Seat paste, preparation method thereof and application of seat paste in wind power tower
By using ordinary silicate cement, fast hard composite sulfaaluminate cement, natural sand and fly ash beads in the seat slurry, its fluidity and settling time are adjusted, and the seat slurry in the wind power tower is solved. The problem of high fluidity or insufficient strength has achieved high strength and suitable fluidity slurry, meeting the construction needs of wind power towers.
Patent Information
- Application Number
- CN202411060393.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-05
- Publication Date
- 2024-11-15
AI Technical Summary
The existing slurry has the problem of too much fluidity or insufficient strength in the wind power steel-concrete tower, which cannot meet the high strength and high fluidity requirements of the wind power tower, and there are risks such as cracking and stratification.
Ordinary silicate cement and fast hard composite sulfur aluminate cement as the basic cementing material, combined with natural sand and fly ash beads, water reducer and cellulose are added to adjust the flow and settling time of the mortar to prepare a A special slurry for cement-based wind power seats has high strength grade, low fluidity and long settling time.
The 28d strength of the seat slurry is greater than 80MPa, the expansion degree is less than 200mm, and the settling time is greater than or equal to 60min, which meets the construction requirements of the wind power tower and improves the stability and use efficiency of the material.
Smart Images

Figure CN118955062A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of building materials, and in particular to a base slurry and a preparation method thereof and application thereof in a wind power tower. Background Art
[0002] Wind power generation is one of the important components of the development and utilization of new energy, and has developed rapidly in recent years. The tower is the main supporting component of the wind turbine. With the rapid development of wind power generation, the size of the wind turbine head is getting larger and larger. The original steel tower can no longer meet the current use requirements, so the current wind turbine towers mostly use a hybrid tower that combines concrete and steel, that is, a steel-concrete tower. The steel-concrete tower is usually a reinforced concrete cylindrical structure, which can be prefabricated in sections and pieces in the prefabrication plant, and then the finished concrete tower segments are spliced and assembled at the construction site. At present, the splicing parts of the concrete tower segments are mostly connected with epoxy resin, which has high strength. However, since epoxy resin and cement concrete are two different materials, the degree of negative temperature shrinkage is different, and there is a risk of cracking and delamination after long-term use.
[0003] At present, some researchers have proposed to use cement-based mortar materials instead of epoxy resin. Since the wind power steel-concrete tower assembly section is small, the joint buffer is required to be greater than 5 cm, and it is also a high-altitude operation, so the requirements for the performance of cement-based mortar are relatively high.
[0004] Seat mortar is a special mortar required in prefabricated concrete structures. Seat mortar is a dry mix composed of cement as the basic binder, fine aggregate, high-performance admixtures and other materials. After adding water and stirring, it has properties such as early strength and high strength, and is suitable for the installation and construction of prefabricated components. However, current seat mortars are usually used in prefabricated concrete beams, columns and shear walls. Since they are not specially designed for wind power steel-concrete towers, most seat mortars have the defects of too high fluidity or insufficient strength grade. Summary of the invention
[0005] In view of this, the present invention provides a base slurry and a preparation method thereof and application in a wind power tower. The base slurry provided by the present invention has high strength grade, low fluidity, and long setting time, and can meet the construction requirements of wind power towers. It is a cement-based base slurry specially used for wind power.
[0006] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0007] A seat slurry comprises the following components in mass fraction: 33-43% of ordinary Portland cement, 6-16% of rapid hardening composite sulphoaluminate cement, 39-49% of sand, 1.5-5% of water reducing agent, 0.3-0.6% of cellulose and 2-4% of fly ash floating beads.
[0008] Preferably, the 28-day compressive strength of the ordinary Portland cement is ≥55 MPa.
[0009] Preferably, the setting time of the fast-hardening composite sulphoaluminate cement is ≤180 min, and the 28-day compressive strength is >42.5 MPa.
[0010] Preferably, the sand is natural sand, the mesh size of the natural sand is 20 to 80 meshes, and the mud content of the natural sand is less than 1wt%.
[0011] Preferably, the water reducer is polycarboxylic acid high performance water reducer powder.
[0012] Preferably, the cellulose is 400 viscosity cellulose.
[0013] Preferably, the water storage rate of the fly ash beads is less than 95%.
[0014] The present invention also provides a method for preparing the seat slurry described in the above scheme, comprising the following steps:
[0015] Ordinary Portland cement, fast-hardening composite sulphoaluminate cement, sand, water reducing agent, cellulose and fly ash beads are mixed to obtain the seat slurry.
[0016] The present invention also provides the use of the seat slurry described in the above scheme or the seat slurry prepared by the preparation method described in the above scheme in a wind power tower.
[0017] Preferably, the seat slurry is mixed with water during application, and the mass of the water is 10-15% of the mass of the seat slurry.
