Modified polyether water reducer as well as preparation method and application thereof

By using modified polyether water reducer prepared by ethylene oxide propylene oxide block polyether and other raw materials, the problems of insufficient water reduction rate and complex operation in UHPC are solved, and efficient water reduction and mechanical performance improvement are achieved , simplifies the process.

CN118955814APending Publication Date: 2024-11-15CHINA WEST CONSTR ACAD OF BUILDING MATERIALS CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411073075.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-06
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The conventional polycarboxylic acid water reducing agent in existing ultra-high performance concrete (UHPC) shows problems such as insufficient water reduction rate, large amount of mixing, long stirring time, large viscosity and insufficient fluidity at low water bonding ratio, and traditional processes High temperature and high pressure reactions are required, and the operation is complicated.

Method used

Ethylene oxide propylene oxide block polyether is used as a modified polyether water reducer, and is prepared by radical polymerization, combining raw materials such as methacrylic acid-β-hydroxyethyl phosphate and maleic anhydride to adjust the molecular structure. and proportions to achieve high water reduction and viscosity reduction effects, and do not rely on high temperature and high pressure reactions.

Benefits of technology

The reversal time of UHPC is significantly improved, the later strength is maintained, and the preparation process is simplified. The molecular structure is adapted to the dispersion of particles of different sizes, which improves the working and mechanical properties of concrete.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004981411230000051
    Figure BDA0004981411230000051
  • Figure BDA0004981411230000091
    Figure BDA0004981411230000091
Patent Text Reader

Abstract

The invention belongs to the technical field of building materials, and particularly relates to a modified polyether water reducer as well as a preparation method and application thereof. The modified polyether water reducer is prepared from the following raw materials: ethylene oxide-propylene oxide block polyether, unsaturated polyoxyethylene ether, acrylic acid, methacrylic acid-beta-hydroxyethyl phosphate and maleic anhydride. The modified polyether water reducer has the characteristics of high water reducing rate, good viscosity reducing effect and the like, can obviously prolong the rewinding time of the expansion degree of UHPC when being applied to a UHPC system, does not influence the later strength of the UHPC, and does not involve high-temperature and high-pressure reactions in the preparation process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of building materials, and specifically relates to a modified polyether water reducing agent and a preparation method and application thereof. Background Art

[0002] Ultra-high performance concrete (UHPC) has excellent properties such as ultra-high strength, high toughness, low permeability and high durability, and is gradually replacing ordinary concrete in some building structures with special technical requirements. However, due to the ultra-high amount of adhesive and ultra-low water-binder ratio design of UHPC, the water reduction rate of conventional polycarboxylate water-reducing agent in UHPC with low water-binder ratio is insufficient, resulting in large dosage, long mixing time, high viscosity and insufficient fluidity of UHPC.

[0003] Xu Wenying et al. developed an ultra-high performance water reducer for UHPC by introducing amino groups into the main chain and side chain at the same time, and hydrophobic groups and hyperbranched structures into the side chain. The water reducer has a low water-cement ratio below 0.2 and has high water reduction rate and viscosity reduction functions. However, this process requires the synthesis of intermediate raw materials such as hyperbranched monomers and polysuccinimide, involves high temperature and high pressure reactions, has a long time cycle and complex operation (Reference: Synthesis and Performance Research of Ultra-High Performance Water Reducer for UHPC, New Building Materials, Issue 001, 2022). Summary of the invention

[0004] The purpose of the present invention is to provide a modified polyether water reducer and a preparation method and application thereof. The modified polyether water reducer has the characteristics of high water reduction rate and good viscosity reduction effect. The application of the modified polyether water reducer in the UHPC system can significantly improve the rewinding time of the UHPC without affecting the later strength of the UHPC. At the same time, the preparation process does not involve high temperature and high pressure reactions.

[0005] Specifically, the present invention provides the following technical solutions:

[0006] A modified polyether water reducer uses ethylene oxide and propylene oxide block polyether as its preparation raw materials.

