Radiation-resistant, high-temperature-resistant and high-emissivity protective coating and preparation method thereof

By using acrylic-modified silicone resin and specific fillers in the coating, a radiation-resistant and high-temperature-resistant protective coating is prepared, which solves the problem of easy cracking and peeling of the coating under high radiation and high temperature environment, and achieves effective protection and temperature reduction of the device. It is suitable for aerospace devices and nuclear reactor equipment.

CN118931382AInactive Publication Date: 2024-11-12NORTHEASTERN UNIV CHINA +1

Patent Information

Application Number
CN202411335616.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-24
Publication Date
2024-11-12
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing coatings are prone to cracking and peeling under high radiation and high temperature environments, failing to effectively protect devices and leading to device damage.

Method used

Using acrylic-modified silicone resin as the matrix, combined with specific fillers and enamel, a radiation-resistant and high-temperature-resistant protective coating is formed. The coating is prepared by ball milling and mixing polyurethane resin, with a coating thickness of 50-120 μm.

Benefits of technology

The coating exhibits excellent stability under nuclear radiation and high temperature environments, reduces device surface temperature, and extends service life, making it suitable for aerospace devices and nuclear reactor equipment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0005058157790000011
    Figure HDA0005058157790000011
  • Figure HDA0005058157790000012
    Figure HDA0005058157790000012
Patent Text Reader

Abstract

The invention provides a radiation-resistant, high-temperature-resistant and high-emissivity protective coating and a preparation method thereof, and belongs to the technical field of material engineering. Comprising 20-30 parts of acrylic acid modified organic silicon resin, 15-20 parts of polyurethane resin, pigment and filler and 2-11 parts of enamel. The pigment filler is prepared from 1 to 3 parts of Ta, 1 to 3 parts of V, 5 to 8 parts of copper chromite black, 5 to 7.5 parts of iron manganese black, 10 to 13 parts of B4C and 1 to 3 parts of Ta2O5; the preparation method comprises the following steps: ball-milling and mixing the acrylic modified organic silicon resin, the pigment filler, the enamel and the diluent, uniformly mixing, adding the polyurethane resin, and uniformly dispersing to obtain the coating. The protective coating prepared by the invention has an excellent protective effect in nuclear radiation and high-temperature environments, and can effectively resist nuclear radiation and improve the heat dissipation rate, so that the surface temperature of a device is reduced, the surface temperature of the device is not increased, and the device is effectively protected.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of material engineering, and in particular relates to a radiation-resistant, high-temperature-resistant and high-emissivity protective coating and a preparation method thereof. Background Art

[0002] In some special environments, such as space, nuclear radiation areas, or high temperature and high radiation environments, devices operating in such environments are easily damaged due to long-term exposure to strong radiation and high temperature. Based on this, in order to protect these devices, coatings are often applied on their surfaces to reduce the impact of strong radiation and high temperature factors.

[0003] However, because the coating is itself in a high-irradiation, high-temperature environment while protecting the device, if the coating itself has limited resistance to high temperature or radiation, its surface will easily crack and fall off during long-term use, making it difficult to effectively protect the devices inside. Summary of the invention

[0004] The purpose of the present invention is to provide a radiation-resistant, high-temperature-resistant and high-emissivity protective coating and a preparation method thereof, which can effectively isolate nuclear radiation and reduce the surface temperature of the device, thereby reducing the degree to which the device is affected by high radiation and high temperature factors, and effectively prolonging the service life of the device.

[0005] The present invention is achieved through the following technical solutions:

[0006] A radiation-resistant, high-temperature-resistant and high-emissivity protective coating, comprising the following components in parts by weight:

[0007] 20-30 parts of acrylic modified silicone resin, 15-20 parts of polyurethane resin, pigments and fillers, and 2-11 parts of enamel;

[0008] The pigment filler comprises 1-3 parts of Ta, 1-3 parts of V, 5-8 parts of copper chrome black, 5-7.5 parts of iron manganese black, 10-13 parts of B4C and 1-3 parts of Ta2O5.

