Water-soluble chelate polymer and method for producing same
By using water-soluble chelating polymers and chelating groups-containing polymer particles in lithium-ion battery electrodes, the problem of manganese or nickel ion dissolution in lithium-ion batteries is solved, and the electrode is improved by high-molecular weight hydrogen ionic alginic acid Performance, achieving efficient cycle life and charging and discharging characteristics extension.
Patent Information
- Application Number
- CN202380031942.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-01-13
- Filing Date
- 2023-01-30
- Publication Date
- 2024-11-15
AI Technical Summary
Dissolution and precipitation of manganese or nickel ions in the active substances of existing lithium-ion battery electrodes leads to reduced circulation characteristics and magnification characteristics, and the use of organic solvents in traditional binders leads to high manufacturing costs and environmental pollution, and high molecular weight hydrogen ionic alginic acid Difficult to obtain and apply.
Anionic polymers with carboxyl, sulfonic acid and/or sulfate groups are used to form a water-soluble chelating polymer through ionic bonding to form a water-soluble chelating polymer for rapid capture of heavy metal ions and use in lithium-ion battery electrodes containing The polymer compound particles of chelating groups and high molecular weight hydrogen ionic alginic acid are used as binders to improve the electrode performance.
It realizes rapid capture of heavy metal ions, extends the cycle life and charge and discharge characteristics of lithium-ion batteries, reduces manufacturing costs, and improves the workability and storage of electrodes.
Smart Images

Figure BDA0005067274560000061 
Figure BDA0005067274560000062 
Figure BDA0005067274560000071
Abstract
Description
Technical Field
[0001] The first embodiment of the present invention relates to a water-soluble chelate polymer and a method for producing the same. Furthermore, the second embodiment of the present invention relates to a chelate polymer and a method for producing the same. Furthermore, the third and fourth embodiments of the present invention relate to a lithium-ion battery electrode mixture composition, a slurry for forming a lithium-ion battery electrode mixture layer, an electrode for a lithium-ion battery, and a lithium-ion battery. Furthermore, the fifth and sixth embodiments of the present invention relate to a composition, an adhesive for lithium-ion battery electrodes, a slurry for forming a lithium-ion battery electrode mixture layer, an electrode for a lithium-ion battery, and a lithium-ion battery. Furthermore, the seventh embodiment of the present invention relates to a high molecular weight hydrogen ion type alginic acid, a method for producing the same, an adhesive for lithium-ion battery electrodes, a slurry for forming a lithium-ion battery electrode mixture layer, an electrode for a lithium-ion battery, and a lithium-ion battery. Background Art
[0002] All along, the chelate resin that imports and forms chelate with the chelate functional group of these metal ions with selectivity between metal ions has excellent selectivity for metal ions, particularly heavy metal ions, therefore, is used to remove heavy metal in water treatment fields such as wastewater treatment.In recent years, in order to meet the requirement of high integration of semiconductor or prolong the life-span of lithium ion battery, the demand for the trace heavy metal ions in the organic solvent is also increasing day by day, and organic solvent is purified by chelate resin.Yet chelate resin in the past is the beaded particle that forms by crosslinking agent height crosslinking such as divinylbenzene, therefore, has the following problem: the diffusion of heavy metal ion to resin interior is slow, and processing speed will be slowed down and liquid will be led to lentamente, otherwise the capture efficiency of heavy metal ion will be reduced.
[0003] In order to solve the problem of above-mentioned pearl-shaped resin, fibrous resin (for example, referring to patent documentation 1,2) has been proposed.The specific surface area of fibrous resin is large, and near the surface, chelating functional groups are imported, so the capture speed of heavy metal ions is fast, which can improve the shortcoming of above-mentioned pearl-shaped resin.But, in recent years, the requirement for the removal level of heavy metal ions is improved day by day, even if use above-mentioned fibrous resin, the situation that can not satisfy the removal level is increasing.
[0004] Prior art literature
[0005] Patent Literature
[0006] Patent Document 1: Japanese Patent Application Publication No. 2000-248467
[0007] Patent Document 2: Japanese Patent Application Publication No. 2013-194339
[0008] Patent Document 3: Japanese Patent Application Publication No. 2000-58055
[0009] Patent Document 4: Japanese Patent Application Publication No. 2000-195548
[0010] Patent Document 5: Japanese Patent Application Laid-Open No. 53-41732
[0011] Patent Document 6: Japanese Patent Application Publication No. 2003-68292
[0012] Patent Document 7: Japanese Patent Application Publication No. 2008-27904
[0013] Patent Document 8: International Publication No. 2012 / 133120
[0014] Patent Document 9: Japanese Patent Application Laid-Open No. 10-92415
[0015] Patent Document 10: Japanese Patent Application Publication No. 2001-15114
[0016] Patent Document 11: Japanese Patent Application Publication No. 2014-96238
[0017] Patent Document 12: Japanese Patent Application Publication No. 2014-195018
[0018] Patent Document 13: Japanese Patent Application Publication No. 2015-191862
[0019] Patent Document 14: International Publication No. 2016 / 052715
[0020] Patent Document 15: Japanese Patent Application Laid-Open No. 10-92415 Summary of the invention
[0021] Problems to be solved by the invention
[0022] The first and second aspects of the present invention aim to provide a water-soluble chelate polymer that can rapidly capture a trace amount of heavy metal ions and reduce the amount of heavy metal ions to below the ppm level in a short period of time.
[0023] However, in recent years, lithium-ion batteries have been widely used as power sources for electrical devices, etc. Furthermore, their use as power sources for electric vehicles is expanding recently, and there is a demand for improved characteristics, such as higher capacity, higher output, longer cycle life, and higher safety.