[0007] Ethylene oxide propylene oxide block polyether, also known as ethylene oxide propylene oxide copolyether, can be regulated by relative molecular weight and the ratio of ethylene oxide to propylene oxide. Ethylene oxide propylene oxide block polyether is divided into EPE type block copolyether and PEP type block copolyether. EPE type block copolyether refers to a block copolyether with a hydrophobic polyoxypropylene group in the middle and a hydrophilic polyoxyethylene group at both ends, such as the Pluronic series of Wyandottc Chemical Co., USA, which uses propylene glycol as an initiator, firstly undergoes addition polymerization with propylene oxide, and then undergoes addition polymerization with ethylene oxide to form a high molecular compound, such as the Pluronic P104 model, whose PPO relative molecular weight is 3000 and PEO content is 40% (mass ratio). PEP type block copolyether is made of polyethylene glycol (PEG) and propylene oxide as raw materials. Under the action of an alkali catalyst, PO monomers are continuously connected to both ends of PEG by anionic polymerization to form PEP type polyether. Its structure is with the hydrophilic group inside and the hydrophobic group outside.

[0008] In the technical solution of the present invention, the ethylene oxide propylene oxide block polyether refers to an EPE type block copolyether.

[0009] Preferably, in the ethylene oxide propylene oxide block polyether, the block ratio of ethylene oxide to propylene oxide is 7:3 to 4:6; more preferably 6:4 to 5:5.

[0010] Preferably, the raw materials for preparing the modified polyether water-reducing agent include both ethylene oxide propylene oxide block polyether and β-hydroxyethyl methacrylate phosphate.

[0011] Preferably, the raw materials for preparing the modified polyether water reducer include: ethylene oxide propylene oxide block polyether, unsaturated polyoxyethylene ether, acrylic acid, β-hydroxyethyl methacrylate phosphate and maleic anhydride.

[0012] Further preferably, the mass ratio of the ethylene oxide propylene oxide block polyether, unsaturated polyoxyethylene ether, acrylic acid, β-hydroxyethyl methacrylate phosphate and maleic anhydride is 1:(2-4):(2-5):(0.2-0.5):(0.3-0.5).

[0013] Further preferably, the unsaturated polyoxyethylene ether is selected from at least one of isopentenyl polyoxyethylene ether, isobutylene polyoxyethylene ether, allyl polyoxyethylene ether and ethylene glycol monovinyl polyoxyethylene ether; more preferably isopentenyl polyoxyethylene ether and / or ethylene glycol monovinyl polyoxyethylene ether.

[0014] Preferably, the molecular weights of the ethylene oxide propylene oxide block polyether and the unsaturated polyoxyethylene ether are both 2200 to 4500 g / mol; more preferably 2400 to 3000 g / mol.

[0015] Preferably, the raw materials for preparing the modified polyether water-reducing agent also contain an initiator and a reducing agent.

[0016] More preferably, the initiator is selected from at least one of ammonium persulfate, potassium persulfate, benzoyl peroxide, azobisisobutyronitrile, and hydrogen peroxide; more preferably potassium persulfate.

[0017] Further preferably, the reducing agent is selected from ascorbic acid, sodium bisulfite, and sodium sulfite; more preferably sodium bisulfite.

[0018] The present invention also provides a method for preparing the modified polyether water reducer, comprising the following steps:

[0019] 1) dissolving β-hydroxyethyl methacrylate phosphate, maleic anhydride and unsaturated polyoxyethylene ether in water to obtain a base solution;

[0020] 2) dissolving ethylene oxide propylene oxide block polyether and acrylic acid in water to obtain a dropping liquid A;

[0021] Dissolve the initiator in water to obtain dropwise solution B;

[0022] Dissolve the reducing agent in water to obtain a dropwise addition liquid C;

[0023] 3) The base liquid is heated to a certain temperature, and then the dropping liquid A, the dropping liquid B and the dropping liquid C are simultaneously dropped into the base liquid to carry out a free radical polymerization reaction. After the dropping is completed, the temperature is kept constant for a period of time to obtain the product.

[0024] Preferably, in step 3), the base liquid is heated to 50-80°C.

[0025] Preferably, in step 3), the dropping time is 2 to 4 hours.

[0026] Preferably, in step 3), the temperature is kept warm for 20 to 60 minutes after the addition is completed.

[0027] The present invention also provides application of the modified polyether water reducer in ultra-high performance concrete with a water-binder ratio of 0.14 to 0.2.

[0028] Preferably, the solid content of the modified polyether water-reducing agent does not exceed 1%.

