High-cycle sodium-ion battery positive electrode material and preparation method thereof, positive electrode plate and sodium-ion battery
By using a sintering process of multi-element polyvalent high-entropy cladding layer and specific metal element ratio on the surface of the positive electrode material of sodium ion battery, the problem of increasing impedance of the cladding material in the prior art is solved, and the cycle performance and stability of the battery are improved , achieving both high capacity and high rate performance.
Patent Information
- Application Number
- CN202411064976.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-05
- Publication Date
- 2024-11-15
Smart Images

Figure CN118970005A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of sodium ion battery positive electrode materials, and in particular to a high-cycle sodium battery positive electrode material and a preparation method thereof, a positive electrode sheet and a sodium ion battery. Background Art
[0002] Compared with lithium-ion batteries, sodium-ion batteries have the following advantages: (1) Sodium materials are abundant and inexpensive; (2) Low-concentration electrolytes can be used to reduce costs; (3) Aluminum foil can be used as the negative electrode current collector, which can further reduce costs; (4) They have a higher theoretical energy density and can store more energy; and (5) They have good safety performance.
[0003] Among them, the positive electrode material of sodium ion batteries has an important influence on the performance of sodium ion batteries. Existing sodium ion positive electrode materials are often coated with materials such as alumina, which increases the material impedance, affects the electrochemical properties of the positive electrode materials, and reduces the cycle performance of sodium ion batteries.
[0004] In view of this, the present invention is proposed. Summary of the invention
[0005] The first purpose of the present invention is to provide a high-cycle sodium battery positive electrode material, in which the coating layer can protect the interface on the surface of the positive electrode material, inhibit the decomposition of the electrolyte, and can consume the residual alkali on the surface, improve the stability of the positive electrode material, and improve the cycle performance of the prepared battery; in addition, the present application uses a multi-element multi-valent surface high-entropy coating to increase the strength of the material, control the particle size distribution, and further improve the cycle performance.
[0006] The second purpose of the present invention is to provide a method for preparing a high-cycle sodium battery positive electrode material, which is simple to operate, easy to implement, has a short process, and is suitable for mass production.
[0007] The third object of the present invention is to provide a positive electrode sheet having excellent cycle performance, high capacity, good rate performance and the like.
[0008] A fourth object of the present invention is to provide a sodium ion battery having good cycle performance and taking into account both high capacity and high rate performance.
[0009] In order to achieve the above-mentioned purpose of the present invention, the following technical solutions are particularly adopted:
[0010] The present invention first provides a high-cycle sodium battery positive electrode material, comprising a base material and a coating layer coated on the surface of the base material;
[0011] The general formula of the matrix material is Na x Cu y Niz Fe u Mn v O 2+q ; Among them, 0.96≤x≤1.01, 0.025≤y≤0.055, 0.28≤z≤0.32, 0.29≤u≤0.34, 0.30≤v≤0.38, -0.04<q≤0.04, y+z+u+v=1;
[0012] The general formula of the coating layer is Na a Mg b Al c A d J e O 2+p ; Wherein, A includes metal elements with an average valence of +4, J includes metal elements with an average valence δ of +5 or +6, 0.8≤a≤1.55, 0.3≤b≤0.7, 0.1≤c≤0.3, 0.2≤d≤0.4, 0<e≤0.4, -0.5≤p≤0.25, b+c+d+e=1.
[0013] Further, A includes at least one of Ti, Hf and Zr.
[0014] Furthermore, J having an average valence of +5 includes at least one of Nb, V and Ta.
[0015] Furthermore, J having an average valence of +6 includes at least one of W and Mo.
[0016] Furthermore, the molar amount of the coating layer is 0.002 to 0.01 of the molar amount of the base material.
[0017] Furthermore, the Shore hardness of the matrix material is 25-45 HV, and the particle strength of the matrix material is ≥80 MPa.
[0018] Furthermore, the Shore hardness of the matrix material is A, the particle strength of the matrix material is B, and the particle size (D 90 -D 10 ) / D 50 is C, the percentage of the peak area I003 of the 003 characteristic diffraction peak in the X-ray diffraction spectrum of the high cycle sodium battery positive electrode material to the peak area I104 of the 104 characteristic diffraction peak I003 / I104×100% is D%, the half-peak width FWHM104 of the 104 characteristic diffraction peak in the X-ray diffraction spectrum of the high cycle sodium battery positive electrode material is E, wherein A, B, C, D, and E satisfy the following relationship: 100≤1000×D×E / B+A+23.5C≤100.5; wherein the unit of A is HV, the unit of B is MPa, the unit of C is 1, and the unit of E is °.
[0019] Furthermore, the particle size D of the high cycle sodium positive electrode material is 10 Satisfy 5.1μm≤D 10 ≤5.4μm.
[0020] Furthermore, the particle size D of the high cycle sodium positive electrode material is 50 Satisfy 9.2μm≤D 50 ≤9.8μm.
[0021] Furthermore, the particle size D of the high cycle sodium positive electrode material is 90 Satisfy 15.9μm≤D 90 ≤16.9μm.
[0022] Furthermore, the particle size (D 90 -D 10 ) / D 50 Satisfy 1.13≤(D 90 -D 10 ) / D 50 ≤1.19.
[0023] Furthermore, the high cycle sodium battery positive electrode material is an O3 type layered oxide.
[0024] Furthermore, in the X-ray diffraction pattern of the high-cycle sodium battery positive electrode material, the percentage of the peak area I003 of the 003 characteristic diffraction peak to the peak area I104 of the 104 characteristic diffraction peak I003 / I104×100% satisfies 88%≤I003 / I104×100%≤132%.
[0025] Furthermore, the half-peak width FWHM104 of the 104 characteristic diffraction peak in the X-ray diffraction spectrum of the high-cycle sodium battery positive electrode material satisfies 0.054≤FWHM104≤0.068.
[0026] Furthermore, at 25° C., the pH of a solution of 2 g of the high-cycle sodium-based cathode material dissolved in 40 mL of water is 12.00 to 12.25.
[0027] Furthermore, the specific surface area of the high cycle sodium positive electrode material is 0.26 to 0.3 m 2 / g.