[0024] The electrode of a lithium-ion battery has a structure in which a porous body composed mainly of powdered active material, conductive additive and binder is stacked and bonded to a current collector. 0.5 Mn 1.5 O4、LiNi 0.5 Mn0.3 Co 0.2 O2、LiNi 0.33 Mn 0.33 Co 0.33 O2、LiNi 0.8 Mn 0.1 Co 0.1 However, during charge and discharge, manganese or nickel in the active material of these lithium composite oxides will dissolve, ionize, precipitate, and accumulate on the negative electrode, resulting in a decrease in cycle characteristics or rate characteristics.
[0025] In order to prevent the degradation of this battery characteristic, a positive electrode material for lithium secondary battery formed by covering the surface of lithium manganate with an organic compound that can provide a ligand is disclosed (for example, see patent document 3.). It is believed that the manganese ions or nickel ions dissolved from the positive electrode active material can be captured by the organic compound that can provide a ligand, but because the organic compound that can provide a ligand is a low molecular compound, it is easy to dissolve and detach from the surface of lithium manganate, and its effect is limited. In addition, it is also disclosed that in a non-aqueous electrolyte secondary battery with a manganese-based positive electrode, a chelating agent or crown ether that forms a complex with manganese is contained in the non-aqueous electrolyte (for example, see patent document 4.). It is believed that the manganese ions or nickel ions dissolved from the positive electrode active material can be captured by the chelating agent or crown ether in the non-aqueous electrolyte, but because the chelating agent or crown ether is dissolved in the non-aqueous electrolyte, it will also diffuse to the negative electrode and be reduced and decomposed at the negative electrode, so the effect is not good.
[0026] The third aspect of the present invention also aims to provide a lithium ion battery electrode mixture composition, a slurry for forming a lithium ion battery electrode mixture layer, a lithium ion battery electrode, and a lithium ion battery that can produce an electrode having excellent charge and discharge characteristics and a prolonged cycle life.
[0027] In addition, it is known that the electrodes of lithium-ion batteries have a structure in which a porous body mainly composed of powdered active materials, conductive additives and binders is stacked and bonded to a current collector. Its performance is not only affected by the characteristics of the active materials, but also greatly affected by the type of binder.
[0028] Polyvinylidene fluoride (PVDF) has always been the mainstream binder for positive electrodes. However, since organic solvents such as N-methylpyrrolidone are used in the manufacture of electrodes, it has the following disadvantages: the increase in supporting equipment related to electrode manufacturing leads to higher costs. For example, emission reduction equipment is required in the slurry preparation process or the electrode sheet coating process, and solvent recovery equipment is required in the electrode sheet drying process; the cost of purchasing or recovering organic solvents is huge, and the operating cost increases; since PVDF has low adhesion to the positive electrode active material, the amount of binder added increases.
[0029] On the other hand, as aqueous adhesives that do not use organic solvents and can be dispersed and dissolved in water, the following are disclosed: using polyvinyl alcohol and methyl cellulose (for example, see Patent Document 5); using xanthan gum (for example, see Patent Document 6); using starch-type polysaccharides such as amylose and amylopectin (for example, see Patent Documents 7 and 8); and using alginic acid or alginic acid derivatives (for example, see Patent Documents 9, 10, 11, 12, and 13). Aqueous adhesives do not require emission reduction equipment when manufacturing electrode plates, and the working environment is also good, so they are preferred, but the combination of active materials and adhesives may lead to problems such as reduced adhesion to the active materials and corrosion of the current collector.
[0030] In addition, it is known that LiMn2O4, LiNi 0.5 Mn 1.5 O4、LiNi 0.5 Mn 0.3 Co 0.2 O2、LiNi 0.33 Mn 0.33 Co 0.33 O2、LiNi 0.8 Mn 0.1 Co 0.1 O2、LiNi 0.8 Co 0.15 Al 0.05 O2、LiMn 0.7 Fe 0.3 PO4 and other lithium composite oxides, but during charge and discharge, manganese or nickel in the active material of these lithium composite oxides will dissolve, ionize, precipitate, and accumulate on the negative electrode, resulting in reduced cycle characteristics or rate characteristics.
[0031] The fourth scheme of the present invention also aims to provide a binder for lithium ion battery electrodes which has excellent workability when making electrodes and can make electrodes with excellent charge and discharge characteristics and extended cycle life, as well as a slurry for forming a lithium ion battery electrode mixture layer, a lithium ion battery electrode and a lithium ion battery using the same.
[0032] The fifth embodiment of the present invention also aims to provide a composition that has excellent workability when making electrodes and can make electrodes with excellent charge and discharge characteristics and extended cycle life, as well as a binder for lithium ion battery electrodes using the composition, a slurry for forming a lithium ion battery electrode mixture layer using the composition, an electrode for a lithium ion battery, and a lithium ion battery.
[0033] The sixth embodiment of the present invention also aims to provide a composition, a binder for lithium-ion battery electrodes using the same, a slurry for forming a lithium-ion battery electrode mixture layer using the same, an electrode for a lithium-ion battery, and a lithium-ion battery. The composition has excellent workability in making electrodes due to its excellent storage, transportability, and operability in a dry state. When used as a binder for lithium-ion battery electrodes, it easily forms ionic compounds by contact with water, thereby making it possible to make electrodes with excellent charge and discharge characteristics and extended cycle life.
[0034] On the other hand, hydrogen ion alginic acid has always been manufactured by the following method: dissolving alginate such as sodium alginate in water, adding acid to the aqueous solution, precipitating water-insoluble hydrogen ion alginic acid and recovering (for example, referring to patent documentation 14). However, in this method, the molecular weight of alginate is reduced due to the effect of acid, and therefore, it is impossible to obtain a hydrogen ion alginic acid of a certain or higher molecular weight. In addition, when it is desired to obtain a hydrogen ion alginic acid of a higher molecular weight by this method, it is necessary to use a material with a higher molecular weight of alginate of a raw material, and the viscosity of the aqueous solution significantly increases, so it can only be produced with a dilute solution of low concentration. In addition, the hydrogen ion alginic acid obtained is also recovered in the form of a hydrogel comprising a large amount of water, so a burden is brought to the drying process, and the productivity is low, which becomes a problem.
