Catalytic material for tail gas treatment and preparation method thereof
By using an amino-functionalized metal organic frame (NH2-UiO-66) in the catalyst to fix and disperse precious metals and coat Al-MOFs on its surface, the poor stability and poisoning of the catalyst in high temperature environment are solved, and efficient Exhaust gas treatment reduces costs and improves the service life of the catalyst.
Patent Information
- Application Number
- CN202411444224.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-16
- Publication Date
- 2024-11-15
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing catalysts have poor stability in high temperature environments, are prone to sintering or agglomeration, and are easily poisoned by toxic substances such as sulfides in the exhaust gas, resulting in a shortened service life, and the use of precious metals is large and the cost is high, which limits its large-scale promotion.
The amino-functionalized metal organic frame (NH2-UiO-66) is used as a support to fix and disperse precious metal catalysts, and the surface of which is coated with Al-MOFs is stabilized by heat treatment to form a catalytic material with excellent catalytic activity and stability.
Improve the stability and activity of the catalyst, extend the service life, reduce the aggregation and sintering of precious metals, enhance the adsorption and conversion efficiency of harmful gases, improve the efficiency of catalytic reactions, and improve durability through cladding protection. sex.
Smart Images

Figure CN118950102A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of automobile exhaust treatment, and in particular to a catalytic material for exhaust gas treatment and a preparation method thereof. Background Art
[0002] Nitrogen oxides (NO x ), carbon monoxide (CO), hydrocarbons (HC) and other harmful gases not only cause serious pollution to the atmospheric environment, but also pose a direct threat to human health. These pollutants in exhaust gas are the main cause of environmental problems such as haze and acid rain, seriously affecting air quality and ecosystems. Therefore, the development of efficient and stable catalytic materials to effectively purify exhaust gas and reduce the emission of harmful substances has become a key issue in achieving sustainable development.
[0003] Although existing catalysts can effectively reduce the emission of harmful gases under certain conditions, they have many defects in practical applications. First, many catalysts have poor stability in high temperature environments and are prone to sintering or agglomeration, resulting in a significant decrease in catalytic activity. Secondly, toxic substances such as sulfides and phosphorus in tail gas can easily poison the catalyst and reduce its service life. In addition, some catalysts require a large amount of precious metals during the manufacturing process, resulting in high costs, which limits their large-scale promotion and application. Therefore, it is urgent to develop a new catalytic material with higher stability, strong anti-poisoning ability, and the ability to maintain high efficiency and activity under complex working conditions to meet the needs of tail gas treatment technology. Summary of the invention
[0004] In view of the above situation, in order to overcome the defects of the prior art, the present invention provides a catalytic material for tail gas treatment and a preparation method thereof. The present invention uses amino-functionalized metal organic framework (NH2-UiO-66) as a carrier to effectively fix and disperse the precious metal catalyst, and then coats Al-MOFs on its surface after heat treatment, and further heat treats and stabilizes it to obtain a catalytic material with excellent catalytic activity and stability.
[0005] In order to achieve the above-mentioned purpose, the technical solution adopted by the present invention is as follows: The present invention proposes a catalytic material for exhaust gas treatment, and the catalytic material includes the following components: NH2-UiO-66, chloroplatinic acid, chloropalladic acid, chlororhodic acid, polyethyleneimine, aluminum salt, organic ligand, and regulator.
[0006] Preferably, the preparation method of NH2-UiO-66 specifically comprises the following steps: A1. Add zirconium chloride, aminoterephthalic acid and acetic acid into DMF, stir and dissolve evenly to form a precursor; A2. Transfer the precursor prepared in step A1 to a reactor, place it in an oven and heat it at 120°C for 24 hours, cool it to room temperature and collect the precipitate by centrifugation, wash the precipitate alternately with ethanol and deionized water three times, place it in a vacuum drying oven at 60°C and dry it for 12 to 24 hours to obtain NH2-UiO-66.
[0007] Preferably, in step A1, the ratio of zirconium chloride to aminoterephthalic acid is 1 mol:2 mol.
[0008] Preferably, in step A1, the ratio of acetic acid and DMF to zirconium chloride is 2-4 mol:10-20 L:1 mol.
[0009] Preferably, the aluminum salt is any one of aluminum chloride, aluminum nitrate and aluminum carbonate, the organic ligand is any one of terephthalic acid, trimesic acid and pyromellitic acid, and the regulator is any one of benzoic acid and formic acid.