[0028] Furthermore, the capacity retention rate of the 26700 battery cell containing the high-cycle sodium battery positive electrode material after 500 cycles at 45° C. is ≥97.5%.
[0029] The present invention further provides a method for preparing the high-cycle sodium battery positive electrode material, comprising the following steps: (a) mixing a sodium source, a copper source and a nickel-iron-manganese ternary precursor and performing a first sintering to obtain a matrix material; (b) mixing the matrix material with a sodium source, a magnesium source, an aluminum source, an A-containing compound and a J-containing compound and performing a second sintering to obtain the high-cycle sodium battery positive electrode material.
[0030] Furthermore, the first sintering temperature is 900-1100° C., and the holding time is 12-16 hours.
[0031] Furthermore, the second sintering temperature is 800-900° C., and the holding time is 10-20 hours.
[0032] The present invention further provides a positive electrode sheet, comprising the high cycle sodium battery positive electrode material.
[0033] The present invention also provides a sodium ion battery, comprising the positive electrode sheet.
[0034] Compared with the prior art, the present invention has the following beneficial effects:
[0035] (1) The composite layered oxide positive electrode material provided by the present invention has a coating layer that can protect the interface on the surface of the positive electrode material, inhibit the decomposition of the electrolyte, and can consume the residual alkali on the surface, thereby improving the stability of the positive electrode material and the cycle performance of the battery; in addition, the present application uses a multi-element multi-valent surface high-entropy coating to increase the strength of the material, control the particle size distribution, and further improve the cycle performance.
[0036] (2) The composite layered oxide positive electrode material provided by the present invention forms a high ion layer conductive coating composed of inactive metal oxides (inactive metals refer to metal elements with unchanged valence) and residual alkali on the surface of the base material, thereby improving the problems of high alkalinity and thermodynamic instability of the material.
[0037] (3) The composite layered oxide positive electrode material provided by the present invention has specific proportions of various metal elements. Even if the molar ratio of the coating layer is 0.002 to 0.01, the battery made from the positive electrode material prepared by the present invention can still maintain its capacity and rate performance without decreasing. More coating materials can reduce the contact between the base material and the electrolyte, reduce side reactions, and thus increase the cycle life of the battery.
[0038] (4) The composite layered oxide positive electrode material provided by the present invention can control the hardness of the material from both microscopic and macroscopic scales by controlling the microscopic particle hardness and Shore hardness of the positive electrode material, thereby improving the compaction density of the material electrode and the compression resistance of the particles, which is beneficial to improving the energy density and cycle performance of the positive electrode material battery cell. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0040] Figure 1 This is an electron microscope image of the high-cycle sodium battery positive electrode material prepared in Example 1 provided by the present invention. DETAILED DESCRIPTION
[0041] The technical scheme of the present invention will be clearly and completely described below in conjunction with the accompanying drawings and specific embodiments, but it will be understood by those skilled in the art that the following described embodiments are part of embodiments of the present invention, rather than all embodiments, and are only used to illustrate the present invention, and should not be considered as limiting the scope of the present invention. Based on the embodiments in the present invention, all other embodiments obtained by those of ordinary skill in the art without making creative work are within the scope of protection of the present invention. If specific conditions are not specified in the embodiments, they are carried out according to normal conditions or conditions recommended by the manufacturer. If the manufacturer is not specified in the reagents or instruments used, they are all conventional products that can be purchased commercially.
[0042] If there is no special explanation, in the present invention, "the first aspect", "the second aspect", "the third aspect", "the fourth aspect", etc. are only used for descriptive purposes and cannot be understood as indicating or implying relative importance or quantity, nor can they be understood as implicitly indicating the importance or quantity of the indicated technical features. Moreover, "the first", "the second", "the third", "the fourth", etc. only serve the purpose of non-exhaustive enumeration and description, and it should be understood that they do not constitute a closed limitation on quantity.
[0043] If there is no special explanation, the "include" and "comprising" mentioned in the present invention represent open-ended or closed-ended expressions. For example, the "include" and "comprising" may represent that other components not listed may also be included or only the listed components may be included or only the listed components may be included.
[0044] If there is no special explanation, in the present invention, "one or more" or "at least one" refers to any one, any two or more of the listed items. Among them, "several" refers to any two or more of the listed items.
[0045] In a first aspect, the present invention provides a high cycle sodium battery positive electrode material, comprising a base material and a coating layer coated on the surface of the base material.
[0046] The general formula of the matrix material is Na x Cuy Ni z Fe u Mn v O 2+q ; Among them, 0.96≤x≤1.01, 0.025≤y≤0.055, 0.28≤z≤0.32, 0.29≤u≤0.34, 0.30≤v≤0.38, -0.04<q≤0.04, y+z+u+v=1.
[0047] Wherein, x includes but is not limited to any point value of 0.96, 0.97, 0.98, 0.99, 1, 1.01 or any range value between them. y includes but is not limited to any point value of 0.025, 0.03, 0.035, 0.04, 0.045, 0.05, 0.055 or any range value between them. z includes but is not limited to any point value of 0.28, 0.29, 0.3, 0.31, 0.32 or any range value between them. u includes but is not limited to any point value of 0.29, 0.30, 0.31, 0.32, 0.33, 0.34 or any range value between them. v includes but is not limited to any point value of 0.30, 0.31, 0.32, 0.33, 0.34, 0.35, 0.36, 0.37, 0.38 or any range value between them. q includes, but is not limited to, any point value of -0.04, -0.03, -0.02, -0.01, 0, 0.01, 0.02, 0.03, 0.04, or a range of values between any two of them.
[0048] The general formula of the coating layer is Na a Mg b Al c A d J e O 2+p ; Wherein, A includes metal elements with an average valence of +4, J includes metal elements with an average valence δ of +5 or +6, 0.8≤a≤1.55, 0.3≤b≤0.7, 0.1≤c≤0.3, 0.2≤d≤0.4, 0<e≤0.4, -0.5≤p≤0.25, b+c+d+e=1.
[0049] Moreover, 2.5≤(2b+3c+4d+eδ) / (b+c+d+e)≤3.5, a+2b+3c+4d+eδ=4+2q, that is, the above general formula satisfies the charge balance (positive and negative valences are 0).