[0035] On the other hand, hydrogen ion alginic acid or alginate, alginic acid derivatives (hereinafter referred to as "alginic acid") can be used as raw materials for lithium ion battery electrode binders (for example, see Patent Document 14, Patent Document 15, Patent Document 10). However, when the molecular weight of the alginic acid is low, there is a problem of cracking or peeling of the electrode due to high adhesion to the current collector.
[0036] The seventh embodiment of the present invention also aims to provide a high molecular weight hydrogen ion type alginic acid useful as a raw material for a binder for lithium ion battery electrodes. Furthermore, another object is to provide a binder for lithium ion battery electrodes, a slurry for forming a lithium ion battery electrode mixture layer, a lithium ion battery electrode, and a lithium ion battery using the high molecular weight hydrogen ion type alginic acid as a raw material.
[0037] Another object of the present invention is to provide a method for producing hydrogen ion-type alginic acid with excellent productivity.
[0038] Solutions for solving problems
[0039] The present inventors have conducted intensive research to solve the above-mentioned problems and have found that the above-mentioned purpose can be achieved by using a water-soluble chelate polymer obtained by introducing a chelate functional group into an anionic polymer having a carboxyl group, a sulfonic acid group and / or a sulfate group via an ionic bond, thereby completing the first embodiment of the present invention.
[0040] That is, the first aspect of the present invention is [1-1] to [1-5] shown below.
[0041] [1-1]
[0042] A water-soluble chelating polymer is formed by ionically bonding an anionic polymer having a carboxyl group, a sulfonic acid group and / or a sulfate group and a chelating functional group having a cationic functional group, wherein the water-soluble chelating polymer contains 0.2 to 6 mmol / g of chelating functional groups and has a weight average molecular weight of 30,000 to 1,000,000.
[0043] [1-2]
[0044] The water-soluble chelate polymer according to the above [1-1], wherein the anionic polymer is an acidic polysaccharide.
[0045] [1-3]
[0046] The water-soluble chelate polymer according to [1-1] or [1-2] above, wherein the chelate functional group is an aminocarboxylic acid group or an aminophosphonic acid group.
[0047] [1-4]
[0048] A method for producing a water-soluble chelate polymer, wherein an anionic polymer having carboxyl groups, sulfonic acid groups and / or sulfate groups is brought into contact with an acid to convert the carboxyl groups, sulfonic acid groups and / or sulfate groups into hydrogen ion types, and then brought into contact with a compound having an amino group and containing a chelate functional group to introduce the chelate functional group into the anionic polymer.
[0049] [1-5]
[0050] The method for producing a water-soluble chelated polymer according to the above-mentioned [1-4] is characterized in that an anionic polymer having a hydrogen ion type carboxyl group, a sulfonic acid group and / or a sulfate group is dispersed in a hydrophobic solvent, a compound having an amino group and containing a chelating functional group is dissolved in water, and the two are mixed to prepare an oil-in-water emulsion, and the chelating functional group is introduced into the anionic polymer.
[0051] [1-6]
[0052] A method for capturing heavy metal ions, comprising adding the water-soluble chelate polymer described in [1-1] to [1-3] to a solution containing heavy metal ions, and capturing the heavy metal ions with the chelate polymer.
[0053] The present inventors speculate as follows about the reason why the above-mentioned object is achieved by the first aspect of the present invention.
[0054] That is, the chelating polymer of the first scheme of the present invention can be made into an aqueous solution and can also be easily coated on a particulate carrier with high polarity and large specific surface area. The coated particulate carrier can quickly adsorb and remove trace heavy metal ions in the organic solvent in a short time due to the synergistic effect of the chelating functional groups arranged near the surface and the large specific surface area.
[0055] Furthermore, if the same effect is to be obtained by using the above-mentioned fibrous chelate resin, the fibrous chelate resin needs to be pulverized to an average particle size of 5 μm or less, but the fibrous chelate resin is difficult to pulverize, which is not suitable from the cost point of view.
[0056] The second aspect of the present invention is [2-1] to [2-9] shown below.
[0057] [2-1]
[0058] A chelate polymer having a structure represented by the following general formula (1) and containing 0.2 to 5 mmol / g of a chelate functional group.
[0059] PS-XA-CL(1)
[0060] (In the formula, PS represents an acidic polysaccharide or a basic polysaccharide. X represents a group represented by -O- or -N(R)-, R represents a hydrogen atom or a hydrocarbon group having 1 to 6 carbon atoms. A represents an organic group having 3 to 30 carbon atoms, and CL represents an organic group having 1 to 30 carbon atoms containing a chelating functional group.)
[0061] [2-2]
[0062] The chelate polymer according to the above-mentioned [2-1] has a structure represented by the following general formula (2).
[0063] [Chemical formula 1]
[0064]
[0065] (In the formula, A and CL have the same meanings as above. M represents a hydrogen atom or an alkali metal ion, and n represents an integer of 10 to 1000.)
[0066] [2-3]
[0067] The chelate polymer according to the above [2-1] or [2-2], which has a weight average molecular weight of 10,000 to 1,000,000.
[0068] [2-4]
[0069] A method for producing a chelate polymer according to the above [2-1], wherein an acidic polysaccharide and / or a basic polysaccharide is reacted with an epihalohydrin and / or a polyfunctional epoxy compound having 2 to 6 epoxy groups, and then reacted with a compound having an amino group and a chelate functional group.
[0070] [2-5]
[0071] A chelate polymer having a structure represented by the following general formula (3) and containing 0.2 to 5 mmol / g of a chelate functional group.
