Composite filler as well as preparation method and application thereof
By modifying the titanium oxide silicate surface and building a thermal conductivity 3D network, the problem of limited thermal conductivity of two-dimensional graphene is solved, and a high-efficiency thermal conductivity network and high-emissivity composite filler are realized, which improves the heat of the thermally conductive film Conductivity and heat dissipation effect enhance environmental adaptability.
Patent Information
- Application Number
- CN202310661015.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-06-06
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2043-06-06
AI Technical Summary
Existing composite fillers are difficult to achieve both the construction of thermal conductivity networks and high emissivity and environmental adaptability requirements, especially the longitudinal thermal conductivity of two-dimensional graphene is limited, resulting in poor application effects in the field of thermally conductive materials.
By modifying the titanium oxide surface of silicate and using the interaction between silicate and graphene, an isotropic thermal conductivity 3D network is constructed to improve the binding force between graphene and titanium oxide, and prepare A composite filler with high efficiency thermal conductivity network, high emissivity and good environmental adaptability are produced.
The thermal conductivity of the thermal conductivity film is increased to 5.593~6.727W·m-1K-1 and the heat dissipation effect are increased to 18.55~25.03%, which expands the use range of composite fillers and enhances its environmental adaptability.
Smart Images

Figure CN119081465A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of thermal conductive fillers, and in particular relates to a composite filler and a preparation method and application thereof. Background Art
[0002] Titanium suboxide is a polycrystalline inorganic material composed of two valence states of titanium oxide in the magneli phase. It has a stable crystal structure and has excellent properties such as high conductivity, acid resistance, acid resistance and wear resistance. So far, research on titanium suboxide has mainly focused on electrode materials and black pigments. Since the thermal conductivity of titanium suboxide is only 10-20W·m - 1 K -1 Compared with most metal oxides, they are not materials with high thermal conductivity. Therefore, there are few reports on research in the field of thermal conductive materials including heat dissipation films, thermal interface materials and thermal grease.
[0003] There are three main ways of heat conduction, including heat conduction, heat convection and heat radiation; among them, heat conduction and heat radiation are properties of the material itself, which are highly controllable and are the main directions of heat transfer research. The main components of heat-related composite materials include an organic binder base and a filler. Graphene has become a hot topic in the field of thermal conductive coating filler research due to its high emissivity and high thermal conductivity (5300W / m·K) close to that of a black body. However, the limitations of two-dimensional materials in longitudinal heat transfer are not conducive to the thermal conductivity of graphene. At present, it is commonly used to reduce graphene agglomeration and increase graphene dispersion by adding silicon dioxide, silicon powder, metal powder and metal oxides, thereby improving the longitudinal thermal conductivity of two-dimensional graphene.
[0004] CN107903751A discloses a graphene heat dissipation coating and a preparation method thereof, wherein the graphene heat dissipation coating comprises, by weight percentage, 35-55% of resin, 1-15% of graphene, 5-10% of functional filler, 0.5-1.5% of leveling agent, 0.05-0.2% of defoamer, 1-3% of dispersant, 3-10% of colorant and 10-40% of solvent; the graphene is one or more of N-type high-purity graphene and functional graphene, and the functional filler is one or more of aluminum nitride, carbon fiber, spherical nano-alumina and alumina fiber. In this technical solution, N-type high-purity graphene with high heat dissipation and radiation, functional graphene with high radiation dielectric loss and functional fillers are combined in a specific mass ratio, so that the graphene radiation and the structure of the filler form a non-gravity stacking bridging structure, the internal space defects of the coating increase, and the coating is given better directional heat transfer performance. At the same time, the spatial infrared radiation area is increased, so that the radiation emissivity and radiation absorption rate achieve the optimal radiation effect, enhance infrared thermal radiation, form a coating with high radiation and high heat transfer performance, and achieve a uniform heat effect of the substrate facing the coating.
[0005] CN114163851A discloses a graphene heat dissipation slurry and its preparation method. The graphene heat dissipation slurry comprises: by weight, 25-80 parts of graphene, 15-50 parts of acrylate, 5-35 parts of thermal conductive filler, 10-40 parts of solvent, 0.01-10 parts of resin acid and 0.01-3 parts of auxiliary agent; the thermal conductive filler is at least one of graphite, fullerene, carbon black, carbon nanotube, carbon fiber, silicon nitride, aluminum nitride, silicon carbide, aluminum, copper, silver, carbon steel, silicon, aluminum oxide or magnesium oxide. This technical solution improves the adhesion of the coating by using straight-chain acrylate modified by resin acid as a polymer binder. The present invention can more effectively reduce the volume occupied by macromolecules, make the coating thinner, thereby increasing the cross-linking density, making the graphene powder or thermal conductive filler more compact, easier to form a thermal conductive path, and improving the thermal conductivity.