[0050] Wherein, a includes but is not limited to any one of 0.8, 0.85, 0.9, 0.95, 1, 1.1, 1.2, 1.3, 1.4, 1.5 or any range between them. b includes but is not limited to any one of 0.3, 0.4, 0.5, 0.6, 0.7 or any range between them. c includes but is not limited to any one of 0.1, 0.15, 0.2, 0.25, 0.3 or any range between them. d includes but is not limited to any one of 0.2, 0.25, 0.3, 0.35, 0.4 or any range between them. e includes but is not limited to any one of 0.01, 0.05, 0.1, 0.15, 0.2, 0.25, 0.3, 0.35, 0.4 or any range between them. p includes, but is not limited to, any one of -0.5, -0.4, -0.3, -0.2, -0.1, 0, 0.1, 0.2, 0.25, or a range of values between any two of them.
[0051] The composite layered oxide positive electrode material provided by the present invention has a base material that provides capacity; the coating layer can protect the interface on the surface of the positive electrode material, inhibit the decomposition of the electrolyte, and can consume the residual alkali on the surface, thereby improving the stability of the positive electrode material.
[0052] Specifically, the present invention adopts high entropy coating (coating of more than 3 elements), and it is a combination of elements with different valence states. Coating of elements with different valence states can increase the surface defect concentration of the material, improve the electronic conductivity and surface stability.
[0053] In some specific embodiments, A includes at least one of Ti, Hf and Zr.
[0054] In some specific embodiments, J having an average valence of +5 includes at least one of Nb, V and Ta.
[0055] In some specific embodiments, J having an average valence of +6 includes at least one of W and Mo.
[0056] The present invention forms a high ion layer conductive coating layer composed of inactive metal oxides (inactive metal refers to metal elements with unchanged valence) and residual alkali (residual alkali on the surface of the substrate material) on the surface of the substrate material, so that problems such as high alkalinity and thermodynamic instability of the material are improved. The positive electrode material of the present invention is a multi-element coating layer.
[0057] A and J in the coating material of the present invention are both high-valent elements with high stability, which can significantly improve the ionic conductivity of the material and have a stable structure.
[0058] In some specific embodiments, the molar amount of the coating layer is 0.002 to 0.01 of the molar amount of the base material, including but not limited to any point value of 0.002, 0.005, 0.006, 0.008, 0.01 or any range value between two of them. If the coating is too much, the material capacity will decrease, and if there are too many coatings, the residual alkali content is insufficient to react with it, and the oxide will cause the material impedance at the battery end to increase.
[0059] The positive electrode material provided by the present invention adopts a specific ratio of each metal element. Even if the molar ratio of the coating layer is 0.002-0.01, the battery made of the positive electrode material prepared by the present invention can still maintain the capacity and rate performance without decreasing. The coating material can reduce the contact between the base material and the electrolyte, reduce side reactions, and thus improve the cycle life of the battery.
[0060] In some specific embodiments, the Shore hardness of the matrix material is 25-45HV, including but not limited to any one of 25HV, 30HV, 35HV, 40HV, and 45HV, or a range between any two of them; the particle strength of the matrix material is ≥80Mpa, including but not limited to any one of 80Mpa, 100Mpa, 110Mpa, 130Mpa, 140Mpa, 150Mpa, 160Mpa, 170Mpa, 180Mpa, 190Mpa, and 200Mpa, or a range between any two of them.
[0061] The present invention controls the hardness of the material from both microscopic and macroscopic scales by controlling the microscopic particle hardness and Shore hardness of the positive electrode material, which can improve the compaction density of the material electrode and the compression resistance of the particles, and is beneficial to improving the energy density and cycle performance of the positive electrode material battery cell.
[0062] In some specific implementations, a sagger of 330 mm×330 mm×100 mm is used, the amount of the sagger is 3 kg, and the Shore hardness of the matrix material obtained after sintering is 25-45 HV, and the particle strength is ≥80 MPa.
[0063] In some specific embodiments, the Shore hardness of the matrix material is A, the particle strength of the matrix material is B, and the particle size (D 90 -D 10 ) / D 50 C(that is, C=(D 90 -D 10 ) / D 50), the percentage of the peak area I003 of the 003 characteristic diffraction peak in the X-ray diffraction spectrum of the high cycle sodium battery positive electrode material to the peak area I104 of the 104 characteristic diffraction peak I003 / I104×100% is D% (D%=I003 / I104×100%, that is, D=I003 / I104×100), and the half-peak width FWHM104 of the 104 characteristic diffraction peak in the X-ray diffraction spectrum of the high cycle sodium battery positive electrode material is E, wherein A, B, C, D, and E satisfy the following relationship: 100≤1000×D×E / B+A+23.5C≤100.5.
[0064] Among them, the unit of A is HV, the unit of B is MPa, the unit of C is 1, and the unit of E is °.
[0065] The value of 1000×D×E / B+A+23.5C includes but is not limited to any one of 100, 100.1, 100.2, 100.3, 100.4, 100.5 or a range of values between any two of them.
[0066] By satisfying the above relationship and controlling the material hardness and particle strength to a certain extent, the crystallinity of the material can be increased; and by controlling the half-peak width to a certain extent, the primary particle size of the material can be effectively controlled.
[0067] In some specific embodiments, the particle size D of the high cycle sodium positive electrode material is 10 Satisfy 5.1μm≤D 10 ≤5.4μm; where D 10 Including but not limited to any point value of 5.1 μm, 5.2 μm, 5.3 μm, 5.4 μm, or a range of values between any two of them.
[0068] In some specific embodiments, the particle size D of the high cycle sodium positive electrode material is 50 Satisfy 9.2μm≤D 50 ≤9.8μm; where D 50 Including but not limited to any point value of 9.2 μm, 9.3 μm, 9.4 μm, 9.5 μm, 9.6 μm, 9.7 μm, 9.8 μm or a range of values between any two of them.
[0069] In some specific embodiments, the particle size D of the high cycle sodium positive electrode material is 90 Satisfy 15.9μm≤D 90 ≤16.9μm; among which D 90 Including but not limited to any point value of 15.9 μm, 16 μm, 16.2 μm, 16.3 μm, 16.5 μm, 16.6 μm, 16.7 μm, 16.9 μm, or a range of values between any two of them.