[0072] [Chemical formula 2]
[0073]
[0074] (In the formula, PS and X have the same meanings as above. B represents a vinyl monomer residue having a chelating functional group and 4 to 30 carbon atoms, D represents a vinyl monomer residue having no chelating functional group and 4 to 30 carbon atoms, and l and m each independently represent an integer of 10 to 500.)
[0075] [2-6]
[0076] The chelate polymer according to the above-mentioned [2-5] has a structure represented by the following general formula (4).
[0077] [Chemical formula 3]
[0078]
[0079] (In the formula, B, D, M, l, m, and n have the same meanings as above.)
[0080] [2-7]
[0081] The chelate polymer according to the above [2-5] or [2-6], which has a weight average molecular weight of 10,000 to 1,000,000.
[0082] [2-8]
[0083] A method for producing a chelate polymer according to the above [2-5], wherein an epoxy group-containing vinyl monomer is graft-polymerized onto an acidic polysaccharide and / or a basic polysaccharide, and then the monomer is reacted with a compound having an amino group and a chelate functional group.
[0084] [2-9]
[0085] A method for capturing heavy metal ions, comprising adding the chelate polymer described in any one of [2-1] to [2-3] and [2-5] to [2-7] to a solution containing heavy metal ions, and capturing the heavy metal ions with the chelate polymer.
[0086] The present inventors speculate as follows about the reason why the above-mentioned object is achieved by the second aspect of the present invention.
[0087] That is, the chelate polymer of the second embodiment of the present invention is water-soluble or water-swellable, has high affinity with highly polar organic solvents, and can be easily crushed to form microparticles, so it can quickly adsorb and remove trace heavy metal ions in polar organic solvents in a short time.
[0088] The third aspect of the present invention is [3-1] to [3-12] shown below.
[0089] [3-1]
[0090] A lithium ion battery electrode mixture composition comprises an electrode mixture comprising an active material, a binder and a conductive auxiliary agent as required, wherein water-insoluble polymer compound particles containing a chelate group are contained, and the binder is a water-soluble polymer.
[0091] [3-2]
[0092] The lithium ion battery electrode mixture composition according to the above [3-1], wherein the water-insoluble polymer compound fine particles containing a chelate group are water-insoluble polysaccharide fine particles containing a chelate group.
[0093] [3-3]
[0094] The lithium ion battery electrode mixture composition according to the above [3-1], wherein the water-soluble polymer is a polysaccharide, a homopolymer or copolymer of (meth)acrylic acid, a homopolymer or copolymer of maleic acid, or a salt thereof.
[0095] [3-4]
[0096] A slurry for forming an electrode mixture layer for a lithium ion battery, comprising the electrode mixture composition according to any one of [3-1] to [3-3] and water.
[0097] [3-5]
[0098] A lithium ion battery electrode comprising the electrode mixture composition described in any one of [3-1] to [3-3] above.
[0099] [3-6]
[0100] A lithium ion battery comprising the electrode for a lithium ion battery described in [3-5] above in an electrode mixture of at least one of a positive electrode and a negative electrode.
[0101] [3-7]
[0102] A lithium ion battery electrode mixture composition comprises an electrode mixture comprising an active material, a binder and a conductive auxiliary agent as required, wherein organic solvent-insoluble polymer compound particles containing a chelating group are contained, and the binder is a fluorine-based resin.
[0103] [3-8]
[0104] The lithium ion battery electrode mixture composition according to the above [3-7], wherein the organic solvent-insoluble polymer compound fine particles containing a chelate group are organic solvent-insoluble polysaccharide fine particles containing a chelate group.
[0105] [3-9]
[0106] The lithium ion battery electrode mixture composition according to the above [3-7], wherein the organic solvent is an amide solvent.
[0107] [3-10]
[0108] A slurry for forming an electrode mixture layer for a lithium ion battery, comprising the electrode mixture composition according to any one of [3-7] to [3-9] above and an organic solvent.
[0109] [3-11]
[0110] A lithium ion battery electrode comprising the electrode mixture composition described in any one of [3-7] to [3-9] above.
[0111] [3-12]
[0112] A lithium ion battery comprising the electrode for a lithium ion battery described in [3-11] above in an electrode mixture of at least one of a positive electrode and a negative electrode.
[0113] The present inventors speculate as follows about the reason why the above-mentioned object is achieved by the third aspect of the present invention.
[0114] That is, by including insoluble polymer compound particles containing chelate groups in the electrode mixture layer, the manganese ions or nickel ions dissolved from the positive electrode active material are captured by the insoluble polymer compound particles containing chelate groups near the active material, therefore, manganese or nickel can be suppressed from precipitating and accumulating to the negative electrode active material, and excellent charge-discharge characteristics and cycle life can be achieved. In addition, it is inferred that since the insoluble polymer compound containing chelate groups is a particle, the capture efficiency of manganese ions or nickel ions is improved.
[0115] The fourth aspect of the present invention is [4-1] to [4-5] shown below.
[0116] [4-1]
[0117] A binder for lithium ion battery electrodes, wherein in the lithium ion battery, the binder for binding an active material, a conductive auxiliary agent and a current collector comprises a polymer compound containing a chelate group.
[0118] [4-2]
[0119] The adhesive according to the above [4-1], wherein the chelate group in the chelate group-containing polymer compound is bonded to the polymer compound via a covalent bond and / or an ionic bond.
[0120] [4-3]
[0121] A slurry for forming a lithium ion battery electrode mixture layer, comprising an active material, a conductive aid, the binder described in [4-1] or [4-2] above, and water.
[0122] [4-4]
[0123] A lithium ion battery electrode comprising the binder described in [4-1] or [4-2] above.
[0124] [4-5]
[0125] A lithium ion battery comprising the electrode described in [4-4] above.