[0009] As some possible implementation methods of the present application, the protective coating comprises the following components in parts by weight:

[0010] 22-28 parts of acrylic modified silicone resin, 16-19 parts of polyurethane resin, pigments and fillers, and 6-10 parts of enamel;

[0011] The pigment filler comprises 1.2-2.5 parts of Ta, 1.2-2.5 parts of V, 5.5-7.5 parts of copper chrome black, 5.5-7 parts of iron manganese black, 10.5-12 parts of B4C and 1.5-2.8 parts of Ta2O5.

[0012] As some possible implementation methods of the present application, the protective coating comprises the following components in parts by weight:

[0013] 26 parts of acrylic modified silicone resin, 18 parts of polyurethane resin, pigments and fillers, and 10 parts of enamel;

[0014] The pigment filler includes 2.2 parts of Ta, 2 parts of V, 6 parts of copper chrome black, 6 parts of iron manganese black, 12 parts of B4C and 2 parts of Ta2O5.

[0015] As some possible implementation modes of the present application, the enamel includes glass powders with multiple different melting points.

[0016] As some possible implementation methods of the present application, the glass powder includes SiO2-B2O3-Al2O3-CaF2-R2O (R is Na or K), SiO2-8B2O3-2.5Li2O-15Al2O3-3Na2O-15CaO-7CaF2 and SiO2-10Al2O3-6B2O3-6Na2O-6K2O-6SrO2.

[0017] As some possible implementation methods of the present application, the protective coating further includes one or more of a defoaming agent, a leveling agent and a dispersant.

[0018] As some possible implementation methods of the present application, the coating has a coating thickness of 50 to 120 μm.

[0019] In addition, to achieve the above purpose, the present invention also provides a method for preparing a radiation-resistant, high-temperature-resistant and high-emissivity protective coating, wherein the acrylic modified silicone resin, pigments, fillers, enamel and diluent are ball-milled and mixed, and after being evenly mixed, polyurethane resin is added and evenly dispersed to obtain the coating.

[0020] Compared with the prior art, the present invention has the following beneficial effects:

[0021] The present invention adopts acrylic modified silicone resin as a matrix, and after adding special fillers and enamel, a protective coating with radiation resistance, high temperature resistance and high emissivity is obtained. The coating has excellent protective effects under nuclear radiation and high temperature environments, can effectively resist nuclear radiation, increase the heat dissipation rate, and thus reduce the surface temperature of the device, so that the surface of the device does not heat up, and effectively protects the device. The coating can be widely used in the outer surface of aerospace / spacecraft, equipment in 3-4 generation advanced sodium-cooled reactors, or the surface of a certain type of hot end component.

[0022] Specifically, the performance indicators of the protective coating in the present invention are as follows:

[0023] Protective coating at 1.7×10 5 At irradiation doses above Gy, the coating does not powder or peel off;

[0024] The protective coating can withstand temperatures of 600-700°C for more than 1000-200 hours, which refers to ultra-high temperature accelerated oxidation behavior. If it is used in actual devices, it can last for more than 3 months to 1 year.

[0025] After the protective coating is applied, the surface temperature of the substrate of the coated sample decreases by about 10% at a high temperature of 600-700°C; in the 9-12μm frequency band, the emissivity at 50°C is ≥0.90, and the emissivity at 650°C is ≥0.85. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 : The surface and cross-sectional morphology of the coating as prepared in Example 3; wherein, Figure 1 (a) is the surface image of the coating as prepared; Figure 1 (b) is the cross-sectional morphology of the coating;

[0027] Figure 2 : The surface and cross-sectional morphology of the coating in Example 3 after high-temperature oxidation at 650°C for 1500h; wherein, Figure 2 (a) is the surface image of the coating as prepared; Figure 2 (b) is the cross-sectional morphology of the coating. DETAILED DESCRIPTION

[0028] In the prior art, coatings used in some special environments, such as space, nuclear radiation areas, or high-temperature and high-radiation environments, are very likely to cause cracking and peeling on the coating surface due to being exposed to high radiation and high temperature for a long time, which makes it difficult for the devices inside to be effectively protected.