[0006] Considering the heat dissipation requirements and environmental adaptability of heat dissipation fillers, the existing composite fillers are difficult to meet the requirements of building a thermal conductive network, high emissivity and environmental adaptability. Therefore, how to provide a thermal conductive composite filler with an efficient thermal conductive network, high emissivity and good environmental adaptability has become a technical problem that needs to be solved urgently. Summary of the invention
[0007] In view of the deficiencies of the prior art, the purpose of the present invention is to provide a composite filler and a preparation method and application thereof. In the present invention, the raw materials for preparing the composite filler are designed, and silicate is further used to modify the surface of titanium oxide, and the interaction between silicate and graphene is used to improve the bonding force between graphene and titanium oxide, thereby constructing an isotropic thermal conductive 3D network, improving the limitation of graphene's two-dimensional thermal conductivity, and obtaining a thermal conductive composite filler with an efficient thermal conductive network, high emissivity and good environmental adaptability.
[0008] To achieve this object, the present invention adopts the following technical solutions:
[0009] In a first aspect, the present invention provides a composite filler, wherein raw materials for preparing the composite filler include titanium dioxide, graphene, a dispersant and a silicate.
[0010] Graphene has become a hot topic in the field of thermal conductive coating fillers due to its high emissivity and high thermal conductivity (5300W / m·K) close to that of a black body. However, the limitations of two-dimensional materials in longitudinal heat transfer are not conducive to graphene's thermal conductivity.
[0011] In the present invention, the raw materials for preparing the composite filler are designed, and silicate is further used to modify the surface of titanium dioxide (Ti4O7), and the graphene is evenly dispersed through conjugation between the dispersant and graphene to avoid agglomeration of the graphene. At the same time, the interaction between the silicate and the graphene improves the bonding force between the graphene and titanium dioxide, thereby constructing an isotropic thermal conductive 3D network, improving the limitation of the two-dimensional thermal conductivity of the graphene, and obtaining a thermal conductive composite filler with a high-efficiency thermal conductive network, high emissivity and good environmental adaptability.
[0012] At the same time, titanium dioxide has good wear resistance and acid and alkali resistance. On the basis of increasing the corrosion protection effect of the organic matrix, it can further enhance the tolerance and environmental adaptability of the composite filler, providing a certain guarantee for expanding the scope of use of the thermally conductive filler.
[0013] The following are preferred technical solutions of the present invention, but are not intended to limit the technical solutions provided by the present invention. Through the following preferred technical solutions, the objectives and beneficial effects of the present invention can be better achieved and realized.
[0014] As a preferred technical solution of the present invention, the mass ratio of titanium dioxide and graphene is 1:(0.2-2.5), for example, it can be 1:0.2, 1:0.4, 1:0.6, 1:0.8, 1:1, 1:1.2, 1:1.4, 1:1.6, 1:1.8, 1:2, 1:2.2 or 1:2.5, etc.
[0015] In the present invention, by controlling the mass ratio of titanium oxide and graphene within a specific range, an isotropic thermal conductive 3D network can be constructed, and a thermal conductive composite filler with an efficient thermal conductive network, high emissivity and good environmental adaptability can be obtained. If the mass ratio of titanium oxide and graphene is too small, it is not conducive to the formation of an isotropic thermal conductive 3D network, resulting in poor heat dissipation effect of the composite filler; if the mass ratio of titanium oxide and graphene is too large, due to the low intrinsic thermal conductivity of titanium oxide, which is 10-20W·m -1 K -1 , resulting in poor thermal conductivity of the prepared composite filler.
[0016] Preferably, based on the mass percentage of the titanium oxide being 100%, the mass percentage of the dispersant is 3-15%, for example, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14% or 15%, etc.
[0017] In the present invention, by controlling the amount of the dispersant within a specific range, the graphene can have a better dispersion effect. If the amount of the dispersant is too little, the dispersion effect of the graphene will be poor, and the graphene will easily agglomerate, resulting in poor thermal conductivity of the composite filler finally prepared; if the dispersant content is too much, the dispersant has no positive effect on the dispersion effect of the graphene.
[0018] Preferably, based on the mass content of the titanium oxide being 100%, the mass percentage of the silicate is 2-10% (for example, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9% or 10%, etc.), and more preferably 4-8%.