[0126] The present inventors speculate as follows about the reason why the above-mentioned object is achieved by the fourth aspect of the present invention.
[0127] That is, by using a polymer compound containing a chelate group in the binder, the chelate group can capture manganese ions or nickel ions dissolved from the positive electrode active material near the positive electrode and / or negative electrode, and inhibit the precipitation and accumulation of the negative electrode active material, thereby achieving excellent charge and discharge characteristics and an extension of the cycle life.
[0128] The fifth aspect of the present invention is [5-1] to [5-6] shown below.
[0129] [5-1]
[0130] A composition comprises a high molecular compound and a low molecular compound containing a chelating group.
[0131] [5-2]
[0132] The composition according to the above [5-1], wherein the polymer compound is a water-soluble polymer compound, and the chelate group-containing low-molecular compound is a water-soluble compound.
[0133] [5-3]
[0134] A binder for lithium-ion battery electrodes, comprising the composition described in [5-1] or [5-2] above.
[0135] [5-4]
[0136] A slurry for forming a lithium ion battery electrode mixture layer, comprising an active material, a conductive aid, the binder described in [5-3] above, and water.
[0137] [5-5]
[0138] A lithium ion battery electrode comprising the binder described in [5-3] above.
[0139] [5-6]
[0140] A lithium ion battery comprising the electrode described in [5-5] above.
[0141] The present inventors speculate as follows about the reason why the above-mentioned object is achieved by the fourth aspect of the present invention.
[0142] That is, it can be considered that when a composition formed by a physical mixture of a polymer compound and a low molecular weight compound containing a chelate group is used in a binder, the binder covers the active material, and the low molecular weight compound containing a chelate group dispersed in the binder efficiently captures manganese ions or nickel ions dissolved from the positive electrode active material near the positive electrode and / or the negative electrode, thereby inhibiting the precipitation and accumulation of manganese or nickel on the negative electrode active material, and achieving excellent charge and discharge characteristics and an extension of the cycle life.
[0143] The sixth aspect of the present invention is [6-1] to [6-8] shown below.
[0144] [6-1]
[0145] A composition comprises hydrogen ion type alginic acid and a compound containing a chelating group.
[0146] [6-2]
[0147] The composition according to [6-1] or [6-2], wherein the chelate group-containing compound is a compound containing at least one basic functional group selected from the group consisting of a primary amino group, a secondary amino group, a tertiary amino group, and an imino group.
[0148] [6-3]
[0149] The composition according to [6-1] above, wherein the chelate group-containing compound is a compound having an aqueous solution having a pH of 3 to 9 when dissolved in water.
[0150] [6-4]
[0151] The composition according to any one of [6-1] to [6-3] above, further comprising an active substance.
[0152] [6-5]
[0153] A binder for lithium-ion battery electrodes, comprising the composition described in any one of [6-1] to [6-3] above.
[0154] [6-6]
[0155] A slurry for forming a lithium ion battery electrode mixture layer, comprising an active material, a conductive aid, the binder described in [6-5] above, and water.
[0156] [6-7]
[0157] A lithium ion battery electrode comprising the binder described in [6-5] above.
[0158] [6-8]
[0159] A lithium ion battery comprising the lithium ion battery electrode described in [6-7] above.
[0160] The seventh aspect of the present invention is [7-1] to [7-6] shown below.
[0161] [7-1]
[0162] A high molecular weight hydrogen ion type alginic acid has a weight average molecular weight of 500,000 to 1,500,000 and a hydrogen ion substitution rate of 80 to 99%.
[0163] [7-2]
[0164] A method for producing hydrogen ion-type alginic acid, wherein at least one of an alkali metal salt of alginate or an alkaline earth metal salt of alginate is dispersed in a poor solvent thereof, and then an acid is added to exchange ions of at least one of the alkali metal salt of alginate or an alkaline earth metal salt of alginate into a hydrogen ion type in a dispersed state.
[0165] [7-3]
[0166] A binder for lithium-ion battery electrodes, comprising the high molecular weight hydrogen ion type alginic acid described in [7-1] above.
[0167] [7-4]
[0168] A slurry for forming a lithium ion battery electrode mixture layer, comprising an active material, a conductive aid, the binder for lithium ion battery electrodes described in [7-3] above, and water.
[0169] [7-5]
[0170] A lithium ion battery electrode comprising an active material, a conductive aid and the binder for lithium ion battery electrodes described in [7-3] above.
[0171] [7-6]
[0172] A lithium ion battery comprising the lithium ion battery electrode described in [7-5] above.
[0173] Effects of the Invention
[0174] According to the first and second aspects of the present invention, a water-soluble chelate polymer capable of rapidly capturing a trace amount of heavy metal ions and reducing the amount of heavy metal ions to below the ppm level in a short period of time can be produced and provided by a simple method.
[0175] According to the third aspect of the present invention, a lithium ion battery electrode mixture composition and a slurry for forming a lithium ion battery electrode mixture layer, as well as a lithium ion battery electrode and a lithium ion battery are provided, which can produce a battery having excellent charge and discharge characteristics and a prolonged cycle life.
[0176] According to the fourth scheme of the present invention, a binder for lithium ion battery electrodes and a slurry for forming a lithium ion battery electrode mixture layer can be provided, which have excellent workability when making electrodes and can make electrodes with excellent charge and discharge characteristics and extended cycle life. Furthermore, by using it, electrodes for lithium ion batteries and lithium ion batteries with excellent charge and discharge characteristics and extended cycle life can also be provided.
[0177] According to the fifth and sixth schemes of the present invention, there can be provided a composition which has excellent workability when making electrodes and can make electrodes with excellent charge and discharge characteristics and extended cycle life, an adhesive for lithium ion battery electrodes, and a slurry for forming a lithium ion battery electrode mixture layer. Furthermore, by using the same, there can be provided electrodes for lithium ion batteries and lithium ion batteries with excellent charge and discharge characteristics and extended cycle life.
