Impact-resistant material and impact-resistant thermal management material
By combining collagen fibers with non-Newtonian gels and designing impact-resistant thermal management materials for sandwich structures, the shortcomings of existing impact-resistant materials in thermal damage protection are solved, and the dual protection performance under impact and high temperature and high heat conditions are achieved. Significantly improves impact resistance and thermal insulation management effect.
Patent Information
- Application Number
- CN202410941790.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-15
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-07-15
AI Technical Summary
Existing impact-resistant materials only have a single impact protection function, and cannot effectively protect other forms of damage such as thermal damage, and lack dual protection performance under impact and high temperature and high heat conditions.
Collagen fibers and non-Newtonian gels are used to prepare impact-resistant materials through a kneading process, and a sandwich structure is designed with collagen fiber-based porous aerogel as the shell to form impact-resistant thermal management materials to achieve dual resistance to mechanical impact and thermal damage. Protect.
The material exhibits excellent impact resistance under impact loads, which can effectively reduce the impact peak force and extend the buffering time. It also has low thermal conductivity, low thermal diffusion coefficient and low infrared emissivity, realizes thermal insulation management and provides more comprehensive protection performance.
Smart Images

Figure CN118956155A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the fields of impact-resistant materials and thermal management, and in particular to an impact-resistant material and an impact-resistant thermal management material. Background Art
[0002] Impact-resistant materials have broad application prospects in personal protection, transportation, aerospace and other fields. (Ishchenko AN, Tabachenko AN, Akinshin RN, et al. Development and investigation of a two-layer metal-ceramic material for protective barriers in conditions of high-speed impact [J]. Technical Physics, 2018, 63(7):988-994. Sisan MM, Eslami-Farsani R. An experimental study on impact resistance of different layup configuration of fiber metal laminates[J]. Fibers and Polymers, 2019, 20(10): 2200-2206. Yuan Z, Yang G, Yang Z, et al. Effect of metal-fiber shear interaction on curing deformation of fiber metal laminates[J]. Arabian Journal for Science and Engineering,2020, 45(7): 5375-5384.).In recent years, researchers have developed a variety of new impact-resistant materials, such as impact-resistant protective materials based on high-performance fibers such as carbon fiber, aramid fiber (Kevlar), and ultra-high molecular weight polyethylene fiber (UHMWPE). The research focus is to improve the impact protection performance of impact-resistant protective materials (Cheeseman BA, Bogetti TA, Ballistic impact intofabric and compliant composite laminates [J]. Composite Structures, 2003, 61:161-173. Park JH, Rutledge GC, Ultrafine high performance polyethylene fibers [J]. Journal of Materials Science, 2018, 53: 3049-3063. Priyanka P, Dixit A, Mali HS, High strength Kevlar fiber reinforced advanced textile composites [J]. Iranian Polymer Journal, 2019, 28: 621-638.). However, flexible impact-resistant materials with only a single impact protection function cannot simultaneously meet the needs of protecting against other forms of damage risks such as thermal damage. Therefore, it is urgent to develop new impact-resistant materials with thermal management functions.
[0003] In view of this, the present invention is proposed. Summary of the invention
[0004] In order to solve the problems in the background technology, the present invention aims to provide an impact-resistant material and an impact-resistant thermal management material.
[0005] A first aspect of the present invention provides an impact-resistant material, which is a collagen fiber reinforced non-Newtonian gel prepared by a mixing process of collagen fibers and non-Newtonian gel.
[0006] Preferably, the mass ratio of the collagen fibers to the non-Newtonian gel is 1:(8-40).
[0007] Preferably, the non-Newtonian gel is made from hydroxy silicone oil, hydrophobic fumed silica and boric acid.
[0008] Preferably, the mixing process uses benzoyl peroxide as a vulcanizing agent.
[0009] The second aspect of the present invention provides an impact-resistant thermal management material, which is a sandwich structure material made of the impact-resistant material as a core material and the collagen fiber-based porous aerogel as a shell layer.
