Method for selectively extracting precious metal silver in solid waste through ionic liquid-like system

Through the combination of ionic liquids and chloride salts, the problems of high corrosion and complex metal recycling in the hydrometallurgy process are solved, and efficient and environmentally friendly precious metal silver recycling is achieved. The silver leaching rate is as high as 94.4% or above, simplifying the Process and reduce costs.

CN118932187APending Publication Date: 2024-11-12SHANGHAI SECOND POLYTECHNIC UNIVERSITY
View PDF 0 Cites 3 Cited by

Patent Information

Application Number
CN202411076034.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-07
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing hydrometallurgical recycling process has problems such as the use of highly corrosive leaching agents, high risk of pollution, and difficulty in efficient recycling of complex metals and trace precious metals, resulting in low recovery rate of precious metals.

Method used

Using an ionic liquid system and chloride salt combination, the pH value, precipitation and filtration can be adjusted by heating and stirring, deionized water to adjust the pH value, precipitation and filtration, so as to selectively extract precious metal silver from solid waste, and the stability and solvation effect of ionic liquids are used to avoid cheap Reduction of metal.

Benefits of technology

It has achieved efficient, low-toxic and environmentally friendly precious metal silver recycling, with silver leaching rate reaching 94.4% or above, reducing the difficulty of high-purity silver recycling, simplifying the process flow and reducing costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118932187A_ABST
    Figure CN118932187A_ABST
Patent Text Reader

Abstract

The invention discloses a method for selectively extracting precious metal silver in solid waste through an ionic liquid-like system. The method comprises the following steps that (1) the silver-containing solid waste is placed in a leaching agent to be heated, stirred and leached, the leaching agent is a combination of ionic-like liquid and chlorine salt, the ionic-like liquid is choline chloride-malonic acid, the molar ratio of choline chloride to malonic acid is 1: 1, and the chlorine salt is FeCl3; 2) adding a proper amount of deionized water into the leached product, and adjusting the pH to be acidic; 3) standing at normal temperature and completely precipitating, and filtering to obtain silver chloride precipitate and filtrate; and 4) removing the deionized water in the filtrate obtained in the step 3) by evaporation, wherein the remaining leaching agent can be recycled. According to the method, a choline chloride-malonic acid (similar ionic liquid)-mild oxidant (Fe < 3 + >)-simple coordination agent (Cl <->) reaction system is used for replacing a traditional strong acid / alkali-strong oxidant system, and selective extraction of the trace precious metal in the solid waste under the green mild reaction system is achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of resources and technology, and more specifically, relates to a method for selectively extracting precious metal silver from solid waste using a quasi-ionic liquid system. Background Art

[0002] In 2019, nearly 53.6 million tons of e-waste were generated worldwide, an increase of 21% compared with five years ago. Despite this, only 17.4% of e-waste was collected and recycled, which means that precious metals and high-value recyclable materials in e-waste are abandoned rather than recycled. Unlike traditional solid waste such as domestic waste, e-waste has the dual attributes of being hazardous and resource-based. From the perspective of resource utilization, the metal and non-metal components contained in e-waste are highly recyclable, especially precious metals, whose grade is dozens or even hundreds of times higher than that of crude ore. The cost of recovering metals from e-waste is much lower than the cost of mining raw ore. However, there are also a variety of heavy metals, such as lead, mercury and cadmium, as well as persistent organic matter, such as polychlorinated biphenyls and brominated flame retardants. If not handled properly, these hazardous substances will cause serious harm to the global ecosystem and human health. For example, waste photovoltaic modules contain harmful metals such as arsenic and cadmium, the junction boxes used on photovoltaic panels contain copper, tin oxide and chromium, and thin-film solar panels also contain cadmium and tellurium, which are all carcinogenic heavy metals. If waste photovoltaic modules are not handled properly, these heavy metals will leach out and cause serious environmental problems; on the other hand, waste photovoltaic modules have high resource value, and the high-quality Ag contained in them is the focus of recycling. It is estimated that 6.87kg of silver can be recycled per ton of retired photovoltaic cells. Appropriate recycling of valuable metal Ag in waste photovoltaic modules can save resources and effectively alleviate the contradiction between supply and demand of precious metal resources. Under the background of global carbon neutrality, the resource utilization of silver in solid waste is of great significance in saving resources, reducing environmental pollution, promoting circular economy and bringing economic benefits.