[0178] According to the seventh aspect of the present invention, it is possible to provide high molecular weight hydrogen ion type alginic acid useful as a raw material of a binder for lithium ion battery electrodes, and the high molecular weight hydrogen ion type alginic acid can be produced with good productivity. BRIEF DESCRIPTION OF THE DRAWINGS
[0179] Figure 1 This is the FT-IR spectrum of the hydrogen ion type alginic acid used in Example 1-1.
[0180] Figure 2 This is the FT-IR spectrum of the chelated polymer obtained in Example 1-1.
[0181] Figure 3 This is a graph comparing the charge-discharge cycle characteristics of the laminated batteries obtained in Example 4-1, Example 4-2, and Comparative Example 4-1. DETAILED DESCRIPTION
[0182] Hereinafter, the first aspect of the present invention will be described in detail.
[0183] A first aspect of the present invention is a water-soluble chelate polymer and a method for producing the same.
[0184] The water-soluble chelating polymer of the first embodiment of the present invention is formed by bonding an anionic polymer having a carboxyl group, a sulfonic acid group and / or a sulfate group and a chelating functional group having a cationic functional group via ionic bonds, wherein the chelating functional group is contained in an amount of 0.2 to 6 mmol / g and the weight average molecular weight is 30,000 to 1,000,000. In the first embodiment of the present invention, "water-soluble" means that the solubility in water is 0.1 to 50 g / 100 g. "Anionic polymer" refers to a polymer that can fix the chelating functional group via ionic bonds, and is a polymer having a carboxyl group, a sulfonic acid group and / or a sulfate group as a functional group for fixing the chelating functional group. Some examples of anionic polymers having a carboxyl group, a sulfonic acid group and / or a sulfate group include: poly(acrylic acid), poly(methacrylic acid), poly(itaconic acid), poly(maleic acid), ethylene-maleic acid copolymer, isobutylene-maleic acid copolymer, methyl vinyl ether-maleic acid copolymer, styrene-maleic acid copolymer, poly(fumaric acid), poly(vinyl sulfonic acid), poly(styrene sulfonic acid), poly(2-sulfoethyl methacrylate), poly(2-sulfoethyl acrylate), poly(3-sulfoethyl acrylate), The present invention relates to vinyl polymers composed of copolymers thereof; carboxymethyl cellulose, gellan gum, alginic acid, sulfated alginic acid, carrageenan, xanthan gum, chondroitin sulfate, heparin, hyaluronic acid, pectinic acid, gum arabic, agar, tragacanth and the like. These polymers can be copolymerized with other monomers within the range of maintaining water solubility. Among these anionic polymers, it is preferred to use acidic polysaccharides having excellent mechanical strength and high oxidation resistance, and it is further preferred to use alginic acid or sulfated alginic acid. The ratio of mannuronic acid to guluronic acid as constituent components of alginic acid is arbitrary, and alginic acid having a high ratio of mannuronic acid that produces a soft gel and alginic acid having a high ratio of guluronic acid that can produce a rigid gel can be used.
[0185] Sulfated polysaccharides into which sulfate groups are introduced are also suitable for use. Sulfate groups are strongly acidic cation exchange groups that can be exchanged with alkaline salts and neutral salts such as NaCl or CaCl2. The sulfate groups are introduced into the hydroxyl group in the polysaccharide structure, and are introduced by replacing the hydrogen of the hydroxyl group with -SO3H. The content of sulfate groups is preferably 0.5 to 5.0 mmol / g. When the sulfate group content is within the above range, the content of chelating functional groups increases and oxidation resistance also improves, so it is preferred.
[0186] In water-soluble chelated polymers, the above-mentioned anionic polymer and the chelating functional group with cationic functional group are bonded via ionic bonds. Chelating functional group refers to a functional group that can form a chelate with a ligand having multiple coordination sites and between polyvalent metal ions. As chelating functional group, it is suitable to use a chelating functional group comprising aminocarboxylic acid group or aminophosphonic acid group. As some examples of the chelating functional group comprising aminocarboxylic acid group, it is possible to enumerate: iminodiacetic acid group, nitrilotriacetic acid group, hydroxyethylglycine group, hydroxyethyliminodiacetic acid group, etc. As some examples of the chelating functional group comprising aminophosphonic acid, it is possible to enumerate: aminomethylphosphonic acid group, nitrilotri(methylphosphonic acid) group, etc.
[0187] The amount of the chelating functional group contained in the water-soluble chelating polymer is 0.2~6mmol / g, is preferably 0.5~5mmol / g. When the content of the chelating functional group is within the scope, heavy metal ions can be captured rapidly, and the heavy metal ion capture amount is also sufficient, so preferred. Here, the amount of the functional group of the water-soluble chelating polymer can be calculated by ultimate analysis.
[0188] The molecular weight of water-soluble chelating polymer is 30,000~1,000,000 in terms of weight average molecular weight, preferably 50,000~1,000,000. When the weight average molecular weight is in this range, sufficient mechanical strength can be ensured, and the viscosity during processing can also be adjusted to the scope without problems, so it is preferred. Here, the weight average molecular weight of water-soluble polymer can be calculated by gel permeation chromatography (GPC) measurement.
[0189] The water-soluble chelated polymer of the first scheme of the present invention has the structure that chelating functional group is bonded via ionic bond and anionic polymer.In order to form ionic bond with anionic polymer, need to have cationic functional group in the compound containing chelating functional group.As the example of cationic functional group, can enumerate: ammonium group, phosphonium group, sulfonium group etc.Here, can confirm that ionic bond is formed in the water-soluble polymer by observing the variation of the spectrogram that obtains based on infrared spectroscopic analysis such as FT-IR.