[0010] Preferably, the collagen fiber-based porous aerogel is a porous aerogel constructed by nano-silica-modified collagen fibers.
[0011] Preferably, the collagen fiber-based porous aerogel is prepared by reacting nano-silica-modified collagen fibers with a sodium alginate solution and then freeze-drying the resultant.
[0012] Preferably, the nano-silica modified collagen fibers are prepared by in-situ hydrolysis of tetraethyl orthosilicate on the surface of collagen fibers.
[0013] Compared with the prior art, the present invention has the following beneficial effects: 1. The impact-resistant material provided by the present invention has excellent impact-resistant protection function, which can reduce the peak impact force by 75.3% and extend the buffering time during impact by 59.9%; 2. Traditional impact-resistant materials only have a single impact-resistant protection function, while the impact-resistant thermal management material provided by the present invention can achieve dual protection against mechanical impact and thermal damage, providing protection for personnel protection under impact loads and high temperature and high heat conditions; 3. The impact-resistant thermal management material provided by the present invention exhibits excellent impact resistance, which can reduce the peak impact force by 70.0% and extend the buffering time during impact by 41.1%. In the mechanical impact test under the same conditions, compared with rigid and soft materials such as steel plates, melamine foams and collagen fiber-based porous aerogels, the impact-resistant thermal management material exhibits more excellent impact protection performance; 4. The shock-resistant thermal management material provided by the present invention has a low thermal conductivity (0.12 W m -1 k -1 )、low thermal diffusivity(0.09 mm 2 s -1 ) and low infrared emissivity (0.78), which can effectively suppress heat exchange methods such as thermal convection / thermal radiation and achieve adiabatic management. BRIEF DESCRIPTION OF THE DRAWINGS
[0014] Figure 1 The storage modulus-shear frequency curves of the impact-resistant material-1 in Example 1, the impact-resistant material-2 in Example 2, the impact-resistant material-3 in Example 3, the impact-resistant material-4 in Example 4, the impact-resistant material-5 in Example 5 and the control sample in Comparative Example 1; Figure 2The peak forces and cushioning times of the impact-resistant material-1 in Example 1, the impact-resistant material-2 in Example 2, the impact-resistant material-3 in Example 3, the impact-resistant material-4 in Example 4 and the impact-resistant material-5 in Example 5 when the drop heights are 25 mm, 50 mm, 75 mm, 100 mm, 125 mm and 150 mm respectively, and the back stereomicroscope pictures after being impacted at the drop height of 150 mm; Figure 3 The peak forces and buffering times of the impact-resistant thermal management material in Example 6 and the blank control in Comparative Example 1 when the drop hammer heights are 50 mm, 75 mm, 100 mm, 125 mm and 150 mm, respectively, and the back stereomicroscope images of the impact-resistant thermal management material in Example 6 after being impacted at drop hammer heights of 50 mm, 75 mm, 100 mm, 125 mm and 150 mm; Figure 4 The peak force and cushioning time of the impact-resistant material-4 in Example 4, the control sample and the blank control in Comparative Example 1 when the drop hammer height is 50 mm, 75 mm, 100 mm, 125 mm and 150 mm respectively; Figure 5 The impact resistance of steel plate, melamine foam, collagen fiber-based porous aerogel in Example 6 and impact-resistant thermal management material are compared; Figure 6 It is the surface temperature difference (ΔT) corresponding to the impact-resistant material-4 in Example 4 and the impact-resistant thermal management material in Example 6 when heated by a heating lamp (250 W) for 30 min. DETAILED DESCRIPTION
[0015] In order to make the purpose, technical scheme and advantages of the present invention clearer, the present invention is further described in detail below in conjunction with specific embodiments and with reference to the accompanying drawings. It should be understood that these descriptions are exemplary only and are not intended to limit the scope of the present invention. In addition, in the following description, the description of known structures and technologies is omitted to avoid unnecessary confusion of the concept of the present invention. In the embodiment, those who do not indicate specific conditions are carried out according to the conditions recommended by normal conditions or manufacturers. Those who do not indicate manufacturers for reagents or instruments used are conventional products that can be obtained by commercial purchase.