[0019] In the present invention, by controlling the amount of silicate within a specific range, the surface of titanium oxide can be activated and used as a "bridge" to connect titanium oxide and graphene, thereby improving the bonding force between titanium oxide and graphene, and thus preparing a composite filler with good thermal conductivity. If the amount of silicate is too small, the modification effect on titanium oxide is poor, and the thermal conductivity of the prepared composite filler is poor; if the amount of silicate is too large, the thermal conductivity will be reduced.
[0020] As a preferred technical solution of the present invention, the average particle size of the titanium oxide is 15 to 25 μm, for example, it can be 15 μm, 16 μm, 17 μm, 18 μm, 19 μm, 20 μm, 21 μm, 22 μm, 23 μm, 24 μm or 25 μm.
[0021] Preferably, the graphene is prepared by a redox method.
[0022] In the present invention, graphene prepared by a redox method is selected as a raw material, so that the graphene surface has oxygen-containing groups, and the oxygen-containing groups on the graphene surface interact with the silicate-modified titanium dioxide particles to improve the bonding force between the graphene and the titanium dioxide.
[0023] The specific preparation method of graphene is as follows: 0.4-0.6 mg mL -1 Hydrazine hydrate is added to a graphene oxide solution, wherein the mass ratio of graphene oxide to hydrazine hydrate is 10:(6-8), the mixed solution is placed in a water bath at 80-95° C., stirred and heated for 1-2 hours, filtered, the filter cake is collected, and then dried at 80-100° C. for 8-12 hours.
[0024] The concentration of graphene oxide in the graphene oxide solution can be 0.4 mg mL -1 , 0.42mg·mL -1 , 0.44mg·mL -1 , 0.46mg·mL -1 , 0.48mg·mL -1 , 0.5mg·mL -1 , 0.52mg·mL -1 , 0.54mg·mL -1 , 0.56mg·mL -1 , 0.58mg·mL -1 or 0.6 mg mL -1 wait.
[0025] The mass ratio of graphene oxide to hydrazine hydrate can be 10:6, 10:6.3, 10:6.6, 10:6.8, 10:7, 10:7.2, 10:7.5, 10:7.8 or 10:8, etc.
[0026] The temperature of the water bath heating can be 80°C, 81°C, 84°C, 86°C, 88°C, 90°C, 92°C or 95°C, etc.
[0027] The heating time can be 1h, 1.5h or 2h, etc.
[0028] The drying temperature can be 80°C, 81°C, 84°C, 86°C, 88°C, 90°C, 92°C, 95°C, 98°C or 100°C, etc.
[0029] The drying time can be 8h, 9h, 10h, 11h or 12h, etc.
[0030] Preferably, the number of layers of the graphene is 3-15 layers, for example, it can be 3 layers, 4 layers, 5 layers, 6 layers, 7 layers, 8 layers, 9 layers, 10 layers, 11 layers, 12 layers, 13 layers, 14 layers or 15 layers.
[0031] As a preferred technical solution of the present invention, the dispersant is selected from any one of dispersant NNO, sodium dodecylbenzene sulfonate, polyvinyl pyrrolidone (PVP), rhodamine 6G, and protoporphyrin, or a combination of at least two thereof.
[0032] Preferably, the silicate has a structural formula as shown in Formula I below:
[0033]
[0034] wherein R1-R4 are each independently selected from a C1-C5 alkyl group (e.g., a methyl group, an ethyl group, a propyl group, a butyl group or a pentyl group);
[0035] Preferably, the silicate is selected from any one of methyl orthosilicate, ethyl orthosilicate, propyl orthosilicate, butyl orthosilicate or pentyl orthosilicate, or a combination of at least two thereof.
[0036] As a preferred technical solution of the present invention, the raw materials for preparing the composite filler also include a solvent.
[0037] Preferably, the solvent is selected from any one of ethanol, water or acetic acid, or a combination of at least two thereof.
[0038] In a second aspect, the present invention provides a method for preparing the composite filler as described in the first aspect, the preparation method comprising the following steps:
[0039] (1) mixing titanium oxide, a silicate and a solvent, and performing a modification treatment to obtain a mixture A containing modified titanium oxide;
[0040] mixing graphene, a dispersant and a solvent to obtain a mixture B;
[0041] (2) Mixing the mixture A and the mixture B, and drying them to obtain the composite filler.
[0042] In the present invention, titanium oxide is surface-modified by using silicate to obtain modified titanium oxide, graphene is evenly dispersed by using a dispersant, and then the silicate groups on the surface of the titanium oxide interact with the graphene to improve the binding force between the titanium oxide and the graphene, and the titanium oxide is dispersed between the graphenes to construct an isotropic thermally conductive 3D network, thereby obtaining a thermally conductive composite filler with an efficient thermally conductive network, high emissivity and good environmental adaptability.