[0190] As an example, a chelate polymer production reaction formula is shown below when alginic acid is used as the anionic polymer and disodium iminodiacetic acid is used as the chelate group-containing compound.
[0191] [Chemical formula 4]
[0192]
[0193] Next, the manufacture method of the chelated polymer of the first scheme of the present invention is described. The water-soluble chelated polymer can be manufactured by the following method: an anionic polymer with carboxyl, sulfonic acid group and / or sulfate group is contacted with acid, after carboxyl, sulfonic acid group and / or sulfate group are converted into hydrogen ion type, it is contacted with a compound containing chelate functional group with amino group or a compound containing chelate functional group with phosphonium group or a compound containing chelate functional group with sulfonium group, and the chelate functional group is imported into the anionic polymer.
[0194] First, an anionic polymer having a carboxyl group, a sulfonic acid group and / or a sulfate group is contacted with an acid to convert the carboxyl group, the sulfonic acid group and / or the sulfate group into a hydrogen ion type. By converting the carboxyl group, the sulfonic acid group and / or the sulfate group into a hydrogen ion type, the amino group and the carboxyl group, the sulfonic acid group and / or the sulfate group in the chelate compound easily form a salt, and the chelate compound can be introduced into the anionic polymer via an ionic bond. The reaction of converting the carboxyl group, the sulfonic acid group and / or the sulfate group in the anionic polymer into a hydrogen ion type is carried out by dissolving the anionic polymer in water and adding an acid. The concentration of the anionic polymer aqueous solution is not particularly limited, but when the concentration is 0.1 to 5%, the operability is excellent and the productivity is also good, so it is preferred. Regarding the reaction temperature, it can be set to any temperature except the temperature range where water solidifies or boils, and specifically, it is preferably 5 to 90°C. The reaction time is also not particularly limited, and is preferably 5 to 120 minutes. The acid used is not particularly limited as long as it is a substance that can reduce the pH to below 2, and hydrochloric acid, sulfuric acid, nitric acid, trifluoroacetic acid, etc. can be used. The amount of acid added can be added so that the pH of the anionic polymer aqueous solution becomes below 2. After the reaction is completed, the hydrogen ion type anionic polymer is precipitated in a gel state, so the precipitated gel is recovered by filtration, etc., and washed with water and dried as needed to separate.
[0195] Furthermore, anionic polymers in which carboxyl groups, sulfonic acid groups and / or sulfate groups have been converted to hydrogen ion types in advance are already commercially available, and when such anionic polymers are used, the above-mentioned acid treatment step is not necessary.
[0196] Next, the anionic polymer converted into hydrogen ion type is contacted with a compound containing a chelating functional group having an amino group, and the chelating functional group is introduced into the anionic polymer. The compound containing a chelating functional group having an amino group refers to a compound having an amino group and a chelating functional group. As the chelating functional group, for example: aminocarboxylic acid group or aminophosphonic acid group etc. can be enumerated. Some specific examples of compounds containing chelating functional groups include: iminodiacetic acid, nitrilotriacetic acid, ethylenediaminetetraacetic acid, N,N-bis(2-hydroxyethyl)glycine, 1,2-diaminocyclohexanetetraacetic acid, diethylenetriaminepentaacetic acid, N-(2-hydroxyethyl)ethylenediaminetriacetic acid, bis(2-aminoethyl)ethylene glycoltetraacetic acid, bis(2-aminophenyl)ethylene glycoltetraacetic acid, N-(2-hydroxyethyl)iminodiacetic acid, tetrakis(2-pyridylmethyl)ethylenediamine, triethylenetetraaminehexaacetic acid, aminomethylphosphonic acid, aminoethylphosphonic acid, aminopropylphosphonic acid, nitrilotri(methylphosphonic acid) and their salts. These chelating compounds having amino groups can be used alone or in combination of two or more. The amount of the compound containing chelating functional groups having amino groups is used in the range of 0.1 to 1 mole relative to 1 mole of carboxyl, sulfonic acid and / or sulfate groups in the anionic polymer.
[0197] The obtained water-soluble chelate polymer can be stored in a state of maintaining an aqueous solution or in a state of being separated into a solid. As a method for separating into a solid, there can be cited: a method of separating by heating the aqueous solution to remove water; or a method of separating by dropping the aqueous solution into alcohol or acetone, which is a poor solvent for the chelate polymer, to precipitate the polymer.
[0198] When making the above-mentioned water-soluble chelated polymer be dissolved in water, even at low concentration, also can show high viscosity, therefore, be difficult to manufacture under high concentration condition.So, found that by making the anionic polymer of carboxyl, sulfonic acid group and / or sulfate group with hydrogen ion type be scattered in hydrophobic solvent, make the compound containing chelating functional group with amino be dissolved in water, and both are mixed and prepare water-in-oil emulsion, even under high concentration condition, also can manufacture this water-soluble chelated polymer, can improve productivity.
[0199] As described above, an anionic polymer having a hydrogen ion type carboxyl group, a sulfonic acid group and / or a sulfate group is obtained by contacting an anionic polymer having a carboxyl group, a sulfonic acid group and / or a sulfate group with an acid. The obtained hydrogen ion type anionic polymer has high hydrophilicity and is therefore insoluble in a hydrophobic solvent. When the two are contacted, a slurry in which the hydrogen ion type anionic polymer is dispersed in a hydrophobic solvent can be obtained. As usable hydrophobic solvents, solvents that are not mutually soluble in water can be cited. As some examples of hydrophobic solvents, higher alcohols such as butanol, hexanol, and octanol can be cited; vegetable oils such as olive oil, palm oil, rapeseed oil, soybean oil, and cottonseed oil; ester solvents such as propyl acetate, butyl acetate, and hexyl acetate; hydrocarbons such as hexane, decane, hexadecane, benzene, toluene, and xylene. The concentration of the slurry is not particularly limited, and the slurry can be prepared at a very high concentration of 10 to 30% by weight. In addition, in order to stabilize the water-in-oil emulsion described later, an emulsifier can be added as needed. Preferred emulsifiers include lipophilic emulsifiers having an HLB (hydrophilic-lipophilic balance) of 7 or less, and specific examples include sorbitan fatty acid esters such as sorbitan monooleate and sorbitan monostearate; sucrose fatty acid esters such as sucrose stearate and sucrose oleate, lecithin, etc. The amount of the emulsifier added is also not particularly limited, and 5 to 30% by weight can be added relative to the hydrophobic solvent.