[0016] Example 1 (1) Preparation of impact-resistant material-1: 7.5 g of hydrophobic fumed silica was dispersed in 150 mL of hydroxy silicone oil, and then 11.5 g of boric acid was added to the mixture. oAfter reacting for 3.0 h at 40 °C, the mixture was cooled to room temperature to obtain elastic non-Newtonian gel (ENG). 40 g of ENG was placed in a torque rheometer at a speed of 120 rpm and a temperature of 80 °C. o C for 2.0 min, then 1.6 g of benzoyl peroxide was added for vulcanization, 1.0 g of collagen fiber was added for mixing after 2.0 min, and the mixture was taken out and allowed to stand for 24 h at 50 o C and 5.0 MPa for 10 min to obtain impact-resistant material-1.
[0017] (2) A rotational rheometer (TA-AR2000ex, USA) was used to perform a frequency sweep test on the impact-resistant material 1 prepared in this example. Figure 1 As shown, in the frequency range of 0.1-100 Hz, the storage modulus of impact-resistant material-1 shows a significant upward trend, increasing from 193 Pa to 0.066 MPa, exhibiting shear hardening characteristics.
[0018] (3) The impact resistance performance of the impact-resistant material 1 prepared in this example was tested: the impact-resistant material 1 was placed on the impact table of the drop hammer impact tester CLC-AI (Beijing Guance Precision Instrument Equipment Co., Ltd.) and fixed, and a hammer head (Φ20 mm, 2.36 kg) was used to drop the hammer at heights of 25 mm, 50 mm, 75 mm, 100 mm, 125 mm and 150 mm to perform a drop hammer impact test. Figure 2 a. Figure 2 As shown in b, the peak forces are 85 N, 110 N, 161 N, 270 N, 363 N and 485 N, and the buffer times are 3.897 ms, 3.653 ms, 3.438 ms, 3.067 ms, 2.933 ms and 2.564 ms, respectively.
[0019] (4) The back side of the impact-resistant material-1 in Example (3) after being impacted at a drop hammer height of 150 mm was photographed using a stereo microscope ( Figure 2 c).
[0020] Example 2 (1) Preparation of impact-resistant material-2: 7.5 g of hydrophobic fumed silica was dispersed in 150 mL of hydroxy silicone oil, and then 11.5 g of boric acid was added to the mixture. o After reacting for 3.0 h at 40 °C, the mixture was cooled to room temperature to obtain elastic non-Newtonian gel (ENG). 40 g of ENG was placed in a torque rheometer at a speed of 120 rpm and a temperature of 80 °C. oC for 2.0 min, then 1.6 g of benzoyl peroxide was added for vulcanization, 2.0 g of collagen fibers were added for mixing after 2.0 min, and the mixture was taken out and allowed to stand for 24 h at 50 o C and 5.0 MPa for 10 min to obtain impact-resistant material-2.
[0021] (2) A rotational rheometer (TA-AR2000ex, USA) was used to perform a frequency sweep test on the impact-resistant material 2 prepared in this embodiment. Figure 1 As shown, in the frequency range of 0.1-100 Hz, the storage modulus of impact-resistant material-2 shows a significant upward trend, from 1093 Pa to 0.13 MPa, exhibiting shear hardening characteristics.