[0029] Based on this, the present invention provides a radiation-resistant, high-temperature-resistant and high-emissivity protective coating, comprising the following components in parts by weight:

[0030] 20-30 parts of acrylic modified silicone resin, 15-20 parts of polyurethane resin, pigments and fillers, and 2-11 parts of enamel;

[0031] The pigment filler comprises 1-3 parts of Ta, 1-3 parts of V, 5-8 parts of copper chrome black, 5-7.5 parts of iron manganese black, 10-13 parts of B4C and 1-3 parts of Ta2O5.

[0032] In the above scheme, acrylic modified silicone resin is used as the matrix of the protective coating, which has excellent heat resistance, weather resistance, acid and alkali resistance, corrosion resistance and strong adhesion. On the basis of the matrix, fillers and enamel are added to form a special nuclear radiation resistance skeleton inside the protective coating, which shows excellent stability in the nuclear radiation environment, while improving the heat dissipation rate, so that the surface temperature / emissivity index does not decrease for a long time. Specifically, oxides such as copper chromium black and iron manganese black have good high-temperature stability and high emissivity. Boron carbide has the characteristics of low density, high strength, high-temperature stability and good chemical stability, and can absorb a large amount of neutrons without forming any radioactive isotopes. Therefore, it is an ideal neutron absorber in nuclear power plants. Enamel can fill the pores in the coating, improve the density of the coating, etc., thereby improving the protective performance of the coating.

[0033] The present invention creates a dual protection mechanism by integrating nuclear radiation resistance components and high emissivity fillers, so that the coating can simultaneously cope with the requirements of nuclear radiation and high-temperature heat dissipation.

[0034] It is worth noting that the emissivity of general coatings can meet higher requirements in the early stage or before being subjected to extreme environments. However, once it is used in high-temperature service, the emissivity will drop rapidly. The present invention can enable the coating to have good high-temperature thermal stability by limiting the filler components. On the other hand, even in the early stage or after the process decomposition, it can still react quickly and produce in situ, and can play a lasting protective role.

[0035] Through the synergistic effect of the above components, the prepared protective coating can integrate radiation resistance, high temperature resistance and high emissivity, which can effectively isolate nuclear radiation and reduce the surface temperature of the device to protect the device.

[0036] Specifically, the performance indicators of the protective coating in the present invention are as follows:

[0037] Protective coating at 1.7×10 5 Gy or above irradiation dose (the nuclear irradiation tests in this application were all completed at 350°C), the coating does not powder or peel off;

[0038] The protective coating can withstand temperatures of 600-700°C for more than 1000-200 hours, which refers to ultra-high temperature accelerated oxidation behavior. If it is used in actual devices, it can last for more than 3 months to 1 year.

[0039] It is worth noting that it is very difficult for traditional organic coatings to break through the temperature limit. The general use temperature is about 120 degrees Celsius. In general, the temperature in a nuclear reactor is about 120 degrees Celsius, that is, traditional organic coatings can barely be used, but in a primary circuit, the general temperature is 300-400 degrees Celsius, and traditional coatings are difficult to apply at this temperature. The organic silicon coating developed by the present invention can increase the use temperature to 600-700 degrees Celsius, which is extremely difficult, and this high temperature environment can be used for some high-temperature hot end components in the nuclear environment, such as heat exchangers and some heat transfer pipelines.

[0040] After the protective coating is applied, the surface temperature of the substrate of the coated sample decreases by about 10% at a high temperature of 600-700°C; in the 9-12μm frequency band, the emissivity at 50°C is ≥0.90; and the emissivity at 650°C is ≥0.85.

[0041] In order to further improve the protective effect of the protective coating, as some possible implementation methods of the present application, the amount of the protective coating is further limited, that is, the protective coating includes the following components in parts by weight:

[0042] 22-28 parts of acrylic modified silicone resin, 16-19 parts of polyurethane resin, pigments and fillers, and 6-10 parts of enamel;

[0043] The pigment filler comprises 1.2-2.5 parts of Ta, 1.2-2.5 parts of V, 5.5-7.5 parts of copper chrome black, 5.5-7 parts of iron manganese black, 10.5-12 parts of B4C and 1.5-2.8 parts of Ta2O5.