[0043] As a preferred technical solution of the present invention, the solvent in the mixture A includes ethanol and / or acetic acid;
[0044] Preferably, the solvent comprises ethanol and acetic acid, and the volume ratio of ethanol to acetic acid is 1:(1-2), for example, it can be 1:1, 1:1.1, 1:1.2, 1:1.3, 1:1.4, 1:1.5, 1:1.6, 1:1.7, 1:1.8, 1:1.9 or 1:2, etc.
[0045] Preferably, the temperature of the modification treatment is room temperature.
[0046] Preferably, the modification treatment time is 44 to 50 hours, for example, it can be 44 hours, 45 hours, 46 hours, 47 hours, 48 hours, 49 hours or 50 hours.
[0047] Preferably, the solvent in the mixture B comprises water and / or ethanol.
[0048] Preferably, the mixing temperature for obtaining the mixture B is room temperature.
[0049] Preferably, the mixing time for obtaining the mixture B is 34 to 40 h, for example, 34 h, 35 h, 36 h, 37 h, 38 h, 39 h or 40 h.
[0050] As a preferred technical solution of the present invention, the mixing time in step (2) is 70 to 75 hours, for example, it can be 70 hours, 71 hours, 72 hours, 73 hours, 74 hours or 750 hours.
[0051] Preferably, the mixing temperature in step (2) is room temperature.
[0052] Preferably, the drying method in step (2) includes freeze-drying.
[0053] Preferably, the drying time in step (2) is 12 to 18 hours, for example, it can be 12 hours, 13 hours, 14 hours, 15 hours, 16 hours, 17 hours or 18 hours.
[0054] In the present invention, the preparation method of the composite filler specifically comprises the following steps:
[0055] (1) mixing titanium suboxide, silicate and solvent, and performing a modification treatment at room temperature for 44 to 50 hours to obtain a mixture A containing modified titanium suboxide;
[0056] At room temperature, graphene, a dispersant and water are mixed for 34 to 40 hours to obtain a mixture B;
[0057] (2) Mixing mixture A and mixture B at room temperature for 70 to 75 hours, and then freeze-drying for 12 to 18 hours to obtain the composite filler.
[0058] In a third aspect, the present invention provides a thermally conductive coating, which includes the following components in parts by weight: 1-5 parts of the composite filler as described in the first aspect and 24 parts of a binder.
[0059] In the present invention, by controlling the mass ratio of the composite filler to the binder within a specific range, the thermal conductive coating prepared has both good thermal conductivity and is not easy to fall off. If the amount of the composite filler is too much, it is easy to fall off and does not meet the application requirements; if the amount of the composite filler is too little, the thermal conductive effect of the prepared thermal conductive filler is poor.
[0060] There is no special restriction on the specific selection of the adhesive in the present invention, and any adhesive commonly used in the art is applicable, including but not limited to adhesive DC184.
[0061] The present invention does not impose any special restrictions on the preparation method of the thermal conductive coating, which illustratively includes but is not limited to: uniformly mixing the composite filler and the binder to obtain the thermal conductive coating.
[0062] The thermal conductive coating can be prepared by the thermal conductive coating provided by the present invention, and its preparation method exemplarily includes but is not limited to: coating the thermal conductive coating on either side of a substrate and then drying to obtain the thermal conductive coating.
[0063] In a fourth aspect, the present invention provides a use of the composite filler as described in the first aspect and the thermally conductive coating as described in the third aspect in a thermally conductive coating, a thermally conductive interface material and a heat sink.
[0064] Compared with the prior art, the present invention has the following beneficial effects:
[0065] The present invention designs the raw materials for preparing the composite filler, further controls the mass ratio of titanium dioxide and graphene in the raw materials for preparing the composite filler within a specific range, controls the amount of silicate within a specific range, and uses graphene with oxygen-containing groups on the surface to construct a composite filler with an isotropic thermal conductive 3D network, improves the limitation of the two-dimensional thermal conductivity of graphene, and thus obtains a thermal conductive composite filler with an efficient thermal conductive network, high emissivity and good environmental adaptability. The thermal conductivity of the thermal conductive film prepared by the composite filler is 5.593-6.727 W·m -1 K -1 The heat dissipation effect is 18.55~25.03%. BRIEF DESCRIPTION OF THE DRAWINGS
[0066] Figure 1 is a scanning electron microscope photograph of titanium oxide used in Example 1 of the present invention;
[0067] Figure 2 This is a transmission electron microscope photograph of the composite filler provided in Example 1 of the present invention. DETAILED DESCRIPTION
[0068] The technical solution of the present invention is further described below in conjunction with the accompanying drawings and through specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.