[0018] The present invention provides a seat slurry, comprising the following components by mass fraction: 33-43% of ordinary Portland cement, 6-16% of fast-hardening composite sulphoaluminate cement, 39-49% of sand, 1.5-5% of water reducer, 0.3-0.6% of cellulose, and 2-4% of fly ash beads. The inventors have found that the seat slurry is applied to the wind power tower frame and needs to meet the following requirements: on the one hand, the mortar is required to have a higher strength grade, and the 28d strength needs to reach more than 80MPa; on the other hand, the mortar is required to have a smaller fluidity (less than 200mm) to avoid excessive vertical flow during construction, resulting in material waste; the third aspect is also required to have a longer initial setting time (greater than or equal to 60min) to meet the construction time requirements. The present invention uses ordinary Portland cement and fast-hardening composite sulphoaluminate cement as basic cementing materials, uses sand as fine aggregate, uses fly ash beads as admixtures, and then adds a water reducer to adjust the fluidity of the mortar. The obtained seat slurry has a high strength grade, low fluidity, and a long setting time. The results of the embodiments show that the 28d strength of the seat slurry of the present invention is greater than 80 MPa, the expansion is less than 200 mm, and the setting time is greater than or equal to 60 min, which can meet the construction requirements of the wind power tower. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 This is the test result of the expansion degree of the seat slurry in Example 1 of the present invention. DETAILED DESCRIPTION
[0020] The invention provides a seat slurry, comprising the following components in mass fraction: 33-43% of ordinary Portland cement, 6-16% of rapid hardening composite sulphoaluminate cement, 39-49% of sand, 1.5-5% of water reducing agent, 0.3-0.6% of cellulose and 2-4% of fly ash floating beads.
[0021] Unless otherwise specified, all raw materials / components used in the present invention are commercially available products.
[0022] In terms of mass fraction, the seat slurry provided by the present invention includes 33-43% of ordinary Portland cement, preferably 36-40%, and more preferably 38%; the 28-day compressive strength of the ordinary Portland cement is preferably ≥55MPa. In a specific embodiment of the present invention, the model of the ordinary Portland cement is preferably p.o52.5; the present invention controls the 28-day strength of ordinary Portland cement to above 55MPa, and can ensure the strength of the seat slurry based on the above-mentioned dosage.
[0023] In terms of mass fraction, the seat slurry provided by the present invention includes 6-16% of fast-hardening composite sulphoaluminate cement, preferably 8-12%, and more preferably 11%; the setting time of the fast-hardening composite sulphoaluminate cement is preferably ≤180min, and the 28-day compressive strength is preferably >42.5MPa; in a specific embodiment of the present invention, the fast-hardening composite sulphoaluminate cement is preferably 42.5 fast-hardening composite sulphoaluminate cement. The present invention uses ordinary Portland cement and fast-hardening composite sulphoaluminate cement in combination, and strictly controls the ratio of ordinary Portland cement and fast-hardening composite sulphoaluminate cement, which can ensure that the seat slurry has high strength both in the early and late stages.
[0024] In terms of mass fraction, the seat slurry provided by the present invention includes 39-49% sand, preferably 42-45%, and more preferably 44%; the sand is preferably natural sand, more preferably dried natural sand, specifically dried river sand; the mesh number of the natural sand is preferably 20-80 mesh, and the mud content of the natural sand is preferably less than 1wt%; in a specific embodiment of the present invention, it is preferred to mix 20-40 mesh natural sand and 40-80 mesh natural sand, and the mass ratio of the 20-40 mesh natural sand and 40-80 mesh natural sand is preferably 1:1. Natural sand has good grain shape and high roundness. Under the same expansion degree, the water consumption is lower, and the natural sand has better firmness. The present invention adds natural sand to the seat slurry, which can reduce water consumption and increase strength.
[0025] In terms of mass fraction, the slurry provided by the present invention includes 1.5-5% water reducer, preferably 5-4%, and more preferably 3.5%; the water reducer is preferably a polycarboxylic acid high-performance water reducer, and more preferably a polycarboxylic acid high-performance water reducer powder; the water reduction rate of the water reducer is preferably ≥30%, and more preferably 30%-32%. In the present invention, the main function of the water reducer is to reduce the amount of water, disperse cement particles, and more fully hydrate to improve the strength of cement; and the present invention uses a water reducer with a higher water reduction rate, which can ensure a lower water-cement ratio. At the same time, the polycarboxylic acid high-performance water reducer used in the present invention has a collapse-preserving effect, which can improve the retention effect.
[0026] In terms of mass fraction, the seat slurry provided by the present invention comprises 0.3-0.6% cellulose, preferably 0.5%; the cellulose is preferably 400 viscosity cellulose. In the present invention, the cellulose can play the role of retaining water, improving workability, and reducing fluidity.