[0010] The present invention also provides a method for preparing a catalytic material for tail gas treatment, which specifically comprises the following steps: S1. Take 2-4 g NH2-UiO-66 and evenly disperse it in 200 mL water, add chloroplatinic acid, chloropalladic acid, chlororhodic acid, and polyethyleneimine, and stir at 300-500 rpm for 12-24 h to obtain an active component solution; S2, filtering the active component solution prepared in step S1 to obtain an active component, placing the active component in a tubular furnace, introducing a nitrogen flow, heating to 600-800° C. and calcining for 2-5 h, cooling to room temperature, washing with water and ethanol alternately three times, and drying to obtain a catalyst intermediate 1; S3, weighing 200-400 mg of the catalyst intermediate 1 prepared in step S2, dispersing it in 50 mL of DMF, and evenly dispersing it by ultrasonication, adding aluminum salt, organic ligand and regulator, stirring and dispersing them evenly, placing them in a reaction kettle, and heating them in an oven at 160° C. for 16-24 h. After naturally cooling to room temperature, washing the precipitate with ethanol and water alternately for three times, and drying them to obtain the catalyst intermediate 2; S4. Placing the catalyst intermediate 2 prepared in step S3 in a tubular furnace, introducing a nitrogen flow, heating to 400-600° C. and calcining for 2-5 h, cooling to room temperature, washing three times with water and ethanol alternately, and drying to obtain a catalytic material for exhaust gas treatment.
[0011] Preferably, in step S1, the mass ratio of chloroplatinic acid, chloropalladic acid, chlororhodic acid, polyethyleneimine and NH2-UiO-66 is 0.1~0.3g: 0.1~0.2g: 0.2~0.5g: 0.2~0.4g: 2g.
[0012] Preferably, the flow rate of the nitrogen gas flow in step S2 and step S4 is 100 mL / min.
[0013] Preferably, in step S3, the usage ratio of the aluminum salt, the organic ligand, the regulator and the catalyst intermediate is 1 mmol: 1 mmol: 2-4 mmol: 200 mg.
[0014] The beneficial effects achieved by the present invention are as follows: The present invention uses an amino-functionalized metal organic framework (NH2-UiO-66) as a carrier to effectively fix and disperse the precious metal catalyst, thereby improving the stability and activity of the catalyst. By evenly dispersing the precious metal in the pores of the MOF, not only is its surface area and opportunity to contact the reactants increased, but also the stability of the catalyst under high temperature and complex reaction conditions is ensured, the aggregation and sintering of the precious metal is reduced, and the service life of the catalyst is extended. At the same time, the introduction of zirconium can effectively promote electron transfer and the activation of reactants. The high coordination number and unique electronic properties of zirconium help to optimize the interaction between the reactants and the active sites of the precious metals and reduce the reaction energy barrier. This makes harmful gases (such as NO x , CO and HC) can be adsorbed and converted by the catalyst more quickly, thereby improving the efficiency of the catalytic reaction.
[0015] In addition, the present invention further enhances the stability of the catalyst by coating an additional layer of heat-treated porous Al-MOFs material on the catalyst surface. This coating layer not only protects the active sites of the precious metals to prevent them from falling off and poisoning in high temperature environments, but also reduces the direct damage of harmful substances in the exhaust gas to the catalyst, thereby effectively improving the durability and activity of the catalyst in the exhaust gas treatment process. This dual protection mechanism makes the catalytic material of the present invention have higher reliability and efficiency in practical applications, meeting the requirements of sustainable development. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] In order to more clearly illustrate the technical solutions in the present invention or the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings in the following description are only for the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0017] Figure 1 is a transmission electron microscope image of the catalytic material prepared in Example 1; Figure 2 is the CO removal rate of the catalytic materials prepared in Examples 1-3 and Comparative Examples 1-2; Figure 3 is the NO removal rate of the catalytic materials prepared in Examples 1-3 and Comparative Examples 1-2; Figure 4 It is the HC removal rate of the catalytic materials prepared in Examples 1-3 and Comparative Examples 1-2. DETAILED DESCRIPTION
[0018] The present invention is further described in detail below through examples and comparative examples, but this should not be understood as the scope of the present invention being limited to the following examples, and all technologies implemented based on the above contents of the present invention belong to the scope of the present invention.
