacuum oven for use;
[0041] S2, evacuating, degassing, and leak checking the CZC crystal growth device to achieve vacuum in the CZC crystal growth device, wherein the vacuum pressure is 10Pa, evacuating and degassing the CZC crystal growth device and filling nitrogen into the CZC crystal growth device are alternately performed 2-3 times by a vacuum pump, a vacuum evacuation interface is set at the bottom of the CZC crystal growth device, nitrogen (purity 7N) is used for degassing, and a nitrogen gas inlet is set at the top of the CZC crystal growth device;
[0042] S3, after step S2 is completed, the top cover and the middle tube are locked by corresponding screws, and the middle tube and the base are locked by corresponding screws, then the vacuum interface and the gas inlet are closed, and then hydrogen is introduced into the CZC crystal growth device to maintain the pressure in the CZC crystal growth device at 0.1 MPa (monitored by a pressure gauge), and then the gas inlet is closed;
[0043] S4, chemical material, start heating the crucible, heat up and melt the InSb polycrystalline material in the crucible, wherein the heater used for heating includes a graphite heater, a graphite double-layer insulation cover and carbon felt, the graphite heater is arranged around the crucible, the graphite double-layer insulation cover is arranged around the graphite heater, and the carbon felt is filled between the inner layer and the outer layer of the graphite double-layer insulation cover. The heater for heating the quartz crucible is the only heating device in the Czochralski crystal growth equipment;
[0044] S5, after the InSb polycrystalline material is completely melted to form a melt, the temperature is raised to 600-800°C, the gas inlet in the Czochralski crystal growth equipment is opened, the vacuum interface is maintained to be vacuumed, and ammonia and hydrogen mixed gas is switched to be introduced, the volume ratio of ammonia in the mixed gas is 15%, the purity of ammonia and hydrogen is 5N, the flow rate of the mixed gas is 3L / min, and the introduction time is 1h. After the introduction time is over, the gas inlet and the vacuum interface are closed, and then the temperature is kept for 15h, and hydrogen is introduced to drive out the gas while the vacuum interface is kept closed. The drive out time is 6h, and then the gas inlet is closed to maintain the hydrogen atmosphere, and the temperature is lowered to 525°C, wherein the formation of the melt is observed and determined through an observation window (not shown, arranged on the top cover), and the temperature is detected by a thermocouple;
[0045] S6, after step S5 is completed, the crystal is grown by the Czochralski method, the pulling rod drives the seed crystal to move downward into the crucible, immerse into the melt from the surface, and then the pulling rod is pulled upward to grow the crystal to form a crystal rod. During the crystal growth process, the quartz crucible and the pulling rod maintain opposite rotation speeds, the rotation speed of the crucible is 1 rpm, the rotation speed of the pulling rod is 3 rpm, the seed crystal is an indium antimonide single crystal with a purity of 7.5N, and the pulling speed is constant at 10 mm / h;
[0046] S7, after the crystal growth is completed, the heating and cooling are stopped, the gas in the Czochralski crystal growth equipment is replaced with nitrogen, the Czochralski crystal growth equipment is opened, and the crystal rod is cut off from the crystal pulling rod.
[0047] Comparative Example 1
[0048] Except that the volume proportion of ammonia in the mixed gas in step S5 is 4%, the rest is the same as in Example 1.
[0049] Comparative Example 2
[0050] Except that the heating, switching to introduce ammonia and nitrogen mixed gas, heat preservation, and introducing hydrogen to reduce the temperature in step S5 are not performed (that is, step 5 is changed to "InSb polycrystalline material is completely melted to form a melt"), the rest is the same as Example 1.
[0051] Figure 2 This is a photograph of the crystal rod of Example 1. Figure 3 This is a photograph of the crystal rod of Comparative Example 1. Figure 4 This is a photograph of the crystal rod of Comparative Example 2.
[0052] from Figure 2 It can be seen that the entire surface of the crystal rod is bright, with no matte area (which means no oxide is attached), no oxide scum particles, and no twin lines (which means a single crystal is obtained).
[0053] from Figure 3 It can be seen that there are scattered oxide scum particles, aggregated oxide scum particles, and concentrated matte areas (i.e., the matte areas indicate the presence of oxide attachment) on the surface of the crystal rod, but no twin lines.
[0054] from Figure 4 It can be seen that there are scattered oxide scum particles, concentrated matte areas, scattered matte areas, and twin lines on the surface of the crystal rod, wherein the twin lines are marked with a fluorescent pen after the crystal rod is taken out of the Czochralski crystal growth device.