[0027] In terms of mass fraction, the seat slurry provided by the present invention includes 2-4% fly ash floating beads, preferably 3%; the water storage rate of the fly ash floating beads is preferably <95%; the particle size of the fly ash floating beads is preferably ≤45μm. In the present invention, the addition of fly ash floating beads can improve the stability of the seat slurry, avoid the problem of excessive use of adhesive material and concentrated hydration heat affecting the stability of the material, and the fly ash floating beads can reduce the water consumption and improve the fluidity of the seat slurry. In the present invention, if the fly ash floating beads are omitted, the water reduction rate will be insufficient, and the water consumption needs to be increased, and the hydration temperature will be too high, with the risk of cracking.
[0028] The present invention also provides a method for preparing the seat slurry described in the above scheme, comprising the following steps:
[0029] Ordinary Portland cement, fast-hardening composite sulphoaluminate cement, sand, water reducing agent, cellulose and fly ash beads are mixed to obtain the seat slurry.
[0030] In the present invention, the mixing is preferably carried out in a mortar mixer; the order of adding the various raw materials during the mixing is preferably: first add sand to the mortar mixer, then add ordinary Portland cement and fast-hardening composite sulphoaluminate cement, and finally add fly ash beads, cellulose and water reducer. After the raw materials are added, continue stirring for 250 to 350 seconds, preferably continue stirring for 300 seconds, to obtain the seat slurry.
[0031] The present invention also provides the application of the seat slurry described in the above scheme or the seat slurry prepared by the preparation method described in the above scheme in a wind power tower; the wind power tower is preferably a wind power steel-concrete tower. In the present invention, the seat slurry is mixed with water during application, and the mass of the water is preferably 10-15% of the mass of the seat slurry, and more preferably 12%. The present invention has no special requirements for the specific application method of the seat slurry, and the method well known to those skilled in the art can be used.
[0032] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0033] The sources of the raw materials in the following embodiments are as follows: Po52.5 ordinary Portland cement was purchased from Jinyu Cement, and the 28-day compressive strength was required to be not less than 55 MPa; 42.5 fast-hardening composite sulphoaluminate cement was purchased from Polar Bear Cement, with a setting time of not more than 180 minutes and a 28-day strength greater than 42.5 MPa; the dried natural sand was selected from Chengde Beiyan Company, with a mesh size of 20 to 80 meshes and a mud content of less than 1wt%; polycarboxylic acid high-performance water-reducing agent powder and 400 viscosity cellulose were purchased from Shijiazhuang Yaxi Building Materials, and fly ash beads were purchased from Quwo County Xudong Building Materials Co., Ltd., and the water storage rate was required to be less than 95%.
[0034] Example 1
[0035] The ingredients of the seat slurry are as follows: 38% of p.o52.5 ordinary Portland cement, 11% of 42.5 fast-hardening composite sulphoaluminate cement, 44% of 20-80 mesh dried natural sand (the mass ratio of 20-40 mesh natural sand to 40-80 mesh natural sand is 1:1), 3.5% of polycarboxylic acid high-performance water-reducing agent powder, 0.5% of 400 viscosity cellulose, and 3% of fly ash beads.
[0036] The preparation method of the seat slurry is as follows: firstly, add dried natural sand into a mortar mixer, then add ordinary silicate cement and fast-hardening composite sulphoaluminate cement, and finally add fly ash beads, cellulose and polycarboxylic acid high-performance water reducing agent. After the raw materials are added, continue stirring for 300 seconds to obtain the seat slurry. When the obtained seat slurry is used, add water and stir, and the amount of water added is 12% of the mass of the seat slurry.
[0037] The compressive strength, flexural strength, chloride ion content and water bleeding rate of the obtained mortar were tested. The experimental test was based on the "Standard for Basic Performance Test Methods of Building Mortar", and the experimental data was determined based on the "Q / GYJP 0001-2023 Internal Standard for High-Strength Mortar for Wind Power Generation" issued by Hebei Jianpeng Industry. The test results are shown in Table 1.
[0038] Table 1 Slurry performance test results
[0039]
[0040] It can be seen from the data in Table 1 that the seat slurry prepared by the present invention has low fluidity, long setting time, high compressive strength and flexural strength, and can meet the construction requirements of wind power towers.
[0041] The expansion degree of the obtained seat slurry was tested, and the test method referred to the "Q / GYJP0001-2023 Internal Standard of High-strength Seat Slurry for Wind Power" issued by Hebei Jianpeng Industry. The results are as follows Figure 1 As shown, take Figure 1 The average value of the diameters in two mutually perpendicular directions is taken as the expansion degree of the slurry. Figure 1 It can be seen that the expansion of the seat slurry is 164 mm, indicating that the fluidity of the seat slurry of the present invention is relatively small and meets the construction requirements of the wind power tower.