[0019] The experimental methods in the following examples are conventional methods unless otherwise specified; the experimental materials used in the following examples and comparative examples are purchased from commercial channels unless otherwise specified.
[0020] Example 1: This example proposes a catalytic material for exhaust gas treatment, which includes the following components: NH2-UiO-66, chloroplatinic acid, chloropalladic acid, chlororhodic acid, polyethyleneimine, aluminum chloride, terephthalic acid, and benzoic acid.
[0021] The preparation method of NH2-UiO-66 specifically comprises the following steps: A1. Add 1 mmol zirconium chloride, 2 mmol aminoterephthalic acid and 4 mmol acetic acid into 15 mL DMF and stir to dissolve evenly to form a precursor. A2. Transfer the precursor prepared in step A1 to a reactor, place it in an oven and heat it at 120°C for 24 hours, cool it to room temperature and collect the precipitate by centrifugation, wash the precipitate alternately with ethanol and deionized water three times, place it in a vacuum drying oven at 60°C and dry it for 12 to 24 hours to obtain NH2-UiO-66.
[0022] This embodiment also provides a method for preparing a catalytic material for tail gas treatment, which specifically includes the following steps: S1. Take 2 g NH2-UiO-66 and evenly disperse it in 200 mL water, add 0.1 g chloroplatinic acid, 0.2 g chloropalladic acid, 0.4 g chlororhodic acid, and 0.3 g polyethyleneimine, and stir at 300 rpm for 24 h to obtain an active component solution; S2, filtering the active component solution prepared in step S1 to obtain an active component, placing the active component in a tubular furnace, introducing a nitrogen flow at a flow rate of 100 mL / min, heating to 800° C. and calcining for 2 h, cooling to room temperature, washing with water and ethanol alternately three times, and drying to obtain a catalyst intermediate 1; S3, weighing 200 mg of the catalyst intermediate 1 prepared in step S2, dispersing it in 50 mL of DMF, and evenly dispersing it by ultrasonication, adding 1 mmol of aluminum chloride, 1 mmol of terephthalic acid, and 4 mmol of benzoic acid, stirring and dispersing it evenly, placing it in a reaction kettle, and heating it in an oven at 160° C. for 24 h. After naturally cooling to room temperature, washing the precipitate with ethanol and water alternately for three times, and drying it to obtain the catalyst intermediate 2; S4. The catalyst intermediate 2 prepared in step S3 is placed in a tubular furnace, a nitrogen flow at a flow rate of 100 mL / min is introduced, the temperature is raised to 600° C. and calcined for 2 h. After cooling to room temperature, the catalyst intermediate 2 is washed three times with water and ethanol alternately, and dried to obtain a catalytic material for exhaust gas treatment.
[0023] Example 2: This example proposes a catalytic material for exhaust gas treatment, which includes the following components: NH2-UiO-66, chloroplatinic acid, chloropalladic acid, chlororhodic acid, polyethyleneimine, aluminum nitrate, trimesic acid, and formic acid.
[0024] The preparation method of NH2-UiO-66 specifically comprises the following steps: A1. Add 1 mmol zirconium chloride, 2 mmol aminoterephthalic acid and 2 mmol acetic acid into 20 mL DMF and stir to dissolve evenly to form a precursor; A2. Transfer the precursor prepared in step A1 to a reactor, place it in an oven and heat it at 120°C for 24 hours, cool it to room temperature and collect the precipitate by centrifugation, wash the precipitate alternately with ethanol and deionized water three times, place it in a vacuum drying oven at 60°C and dry it for 12 to 24 hours to obtain NH2-UiO-66.
[0025] This embodiment also provides a method for preparing a catalytic material for tail gas treatment, which specifically includes the following steps: S1. Take 3 g NH2-UiO-66 and evenly disperse it in 200 mL water, add 0.3 g chloroplatinic acid, 0.1 g chloropalladic acid, 0.2 g chlororhodic acid, and 0.4 g polyethyleneimine, and stir at 300-500 rpm for 12 h to obtain an active component solution; S2, filtering the active component solution prepared in step S1 to obtain an active component, placing the active component in a tubular furnace, introducing a nitrogen flow at a flow rate of 100 mL / min, heating to 600° C. and calcining for 5 h, cooling to room temperature, washing with water and ethanol alternately three times, and drying to obtain a catalyst intermediate 1; S3, weighing 400 mg of the catalyst intermediate 1 prepared in step S2, dispersing it in 50 mL of DMF, and evenly dispersing it by ultrasonication, adding 1 mmol of aluminum salt, 1 mmol of trimesic acid and 2 mmol of formic acid, stirring and dispersing it evenly, and placing it in a reaction kettle, placing it in an oven and heating it at 160° C. for 16 h, cooling it naturally to room temperature, and then washing the precipitate with ethanol and water alternately three times, and drying it to obtain the catalyst intermediate 2; S4. The catalyst intermediate 2 prepared in step S3 is placed in a tubular furnace, a nitrogen flow at a flow rate of 100 mL / min is introduced, the temperature is raised to 400° C. and calcined for 5 h. After cooling to room temperature, the catalyst intermediate 2 is washed three times with water and ethanol alternately, and dried to obtain a catalytic material for exhaust gas treatment.