[0055] The above detailed description is used to describe multiple exemplary embodiments, but this document is not intended to be limited to the explicitly disclosed combinations. Therefore, unless otherwise stated, the various features disclosed herein can be combined together to form multiple additional combinations that are not shown for the sake of simplicity.
Claims
1. A method for growing indium antimonide crystals, It is characterized in that Includes steps: S1, loading, loading InSb polycrystalline material into a crucible, the purity of the InSb polycrystalline material being above 7.5N; S2, evacuating the CZC crystal growth device, removing air, and checking for leaks, so that the CZC crystal growth device reaches a vacuum; S3, introducing hydrogen into the CZC crystal growth device to maintain the pressure in the CZC crystal growth device at 0.1 MPa; S4, melting the material, turning on the heating of the crucible to increase the temperature and melt the InSb polycrystalline material in the crucible; S5, after the InSb polycrystalline material is completely melted to form a melt, the temperature is raised to 600-800°C, and a mixture of ammonia and hydrogen is introduced, wherein the volume ratio of ammonia in the mixture is 5-20%, and the purity of ammonia and hydrogen is above 5N, and the mixture is kept warm for 10-20 hours, and then hydrogen is introduced to drive out the gas, and the hydrogen atmosphere is maintained, and the temperature is lowered to 525°C; S6, after step S5 is completed, growing crystals by the Czochralski method.
2. The indium antimonide crystal growth method according to claim 1, It is characterized in that In step S1 , the crucible is a quartz crucible.
3. The indium antimonide crystal growth method according to claim 1, It is characterized in that In step S1, the InSb polycrystalline material is a zone melting polycrystalline material, which is cleaned with aqua regia, rinsed with deionized water for more than 3 times, and dried in a vacuum oven for later use.
4. The indium antimonide crystal growth method according to claim 1, It is characterized in that In step S2, the vacuum pressure reached is 10Pa.
5. The indium antimonide crystal growth method according to claim 1, It is characterized in that In step S2, nitrogen gas with a concentration of 7N is used as the flushing gas.
6. The indium antimonide crystal growth method according to claim 1, It is characterized in that In step S3 , after the pressure in the CZC crystal growth apparatus reaches 0.1 MPa, the gas inlet in the CZC crystal growth apparatus is closed.
7. The indium antimonide crystal growth method according to claim 1, It is characterized in that In step S4, the heater used for heating includes a graphite heater, a graphite double-layer insulation cover and carbon felt. The graphite heater is arranged around the crucible, the graphite double-layer insulation cover is arranged around the graphite heater, and the carbon felt is filled between the inner layer and the outer layer of the graphite double-layer insulation cover. The heater for heating the quartz crucible is the only heating device in the Czochralski crystal growth equipment.
8. The indium antimonide crystal growth method according to claim 1, It is characterized in that In step S5, Switching to introduce ammonia and hydrogen mixed gas is as follows: opening the gas inlet in the Czochralski crystal growth device, maintaining the vacuum interface to evacuate, the flow rate of the mixed gas is 1-3L / min, and the introduction time is 1-2h; after the introduction time is over, closing the gas inlet and the vacuum interface, and then keeping warm; The hydrogen gas is introduced to drive out the gas while opening the gas inlet in the Czochralski crystal growth equipment and keeping the vacuum interface closed. The driving time is 5-7 hours, and the hydrogen atmosphere is maintained in a state where both the gas inlet and the vacuum interface are closed.
9. The indium antimonide crystal growth method according to claim 1, It is characterized in that In step S6, the pulling rod drives the seed crystal to move downward into the crucible and immerse into the melt from the surface. Then, the pulling rod pulls the crystal upward to grow the crystal to form a crystal rod. During the crystal growth process, the quartz crucible and the pulling rod maintain opposite rotation speeds. The rotation speed of the crucible is 0.5-1.5rpm, and the rotation speed of the pulling rod is 2-4rpm. The seed crystal is an indium antimonide single crystal with a purity of 7.5N, and the pulling speed is constant at 5-15mm / h.
10. The indium antimonide crystal growth method according to claim 9, It is characterized in that Also includes the steps: S7, after the crystal growth is completed, the heating and cooling are stopped, the gas in the Czochralski crystal growth equipment is replaced with nitrogen, the Czochralski crystal growth equipment is opened, and the crystal rod is cut off from the crystal pulling rod.