[0042] The setting time (initial setting time) of the obtained seat slurry was tested. The test method referred to the "Q / GYJP 0001-2023 Enterprise Internal Standard of High-strength Seat Slurry for Wind Power" issued by Hebei Jianpeng Industry. The results showed that the setting time of the seat slurry was 60 minutes.
[0043] Example 2
[0044] The ingredients of the seat slurry are as follows: 39% of p.o52.5 ordinary Portland cement, 10% of 42.5 fast-hardening composite sulphoaluminate cement, 43% of 20-80 mesh dried natural sand (the mass ratio of 20-40 mesh natural sand to 40-80 mesh natural sand is 1:1), 3.4% of polycarboxylic acid high-performance water-reducing agent powder, 0.6% of 400 viscosity cellulose, and 4% of fly ash beads.
[0045] The preparation method is the same as that in Example 1.
[0046] Example 3
[0047] The ingredients of the seat slurry are as follows: 36.5% p.o52.5 ordinary Portland cement, 12.5% 42.5 fast-hardening composite sulphoaluminate cement, 46.4% 20-80 mesh dried natural sand (the mass ratio of 20-40 mesh natural sand to 40-80 mesh natural sand is 1:1), 2% polycarboxylic acid high-performance water-reducing agent powder, 0.6% 400 viscosity cellulose, and 2% fly ash beads.
[0048] The preparation method is the same as that in Example 1.
[0049] Example 4
[0050] The ingredients of the seat slurry are as follows: 40% of p.o52.5 ordinary Portland cement, 12% of 42.5 fast-hardening composite sulphoaluminate cement, 40.7% of 20-80 mesh dried natural sand (the mass ratio of 20-40 mesh natural sand to 40-80 mesh natural sand is 1:1), 4% of polycarboxylic acid high-performance water-reducing agent powder, 0.3% of 400 viscosity cellulose, and 3% of fly ash beads.
[0051] The preparation method is the same as that in Example 1.
[0052] The fluidity, setting time, compressive strength, flexural strength, chloride ion content and water seepage rate of Examples 2 to 4 were tested, and the results were similar to those of Example 1. The 28d strength of the slurry was greater than 80 MPa, the fluidity was less than 200 mm, and the setting time was greater than or equal to 60 min (60 to 80 min), which met the construction requirements of the wind power tower.
[0053] Comparative Example 1
[0054] Other conditions were the same as those in Example 1, except that the 42.5 fast-hardening composite sulphoaluminate cement was replaced with p.o.52.5 ordinary Portland cement. The results showed that the setting time of the obtained slurry was greatly prolonged, and the 1d strength was greatly reduced.
[0055] Comparative Example 2
[0056] Other conditions were the same as those in Example 1, except that the fly ash beads were replaced with S95 mineral powder; the results showed that the resulting slurry could not be completely hydrated when the water addition amount was 12%.
[0057] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A seat slurry, characterized in that: The invention comprises the following components in mass fraction: 33-43% of ordinary Portland cement, 6-16% of rapid hardening composite sulphoaluminate cement, 39-49% of sand, 1.5-5% of water reducing agent, 0.3-0.6% of cellulose and 2-4% of fly ash floating beads.
2. The seat slurry according to claim 1, characterized in that: The 28-day compressive strength of the ordinary Portland cement is ≥55MPa.
3. The seat slurry according to claim 1, characterized in that: The setting time of the fast-hardening composite sulphoaluminate cement is ≤180 min, and the 28-day compressive strength is >42.5 MPa.
4. The seat slurry according to claim 1, characterized in that: The sand is natural sand, the mesh number of the natural sand is 20-80 meshes, and the mud content of the natural sand is less than 1wt%.
5. The seat slurry according to claim 1, characterized in that: The water reducing agent is a polycarboxylic acid high performance water reducing agent.
6. The seat slurry according to claim 1, characterized in that: The cellulose is 400 viscosity cellulose.
7. The seat slurry according to claim 1, characterized in that: The water storage rate of the fly ash floating beads is less than 95%.
8. The method for preparing the seat slurry according to any one of claims 1 to 7, characterized in that: The following steps are involved: Ordinary Portland cement, fast-hardening composite sulphoaluminate cement, sand, water reducing agent, cellulose and fly ash beads are mixed to obtain the seat slurry.
9. Use of the base slurry according to any one of claims 1 to 7 or the base slurry prepared by the preparation method according to claim 8 in a wind power tower.
10. The use according to claim 9, characterized in that: When used, the seat slurry is mixed with water, and the mass of the water is 10-15% of the mass of the seat slurry.