[0026] Example 3: This example proposes a catalytic material for exhaust gas treatment, which includes the following components: NH2-UiO-66, chloroplatinic acid, chloropalladic acid, chlororhodic acid, polyethyleneimine, aluminum carbonate, pyromellitic acid, and benzoic acid.
[0027] The preparation method of NH2-UiO-66 specifically comprises the following steps: A1. Add 1 mmol zirconium chloride, 2 mmol aminoterephthalic acid and 3 mmol acetic acid into 10 mL DMF and stir to dissolve evenly to form a precursor; A2. Transfer the precursor prepared in step A1 to a reactor, place it in an oven and heat it at 120°C for 24 hours, cool it to room temperature and collect the precipitate by centrifugation, wash the precipitate alternately with ethanol and deionized water three times, place it in a vacuum drying oven at 60°C and dry it for 16 hours to obtain NH2-UiO-66.
[0028] This embodiment also provides a method for preparing a catalytic material for tail gas treatment, which specifically includes the following steps: S1. Take 3 g NH2-UiO-66 and disperse it evenly in 200 mL water, add 0.2 g chloroplatinic acid, 0.1 g chloropalladic acid, 0.5 g chlororhodic acid, and 0.2 g polyethyleneimine, and stir at 400 rpm for 16 h to obtain an active component solution; S2, filtering the active component solution prepared in step S1 to obtain an active component, placing the active component in a tubular furnace, introducing a nitrogen flow at a flow rate of 100 mL / min, heating to 700° C. and calcining for 4 h, cooling to room temperature, washing with water and ethanol alternately three times, and drying to obtain a catalyst intermediate 1; S3, weighing 300 mg of the catalyst intermediate 1 prepared in step S2, dispersing it in 50 mL of DMF, and evenly dispersing it by ultrasonication, adding 1 mmol of aluminum carbonate, 1 mmol of pyromellitic acid, and 3 mmol of benzoic acid, stirring and dispersing it evenly, placing it in a reaction kettle, and heating it in an oven at 160° C. for 20 h. After naturally cooling to room temperature, washing the precipitate with ethanol and water alternately for three times, and drying it to obtain the catalyst intermediate 2; S4. The catalyst intermediate 2 prepared in step S3 is placed in a tubular furnace, a nitrogen flow at a flow rate of 100 mL / min is introduced, the temperature is raised to 500° C. and calcined for 4 h. After cooling to room temperature, the catalyst intermediate 2 is washed three times with water and ethanol alternately, and dried to obtain a catalytic material for exhaust gas treatment.
[0029] Comparative Example 1: This comparative example proposes a catalytic material for exhaust gas treatment, which differs from Example 1 only in that NH2-UiO-66 is replaced with clay ceramic of the same mass, and the other components, component contents, and experimental steps are the same as those in Example 1.
[0030] Comparative Example 2: This comparative example proposes a catalytic material for exhaust gas treatment, which differs from Example 1 only in that aluminum chloride, terephthalic acid and benzoic acid are not added, and the remaining components, component contents, and experimental steps are the same as those in Example 1. The catalytic material includes the following components: NH2-UiO-66, chloroplatinic acid, chloropalladic acid, chlororhodic acid, and polyethyleneimine.
[0031] The preparation method of NH2-UiO-66 specifically comprises the following steps: A1. Add 1 mmol zirconium chloride, 2 mmol aminoterephthalic acid and 4 mmol acetic acid into 15 mL DMF and stir to dissolve evenly to form a precursor. A2. Transfer the precursor prepared in step A1 to a reactor, place it in an oven and heat it at 120°C for 24 hours, cool it to room temperature and collect the precipitate by centrifugation, wash the precipitate alternately with ethanol and deionized water three times, place it in a vacuum drying oven at 60°C and dry it for 12 to 24 hours to obtain NH2-UiO-66.