[0070] In some specific embodiments, the particle size (D 90 -D 10 ) / D 50 Satisfy 1.13≤(D 90 -D 10 ) / D 50 ≤1.19; where (D 90 -D 10 ) / D 50 The value of includes but is not limited to any one of 1.13, 1.14, 1.15, 1.16, 1.17, 1.18, 1.19 or a range of values between any two of them.
[0071] The present invention controls the particle size of the high-cycle sodium battery positive electrode material to meet the above range, so that the particle size distribution is dispersed, which is beneficial to improving the cycle performance of the material.
[0072] In some specific embodiments, the high cycle sodium battery positive electrode material is an O3 type layered oxide. Specifically, the base material is an O3 type layered oxide structure, and the coating layer is amorphous.
[0073] In some specific embodiments, in the X-ray diffraction spectrum of the high-cycle sodium positive electrode material, the percentage of the peak area I003 of the 003 characteristic diffraction peak to the peak area I104 of the 104 characteristic diffraction peak I003 / I104×100% satisfies 88%≤I003 / I104×100%≤132%, wherein I003 / I104×100% includes but is not limited to any point value of 88%, 89%, 90%, 95%, 96%, 100%, 102%, 105%, 110%, 120%, 130%, 132% or any range value between two of them. In this way, the exposure of the crystal planes corresponding to the transition metal and Na can be kept within a certain range, and the material can have certain air stability and certain active interface.
[0074] In some specific embodiments, the half-peak width FWHM104 of the 104 characteristic diffraction peak in the X-ray diffraction spectrum of the high-cycle sodium positive electrode material satisfies 0.054≤FWHM104≤0.068; wherein FWHM104 includes but is not limited to any point value of 0.054, 0.058, 0.059, 0.06, 0.061, 0.064, 0.067, 0.068 or a range value between any two thereof. The primary particle size of the positive electrode material obtained by the present invention is suitable.
[0075] In some specific embodiments, at 25°C, the pH of the solution formed after 2g of the high-cycle sodium cathode material is dissolved in 40mL of water is 12.00-12.25; including but not limited to any point value of 12.00, 12.04, 12.05, 12.10, 12.15, 12.20, 12.25 or a range value between any two of them. It can be seen that the high-cycle sodium cathode material provided by the present invention has good air stability.
[0076] In some specific embodiments, the specific surface area of the high cycle sodium positive electrode material is 0.26 to 0.3 m 2 / g; including but not limited to 0.26m 2 / g, 0.27m 2 / g, 0.28m 2 / g, 0.29m 2 / g, 0.3m 2 / g or any point value or range value between any two of them. The high cycle sodium positive electrode material provided by the present invention has a small specific surface area, wherein the smaller the specific surface area, the smaller the contact area between the material and the electrolyte, the fewer side reactions, and the better the cycle performance.
[0077] In some specific embodiments, the capacity retention rate of the 26700 battery cell containing the high cycle sodium battery positive electrode material after 500 cycles at 45°C is ≥97.5%, including but not limited to any one of 97.5%, 97.7%, 97.8%, 98%, 98.3%, 98.5%, 98.6%, 98.8%, 99%, 99.5% or the range between any two of them.
[0078] In some specific embodiments, the chemical formula of the high cycle sodium positive electrode material is Na x Cu y Ni z Fe u Mn v O 2+q / β(Na a Mg b Al c A d J e O 2+p ), where β is the coating amount, i.e., the ratio of the molar amount of the coating layer to the molar amount of the base material, β = 0.002 to 0.01. It can be understood that in this chemical formula, Na x Cu y Ni z Fe u Mn v O 2+q Refers to the base material, Na a Mg b Alc A d J e O 2+p Refers to the coating material of the coating layer.
[0079] In a second aspect, the present invention provides a method for preparing the above-mentioned high cycle sodium battery positive electrode material, comprising the following steps:
[0080] (a) According to the target chemical formula of the matrix material, a sodium source, a copper source and a nickel-iron-manganese ternary precursor are uniformly mixed and then first sintered, and then cooled to obtain the matrix material.
[0081] (b) According to the target chemical formula and coating amount of the coating layer, the base material is mixed evenly with the sodium source, the magnesium source, the aluminum source, the A-containing compound and the J-containing compound, and then a second sintering is performed, and the high-cycle sodium battery positive electrode material is obtained after cooling.
[0082] The method for preparing a high-cycle sodium battery positive electrode material provided by the present invention is simple to operate, easy to implement, has a short process, is suitable for mass production, and the high-cycle sodium battery positive electrode material prepared by the method has good cycle stability.
[0083] In some specific embodiments, the temperature of the first sintering is 900-1100°C, including but not limited to any one of 900°C, 950°C, 1000°C, 1050°C, 1100°C or a range between any two of them; the holding time of the first sintering is 12-16h, including but not limited to any one of 12h, 13h, 14h, 15h, 16h or a range between any two of them.
[0084] In some specific embodiments, the temperature of the second sintering is 800-900°C, including but not limited to any one of 800°C, 820°C, 840°C, 850°C, 880°C, 900°C or a range between any two of them; the holding time of the second sintering is 10-20h, including but not limited to any one of 10h, 12h, 14h, 15h, 18h, 20h or a range between any two of them.
[0085] In some specific embodiments, the first sintering and the second sintering are both performed in an oxygen-containing atmosphere, such as an air atmosphere or an oxygen atmosphere. Preferably, the gas flow rate of the oxygen-containing atmosphere is 10 to 30 L / min.
[0086] In some specific implementations, the sodium source, the copper source and the nickel-iron-manganese ternary precursor are mixed, placed in a sagger of 330 mm×330 mm×100 mm with a filling volume of 3 kg, and then sintered.
[0087] In some specific implementations, after the first sintering, the obtained material is subjected to a Shore hardness test and a particle strength test. The Shore hardness of the base material used for the second sintering needs to meet 25-45HV, and the particle strength needs to meet ≥80Mpa.
[0088] In some specific embodiments, the first sintering further includes the steps of first crushing and first screening, specifically, the first crushing and first screening are performed after the Shore hardness test and the particle strength test, and the mesh number of the sieve used for the first screening is 325-400 mesh; including but not limited to any one of 325 mesh, 350 mesh, 375 mesh, 400 mesh or the range value between any two of them.