[0003] In the recovery of precious metals, the earliest method used was hydrometallurgy, such as aqua regia and cyanidation. This type of method is simple and has high recovery efficiency. It can recover precious metals such as gold and silver from the liquid phase of electronic waste and has a good recovery effect on non-ferrous metals. However, most hydrometallurgical methods consume a large amount of leaching agents, and the leaching agents are relatively corrosive, which may cause corrosion to the equipment. A large amount of waste liquid is also difficult to handle and may pollute the environment. In addition, most hydrometallurgical methods cannot handle complex metals. They can only leach precious metals exposed on the surface. Metals that are easily covered by other impurities cannot be leached. During leaching, a large amount of base metals will also be leached, resulting in a decrease in the recovery rate of precious metals. It is difficult to achieve efficient recovery of trace precious metals in a single system. Summary of the invention

[0004] In view of this, in order to solve the shortcomings and defects of the existing recycling process, the purpose of the present invention is to provide a method for selectively extracting precious metal silver from solid waste using a quasi-ionic liquid system. The method is based on a quasi-ionic liquid, which has the advantages of high stability, good solvation effect, simple synthesis, and no need for purification, and is suitable for establishing a process route for efficient resource recovery of precious metals in a mild reaction system. The technical solution of the present invention is specifically described as follows.

[0005] The present invention provides a method for selectively extracting precious metal silver from solid waste using an ionic liquid system, comprising the following steps: 1) adding the silver-containing solid waste to a leaching agent, stirring and leaching under heating conditions, and cooling to room temperature after the leaching is complete; wherein: the leaching agent is a combination of a quasi-ionic liquid and a chloride salt, the quasi-ionic liquid is choline chloride-malonic acid, the molar ratio of choline chloride to malonic acid is 1:1, and the chloride salt is FeCl3; 2) Add appropriate amount of deionized water to the leached product and stir thoroughly until precipitation is complete. During the stirring process, adjust the pH value to 2-3; 3) After the precipitation is completely completed at room temperature, the silver chloride precipitate and the filtrate are obtained by filtration, and the silver chloride precipitate is recovered; 4) The deionized water in the filtrate obtained in step 3) is evaporated and removed, and the remaining leaching agent is recycled.

[0006] In the present invention, in step 1), the silver-containing solid waste is discarded photovoltaic panels or discarded silver-plated parts.

[0007] In the present invention, in step 1), the liquid-solid ratio of the quasi-ionic liquid system to the silver-containing waste is 20:1-150:1 mL / g, and the chloride concentration in the leaching agent is 0.2-0.8 mol / L.

[0008] In the present invention, in step 1), the leaching temperature is 60-100° C., and the leaching time is 30-100 min.

[0009] In the present invention, in step 1), the chloride concentration in the leaching agent is 0.5 mol / L, the leaching temperature is 80° C., and the leaching time is 50 min.

[0010] In the present invention, in step 2), the mass ratio of the amount of deionized water added to the mass ratio of the ionic liquid-like reaction system in step (1) is 0.5:1-2:1. In step 2), the pH value is adjusted to 2-3 by adding dilute nitric acid; the reason for adjusting the pH value to 2-3 is that the dissolution area of ​​the base metal is relatively stable, so that when the silver chloride is selectively reduced and precipitated, other leached base metals in the system can be avoided from being reduced, and the selectivity is higher.

[0011] In the present invention, in step 3), the room temperature static precipitation reaction time is 30 to 200 minutes.

[0012] Compared with the prior art, the present invention has the following beneficial effects: The invention has the advantages of simple process, low toxicity, environmental protection, convenient operation and low cost. The ionic liquid-chloride salt system is adopted to replace the traditional strong acid and strong base oxidant system, which shows the characteristics of high stability, good solvation effect, simple synthesis and no need for purification of the ionic liquid. While selectively recovering the precious metal silver in the solid waste, the reduction of other metals in the solid waste is avoided, and the difficulty of recovering high-purity silver is reduced, which provides ideas and practical basis for realizing the recovery of precious metal silver in solid waste. BRIEF DESCRIPTION OF THE DRAWINGS

[0013] Figure 1 The present invention is a process flow chart of a method for selectively extracting precious metal silver from solid waste using a quasi-ionic liquid system.