[0044] In order to further improve the protective effect of the protective coating, as some possible implementation methods of the present application, the amount of the protective coating is further limited, that is, the protective coating includes the following components in parts by weight:

[0045] 26 parts of acrylic modified silicone resin, 18 parts of polyurethane resin, pigments and fillers, and 10 parts of enamel;

[0046] The pigment filler includes 2.2 parts of Ta, 2 parts of V, 6 parts of copper chrome black, 6 parts of iron manganese black, 12 parts of B4C and 2 parts of Ta2O5.

[0047] In order to further improve the protective effect of the protective coating, as some possible implementation methods of the present application, the components of the enamel are further limited, that is, the enamel includes glass powders with multiple different melting points.

[0048] In this solution, the glass powder in the coating can adjust the thermal expansion coefficient of the coating on the one hand, and can also serve as a secondary binder to repair defects such as cracks and holes caused by the thermal decomposition of organic resins caused by high temperature on the other hand; and in order to adapt the coating to the use environment of different temperatures, glass powders with different melting points need to be selected for adaptation.

[0049] In order to further improve the protective effect of the protective coating, as some feasible embodiments of the present application, the components of the enamel are further limited, that is, the glass powder includes SiO2-B2O3-Al2O3-CaF2-R2O (R is Na or K), SiO2-8B2O3-2.5Li2O-15Al2O3-3Na2O-15CaO-7CaF2 and SiO2-10Al2O3-6B2O3-6Na2O-6K2O-6SrO2.

[0050] In order to further improve the adhesion and density of the coating prepared by the protective coating, as some feasible embodiments of the present application, the components of the protective coating are further limited, that is, the protective coating also includes one or more of a defoamer, a leveling agent and a dispersant, wherein the defoamer, the leveling agent or the dispersant is 0.1-0.3 parts each.

[0051] In order to further improve the protective effect of the protective coating, as some of the embodiments of the present application, the coating thickness of the coating is further limited, that is, the coating thickness of the coating is 50 to 120 μm. If the coating thickness is too small, the radiation resistance, corrosion resistance, high temperature resistance and emissivity will be weakened. If the coating thickness is too thick, it is very easy to crack and peel off, affecting the protective effect.

[0052] The invention prepares the coating by uniformly grinding acrylic modified organic silicon resin, pigments and fillers and enamel with ball mills and then fully mixing with polyurethane resin. The preparation method is simple, fast and low in cost.

[0053] The preparation of the protective coating described in the present application is further described in detail below in conjunction with specific implementation methods.

[0054] Wherein, various raw materials in the examples are commercially available products.

[0055] Example 1

[0056] 28 parts of acrylic modified silicone resin, 1.8 parts of Ta, 3 parts of V, 5 parts of copper chrome black, 6 parts of iron manganese black, 10 parts of B4C and 1.5 parts of Ta2O5, 2 parts of SiO2-B2O3-Al2O3-CaF2-Na2O, 3.5 parts of SiO2-8B2O3-2.5Li2O-15Al2O3-3Na2O-15CaO-7CaF2, 2 parts of SiO2-10Al2O3-6B2O3-6Na2O-6K2O-6SrO 2. 8 parts of enamel (selected from the enamel powder in Example 1 in the patent with application number CN201810069695.7), 11 parts of diluent (xylene), 0.1 parts of leveling agent (BYK-354), 0.2 parts of defoaming agent (BYK-052) and 0.2 parts of wetting agent (Dow Chemical BD-405) are ball-milled and mixed. After mixing evenly, 20 parts of polyurethane resin are added and dispersed at a speed of 1500-2500 rpm for 20-40 minutes to obtain the coating.

[0057] The coating is sprayed, brushed or dipped on a 304 stainless steel surface that has been sandblasted, and cured at 120° C. to obtain a 80 μm protective coating. The protective coating is observed under an electron microscope, and no cracks are found, and the density is greater than 90%.

[0058] The specific properties of the protective coating are as follows:

[0059] 1.7×10 5 After irradiation with γ-rays of 1000 Gy, the coating only oxidized and discolored on the surface, and the coating was intact without any powdering or peeling.