[0089] Preferably, the first crushing and the first screening specifically include: through a rotary mill, an air flow mill, and an ultrasonic vibrating screen, and the process parameters are: a rotary mill gap of 200 μm, an air flow mill grinding pressure of 0.4-0.5 MPa, an extension frequency of 90-130 Hz, and an induced draft fan frequency of 30-40 Hz.
[0090] In some specific embodiments, the second sintering further includes a second crushing and a second screening step, and the mesh size of the sieve used for the second screening is 325-400 mesh; including but not limited to any point value of 325 mesh, 350 mesh, 375 mesh, 400 or a range value between any two of them.
[0091] In some specific embodiments, the particle size D of the nickel-iron-manganese ternary precursor is 50 =4~5μm, particle size D min ≥1μm, particle size D 90 ≤10μm, particle size D max ≤15μm, specific surface area 10~20m 2 / g.
[0092] In some specific embodiments, the tap density TD of the nickel-iron-manganese ternary precursor is ≥ 1.3 g / cm 3 .
[0093] In some specific embodiments, the molar ratio of Ni, Fe and Mn elements in the nickel-iron-manganese ternary precursor is the ratio of z, u and v, that is, 0.28-0.32: 0.30-0.34: 0.30-0.38.
[0094] In some specific implementations, the S content in the nickel-iron-manganese ternary precursor is ≤0.2wt%.
[0095] In some specific embodiments, the particle morphology of the nickel-iron-manganese ternary precursor is spherical or ellipsoidal, without obvious fine powder particles.
[0096] In some specific embodiments, the sodium source in step (a) and step (b) includes any Na-containing compound commonly used in the art, such as sodium carbonate, sodium nitrate, sodium acetate, sodium citrate, sodium oxalate, etc., but is not limited thereto.
[0097] In some specific embodiments, the copper source includes a compound containing Cu, such as copper oxide, copper hydroxide, basic copper carbonate, copper chloride, copper nitrate, copper acetate, etc., but is not limited thereto.
[0098] In some specific embodiments, the magnesium source includes a compound containing Mg, such as magnesium oxide, magnesium hydroxide, magnesium carbonate, magnesium acetate, magnesium nitrate, etc., but is not limited thereto.
[0099] In some specific embodiments, the aluminum source includes a compound containing Al, such as aluminum oxide, aluminum hydroxide, aluminum acetate, aluminum nitrate, etc., but is not limited thereto.
[0100] In some specific embodiments, the A-containing compound includes oxides, chlorides, carbonates, etc. containing A, but is not limited thereto. A includes at least one of Ti, Hf and Zr. The J-containing compound includes oxides, chlorides, carbonates, etc. containing J, but is not limited thereto. J includes at least one of Nb, V, Ta, W and Mo.
[0101] As an example; Ti-containing compounds such as TiO 2 、TiCl 4 , tetrabutyl titanate, etc.; Hf-containing compounds such as HfO 2 , HfCl 4 etc.; Zr-containing compounds such as ZrO 2 、ZrCl 4 etc.; Nb-containing compounds such as Nb 2 O 5 、NbO 2 , Nb 2 O 3 , NbS 2 、NbCl 5 etc.; compounds containing V such as VO, V 2 O 3 , VO 2 、V 2 O 5 , Vanadyl Oxalate, VCl 4 etc.; Ta-containing compounds such as Ta 2 O 5 ; W-containing compounds such as H 3 WO 4 , WO 3 , WS 2 etc.; Mo-containing compounds such as MoO 2、Mo 4 O 11 、Mo 17 O 47 、Mo 5 O 14 、Mo 8 O 23 、MoO 3 wait.
[0102] In a third aspect, the present invention provides a positive electrode sheet comprising the above-mentioned high cycle sodium battery positive electrode material.
[0103] The positive electrode sheet provided by the present invention has the advantages of excellent cycle performance, high capacity, good rate performance, etc.
[0104] Optionally, the positive electrode sheet further includes a binder and / or a conductive agent, which is not limited in the present invention.
[0105] In a fourth aspect, the present invention provides a sodium ion battery comprising the above-mentioned positive electrode sheet.
[0106] The sodium ion battery provided by the present invention has good cycle performance and takes into account both high capacity and high rate performance.
[0107] Optionally, the sodium ion battery further includes a negative electrode sheet, a separator and an electrolyte, which is not limited in the present invention.
[0108] The embodiments of the present invention will be described in detail below in conjunction with the examples, but it will be appreciated by those skilled in the art that the following examples are only used to illustrate the present invention and should not be considered as limiting the scope of the present invention. If no specific conditions are specified in the examples, the conditions are carried out according to normal conditions or the conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be obtained commercially.
[0109] Example 1
[0110] The method for preparing a high cycle sodium battery positive electrode material provided in this embodiment comprises the following steps:
[0111] According to the chemical formula Na x Cu y Ni z Fe u Mn v O 2+q / β(Na a Mg b Al c A d J e O 2+p) wherein β=0.006, a=1.05, b=0.5, c=0.15, d=0.3, e=0.05, x=1.0, y=0.04, z=0.30, u=0.32, v=0.34, q=0, p=0, A is Zr, and J is Nb, a high cycle sodium positive electrode material is prepared:
[0112] According to the ratio in the target chemical formula, weigh the sodium source Na 2 CO 3 , copper source CuO, and nickel iron manganese ternary precursors, use a high-speed mixer to mix the three at high speed until there is no obvious white spot visually, and obtain a mixed material; the mixed material is placed in a 330mm×330mm×100mm sagger, with a filling amount of 3kg, and sintered at 1000℃ for 12h (i.e., the first sintering) in a box-type atmosphere furnace with an air flow of 20L / min. After cooling, the material block is tested for Shore hardness and particle strength. The Shore hardness meets 25-45HV, and the particle strength meets ≥80Mpa. Then the base material is obtained through a rotary mill, an air flow mill, and an ultrasonic vibrating screen. The process parameters are: a rotary mill gap of 200μm, a jet mill grinding pressure of 0.45Mpa, a branch machine frequency of 100Hz, a draft fan frequency of 35Hz, and a screen mesh of 350 meshes.