[0014] Figure 2 The following are the SEM images and EDS spectra of the silver chloride precipitate in Example 1.

[0015] Figure 3 This is the XRD spectrum analysis of the silver chloride precipitate in Example 1. DETAILED DESCRIPTION

[0016] The following are specific embodiments of the present invention and the accompanying drawings to further describe the technical solutions of the present invention, but the present invention is not limited to these embodiments.

[0017] Figure 1 The present invention is a process flow chart of a method for selectively extracting precious metal silver from solid waste using a quasi-ionic liquid system.

[0018] Example 1 Waste photovoltaic silicon wafers ICP-OES measured that the silver content in the discarded solar silicon wafers was 0.0237%, the lead content was 0.0461%, and the aluminum content was 8.1526%. 0.4g of discarded photovoltaic silicon wafers were placed in 50mL of choline chloride-malonic acid (molar ratio 1:1) solvent containing 0.5mol / L FeCl3, and heated and leached for 50min at 80℃ with magnetic stirring (600rpm); after the leaching was completed, it was cooled to room temperature, 50mL of deionized water was added to the leachate, stirred at room temperature, and allowed to stand for 60min until precipitation was complete. During the stirring process, acid was added to adjust the pH value to between 2-3. After complete precipitation, it was filtered, and the obtained precipitate was washed and dried to obtain the AgCl product. The product was analyzed by SEM-EDS and XRD. The SEM image and EDS spectrum of the precipitate are shown in the figure. Figure 2 As shown in the XRD spectrum Figure 3 As shown in the figure, the silver grid lines in the photovoltaic silicon wafer before leaching are metallic silver. After leaching, the silver grid lines become lighter, proving that silver is effectively leached.

[0019] The SEM-EDS results showed that the product was mainly silver, and the XRD spectrum was consistent with the standard spectrum of silver chloride. The leached waste photovoltaic silicon wafers were digested, and their silver content was measured by ICP-OES. Compared with the original sample, the silver leaching rate was calculated to be 94.4%, indicating that the method of the present invention can efficiently recover silver from waste photovoltaic modules.

[0020] Example 2 Silver-plated parts ICP-OES measured the silver content of the silver-plated parts to be 0.5435%, the nickel content to be 0.5057%, and the copper content to be 82.6%. Take 2.9g of the silver-plated parts and put them into 100mL of choline chloride-malonic acid (molar ratio 1:1) solvent containing 0.5mol / L FeCl3, and heat and leach for 50min under magnetic stirring (600rpm) at 80℃; after the leaching is completed, cool to room temperature, add 100mL of deionized water to the leachate, stir at room temperature, and stand for 60min until the precipitation is complete. During the stirring process, add acid to adjust the pH value to between 2-3. Filter, wash and dry the obtained precipitate to obtain the AgCl product. The silver coating in the silver-plated parts raw material adheres to the surface of the copper-nickel alloy. After leaching, the silver coating disappears. It is calculated that the silver leaching rate in the silver-plated parts can reach more than 99.9%. It is confirmed that the silver is effectively leached.

[0021] Comparative Example 1 Waste photovoltaic silicon wafers The leaching material in this comparative example is waste photovoltaic silicon wafers. The difference from Example 1 is that the chloride salt in the choline chloride-malonic acid-chloride salt system is anhydrous cupric chloride. The specific implementation process is as follows: ICP-OES measured the silver content of the discarded solar silicon wafer to be 0.0237%, the lead content to be 0.0461%, and the aluminum content to be 8.1526%. Take 0.4g of discarded photovoltaic silicon wafers in 50mL of choline chloride-malonic acid (molar ratio 1:1) solvent containing 0.5mol / L anhydrous CuCl2, and heat and leach for 50min under magnetic stirring (600rpm) at 80°C; the silver grid lines in the photovoltaic silicon wafers before leaching are metallic silver, and the silver grid lines become slightly lighter after leaching, indicating that silver is leached, and the discarded photovoltaic silicon wafers after leaching are digested, and their silver content is measured by ICP-OES. Compared with the original sample, it is calculated that the silver leaching rate in the discarded photovoltaic silicon wafers under the choline chloride-malonic acid-CuCl2 system is 41.58%, which is much lower than the silver leaching rate in the discarded photovoltaic silicon wafers under the choline chloride-malonic acid-FeCl3 system in Example 1.