[0060] The coating has no powdering or peeling after continuous high temperature resistance for 1000 hours at 600℃; and no powdering or peeling after continuous high temperature resistance for 200 hours at 700℃.

[0061] At a high temperature of 650℃, the substrate surface temperature drops by 6.5±1℃; in the 9-12μm frequency band, the emissivity at 50℃ is ≥0.90; the emissivity at 650℃ is ≥0.85;

[0062] Mechanical strength: Adhesion strength is 9.8Mpa, impact strength is 30cm, and flexibility is 2rank.

[0063] Example 2

[0064] 25 parts of acrylic modified silicone resin, 2 parts of Ta, 1.8 parts of V, 5.5 parts of copper chrome black, 6 parts of iron manganese black, 10.5 parts of B4C and 2 parts of Ta2O5, 2.5 parts of SiO2-B2O3-Al2O3-CaF2-Na2O, 2.5 parts of SiO2-8B2O3-2.5Li2O-15Al2O3-3Na2O-15CaO-7CaF2, 3.5 parts of SiO2-10Al2O3-6B2O3-6N a2O-6K2O-6SrO2, 8.5 parts of enamel (selected from the enamel powder in Example 1 in the patent with application number CN201810069695.7), 10 parts of diluent (xylene), 0.1 parts of leveling agent (BYK-354), 0.2 parts of defoaming agent (BYK-052) and 0.2 parts of wetting agent (Dow Chemical BD-405) are ball-milled and mixed. After mixing evenly, 18 parts of polyurethane resin are added and dispersed evenly to obtain the coating.

[0065] The coating is sprayed, brushed or dipped on a 304 stainless steel surface that has been sandblasted, and cured at 120° C. to obtain a 80 μm protective coating. The protective coating is observed under an electron microscope, and no cracks are found, and the density is greater than 90%.

[0066] The specific properties of the protective coating are as follows:

[0067] 1.7×10 5 After irradiation with γ-rays of 1000 Gy, the coating only oxidized and discolored on the surface, and the coating was intact without any powdering or peeling.

[0068] The coating has no powdering or peeling after continuous high temperature resistance for 1200h at 600℃ and 230h at 700℃.

[0069] At a high temperature of 650℃, the substrate surface temperature drops by 6.7±1℃; in the 9-12μm frequency band, the emissivity at 50℃ is ≥0.90; the emissivity at 650℃ is ≥0.85;

[0070] Mechanical strength: Adhesion strength is 10.05Mpa, impact strength is 33cm, and flexibility is 2rank.

[0071] Example 3

[0072] 26 parts of acrylic modified silicone resin, 2.2 parts of Ta, 2 parts of V, 6 parts of copper chrome black, 6 parts of iron manganese black, 12 parts of B4C and 2 parts of Ta2O5, 3.5 parts of SiO2-B2O3-Al2O3-CaF2-Na2O, 3.5 parts of SiO2-8B2O3-2.5Li2O-15Al2O3-3Na2O-15CaO-7CaF2, 3 parts of SiO2-10Al2O3-6B2O3-6Na2O -6K2O-6SrO2, 10 parts of enamel (selected from the enamel powder in Example 1 in the patent with application number CN201810069695.7), 11.5 parts of diluent (xylene), 0.1 parts of leveling agent (BYK-354), 0.2 parts of defoaming agent (BYK-052) and 0.2 parts of wetting agent (Dow Chemical BD-405) are ball-milled and mixed. After the mixture is evenly mixed, 18 parts of polyurethane resin are added and the coating is obtained after being evenly dispersed.

[0073] The coating was sprayed, brushed or dipped on the surface of 304 stainless steel treated by surface sandblasting, and cured at 120°C to obtain a 80 μm protective coating. The protective coating was observed under an electron microscope, and its surface and cross-sectional morphology were as follows: Figure 1 As shown, no cracks were found and the density was >90%.

[0074] The specific properties of the protective coating are as follows:

[0075] 1.7×10 5 After irradiation with γ-rays of 1000 Gy, the coating only oxidized and discolored on the surface, and the coating was intact without any powdering or peeling.