[0029] The beneficial effects of the present invention are at least:

[0030] 1) The modified polyether water-reducing agent provided by the present invention uses ethylene oxide propylene oxide block polyether in the preparation of raw materials. The dispersing effect of traditional polycarboxylic acid water-reducing agents mainly relies on the steric hindrance effect of the side chain. Compared with the hydrophobic methyl groups of ethylene oxide propylene oxide block polyethers, which are far away from water molecules, the steric hindrance effect is stronger; at the same time, ethylene oxide propylene oxide block polyethers are easy to curl up and fold, and the molecular volume is smaller, which is relatively easier to insert into the particle gaps of ultra-high performance concrete with ultra-low water-cement ratio (UHPC system cementitious materials are based on the most compact packing design, and the gaps between ultra-fine powder particles are much smaller than those of ordinary concrete), thereby exerting their steric hindrance effect and reducing the viscosity of concrete;

[0031] 2) The modified polyether water reducer provided by the present invention uses methyl methacrylate-β-hydroxyethyl phosphate with a phosphoric acid structure in the preparation raw material, and the structure can be hydrolyzed under alkaline conditions to release phosphoric acid groups. Compared with adsorption groups such as carboxyl groups, phosphoric acid groups have stronger adsorption capacity on the surface of micro-nano materials such as silica fume. The structure is adsorbed on the surface of silica fume and synergistically acts with ethylene oxide propylene oxide block polyether to achieve full dispersion of particles such as silica fume. At the same time, the structure is slowly released in the slurry, which can achieve continuous maintenance of UHPC workability;

[0032] 3) The modified polyether water reducer provided by the present invention is added to the reaction system by dropwise addition during the preparation process of the ethylene oxide propylene oxide block polyether, and maleic anhydride is introduced to adjust the main chain structure of the water reducer. The prepared water reducer has a wider molecular weight distribution range, wherein molecules with larger molecular weight and molecular size can adsorb larger cement particles, while molecules with smaller molecular weight and molecular size can adsorb micro-nano powders, thereby achieving comprehensive adsorption and dispersion of particles of different sizes;

[0033] 4) The modified polyether water reducer provided by the present invention further improves the concrete working performance and mechanical properties of the water reducer by optimizing the raw material composition, the block ratio of ethylene oxide and propylene oxide, and the selection of the initiator. DETAILED DESCRIPTION

[0034] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention is described clearly and completely below. The following embodiments are used to illustrate the present invention, but are not used to limit the scope of the present invention. If no specific technology or conditions are specified in the embodiments, the technology or conditions described in the literature in the field or the product instructions are used.

[0035] In the following examples, information of each reagent used is shown in Table 1.

[0036] Table 1 Information of reagents used in the examples

[0037]

[0038] Example 1

[0039] Preparation of S1 base solution: Add 0.2 mol of β-hydroxyethyl methacrylate phosphate, 0.5 mol of maleic anhydride, 2 mol of 2400 g / mol isopentyl polyoxyethylene ether, and 4800 g of deionized water into a 20000 mL four-necked flask, stir until completely dissolved, and heat to 60°C.

[0040] Preparation of S2 Dropping Liquid A: Add 1 mol of 3000 g / mol ethylene oxide propylene oxide block (EO / PO) polyether (wherein the EO / PO block ratio is 7:3), 4 mol of acrylic acid, and 3000 g of deionized water into a dropping bottle, and stir at room temperature until completely dissolved to obtain Dropping Liquid A.

[0041] Preparation of S3 Dropping Liquid B: Add 10 g of azobisisobutyronitrile and 300 g of deionized water into a dropping bottle, and stir at room temperature until completely dissolved to obtain Dropping Liquid B.

[0042] Preparation of S4 Dropping Liquid C: Add 5 g of sodium bisulfite and 300 g of deionized water into a dropping bottle, and stir at room temperature until completely dissolved to obtain Dropping Liquid C.

[0043] Preparation of S5 water reducing agent: Add A, B and C materials to the base liquid at the same time for 3 hours. Keep warm for 30 minutes after the addition is completed to obtain the ultra-high performance concrete water reducing agent.

[0044] The weight average molecular weight of the ultra-high performance concrete water reducing agent prepared in Example 1 tested by an external standard method is 55,000 g / mol, and the residual rate of the polyether macromonomer is less than 2%.