[0069] The sources of some components in the following examples and comparative examples are as follows:
[0070] Titanium dioxide: Longxing Titanium Industry, purity 99%;
[0071] Graphene oxide: Sichuan Hengli Shengtai Graphene Technology Co., Ltd., 1.5 layers, 4 microns in diameter;
[0072] Dispersant NNO: Shanghai MacLean Biochemical Technology Co., Ltd., 95%;
[0073] Dispersant sodium dodecylbenzene sulfonate: Shanghai MacLean Biochemical Technology Co., Ltd., 95%;
[0074] Polyvinylpyrrolidone (PVP): Shanghai MacLean Biochemical Technology Co., Ltd., degree of polymerization is 58,000.
[0075] Example 1
[0076] This embodiment provides a composite filler and a preparation method thereof. The raw materials for preparing the composite filler include the following components in parts by weight:
[0077] 10 parts of titanium oxide, 5 parts of graphene, 0.8 parts of dispersant NNO and 0.4 parts of tetraethyl orthosilicate.
[0078] The preparation method of the composite filler is as follows:
[0079] (1) titanium dioxide (10 parts), tetraethyl orthosilicate (0.4 parts) and a solvent (250 parts, composed of ethanol and acetic acid in a volume ratio of 1:1.4) were mixed and subjected to a modification treatment at room temperature for 48 hours to obtain a mixture A containing modified titanium dioxide;
[0080] At room temperature, graphene (5 parts), dispersant NNO (0.8 parts) and water (250 parts) were mixed for 38 hours to obtain mixture B;
[0081] (2) Mixture A and mixture B were mixed at room temperature for 48 hours, and then freeze-dried for 15 hours to obtain the composite filler.
[0082] The structure of titanium oxide was tested and characterized using a scanning electron microscope. The test results are as follows: Figure 1 As shown by Figure 1 It can be seen that titanium dioxide has a network structure, which is conducive to building a continuous thermal conductive network.
[0083] The structure of the composite filler was tested and characterized using a transmission electron microscope. The test results are as follows: Figure 2 As shown. Figure 2 It can be seen that in this embodiment, a uniformly dispersed composite filler is obtained by designing the raw materials for preparing the composite filler, wherein the graphene is distributed in the middle of the pores of the titanium oxide.
[0084] Example 2
[0085] This embodiment provides a composite filler and a preparation method thereof. The raw materials for preparing the composite filler include the following components in parts by weight:
[0086] 10 parts of titanium oxide, 15 parts of graphene, 1 part of dispersant sodium dodecylbenzene sulfonate and 0.5 parts of ethyl orthosilicate.
[0087] The preparation method of the composite filler is as follows:
[0088] (1) titanium dioxide (10 parts), tetraethyl orthosilicate (0.5 parts) and a solvent (250 parts, composed of ethanol and acetic acid in a volume ratio of 1:1.4) were mixed and subjected to a modification treatment at room temperature for 44 hours to obtain a mixture A containing modified titanium dioxide;
[0089] At room temperature, graphene (15 parts), dispersant sodium dodecylbenzene sulfonate (1 part) and water (300 parts) were mixed for 40 hours to obtain a mixture B;
[0090] (2) Mixture A and mixture B were mixed at room temperature for 10 hours, and then freeze-dried for 15 hours to obtain the composite filler.
[0091] Example 3
[0092] This embodiment provides a composite filler and a preparation method thereof. The raw materials for preparing the composite filler include the following components in parts by weight:
[0093] 10 parts of titanium oxide, 3 parts of graphene, 0.3 parts of rhodamine 6G and 0.8 parts of tetraethyl orthosilicate.
[0094] The preparation method of the composite filler is as follows:
[0095] (1) mixing titanium oxide (10 parts), tetraethyl orthosilicate (0.8 parts) and a solvent (250 parts, composed of ethanol and acetic acid in a volume ratio of 1:1) and performing a modification treatment at room temperature for 48 hours to obtain a mixture A containing modified titanium oxide;
[0096] Graphene (3 parts), rhodamine 6G (0.3 parts) and water (200 parts) were mixed at room temperature for 38 hours to obtain mixture B;
[0097] (2) Mixture A and mixture B were mixed at room temperature for 70 hours, and then freeze-dried for 18 hours to obtain the composite filler.
[0098] Example 4
[0099] This embodiment provides a composite filler and a preparation method thereof. The raw materials for preparing the composite filler include the following components in parts by weight:
[0100] 10 parts of titanium dioxide, 50 parts of graphene, 1.5 parts of PVP and 0.2 parts of tetraethyl orthosilicate.