[0022] (3) The impact resistance of the impact-resistant material 2 prepared in this example was tested: the impact-resistant material 2 was placed on the impact table of the drop hammer impact tester CLC-AI (Beijing Guance Precision Instrument Equipment Co., Ltd.) and fixed, and a hammer head (Φ20 mm, 2.36 kg) was used to drop the hammer at heights of 25 mm, 50 mm, 75 mm, 100 mm, 125 mm and 150 mm to perform a drop hammer impact test. Figure 2 a. Figure 2 As shown in b, the peak forces are 94 N, 121 N, 157 N, 232 N, 310 N and 407 N, and the buffer times are 3.551 ms, 3.483 ms, 3.321 ms, 3.150 ms, 3.005 ms and 2.678 ms, respectively.
[0023] (4) The back side of the impact-resistant material-2 in Example (3) after being impacted at a drop hammer height of 150 mm was photographed using a stereo microscope ( Figure 2 c).
[0024] Example 3 (1) Preparation of impact-resistant material-3: 7.5 g of hydrophobic fumed silica was dispersed in 150 mL of hydroxy silicone oil, and then 11.5 g of boric acid was added to the mixture. o After reacting for 3.0 h at 40 °C, the mixture was cooled to room temperature to obtain elastic non-Newtonian gel (ENG). 40 g of ENG was placed in a torque rheometer at a speed of 120 rpm and a temperature of 80 °C. o C for 2.0 min, then 1.6 g of benzoyl peroxide was added for vulcanization, 3.0 g of collagen fibers were added for kneading after 2.0 min, and the mixture was taken out and allowed to stand for 24 h at 50o C and 5.0 MPa for 10 min to obtain impact-resistant material-3.
[0025] (2) A rotational rheometer (TA-AR2000ex, USA) was used to perform a frequency sweep test on the impact-resistant material 3 prepared in this embodiment. Figure 1 As shown, in the frequency range of 0.1-100 Hz, the storage modulus of impact-resistant material-3 shows a significant upward trend, increasing from 1260 Pa to 0.16 MPa, exhibiting shear hardening characteristics.
[0026] (3) The impact resistance performance of the impact-resistant material 3 prepared in this example was tested: the impact-resistant material 3 was placed on the impact table of the drop hammer impact tester CLC-AI (Beijing Guance Precision Instrument Equipment Co., Ltd.) and fixed, and a hammer head (Φ20 mm, 2.36 kg) was used to drop the hammer at heights of 25 mm, 50 mm, 75 mm, 100 mm, 125 mm and 150 mm to perform a drop hammer impact test. Figure 2 a. Figure 2 As shown in b, the peak forces are 96 N, 119 N, 156 N, 217 N, 271 N and 354 N, and the buffer times are 3.383 ms, 3.397 ms, 3.367 ms, 3.295 ms, 3.171 ms and 2.749 ms, respectively.
[0027] (4) The back side of the impact-resistant material-3 in Example (3) after being impacted at a drop hammer height of 150 mm was photographed using a stereo microscope ( Figure 2 c).
[0028] Example 4 (1) Preparation of impact-resistant material-4: 7.5 g of hydrophobic fumed silica was dispersed in 150 mL of hydroxy silicone oil, and then 11.5 g of boric acid was added to the mixture. o After reacting for 3.0 h at 40 °C, the mixture was cooled to room temperature to obtain elastic non-Newtonian gel (ENG). 40 g of ENG was placed in a torque rheometer at a speed of 120 rpm and a temperature of 80 °C. o C for 2.0 min, then 1.6 g of benzoyl peroxide was added for vulcanization, 4.0 g of collagen fibers were added for mixing after 2.0 min, and the mixture was taken out and allowed to stand for 24 h at 50 o C and 5.0 MPa for 10 min to obtain impact-resistant material-4.
[0029] (2) A rotational rheometer (TA-AR2000ex, USA) was used to perform a frequency sweep test on the impact-resistant material 4 prepared in this embodiment. Figure 1 As shown, in the frequency range of 0.1-100 Hz, the storage modulus of impact-resistant material-4 shows a significant upward trend, increasing from 3814 Pa to 0.29 MPa, exhibiting shear hardening characteristics.