[0032] This embodiment also provides a method for preparing a catalytic material for tail gas treatment, which specifically includes the following steps: S1. Take 2 g NH2-UiO-66 and evenly disperse it in 200 mL water, add 0.1 g chloroplatinic acid, 0.2 g chloropalladic acid, 0.4 g chlororhodic acid, and 0.3 g polyethyleneimine, and stir at 300 rpm for 24 h to obtain an active component solution; S2. Filter the active component solution prepared in step S1 to obtain an active component, place the active component in a tubular furnace, introduce a nitrogen flow with a flow rate of 100 mL / min, heat to 800° C. and calcine for 2 h, cool to room temperature, wash three times with water and ethanol alternately, and dry to obtain a catalytic material for exhaust gas treatment.
[0033] Experimental Example 1: The microstructure of the catalytic material prepared in Example 1 was observed using a scanning electron microscope.
[0034] Figure 1 This is a transmission electron microscope image of the catalytic material prepared in Example 1. As shown in the figure, the catalytic material has a two-layer structure. The outer layer is coated with Al-MOFs that collapsed after calcination, which can effectively protect the active components of the inner layer, indicating that the catalytic material for exhaust gas treatment proposed in the present invention was successfully prepared.
[0035] Experimental Example 2: Simulation Experiment Performance Test 1 g of the catalytic material prepared in Examples 1-3 and Comparative Examples 1-2 was respectively placed in a quartz tube, the quartz tube was placed in a tubular furnace, and a mixed gas was introduced, the mixed gas included 10000 ppm carbon monoxide (CO), 2000 ppm nitric oxide (NO), 4000 ppm hydrocarbons (HC, 2000 ppm C3H8, 2000 ppm C3H6), inert gas N2 was used as a carrier, the gas flow rate was 100 mL / min, the temperature was set to 500°C, the concentrations of CO, NO and HC in the outlet gas were measured every 30 min, and the removal rate of each gas was calculated.
[0036] Figure 2 is the CO removal rate of the catalytic materials prepared in Examples 1-3 and Comparative Examples 1-2; Figure 3 is the NO removal rate of the catalytic materials prepared in Examples 1-3 and Comparative Examples 1-2; Figure 4 It is the HC removal rate of the catalytic materials prepared in Examples 1-3 and Comparative Examples 1-2. As shown in the figure, the catalytic effect of the catalytic materials in Examples 1-3 is excellent, and the removal effect is significantly improved compared with Comparative Example 1, indicating that NH2-UiO-66 as a carrier can effectively improve the catalytic activity. However, the catalytic activity of the catalytic material prepared in Comparative Example 2 decreases over time, which indicates that the catalytic material prepared in Comparative Example 2 is not protected by the Al-MOFs thermal degradation material, and the catalytic active sites are gradually poisoned and fail.
[0037] Experimental Example 3: Actual Application Performance Testing 50 fuel vehicles that meet national emission standards were randomly selected, and the catalytic materials in Examples 1-3 and Comparative Examples 1-2 were applied to the exhaust purification systems of these vehicles to replace the original commercial catalysts. The 50 vehicles were divided into five groups, with ten vehicles in each group. Ten vehicles for each catalyst were set up for parallel experiments. The vehicles drove 500 km normally, and the exhaust gas of the vehicles was tested every 100 km to record the carbon monoxide (CO), nitrogen oxides (NO x The emissions of ) and hydrocarbons (HC) were averaged after 500 km. The test results are shown in Table 1.
[0038] Table 1 Practical application test results
[0039] Table 1 shows the actual application test results of the catalytic materials prepared in Examples 1-3 and Comparative Examples 1-2. As shown in the table, the catalytic materials prepared in Examples 1-3 have excellent catalytic conversion effects, and their performance is much better than that of the catalytic materials prepared in Comparative Example 1, indicating that NH2-UiO-66 as a carrier can well disperse the active components and improve the catalytic performance. The performance of the catalytic material prepared in Comparative Example 2 is slightly lower than that of the embodiment, because during use, the catalytic material prepared in Comparative Example 2 is not protected by the outer layer material, and the catalytic active sites gradually fail.