[0101] The preparation method of the composite filler is as follows:
[0102] (1) titanium dioxide (10 parts), tetraethyl orthosilicate (0.2 parts) and ethanol (250 parts) were mixed and subjected to a modification treatment at room temperature for 50 hours to obtain a mixture A containing modified titanium dioxide;
[0103] At room temperature, graphene (50 parts), PVP (1.5 parts) and water (500 parts) were mixed for 34 hours to obtain mixture B;
[0104] (2) Mixture A and mixture B were mixed at room temperature for 75 hours and then freeze-dried for 12 hours to obtain the composite filler.
[0105] Example 5
[0106] This embodiment provides a composite filler and a preparation method thereof. The raw materials for preparing the composite filler include the following components in parts by weight:
[0107] 10 parts of titanium dioxide, 30 parts of graphene, 1.2 parts of protoporphyrin and 1 part of tetraethyl orthosilicate.
[0108] The preparation method of the composite filler is as follows:
[0109] (1) mixing titanium oxide (10 parts), tetraethyl orthosilicate (1 part) and a solvent (250 parts, composed of ethanol and acetic acid in a volume ratio of 1:1.5) and performing a modification treatment at room temperature for 44 hours to obtain a mixture A containing modified titanium oxide;
[0110] At room temperature, graphene (30 parts), protoporphyrin (1.2 parts) and water (400 parts) were mixed for 40 hours to obtain a mixture B;
[0111] (2) Mixture A and mixture B were mixed at room temperature for 70 hours and then freeze-dried for 15 hours to obtain the composite filler.
[0112] Example 6
[0113] This embodiment provides a composite filler and a preparation method thereof, which is different from Embodiment 1 only in that the weight proportion of graphene in the raw material for preparing the composite filler is 2 parts, and other conditions are the same as those in Embodiment 1.
[0114] Example 7
[0115] This embodiment provides a composite filler and a preparation method thereof, which is different from Embodiment 1 only in that the weight proportion of graphene in the raw material for preparing the composite filler is 20 parts, and other conditions are the same as those in Embodiment 1.
[0116] Example 8
[0117] This embodiment provides a composite filler and a preparation method thereof, which is different from Embodiment 1 only in that the weight proportion of graphene in the raw materials for preparing the composite filler is 25 parts, and other conditions are the same as those in Embodiment 1.
[0118] Example 9
[0119] This embodiment provides a composite filler and a preparation method thereof, which is different from Embodiment 1 only in that the weight portion of graphene in the raw material for preparing the composite filler is 1 part, and other conditions are the same as those in Embodiment 1.
[0120] Example 10
[0121] This embodiment provides a composite filler and a preparation method thereof, which is different from Embodiment 1 only in that the weight portion of ethyl orthosilicate in the raw material for preparing the composite filler is 0.2 parts, and other conditions are the same as those in Embodiment 1.
[0122] Embodiment 11
[0123] This embodiment provides a composite filler and a preparation method thereof, which is different from Embodiment 1 only in that the weight portion of ethyl orthosilicate in the raw material for preparing the composite filler is 0.7 parts, and other conditions are the same as those in Embodiment 1.
[0124] Example 12
[0125] This embodiment provides a composite filler and a preparation method thereof, which is different from Embodiment 1 only in that the weight portion of ethyl orthosilicate in the raw material for preparing the composite filler is 1 part, and other conditions are the same as those in Embodiment 1.
[0126] Example 13
[0127] This embodiment provides a composite filler and a preparation method thereof, which is different from Embodiment 1 only in that the weight portion of ethyl orthosilicate in the raw material for preparing the composite filler is 0.1 parts, and other conditions are the same as those in Embodiment 1.
[0128] Embodiment 14
[0129] This embodiment provides a composite filler and a preparation method thereof, which is different from Embodiment 1 only in that the weight portion of ethyl orthosilicate in the raw material for preparing the composite filler is 1.2 parts, and other conditions are the same as those in Embodiment 1.
[0130] Embodiment 15
[0131] This embodiment provides a composite filler and a preparation method thereof. The only difference from Example 1 is that the graphene in Example 1 is replaced by graphene without oxygen-containing groups on the surface (graphene synthesized by combustion method, purchased from the Institute of Chemistry), and other conditions are the same as those in Example 1.
[0132] Comparative Example 1
[0133] This comparative example provides a composite filler and a preparation method thereof, wherein the composite filler comprises the following components in parts by weight:
[0134] 10 parts of titanium oxide, 15 parts of graphene, and 1 part of sodium dodecylbenzene sulfonate.