[0030] (3) The impact resistance of the impact-resistant material 4 prepared in this example was tested: the impact-resistant material 4 was placed on the impact table of the drop hammer impact tester CLC-AI (Beijing Guance Precision Instrument Equipment Co., Ltd.) and fixed, and a hammer head (Φ20 mm, 2.36 kg) was used to drop the hammer at heights of 25 mm, 50 mm, 75 mm, 100 mm, 125 mm and 150 mm to perform a drop hammer impact test. Figure 2 a. Figure 2 As shown in b, the peak forces are 98 N, 119 N, 160 N, 210 N, 252 N and 297 N, and the buffer times are 3.533 ms, 3.442 ms, 3.320 ms, 3.339 ms, 3.119 ms and 3.071 ms, respectively.
[0031] (4) The back side of the impact-resistant material-4 in Example (3) after being impacted at a drop hammer height of 150 mm was photographed using a stereo microscope ( Figure 2 c).
[0032] (5) The thermal properties of the impact-resistant material 4 prepared in this example were tested. The thermal conductivity of the impact-resistant material 4 was 0.16 W m -1 k -1 , thermal diffusion coefficient is 0.10 mm 2 s -1 .
[0033] (6) The infrared emissivity of the impact-resistant material 4 prepared in this embodiment was tested. The infrared emissivity of the impact-resistant material 4 was 0.92.
[0034] (7) Heat the impact-resistant material-4 prepared in this example with a heating lamp (250 W) for 30 min. Figure 6 As shown in Figure 2, after 30 minutes, the surface temperature of impact-resistant material-4 increased by 16.3 o C. Further linear fitting of the temperature change curve of impact-resistant material-4 within 30 minutes shows that the slope of the fitting straight line of impact-resistant material-4 is 2.52.
[0035] Example 5 (1) Preparation of impact-resistant material-5: 7.5 g of hydrophobic fumed silica was dispersed in 150 mL of hydroxy silicone oil, and then 11.5 g of boric acid was added to the mixture. o After reacting for 3.0 h at 40 °C, the mixture was cooled to room temperature to obtain elastic non-Newtonian gel (ENG). 40 g of ENG was placed in a torque rheometer at a speed of 120 rpm and a temperature of 80 °C. o C for 2.0 min, then 1.6 g of benzoyl peroxide was added for vulcanization, 5.0 g of collagen fibers were added for kneading after 2.0 min, and the mixture was taken out and allowed to stand for 24 h at 50 o C and 5.0 MPa for 10 min to obtain impact-resistant material-5.
[0036] (2) A rotational rheometer (TA-AR2000ex, USA) was used to perform a frequency sweep test on the impact-resistant material 5 prepared in this embodiment. Figure 1 As shown, in the frequency range of 0.1-100 Hz, the storage modulus of impact-resistant material-5 shows a significant upward trend, increasing from 8439 Pa to 0.32 MPa, exhibiting shear hardening characteristics.
[0037] (3) The impact resistance performance of the impact-resistant material 5 prepared in this example was tested: the impact-resistant material 5 was placed on the impact table of the drop hammer impact tester CLC-AI (Beijing Guance Precision Instrument Equipment Co., Ltd.) and fixed, and a hammer head (Φ20 mm, 2.36 kg) was used to drop the hammer at heights of 25 mm, 50 mm, 75 mm, 100 mm, 125 mm and 150 mm to perform a drop hammer impact test. Figure 2 a. Figure 2 As shown in b, the peak forces are 105 N, 138 N, 154 N, 200 N, 250 N and 297 N, and the buffer times are 3.415 ms, 3.265 ms, 3.489 ms, 3.397 ms, 3.221 ms and 3.104 ms, respectively.
[0038] (4) The back side of the impact-resistant material-5 in Example (3) after being impacted at a drop hammer height of 150 mm was photographed using a stereo microscope ( Figure 2 c).