[0113] According to the ratio in the target chemical formula, the base material and Na 2 CO 3 Mg(OH) 2 、Al 2 O 3 、ZrO 2 and Nb 2 O 5 The mixture was mixed evenly, and then sintered in a box-type atmosphere furnace at 850° C. for 14 h at an air flow rate of 20 L / min (i.e., the second sintering), and then subjected to rotary grinding and 325-mesh vibrating sieve to obtain a high-cycle sodium battery positive electrode material.
[0114] like Figure 1 The electron microscope image of the high cycle sodium positive electrode material prepared in this embodiment is shown. The electron microscope test uses the JEOL S4800 model with an acceleration voltage of 5KV.
[0115] Example 2
[0116] The method for preparing a high-cycle sodium battery positive electrode material provided in this embodiment comprises the following steps:
[0117] According to the chemical formula Na x Cu y Ni z Fe u Mn v O 2+q / β(Na aMg b Al c A d J e O 2+p ) wherein β=0.005, a=0.99, b=0.40, c=0.25, d=0.25, e=0.10, x=1.0, y=0.035, z=0.305, u=0.32, v=0.34, q=0, p=0.02, A is Ti, and J is Nb, a high cycle sodium positive electrode material is prepared:
[0118] According to the ratio in the target chemical formula, weigh the sodium source Na 2 CO 3 , copper source CuO, and nickel iron manganese ternary precursor, use a high-speed mixer to mix the three at high speed until there is no obvious white spot visually, and obtain a mixed material; the mixed material is placed in a 330mm×330mm×100mm sagger, with a filling amount of 3kg, and sintered at 1100℃ for 12h (i.e., the first sintering) in a box-type atmosphere furnace with an air flow of 20L / min. After cooling, the material block is tested for Shore hardness and particle strength. The Shore hardness meets 25-45HV, and the particle strength meets ≥80Mpa. Then the base material is obtained through a rotary mill, an air flow mill, and an ultrasonic vibrating screen. The process parameters are: a rotary mill gap of 200μm, a jet mill grinding pressure of 0.4Mpa, a branch machine frequency of 90Hz, a draft fan frequency of 30Hz, and a screen mesh of 325 meshes.
[0119] According to the ratio in the target chemical formula, the base material and Na 2 CO 3 Mg(OH) 2 、Al 2 O 3 、TiO 2 and Nb 2 O 5 The mixture was mixed evenly, and then sintered at 900° C. for 10 h (i.e., the second sintering) in a box-type atmosphere furnace at an air flow rate of 20 L / min. After being subjected to rotary milling and 325-mesh vibrating sieve, a high-cycle sodium battery positive electrode material was obtained.
[0120] Example 3
[0121] The method for preparing the high cycle sodium battery positive electrode material provided in this embodiment comprises the following steps:
[0122] According to the chemical formula Na x Cu y Ni z Fe u Mn v O 2+q / β(Na a Mg bAl c A d J e O 2+p ) wherein β=0.004, a=1.0, b=0.35, c=0.20, d=0.3, e=0.15, x=0.985, y=0.045, z=0.315, u=0.29, v=0.35, q=-0.01, p=0.2, A is Zr, J is W, and a high cycle sodium positive electrode material is prepared:
[0123] According to the ratio in the target chemical formula, weigh the sodium source Na 2 CO 3 , copper source CuO, and nickel iron manganese ternary precursor, use a high-speed mixer to mix the three at high speed until there is no obvious white spot visually, and obtain a mixed material; the mixed material is placed in a 330mm×330mm×100mm sagger, with a filling amount of 3kg, and sintered at 900℃ for 16h (i.e., the first sintering) in a box-type atmosphere furnace with an air flow of 20L / min. After cooling, the material block is tested for Shore hardness and particle strength. The Shore hardness meets 25-45HV, and the particle strength meets ≥80Mpa. Then the base material is obtained through a rotary mill, an air flow mill, and an ultrasonic vibrating screen. The process parameters are: a rotary mill gap of 200μm, a jet mill grinding pressure of 0.5Mpa, a branch machine frequency of 120Hz, a draft fan frequency of 40Hz, and a screen mesh of 375 meshes.
[0124] According to the ratio in the target chemical formula, the base material and Na 2 CO 3 Mg(OH) 2 、Al 2 O 3 、ZrO 2 and WO 3 The mixture was mixed evenly, and then sintered at 800° C. for 20 h (i.e., the second sintering) in a box-type atmosphere furnace at an air flow rate of 20 L / min. After being subjected to a rotary mill and a 325-mesh vibrating sieve, a high-cycle sodium battery positive electrode material was obtained.
[0125] Example 4
[0126] The method for preparing the high cycle sodium positive electrode material provided in this embodiment comprises the following steps:
[0127] According to the chemical formula Na x Cu y Ni z Fe u Mn v O 2+q / β(Na a Mg b Al c A dJ e O 2+p ) wherein β=0.007, a=1.54, b=0.6, c=0.20, d=0.1, e=0.1, x=0.98, y=0.035, z=0.305, u=0.33, v=0.33, q=-0.015, p=0.17, A is Ti, J is W, and a high cycle sodium positive electrode material is prepared:
[0128] According to the ratio in the target chemical formula, weigh the sodium source Na 2 CO 3 , copper source CuO, and nickel iron manganese ternary precursor, use a high-speed mixer to mix the three at high speed until there is no obvious white spot visually, and obtain a mixed material; the mixed material is placed in a 330mm×330mm×100mm sagger, with a filling amount of 3kg, and sintered at 950℃ for 14h (i.e., the first sintering) in a box-type atmosphere furnace with an air flow of 20L / min. After cooling, the material block is tested for Shore hardness and particle strength. The Shore hardness meets 25-45HV, and the particle strength meets ≥80Mpa. Then the base material is obtained through a rotary mill, an air flow mill, and an ultrasonic vibrating screen. The process parameters are: a rotary mill gap of 200μm, a jet mill grinding pressure of 0.45Mpa, a branch machine frequency of 130Hz, a draft fan frequency of 35Hz, and a screen mesh of 400 meshes.