[0135] The preparation method of the composite filler is as follows:
[0136] (1) mixing graphene, sodium dodecylbenzene sulfonate and water (300 parts) at room temperature for 38 hours to obtain a mixture;
[0137] (2) The mixture was mixed with titanium oxide at room temperature for 72 hours and then freeze-dried for 15 hours to obtain the composite filler.
[0138] Comparative Example 2
[0139] This comparative example provides a composite filler and a preparation method thereof, wherein the composite filler comprises the following components in parts by weight:
[0140] 10 parts of titanium oxide, 5 parts of graphene and 0.4 parts of tetraethyl orthosilicate.
[0141] The preparation method of the composite filler is as follows:
[0142] (1) titanium dioxide, tetraethyl orthosilicate and a solvent (250 parts, composed of ethanol and acetic acid in a volume ratio of 1:1.4) were mixed and subjected to a modification treatment at room temperature for 48 hours to obtain a mixture A containing modified titanium dioxide;
[0143] (2) Mixture A and graphene were mixed at room temperature for 72 hours, and then freeze-dried for 15 hours to obtain the composite filler.
[0144] Comparative Example 3
[0145] This comparative example provides a composite filler and a preparation method thereof, wherein the composite filler comprises the following components in parts by weight:
[0146] 5 parts of boron nitride, 10 parts of graphene, and 0.8 parts of rhodamine 6G.
[0147] The preparation method of the composite filler is as follows:
[0148] (1) mixing graphene, rhodamine 6G and water (300 parts) at room temperature for 38 hours to obtain a mixture;
[0149] (2) The mixture was mixed with boron nitride at room temperature for 72 hours and then freeze-dried for 15 hours to obtain the composite filler.
[0150] The composite fillers provided in the above embodiments and comparative examples are used to prepare a thermally conductive film, and the performance of the thermally conductive film is tested. The preparation method of the thermally conductive film is as follows:
[0151] The composite filler (2 parts) and the binder (24 parts) provided in the above-mentioned embodiment and comparative example are respectively mixed evenly, coated evenly on a substrate (aluminum alloy 6061) by a spray gun, and heated and cured to obtain the thermal conductive film.
[0152] The performance test method for thermal conductive film is as follows:
[0153] Thermal conductivity: The thermal conductivity was measured in air at room temperature using Hot Disk TPS 2500S.
[0154] Heat dissipation effect: On a heating platform with a length and width of 15cm×25cm and a stable heating power of 560W, a K-type thermocouple was used to test the temperature of the film surface.
[0155] The performance test results are shown in Table 1 below:
[0156] Table 1
[0157]
[0158]
[0159] As can be seen from the above table, the present invention designs the raw materials for preparing the composite filler, further controls the mass ratio of titanium dioxide and graphene in the raw materials for preparing the composite filler within a specific range, and controls the amount of silicate within a specific range, and uses graphene with oxygen-containing groups on the surface to construct a composite filler with an isotropic thermal conductive 3D network, thereby improving the limitation of the two-dimensional thermal conductivity of graphene, and thus obtaining a thermally conductive composite filler with an efficient thermal conductive network, high emissivity and good environmental adaptability. The thermal conductivity of the thermally conductive film prepared from the composite filler is 5.593-6.727 W·m -1 K -1 The heat dissipation effect is 18.55~25.03%.
[0160] The present invention can further improve the thermal conductivity and heat dissipation effect of the thermal conductive film by further optimizing the amount of silicate used, and its thermal conductivity is ≥6.102W·m -1 K -1 , specifically 6.102~6.727W·m -1 K -1 , the heat dissipation effect is ≥20.09%, specifically 20.09~25.03%.
[0161] Compared with Example 1, if the mass ratio of titanium dioxide and graphene in the composite filler is too small (Examples 4-5) or too large (Example 9), the thermal conductivity of the prepared composite filler is poor.
[0162] Compared with Example 1, if the amount of silicate in the composite filler is too small (Example 13), its modification of titanium dioxide is poor, and it is difficult to construct a 3D thermal conductive network, and the thermal conductivity of the composite filler prepared thereby is poor; if the amount of silicate in the composite filler is too large (Example 14), it will cause waste of raw materials.
[0163] Compared with Example 1, if graphene without oxygen-containing groups on the surface is selected (Example 15), the silica surface modified with silicate is difficult to interact with the graphene without oxygen-containing groups on the surface, and it is difficult to construct a 3D thermal conductive network. The thermal conductivity of the composite filler prepared in this way is poor.