[0045] Example 2

[0046] Preparation of S1 base solution: Add 0.2 mol of β-hydroxyethyl methacrylate phosphate, 0.5 mol of maleic anhydride, 2 mol of 2400 g / mol isopentyl polyoxyethylene ether, and 4800 g of deionized water into a 20000 mL four-necked flask, stir until completely dissolved, and heat to 60°C.

[0047] Preparation of S2 Dropping Liquid A: Add 4 mol of acrylic acid and 3000 g of deionized water into a dropping bottle, and stir at room temperature until completely dissolved to obtain Dropping Liquid A.

[0048] Preparation of S3 Dropping Liquid B: Add 10 g of azobisisobutyronitrile and 300 g of deionized water into a dropping bottle, and stir at room temperature until completely dissolved to obtain Dropping Liquid B.

[0049] Preparation of S4 Dropping Liquid C: Add 5 g of sodium bisulfite and 300 g of deionized water into a dropping bottle, and stir at room temperature until completely dissolved to obtain Dropping Liquid C.

[0050] Preparation of S5 water reducing agent: Add materials A, B and C to the base liquid at the same time for 3 hours. After the addition is completed, keep warm for 30 minutes to obtain the ultra-high performance concrete water reducing agent.

[0051] The weight average molecular weight of the ultra-high performance concrete water reducing agent prepared in Example 2 tested by the external standard method is 56,000 g / mol, and the residual rate of the polyether macromonomer is less than 2%.

[0052] Example 3

[0053] Preparation of S1 base solution: add 0.5 mol of maleic anhydride, 2 mol of 2400 g / mol isopentyl polyoxyethylene ether, and 4800 g of deionized water into a 20000 mL four-necked flask, stir until completely dissolved, and heat to 60°C.

[0054] Preparation of S2 Dropping Liquid A: Add 1 mol of 3000 g / mol ethylene oxide propylene oxide block (EO / PO) polyether (wherein the EO / PO block ratio is 6:4), 4 mol of acrylic acid, and 3000 g of deionized water into a dropping bottle, and stir at room temperature until completely dissolved to obtain Dropping Liquid A.

[0055] Preparation of S3 Dropping Liquid B: Add 10 g of azobisisobutyronitrile and 300 g of deionized water into a dropping bottle, and stir at room temperature until completely dissolved to obtain Dropping Liquid B.

[0056] Preparation of S4 Dropping Liquid C: Add 5 g of sodium bisulfite and 300 g of deionized water into a dropping bottle, and stir at room temperature until completely dissolved to obtain Dropping Liquid C.

[0057] Preparation of S5 water reducing agent: Add materials A, B and C to the base liquid at the same time for 3 hours. After the addition is completed, keep warm for 30 minutes to obtain the ultra-high performance concrete water reducing agent.

[0058] The weight average molecular weight of the ultra-high performance concrete water reducing agent prepared in Example 3 tested by the external standard method is 48,000 g / mol, and the residual rate of the polyether macromonomer is less than 2%.

[0059] Example 4

[0060] Preparation of S1 base solution: add 0.2 mol of β-hydroxyethyl methacrylate phosphate, 2 mol of 2400 g / mol isopentyl polyoxyethylene ether, and 4800 g of deionized water into a 20000 mL four-necked flask, stir until completely dissolved, and heat to 60°C.

[0061] Preparation of S2 Dropping Liquid A: Add 1 mol of 3000 g / mol ethylene oxide propylene oxide block (EO / PO) polyether (wherein the EO / PO block ratio is 6:4), 4 mol of acrylic acid, and 3000 g of deionized water into a dropping bottle, and stir at room temperature until completely dissolved to obtain Dropping Liquid A.

[0062] Preparation of S3 Dropping Liquid B: Add 10 g of azobisisobutyronitrile and 300 g of deionized water into a dropping bottle, and stir at room temperature until completely dissolved to obtain Dropping Liquid B.

[0063] Preparation of S4 Dropping Liquid C: Add 5 g of sodium bisulfite and 300 g of deionized water into a dropping bottle, and stir at room temperature until completely dissolved to obtain Dropping Liquid C.

[0064] Preparation of S5 water reducing agent: Add materials A, B and C to the base liquid at the same time for 3 hours. After the addition is completed, keep warm for 30 minutes to obtain the ultra-high performance concrete water reducing agent.