[0022] Comparative Example 2 Silver-plated parts The leached material in this comparative example is a silver-plated part, which is different from Example 2 in that the chloride salt in the choline chloride-malonic acid-chloride salt system is anhydrous cupric chloride. The specific implementation process is as follows: ICP-OES measured the silver content of the silver-plated part to be 0.5435%, the nickel content to be 0.5057%, and the copper content to be 82.6%. Take 2.9g of the silver-plated part and put it into 100mL of choline chloride-malonic acid (molar ratio 1:1) solvent containing 0.5mol / L CuCl2 and heat and leach for 50min under magnetic stirring (600rpm) at 80℃; after the leaching, it can be clearly seen that the silver coating attached to the surface of the copper-nickel alloy in the raw material of the silver-plated part has not completely disappeared, and there are still large pieces of silver coating attached. The silver content was detected by ICP-OES and the silver leaching rate in the silver-plated parts under the choline chloride-malonic acid-CuCl2 system was calculated to be 56.21%, which is much lower than the silver leaching rate in the silver-plated parts under the choline chloride-malonic acid-FeCl3 system in Example 2.

[0023] The above descriptions are only several preferred implementation examples of the present invention. Several improvements and optimizations made by those skilled in the art without departing from the principles of the present application should also be regarded as within the protection scope of the present application.

Claims

1. A method for selectively extracting precious metal silver from solid waste using an ionic liquid system, characterized in that: The steps include: 1) adding the silver-containing solid waste to a leaching agent, stirring and leaching under heating conditions, and cooling to room temperature after the leaching is complete; wherein: the leaching agent is a combination of a quasi-ionic liquid and a chloride salt, the quasi-ionic liquid is choline chloride-malonic acid, the molar ratio of choline chloride to malonic acid is 1:1, and the chloride salt is FeCl3; 2) Add appropriate amount of deionized water to the leached product and stir thoroughly until precipitation is complete. During the stirring process, adjust the pH value to 2-3; 3) After the precipitation is completely completed at room temperature, the silver chloride precipitate and the filtrate are obtained by filtration, and the silver chloride precipitate is recovered; 4) The deionized water in the filtrate obtained in step 3) is evaporated and removed, and the remaining leaching agent is recycled.

2. The method for selectively extracting precious metal silver from solid waste using a quasi-ionic liquid system according to claim 1, characterized in that: In step 1), the silver-containing solid waste is discarded photovoltaic panels or discarded silver-plated parts.

3. The method for selectively extracting precious metal silver from solid waste using a quasi-ionic liquid system according to claim 1, characterized in that: In step 1), the liquid-solid ratio of the ionic liquid system to the silver-containing waste is 20:1~150:1mL / g, and the chloride concentration in the leaching agent is 0.2~0.8mol / L.

4. The method for selectively extracting precious metal silver from solid waste using a quasi-ionic liquid system according to claim 1, characterized in that: In step 1), the leaching temperature is 60-100°C, and the leaching time is 30-100 minutes.

5. The method for selectively extracting precious metal silver from solid waste using a quasi-ionic liquid system according to claim 1, characterized in that: In step 1), the chloride concentration in the leaching agent is 0.5 mol / L, the leaching temperature is 80° C., and the leaching time is 50 min.

6. The method for selectively extracting precious metal silver from solid waste using a quasi-ionic liquid system according to claim 1, characterized in that: In step 2), the mass ratio of the amount of deionized water added to the quasi-ionic liquid reaction system in step (1) is 0.5:1 to 2:

1.

7. The method for selectively extracting precious metal silver from solid waste using a quasi-ionic liquid system according to claim 1, characterized in that: In step 2), the pH value is adjusted to 2-3 with dilute nitric acid.

8. The method for selectively extracting precious metal silver from solid waste using a quasi-ionic liquid system according to claim 1, characterized in that: In step 3), the room temperature static precipitation reaction time is 30 to 200 minutes.

Citation Information

Cited By

  • Method for extracting silver in solid waste in eutectic system

    CN121087289A

  • Directional extraction method for silver in photovoltaic cell based on eutectic solvent

    CN121852716A

  • A method for directional extraction of silver in photovoltaic cells based on a deep eutectic solvent

    CN121852716B