[0076] The surface and cross-sectional morphology of the steel sheet can withstand high temperature for 1350 hours at 600°C. Figure 2 As shown (where Figure 1 and Figure 2 Among them, the dark gray ones are resins, some light gray ones are non-metallic fillers and enamels, and the bright white ones are metal fillers). The coating does not show any powdering or peeling. It can withstand high temperatures for 300 hours at 700°C without any powdering or peeling. Figure 1 (a) It can be seen that the original coating surface is dense, the filler is evenly dispersed, and there are no defects such as micro cracks; Figure 2 (a) It can be seen that after high-temperature oxidation, the coating surface is smooth and no cracks or holes are found. Figure 1 (b) and Figure 2 The cross-sectional morphology of (b) shows that the coating is well bonded to the substrate, there is no obvious oxide layer between the substrate and the coating, and the substrate is well protected.

[0077] At a high temperature of 650℃, the substrate surface temperature drops by 7±1.2℃; in the 9-12μm frequency band, the emissivity at 50℃ is ≥0.90; the emissivity at 650℃ is ≥0.85;

[0078] Mechanical strength: Adhesion strength is 9.76Mpa, impact strength is 29cm, and flexibility is 2rank.

[0079] From the performance of the above-mentioned Examples 1-3, it can be seen that the protective coating prepared in the present invention has excellent radiation resistance, high temperature resistance, and emissivity, and also has strong adhesion strength and impact strength.

[0080] Comparative Example 1

[0081] Compared with Example 3, the enamel was removed and the other parameters were the same as Example 3.

[0082] The coating is sprayed, brushed or dipped onto a 304 stainless steel surface that has been sandblasted, and cured at 120° C. to obtain a 80 μm protective coating.

[0083] The specific properties of the protective coating are as follows:

[0084] 1.7×10 5 After irradiation with γ-rays of 100 Gy, the coating surface showed powdering and peeling;

[0085] After continuous high temperature resistance for 850 hours at 600℃, the coating showed powdering and peeling; after continuous high temperature resistance for 150 hours at 700℃, the coating showed powdering and peeling;

[0086] At a high temperature of 650℃, the surface temperature of the substrate drops by 4.5±1℃; in the 9-12μm frequency band, the emissivity at 50℃ is <0.90; the emissivity at 650℃ is <0.85.

[0087] Comparative Example 2

[0088] Compared with Example 3, the metal powder is removed, and the other parameters are the same as Example 3.

[0089] The coating is sprayed, brushed or dipped onto a 304 stainless steel surface that has been sandblasted, and cured at 120° C. to obtain a 80 μm protective coating.

[0090] The specific properties of the protective coating are as follows:

[0091] 1.7×10 5 After irradiation with γ-rays of Gy, the coating showed powdering and peeling;

[0092] After continuous high temperature resistance at 600℃ for 800h, the coating showed powdering and peeling; after continuous high temperature resistance at 700℃ for 150h, the coating showed powdering and peeling.

[0093] Comparative Example 3

[0094] Compared with Example 3, the acrylic modified silicone resin is replaced by epoxy resin, and the other parameters are the same as Example 3.

[0095] The coating is sprayed, brushed or dipped onto a 304 stainless steel surface that has been sandblasted, and cured at 120° C. to obtain a 80 μm protective coating.

[0096] The protective coating cannot be used at 600-700°C; in the 9-12 μm frequency band, the emissivity at 50°C is ≤0.90, and it cannot be used at 650°C.

[0097] Comparative Example 4

[0098] Compared with Example 3, the dosage of each component in the protective coating is changed, and the other parameters are the same as Example 3. The dosage after the change is as follows:

[0099] 26 parts of acrylic modified silicone resin, 1 part of Ta, 2 parts of V, 8 parts of copper chrome black, 6 parts of iron manganese black, 5 parts of B4C and 2 parts of Ta2O5, 6 parts of SiO2-B2O3-Al2O3-CaF2-Na2O, 3.5 parts of SiO2-8B2O3-2.5Li2O-15Al2O3-3Na2O-15CaO-7CaF2 and 3 parts of SiO2-10Al2O3-6B2O3-6Na2O-6K2O-6SrO2.