[0065] The weight average molecular weight of the ultra-high performance concrete water reducing agent prepared in Example 4 tested by the external standard method is 57000 g / mol, and the residual rate of the polyether macromonomer is less than 2%.

[0066] Example 5

[0067] Preparation of S1 base solution: Add 0.2 mol of β-hydroxyethyl methacrylate phosphate, 0.5 mol of maleic anhydride, 2 mol of 2400 g / mol isopentyl polyoxyethylene ether, and 4800 g of deionized water into a 20000 mL four-necked flask, stir until completely dissolved, and heat to 60°C.

[0068] Preparation of S2 Dropping Liquid A: Add 1 mol of 3000 g / mol ethylene oxide propylene oxide block (EO / PO) polyether (wherein the EO / PO block ratio is 5:5), 4 mol of acrylic acid, and 3000 g of deionized water into a dropping bottle, and stir at room temperature until completely dissolved to obtain Dropping Liquid A.

[0069] Preparation of S3 Dropping Liquid B: Add 10 g of azobisisobutyronitrile and 300 g of deionized water into a dropping bottle, and stir at room temperature until completely dissolved to obtain Dropping Liquid B.

[0070] Preparation of S4 Dropping Liquid C: Add 5 g of sodium bisulfite and 300 g of deionized water into a dropping bottle, and stir at room temperature until completely dissolved to obtain Dropping Liquid C.

[0071] Preparation of S5 water reducing agent: Add materials A, B and C to the base liquid at the same time for 3 hours. After the addition is completed, keep warm for 30 minutes to obtain the ultra-high performance concrete water reducing agent.

[0072] The weight average molecular weight of the ultra-high performance concrete water reducing agent prepared in Example 5 tested by the external standard method is 55,000 g / mol, and the residual rate of the polyether macromonomer is less than 2%.

[0073] Example 6

[0074] Preparation of S1 base solution: Add 0.2 mol of β-hydroxyethyl methacrylate phosphate, 0.5 mol of maleic anhydride, 2 mol of 2400 g / mol isopentyl polyoxyethylene ether, and 4800 g of deionized water into a 20000 mL four-necked flask, stir until completely dissolved, and heat to 60°C.

[0075] Preparation of S2 Dropping Liquid A: Add 1 mol of 3000 g / mol ethylene oxide propylene oxide block (EO / PO) polyether (wherein the EO / PO block ratio is 5:5), 4 mol of acrylic acid, and 3000 g of deionized water into a dropping bottle, and stir at room temperature until completely dissolved to obtain Dropping Liquid A.

[0076] Preparation of S3 Dropping Liquid B: Add 8 g of potassium persulfate and 300 g of deionized water into a dropping bottle, and stir at room temperature until completely dissolved to obtain Dropping Liquid B.

[0077] Preparation of S4 Dropping Liquid C: Add 5 g of sodium bisulfite and 300 g of deionized water into a dropping bottle, and stir at room temperature until completely dissolved to obtain Dropping Liquid C.

[0078] Preparation of S5 water reducing agent: Add materials A, B and C to the base liquid at the same time for 3 hours. After the addition is completed, keep warm for 30 minutes to obtain the ultra-high performance concrete water reducing agent.

[0079] The weight average molecular weight of the ultra-high performance concrete water reducing agent prepared in Example 6 tested by the external standard method is 45,000 g / mol, and the residual rate of the polyether macromonomer is less than 2%.

[0080] Test example

[0081] The ultra-high performance concrete water reducing agent obtained in Examples 1-6 of the present invention was tested for concrete working performance and mechanical properties. Refer to Q510101ZJJC 001-2021 "Ultra-high Performance Concrete Admixtures", "Standard for Mechanical Properties of Ordinary Concrete" GB / T50081-2002 and "Concrete Admixtures" GB8076-2012. The test results are shown in Table 2.

[0082] The concrete formula ratio is: 16kg of base cement, 4kg of silica fume, 20kg of machine-made sand (modulus coefficient 2.4), and 0.180 of water-cement ratio.