[0129] According to the ratio in the target chemical formula, the base material and Na 2 CO 3 Mg(OH) 2 、Al 2 O 3 、TiO 2 and WO 3 The mixture was mixed evenly, and then sintered at 830° C. for 12 h (i.e., the second sintering) in a box-type atmosphere furnace at an air flow rate of 20 L / min. The high-cycle sodium battery positive electrode material was obtained by grinding with a rotary wheel and screening with a 325-mesh vibration screen.
[0130] Example 5
[0131] The method for preparing the high cycle sodium battery positive electrode material provided in this embodiment comprises the following steps:
[0132] According to the chemical formula Na x Cu y Ni z Fe u Mn v O 2+q / β(Na a Mg b Al c A d J e O 2+p) wherein β=0.006, a=1.05, b=0.5, c=0.15, d=0.3, e=0.05, x=1.0, y=0.04, z=0.30, u=0.32, v=0.34, q=0, p=0, A is Zr, and J is V, a high cycle sodium positive electrode material is prepared:
[0133] According to the ratio in the target chemical formula, weigh the sodium source Na 2 CO 3 , copper source CuO, and nickel iron manganese ternary precursor, use a high-speed mixer to mix the three at high speed until there is no obvious white spot visually, and obtain a mixed material; the mixed material is placed in a 330mm×330mm×100mm sagger, with a filling amount of 3kg, and sintered at 1050℃ for 15h (i.e., the first sintering) in a box-type atmosphere furnace with an air flow of 20L / min. After cooling, the material block is tested for Shore hardness and particle strength. The Shore hardness meets 25-45HV, and the particle strength meets ≥80Mpa. Then the base material is obtained through a rotary mill, an air flow mill, and an ultrasonic vibrating screen. The process parameters are: a rotary mill gap of 200μm, a jet mill grinding pressure of 0.45Mpa, a branch machine frequency of 100Hz, a draft fan frequency of 35Hz, and a screen mesh of 325 meshes.
[0134] According to the ratio in the target chemical formula, the base material and Na 2 CO 3 Mg(OH) 2 、Al 2 O 3 、ZrO 2 and VO 2 The mixture was mixed evenly, and then sintered at 880° C. for 18 h (i.e., the second sintering) in a box-type atmosphere furnace at an air flow rate of 20 L / min, and then subjected to rotary grinding and 325-mesh vibrating sieve to obtain a high-cycle sodium battery positive electrode material.
[0135] Example 6
[0136] The preparation method of the high cycle sodium positive electrode material provided in this embodiment is basically the same as that in embodiment 1, except that A in the target chemical formula is Hf (the value of d remains unchanged), and ZrO 2 Replaced by HfO 2 .
[0137] Example 7
[0138] The preparation method of the high cycle sodium positive electrode material provided in this embodiment is basically the same as that in embodiment 1, except that J in the target chemical formula is Ta (the value of e remains unchanged), and Nb 2 O 5 Replace with Ta 2 O 5 .
[0139] Example 8
[0140] The preparation method of the high cycle sodium positive electrode material provided in this embodiment is basically the same as that in embodiment 1, except that J in the target chemical formula is Mo (the value of e remains unchanged), and Nb 2 O 5 Replaced by MoO 3 .
[0141] Comparative Example 1
[0142] The positive electrode material provided in this comparative example is the base material prepared in Example 1, namely Na x Cu y Ni z Fe u Mn v O 2+q , where x=1.0, y=0.04, z=0.30, u=0.32, v=0.34, q=0.
[0143] Comparative Example 2
[0144] The preparation method of the positive electrode material provided in this comparative example is basically the same as that of Example 1, except that β in the target chemical formula is 0.03, that is, the coating amount is different.
[0145] Comparative Example 3
[0146] The preparation method of the positive electrode material provided in this comparative example is basically the same as that in Example 1, the difference is that d=0, e=0, a=1.5, b=0.5, c=0.5, p=0 in the target chemical formula, that is, the coating layer does not contain A and J.
[0147] Experimental example
[0148] The Shore hardness (i.e., A) and particle strength (i.e., B) of the matrix material in each embodiment and each comparative example were tested respectively, and the particle size D of the positive electrode material prepared in each embodiment and each comparative example was tested respectively. 10 , particle size D 50 , particle size D 90 , and specific surface area (abbreviated as BET, unit is m 2 / g), XRD test was performed on the positive electrode materials prepared in each embodiment and each comparative example to obtain the peak area I003 of the 003 characteristic diffraction peak, the peak area I104 of the 104 characteristic diffraction peak, and the half-peak width FWHM104 of the 104 characteristic diffraction peak (i.e., E, °), and the pH of the aqueous solution of the positive electrode materials prepared in each embodiment and each comparative example was tested, and C=(D 90 -D 10 ) / D 50, D%=I003 / I104×100% (i.e. D=I003 / I104×100), and 1000×D×E / B+A+23.5C (abbreviated as X in Table 1), the results are shown in Table 1.
[0149] Among them, Shore hardness test: use the Shore hardness tester of Dongguan Sanliang Measuring Tools Co., Ltd.
[0150] Particle strength test: Tested using Shimadzu MCT micro compressor.
[0151] Particle size test: 3000 laser particle size distribution analyzer (Malvern), dispersion conditions: ultrasonicate deionized water and the substance to be tested for 60s (ultrasonic intensity 30%); test conditions: set the refractive index to 1.5, the absorbance to 1.0, the pump speed to 2000rpm, the laser intensity to greater than 70%, and the shading degree to 8-20%.
[0152] Specific surface area test: BSD-660S dynamic adsorption specific surface area analyzer; test method: pretreatment: weigh 5.000±0.01g of material and degas at 150℃ for 60min; adsorbent: nitrogen.
[0153] XRD test: using Bruker D8 advance, test range 10-80°, 5° / min.
[0154] pH test: Test equipment: Mettler Toledo FE-28 pH meter, Test method: Weigh 2±0.001g sample and dissolve it in 40ml pure water at 25℃, stir for 10min, and let it stand for 5min.
[0155] Furthermore, the positive electrode materials prepared in each embodiment and each comparative example were used as positive electrode active materials to make 26700 battery cells, and the capacity retention rate of each 26700 battery cell was tested after 500 cycles at a voltage of 2-4V, a charge and discharge rate of 1C / 1C, and 45°C. The results are shown in Table 1.