[0039] Example 6 (1) Preparation of shock-resistant thermal management material: 1.5 g collagen fiber was added to 30 mL ethanol-water (1:1 v / v) mixed solution, and then 3.9 g tetraethyl orthosilicate was added. oC, stirred for 4.0 h, then ammonia was added dropwise to adjust the pH to 9.0, and then o C and continue to react for 4.0 h. After the reaction is completed, the nano-silica modified collagen fibers can be obtained after drying. 0.3 g of sodium alginate was added to 30 mL of deionized water and stirred at 30 ° C for 0.5 h. Subsequently, 1.5 g of nano-silica modified collagen fibers were added to the above sodium alginate aqueous solution and stirred for 2.0 h. The above mixture was freeze-dried to obtain a collagen fiber-based porous aerogel. The impact-resistant material-4 prepared in Example 4 was used as the core material and the collagen fiber-based porous aerogel was used as the shell layer. o C and 5.0 MPa for 10 min to obtain the shock-resistant thermal management material.
[0040] (2) The collagen fiber-based porous aerogel prepared in this example was placed on top of glass to conduct an impact protection experiment. Figure 5 As shown in the figure, the peak force after impact is 118.28 N, the buffer time is 2.32 ms, and the glass is broken after impact.
[0041] (3) The infrared emissivity of the collagen fiber-based porous aerogel prepared in this example was tested. The infrared emissivity of the collagen fiber-based porous aerogel was 0.84.
[0042] (4) The impact resistance performance of the impact-resistant thermal management material prepared in this embodiment was tested: the impact-resistant thermal management material was placed on the impact table of the drop hammer impact tester CLC-AI (Beijing Guance Precision Instrument Equipment Co., Ltd.) and fixed, and a hammer head (Φ20 mm, 2.36 kg) was used to drop the hammer at heights of 50 mm, 75 mm, 100 mm, 125 mm and 150 mm to perform a drop hammer impact test. Figure 3 a. Figure 3 As shown in b, the peak forces are 156 N, 223 N, 236 N, 269 N and 361 N, and the buffer times are 2.779 ms, 2.730 ms, 2.633 ms, 2.652 ms and 2.707 ms, respectively.
[0043] (5) Take a stereo microscope photo of the back side of the impact-resistant thermal management material in Example (2) after it is impacted ( Figure 3 c).
[0044] (6) The impact-resistant thermal management material prepared in this example is placed on top of the glass to conduct an impact-resistant protection experiment. Figure 5 As shown in the figure, the peak force after impact is 63.78 N, the buffer time is 3.99 ms, and the glass is intact after impact.
[0045] (7) The thermal performance test of the shock-resistant thermal management material prepared in this embodiment was carried out. The thermal conductivity of the shock-resistant thermal management material was 0.12 W m -1 k -1 , the thermal diffusion coefficient is 0.09 mm 2 s -1 .
[0046] (8) The infrared emissivity test of the impact-resistant thermal management material prepared in this embodiment was performed, and the infrared emissivity of the impact-resistant thermal management material was 0.78.
[0047] (9) The impact-resistant thermal management material prepared in this example was heated with a heating lamp (250 W) for 30 min. Figure 6 As shown in Figure 2, after 30 minutes, the surface temperature of the impact-resistant thermal management material increased by 12.3 o C. Further linear fitting of the temperature change curve of the shock-resistant thermal management material within 30 min shows that the slope of the fitting straight line of the shock-resistant thermal management material is 1.45.
[0048] Comparative Example 1 (1) Preparation of control sample: 7.5 g of hydrophobic fumed silica was dispersed in 150 mL of hydroxy silicone oil, and then 11.5 g of boric acid was added to the above mixture. o After reacting for 3.0 h at 40 °C, the mixture was cooled to room temperature to obtain elastic non-Newtonian gel (ENG). 40 g of ENG was placed in a torque rheometer at a speed of 120 rpm and a temperature of 80 °C. o C for 2.0 min, then 1.6 g of benzoyl peroxide was added for vulcanization. After 4.0 min, the mixture was taken out and allowed to stand for 24 h. o The mixture was hot-pressed at 400 °C and 5.0 MPa for 10 min to obtain a control sample.