[0040] The present invention and its implementation methods are described above, which is not restrictive. The drawings are only one of the implementation methods of the present invention, and the actual application is not limited thereto. In short, if ordinary technicians in the field are inspired by it and design methods and embodiments similar to the technical solution without creativity without departing from the purpose of the invention, they should all fall within the protection scope of the present invention.
Claims
1. A catalytic material for tail gas treatment, It is characterized in that The catalytic material comprises the following components: NH 2 -UiO-66, chloroplatinic acid, chloropalladic acid, chlororhodic acid, polyethyleneimine, aluminum salt, organic ligand, regulator; The NH 2 -The preparation method of UiO-66 specifically comprises the following steps: A1. Add zirconium chloride, aminoterephthalic acid and acetic acid into DMF, stir and dissolve evenly to form a precursor; A2. The precursor prepared in step A1 was transferred to a reactor, heated at 120°C for 24 h, cooled to room temperature, and centrifuged to collect the precipitate. The precipitate was washed alternately with ethanol and deionized water three times, and dried to obtain NH 2 -UiO-66.
2. A catalytic material for exhaust gas treatment according to claim 1, It is characterized in that In the step A1, the ratio of zirconium chloride to aminoterephthalic acid is 1 mol:2 mol.
3. A catalytic material for exhaust gas treatment according to claim 2, It is characterized in that In the step A1, the usage ratio of acetic acid and DMF to zirconium chloride is 2-4 mol:10-20 L:1 mol.
4. A catalytic material for tail gas treatment according to claim 3, It is characterized in that The aluminum salt is any one of aluminum chloride, aluminum nitrate and aluminum carbonate, the organic ligand is any one of terephthalic acid, trimesic acid and pyromellitic acid, and the regulator is any one of benzoic acid and formic acid.
5. A method for preparing a catalytic material for tail gas treatment according to any one of claims 1 to 4, It is characterized in that The specific steps include: S1, take 2~4 g NH 2 -UiO-66 was evenly dispersed in 200 mL of water, and chloroplatinic acid, chloropalladic acid, chlororhodic acid, and polyethyleneimine were added, and stirred at 300-500 rpm for 12-24 h to obtain an active component solution; S2, filtering the active component solution prepared in step S1 to obtain an active component, placing the active component in a tubular furnace, introducing a nitrogen flow, heating to 600-800° C. and calcining for 2-5 h, cooling to room temperature, washing with water and ethanol alternately three times, and drying to obtain a catalyst intermediate 1; S3, weighing 200-400 mg of the catalyst intermediate 1 prepared in step S2, dispersing it in 50 mL of DMF, and evenly dispersing it by ultrasonication, adding aluminum salt, organic ligand and regulator, stirring and dispersing it evenly, and placing it in a reactor, heating it at 160° C. for 16-24 h, cooling it naturally to room temperature, and then washing the precipitate with ethanol and water alternately three times, and drying it to obtain the catalyst intermediate 2; S4. Placing the catalyst intermediate 2 prepared in step S3 in a tubular furnace, introducing a nitrogen flow, heating to 400-600° C. and calcining for 2-5 h, cooling to room temperature, washing three times with water and ethanol alternately, and drying to obtain a catalytic material for exhaust gas treatment.
6. The method for preparing the catalytic material for tail gas treatment according to claim 5, It is characterized in that In the step S1, chloroplatinic acid, chloropalladic acid, chlororhodic acid, polyethyleneimine and NH 2 -The mass ratio of UiO-66 is 0.1~0.3g:0.1~0.2g:0.2~0.5g:0.2~0.4g:2g.
7. The method for preparing the catalytic material for tail gas treatment according to claim 6, It is characterized in that In the step S3, the dosage ratio of the aluminum salt, the organic ligand, the regulator and the catalyst intermediate is 1 mmol: 1 mmol: 2-4 mmol: 200 mg.
Citation Information
Patent Citations
Preparation of active carbon fiber-metal organic framework composite material, and composite material and application
CN106807329A
SCR (Selective Catalytic Reduction) denitrification catalyst capable of resisting potassium intoxication and preparation method thereof
CN107185593A
Defective MIL-53 (Al) metal organic framework and preparation method and application thereof
CN107899559A
Method for preparing tail gas catalysis purifier
CN108187753A
Pt NPs@MOFs photocatalyst and preparation method and application thereof
CN108620132A