[0164] Compared with Example 1, if the raw materials for preparing the composite filler do not contain silicate (Comparative Example 1), it is difficult to build an interactive "bridge" between titania and graphene, the bonding force between titania and graphene is poor, and the performance of the prepared composite filler is poor; if the raw materials for preparing the composite filler do not contain a dispersant (Comparative Example 2), graphene is easy to agglomerate, and the thermal conductivity of the prepared composite filler is poor; if the modified titania in the composite filler is replaced with boron nitride (Comparative Example 3), it is difficult to obtain a 3D thermal conductive network, and the thermal conductivity of the obtained composite filler is also poor.
[0165] In summary, the present invention designs the raw materials for preparing the composite filler, further controls the mass ratio of titanium dioxide and graphene in the raw materials for preparing the composite filler within a specific range, and controls the amount of silicate within a specific range, and simultaneously uses graphene with oxygen-containing groups on the surface to construct a composite filler with an isotropic thermally conductive 3D network, thereby improving the limitations of the two-dimensional thermal conductivity of graphene, and thus obtaining a thermally conductive composite filler with an efficient thermally conductive network, high emissivity and good environmental adaptability.
[0166] The applicant declares that the present invention illustrates the detailed process flow of the present invention through the above-mentioned embodiments, but the present invention is not limited to the above-mentioned detailed process flow, that is, it does not mean that the present invention must rely on the above-mentioned detailed process flow to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of various raw materials of the product of the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.
Claims
1. A composite filler, characterized in that: The raw materials for preparing the composite filler include titanium dioxide, graphene, a dispersant and silicate.
2. The composite filler according to claim 1, characterized in that: The mass ratio of titanium dioxide to graphene is 1:(0.2-2.5); Preferably, based on the mass content of the titanium oxide being 100%, the mass percentage of the dispersant is 3-15%; Preferably, based on the mass percentage of the titanium oxide being 100%, the mass percentage of the silicate is 2-10%, and more preferably 4-8%.
3. The composite filler according to claim 1 or 2, characterized in that: The average particle size of the titanium oxide is 15 to 25 μm; Preferably, the graphene is prepared by a redox method; Preferably, the number of graphene layers is 3-15.
4. The composite filler according to any one of claims 1 to 3, characterized in that: The dispersant is selected from any one of dispersant NNO, dispersant sodium dodecylbenzene sulfonate, polyvinyl pyrrolidone, rhodamine 6G, and protoporphyrin, or a combination of at least two thereof; Preferably, the silicate has a structural formula as shown in Formula I below: Wherein, R1-R4 are each independently selected from C1-C5 alkyl; Preferably, the silicate is selected from any one of methyl orthosilicate, ethyl orthosilicate, propyl orthosilicate, butyl orthosilicate or pentyl orthosilicate, or a combination of at least two thereof.
5. The composite filler according to any one of claims 1 to 4, characterized in that: The raw materials for preparing the composite filler also include a solvent; Preferably, the solvent is selected from any one of ethanol, water or acetic acid, or a combination of at least two thereof.
6. A method for preparing a composite filler according to any one of claims 1 to 5, characterized in that: The preparation method comprises the following steps: (1) mixing titanium oxide, a silicate and a solvent, and performing a modification treatment to obtain a mixture A containing modified titanium oxide; mixing graphene, a dispersant and a solvent to obtain a mixture B; (2) Mixing the mixture A and the mixture B, and drying them to obtain the composite filler.
7. The preparation method according to claim 6, characterized in that: The solvent in the mixture A includes ethanol and / or acetic acid; Preferably, the solvent comprises ethanol and acetic acid, and the volume ratio of ethanol to acetic acid is 1:(1-2); Preferably, the modification treatment time is 44 to 50 hours; Preferably, the mixing time for obtaining the mixture B is 34 to 40 hours.
8. The preparation method according to claim 6 or 7, characterized in that: The mixing time in step (2) is 70 to 75 hours; Preferably, the drying method in step (2) comprises freeze drying; Preferably, the drying time in step (2) is 12 to 18 hours.
9. A thermally conductive coating, characterized in that: The thermal conductive coating comprises the following components in parts by weight: 1-5 parts of the composite filler according to any one of claims 1 to 6 and 24 parts of a binder.
10. Use of the composite filler according to any one of claims 1 to 5 or the thermally conductive coating according to claim 9 in a thermally conductive coating, a thermally conductive interface material and a heat sink.
Citation Information
Patent Citations
Graphene-containing heat-dissipating coating and preparation method thereof
CN107903751A
Graphene heat dissipation slurry and preparation method thereof
CN114163851A
Magnetic titanate / graphene oxide molecularly imprinted photocatalytic composite material and preparation method thereof
CN105562112A
Composite heat-conducting filler as well as preparation method and application thereof
CN115536905A
Modification method for graphene, modified graphene, and composition containing graphene
US20210017436A1