[0083] Table 2. Comparative data of admixture performance

[0084]

[0085] It can be seen from Table 2 that the overall water reduction rate of the ultra-high performance concrete water reducer prepared by the method of the present invention reaches more than 35%, among which Examples 1, 5, and 6 have better overall performance. In Example 2, no ethylene oxide propylene oxide block polyether is added to the synthetic raw materials, and its adsorption and dispersion of silica fume is relatively weak, so the overall expansion is relatively low, and the drum reversing time is significantly increased, indicating that the viscosity is increased; in Example 3, no methacrylate-β-hydroxyethyl phosphate is added to the synthetic raw materials, and the loss over time is relatively large; in Example 4, no maleic anhydride is added, and the adsorption and dispersion of concrete adhesive is relatively weak, and the overall fluidity is slightly lower than that of Examples 1, 5, and 6.

[0086] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A modified polyether water reducer, characterized in that: Ethylene oxide and propylene oxide block polyether are used as the preparation raw materials.

2. The modified polyether water reducer according to claim 1, characterized in that In the ethylene oxide propylene oxide block polyether, the block ratio of ethylene oxide to propylene oxide is 7:3 to 4:6, preferably 6:4 to 5:

5.

3. The modified polyether water reducer according to claim 1 or 2, characterized in that: The modified polyether water-reducing agent is prepared by using ethylene oxide propylene oxide block polyether and methacrylate-β-hydroxyethyl phosphate as raw materials.

4. The modified polyether water reducer according to claim 1 or 2, characterized in that: The raw materials for preparing the modified polyether water reducer include: ethylene oxide propylene oxide block polyether, unsaturated polyoxyethylene ether, acrylic acid, methacrylate-β-hydroxyethyl phosphate and maleic anhydride.

5. The modified polyether water reducer according to claim 4, characterized in that: The mass ratio of the ethylene oxide propylene oxide block polyether, unsaturated polyoxyethylene ether, acrylic acid, methacrylate-β-hydroxyethyl phosphate and maleic anhydride is 1:(2-4):(2-5):(0.2-0.5):(0.3-0.5).

6. The modified polyether water reducer according to claim 4, characterized in that: The unsaturated polyoxyethylene ether is selected from at least one of isopentenyl polyoxyethylene ether, isobutylene polyoxyethylene ether, allyl polyoxyethylene ether and ethylene glycol monovinyl polyoxyethylene ether; preferably isopentenyl polyoxyethylene ether and / or ethylene glycol monovinyl polyoxyethylene ether.

7. The modified polyether water reducer according to claim 4, characterized in that: The molecular weights of the ethylene oxide propylene oxide block polyether and the unsaturated polyoxyethylene ether are both 2200 to 4500 g / mol, preferably 2400 to 3000 g / mol.

8. The modified polyether water reducer according to claim 1 or 2, characterized in that: The raw materials for preparing the modified polyether water-reducing agent also contain an initiator and a reducing agent; Preferably, the initiator is selected from at least one of ammonium persulfate, potassium persulfate, benzoyl peroxide, azobisisobutyronitrile, and hydrogen peroxide; more preferably potassium persulfate; And / or, the reducing agent is selected from ascorbic acid, sodium bisulfite, and sodium sulfite; more preferably sodium bisulfite.

9. The method for preparing the modified polyether water reducer according to any one of claims 1 to 8, characterized in that: The following steps are involved: 1) dissolving β-hydroxyethyl methacrylate phosphate, maleic anhydride and unsaturated polyoxyethylene ether in water to obtain a base solution; 2) dissolving ethylene oxide propylene oxide block polyether and acrylic acid in water to obtain a dropping liquid A; Dissolve the initiator in water to obtain dropwise solution B; Dissolve the reducing agent in water to obtain a dropwise addition liquid C; 3) heating the base liquid to a certain temperature, then simultaneously dropping the drop liquid A, the drop liquid B and the drop liquid C into the base liquid to carry out a free radical polymerization reaction, and keeping the temperature for a period of time after the drop addition is completed, to obtain; Preferably, in step 3), the base liquid is heated to 50-80° C.; And / or, in step 3), the dropping time is 2 to 4 hours; And / or, in step 3), the temperature is kept warm for 20 to 60 minutes after the addition is completed.

10. Use of the modified polyether water-reducing agent according to any one of claims 1 to 8 in ultra-high performance concrete with a water-binder ratio of 0.14 to 0.2; Preferably, the solid content of the modified polyether water-reducing agent does not exceed 1%.