[0156] Among them, the composition of the positive electrode sheet in the 26700 battery cell is: the mass ratio of positive electrode active material: conductive carbon: binder PVDF = 96:2:2; the composition of the negative electrode sheet in the 26700 battery cell is: the mass ratio of hard carbon: conductive carbon: binder PVDF = 95:2:3; the separator in the 26700 battery cell is: 9μm PP+1.5μm alumina.
[0157] Table 1 Physical and chemical properties and cycle performance test results
[0158]
[0159] It can be seen from Table 1 that the positive electrode materials prepared in each embodiment have excellent cycle performance, which is significantly higher than that of each comparative example. This shows that the positive electrode material provided by the present invention can reduce the side reaction with the electrolyte, thereby improving the cycle performance of the prepared battery.
[0160] Although the present invention has been illustrated and described with specific embodiments, it should be appreciated that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Those skilled in the art should understand that the technical solutions described in the above embodiments may be modified, or some or all of the technical features thereof may be replaced by equivalents without departing from the spirit and scope of the present invention. However, these modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments of the present invention. Therefore, this means that all such replacements and modifications within the scope of the present invention are included in the appended claims.
Claims
1. A high cycle sodium positive electrode material, characterized in that: It comprises a base material and a coating layer coated on the surface of the base material; The general formula of the matrix material is Na x Cu y Ni z Fe u Mn v O 2+q ; Among them, 0.96≤x≤1.01, 0.025≤y≤0.055, 0.28≤z≤0.32, 0.29≤u≤0.34, 0.30≤v≤0.38, -0.04<q≤0.04, y+z+u+v=1; The general formula of the coating layer is Na a Mg b Al c A d J e O 2+p ; Wherein, A includes metal elements with an average valence of +4, J includes metal elements with an average valence δ of +5 or +6, 0.8≤a≤1.55, 0.3≤b≤0.7, 0.1≤c≤0.3, 0.2≤d≤0.4, 0<e≤0.4, -0.5≤p≤0.25, b+c+d+e=1.
2. The high cycle sodium positive electrode material according to claim 1, characterized in that: At least one of the following conditions is met: (1) A includes at least one of Ti, Hf and Zr; (2) J having an average valence of +5 includes at least one of Nb, V and Ta; (3) J having an average valence of +6 includes at least one of W and Mo.
3. The high cycle sodium battery positive electrode material according to claim 1, characterized in that: The molar amount of the coating layer is 0.002 to 0.01 of the molar amount of the base material.
4. The high cycle sodium battery positive electrode material according to claim 1, characterized in that: The Shore hardness of the matrix material is 25-45 HV, and the particle strength of the matrix material is ≥80 MPa.
5. The high cycle sodium battery positive electrode material according to claim 1, characterized in that: The Shore hardness of the matrix material is A, the particle strength of the matrix material is B, and the particle size (D 90 -D 10 ) / D 50 is C, the percentage of the peak area I003 of the 003 characteristic diffraction peak in the X-ray diffraction spectrum of the high cycle sodium positive electrode material to the peak area I104 of the 104 characteristic diffraction peak I003 / I104×100% is D%, and the half-peak width FWHM104 of the 104 characteristic diffraction peak in the X-ray diffraction spectrum of the high cycle sodium positive electrode material is E, wherein A, B, C, D, and E satisfy the following relationship: 100≤1000×D×E / B+A+23.5C≤100.5; Among them, the unit of A is HV, the unit of B is MPa, the unit of C is 1, and the unit of E is °.
6. The high cycle sodium battery positive electrode material according to claim 1, characterized in that: At least one of the following conditions is met: (1) The particle size D of the high cycle sodium positive electrode material 10 Satisfy 5.1μm≤D 10 ≤5.4μm; (2) The particle size D of the high cycle sodium positive electrode material 50 Satisfy 9.2μm≤D 50 ≤9.8μm; (3) The particle size D of the high cycle sodium positive electrode material 90 Satisfy 15.9μm≤D 90 ≤16.9μm; (4) The particle size (D 90 -D 10 ) / D 50 Satisfy 1.13≤(D 90 -D 10 ) / D 50 ≤1.19; (5) The high cycle sodium battery positive electrode material is an O3 type layered oxide; (6) In the X-ray diffraction spectrum of the high cycle sodium positive electrode material, the percentage of the peak area I003 of the 003 characteristic diffraction peak to the peak area I104 of the 104 characteristic diffraction peak I003 / I104×100% satisfies 88%≤I003 / I104×100%≤132%; (7) The half-peak width FWHM104 of the 104 characteristic diffraction peak in the X-ray diffraction spectrum of the high-cycle sodium positive electrode material satisfies 0.054≤FWHM104≤0.068; (8) At 25° C., the pH of a solution of 2 g of the high cycle sodium cathode material dissolved in 40 mL of water is 12.00 to 12.25; (9) The specific surface area of the high cycle sodium positive electrode material is 0.26 to 0.3 m 2 / g; (10) The capacity retention rate of a 26700 battery cell containing the high-cycle sodium battery positive electrode material after 500 cycles at 45°C is ≥97.5%.
7. The method for preparing a high cycle sodium battery positive electrode material according to any one of claims 1 to 6, characterized in that: The steps include: (a) mixing a sodium source, a copper source and a nickel-iron-manganese ternary precursor and then performing a first sintering to obtain a matrix material; (b) mixing the matrix material with a sodium source, a magnesium source, an aluminum source, an A-containing compound and a J-containing compound, and then performing a second sintering to obtain the high-cycle sodium battery positive electrode material.
8. The method for preparing a high cycle sodium positive electrode material according to claim 7, characterized in that: At least one of the following conditions is met: (1) The first sintering temperature is 900-1100° C. and the holding time is 12-16 hours; (2) The second sintering temperature is 800-900°C and the holding time is 10-20h.
9. A positive electrode sheet, characterized in that: It comprises the high cycle sodium battery positive electrode material as described in any one of claims 1 to 6.
10. A sodium ion battery, characterized in that: Comprising the positive electrode sheet as claimed in claim 9.
Citation Information
Cited By
Coated sodium ion battery positive electrode material as well as preparation method and application thereof
CN119275262A
Coated sodium ion battery positive electrode material and preparation method and application thereof