[0049] (2) A rotational rheometer (TA-AR2000ex, USA) was used to perform a frequency sweep test on the control sample prepared in this example. Figure 1 As shown, in the frequency range of 0.1-100 Hz, the storage modulus of the control sample showed a significant upward trend, increasing from 22.62 Pa to 0.034 MPa, showing shear hardening characteristics.
[0050] (3) The control sample prepared in this example was tested for impact resistance: the control sample was placed on the impact table of a drop hammer impact tester CLC-AI (Beijing Guance Precision Instrument Equipment Co., Ltd.) and fixed, and a hammer head (Φ20 mm, 2.36 kg) was used to drop the sample at heights of 50 mm, 75 mm, 100 mm, 125 mm, and 150 mm to perform a drop hammer impact test. Figure 4 a. Figure 4 As shown in Figure 2(b), the peak forces are 154 N, 265 N, 406 N, 527 N and 629 N, and the buffer times are 3.406 ms, 3.139 ms, 3.037 ms, 2.813 ms and 2.721 ms, respectively. When no test sample is placed on the impact table, it is set as a blank control. The peak forces are 571 N, 743 N, 875 N, 1076 N and 1203 N, and the buffer times are 1.142 ms, 1.608 ms, 2.057 ms, 1.874 ms and 1.918 ms, respectively.
[0051] Comparative Example 2 The steel plate is placed on top of the glass to conduct the impact protection test. Figure 5 As shown in the figure, the peak force after impact is 258.54 N, the buffering time is 1.06 ms, and the glass is broken after impact. When no buffer material is placed on the glass, the peak force after impact is 256.07 N, the buffering time is 0.69 ms, and the glass is severely broken after impact.
[0052] Comparative Example 3 Commercial melamine foam was placed on top of glass for impact protection experiments. Figure 5 As shown, the peak force after impact is 231.29 N, the buffer time is 1.86 ms, and the glass is broken after impact.
[0053] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the above embodiments, it should be understood by those skilled in the art that the technical solutions described in the above embodiments may still be modified, or some or all of the technical features thereof may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. An impact-resistant material, characterized in that: The material is a collagen fiber reinforced non-Newtonian gel prepared by mixing collagen fiber and non-Newtonian gel through a kneading process.
2. The impact-resistant material according to claim 1, characterized in that: The mass ratio of the collagen fibers to the non-Newtonian gel is 1:(8-40).
3. The impact-resistant material according to claim 1, characterized in that: The non-Newtonian gel is prepared from hydroxy silicone oil, hydrophobic fumed silica and boric acid.
4. The impact-resistant material according to claim 1, characterized in that: The mixing process uses benzoyl peroxide as a vulcanizing agent.
5. A shock-resistant thermal management material, characterized in that: The material is a sandwich structure material made of the impact-resistant material described in claim 1 as a core material and a collagen fiber-based porous aerogel as a shell layer.
6. The impact-resistant thermal management material according to claim 5, characterized in that: The collagen fiber-based porous aerogel is a porous aerogel constructed by nano-silicon dioxide-modified collagen fibers.
7. The impact-resistant thermal management material according to claim 6, characterized in that: The nano-silicon dioxide modified collagen fibers are prepared by in-situ hydrolysis of ethyl orthosilicate on the surface of the collagen fibers.
Citation Information
Patent Citations
Strong and tough structural wood materials, and methods for fabricating and use thereof
CN110914029A
Method for preparing composite aerogel flame-retardant material from waste leather
CN111234298A
Impact-resistant wearable material, wearable sensing material and preparation method
CN114573865A
High-strength and tear-resistant leather materials and methods of manufacture
US11499267B1
Strong and tough structural wood materials, and methods for fabricating and use thereof
WO2018191181A1