[0100] The coating is sprayed, brushed or dipped onto a 304 stainless steel surface that has been sandblasted, and cured at 120° C. to obtain a 80 μm protective coating.

[0101] The specific properties of the protective coating are as follows:

[0102] 1.7×10 5 After irradiation with γ-rays of 100 Gy, the coating surface showed powdering and peeling;

[0103] After continuous high temperature resistance at 600℃ for 700h, the coating showed powdering and peeling; after continuous high temperature resistance at 700℃ for 140h, the coating showed powdering and peeling.

[0104] It can be seen from this that in the protective coating of the present invention, the dosage relationship of each component is extremely important. Excessive or insufficient dosage of a single component will affect the overall performance of the protective coating.

Claims

1. A radiation-resistant, high-temperature-resistant and high-emissivity protective coating, It is characterized in that It includes the following components by weight: 20-30 parts of acrylic modified silicone resin, 15-20 parts of polyurethane resin, pigments and fillers, and 2-11 parts of enamel; The pigment and filler include 1-3 parts Ta, 1-3 parts V, 5-8 parts copper chrome black, 5-7.5 parts iron manganese black, 10-13 parts B 4 C and 1-3 parts Ta 2 O 5 .

2. A radiation-resistant, high-temperature-resistant and high-emissivity protective coating according to claim 1, It is characterized in that It includes the following components by weight: 22-28 parts of acrylic modified silicone resin, 16-19 parts of polyurethane resin, pigments and fillers, and 6-10 parts of enamel; The pigment and filler include 1.2-2.5 parts of Ta, 1.2-2.5 parts of V, 5.5-7.5 parts of copper chrome black, 5.5-7 parts of iron manganese black, 10.5-12 parts of B 4 C and 1.5-2.8 parts Ta 2 O 5 .

3. A radiation-resistant, high-temperature-resistant and high-emissivity protective coating according to claim 1, It is characterized in that It includes the following components by weight: 26 parts of acrylic modified silicone resin, 18 parts of polyurethane resin, pigments and fillers, and 10 parts of enamel; The pigments and fillers include 2.2 parts Ta, 2 parts V, 6 parts copper chrome black, 6 parts iron manganese black, 12 parts B 4 C and 2 parts Ta 2 O 5 .

4. A radiation-resistant, high-temperature-resistant and high-emissivity protective coating according to claim 1, It is characterized in that The enamel comprises a plurality of glass powders having different melting points.

5. The radiation-resistant, high-emissivity protective coating according to claim 2, It is characterized in that The glass powder includes SiO 2 -B 2 O 3 -Al 2 O 3 -CaF 2 -R 2 O、SiO 2 -8B 2 O 3 -2.5Li 2 O-15Al 2 O 3 -3Na 2 O-15CaO-7CaF 2 and SiO 2 -10Al 2 O 3 -6B 2 O 3 -6Na 2 O-6K 2 O-6SrO 2 ; Wherein, R is Na or K.

6. A radiation-resistant, high-temperature-resistant and high-emissivity protective coating according to claim 1, It is characterized in that It also includes one or more of a defoamer, a leveling agent and a dispersant.

7. The radiation-resistant, high-temperature-resistant and high-emissivity protective coating according to claim 1, It is characterized in that The coating thickness of the coating is 50 to 120 μm.

8. The method for preparing the radiation-resistant, high-temperature-resistant and high-emissivity protective coating according to any one of claims 1 to 5, It is characterized in that The acrylic modified silicone resin, pigments, fillers, enamel and diluent are ball-milled and mixed, and after being uniformly mixed, polyurethane resin is added and uniformly dispersed to obtain the coating.

Citation Information

Patent Citations

  • Nuclear irradiation-resistant, corrosion-resistant and high-temperature-resistant multifunctional integrated organic silicon coating and preparation method thereof

    CN115160924A

  • Temperature control coating with long service life, temperature resistance and high emissivity and preparation process of temperature control coating

    CN117186729A

Cited By

  • Radiation-resistant, high-temperature-resistant and high-emissivity protective coating as well as preparation method and application thereof

    CN120795793A