[0200] The aqueous solution of the chelate functional group-containing compound having an amino group can be prepared by dissolving the chelate functional group-containing compound having an amino group in water. In order to improve productivity, the concentration of the aqueous solution is preferably as high as possible, preferably 10 to 30% by weight.
[0201] The slurry formed by dispersing the above-mentioned hydrogen ion type anionic polymer in a hydrophobic solvent is contacted and mixed with the aqueous solution of the above-mentioned amino group-containing chelating functional group compound to obtain an oil-in-water emulsion. There is no restriction on the contact and mixing method. The method of adding the chelating compound aqueous solution to the anionic polymer dispersion is easy to prepare a uniform water-soluble chelating polymer, so it is preferred. In order to stably maintain the oil-in-water emulsion, the temperature when the two are contacted and mixed is preferably a relatively low temperature of 0 to 15°C. The time required for contact and mixing is not particularly limited, and is preferably about 10 minutes to 5 hours. In addition, in order to maintain uniform contact and mixing, the stirring blade is preferably a large blade such as FULLZONE or MAXBLEND.
[0202] There is no particular limitation on the method for separating the water-soluble chelate polymer from the obtained water-in-oil emulsion. Examples thereof include: a method of removing water by heating the water-in-oil emulsion and then separating the water-soluble chelate polymer particles by filtration; or a method of separating the water-soluble chelate polymer particles by dropping the water-in-oil emulsion into a solvent (such as acetone or lower alcohol) mixed with water and a hydrophobic solvent.
[0203] The above-mentioned water-soluble chelating polymer can be made into an aqueous solution and can also be easily coated on a microparticle carrier with high polarity and large specific surface area. The coated microparticle carrier can quickly adsorb and remove trace heavy metal ions in organic solvents in a short period of time due to the synergistic effect of the chelating functional groups arranged near the surface and the large specific surface area. Therefore, it can be suitable for use in the purification of organic solvents for semiconductor manufacturing that requires high purity.
[0204] A water-soluble chelate polymer can be added to a solution containing heavy metal ions to capture the heavy metal ions with the chelate polymer.
[0205] Hereinafter, the second aspect of the present invention will be described in detail.
[0206] A second aspect of the present invention is a chelate polymer and a method for producing the same.
[0207] More specifically, the chelate polymer in the second embodiment of the present invention is represented by the chelate polymer (I) or the chelate polymer (II) described below.
[0208] The second embodiment of the present invention is a chelate polymer (I) having a structure represented by the following general formula (1) and containing 0.2 to 5 mmol / g of a chelate functional group.
[0209] PS-XA-CL(1)
[0210] (In the formula, PS represents an acidic polysaccharide or a basic polysaccharide. X represents a group represented by -O- or -N(R)-, R represents a hydrogen atom or a hydrocarbon group having 1 to 6 carbon atoms. A represents an organic group having 3 to 30 carbon atoms, and CL represents an organic group having 1 to 30 carbon atoms containing a chelating functional group.)
[0211] The chelate polymer (I) of the second embodiment of the present invention is represented by the above general formula (1), and is obtained by introducing a chelate functional group into an acidic polysaccharide or a basic polysaccharide via a covalent bond.
[0212] In the formula, PS represents acidic polysaccharide or alkaline polysaccharide. Acidic polysaccharide refers to polysaccharide containing functional groups showing acidity such as carboxyl or sulfate group, as these examples, can enumerate: carboxymethyl cellulose, gellan gum, alginic acid, sulfated alginic acid, carrageenan, xanthan gum, chondroitin sulfate, heparin, hyaluronic acid, pectic acid, gum arabic, agar, tragacanth or their salt. And then, can also be mixed with neutral polysaccharide or other water-soluble polymers in the scope of not significantly reducing chelating functional group content. In addition, as long as water or organic solvent have swelling property, then cross-linked structure can also be introduced. In these acidic polysaccharides, alginic acid, sulfated alginic acid or their salt are due to excellent oxidation resistance, mechanical strength is also higher, therefore preferably used. The ratio of mannuronic acid to guluronic acid as constituent components of alginic acid is arbitrary, and either alginic acid having a high mannuronic acid ratio which produces a soft gel or alginic acid having a high guluronic acid ratio which produces a rigid gel can be used.
[0213] On the other hand, basic polysaccharides refer to polysaccharides containing a functional group showing basicity such as an amino group, and examples of these include chitosan.
[0214] Sulfated polysaccharides into which sulfate groups are introduced are also suitable for use. Sulfate groups are strongly acidic cation exchange groups that can undergo ion exchange not only with alkaline salts but also with neutral salts such as NaCl or CaCl2. The sulfate groups are introduced into the site of the hydroxyl groups contained in the polysaccharide structure, and are introduced by replacing the hydrogen of the hydroxyl groups with -SO3H. The content of sulfate groups in the polysaccharide is preferably 0.5 to 5.0 mmol / g. When the sulfate group content is within the above range, the content of chelating functional groups increases and oxidation resistance also improves, so it is preferred.
[0215] X represents a group represented by -O- or -N(R)-, and R represents a hydrogen atom or a hydrocarbon group having 1 to 6 carbon atoms. Examples of the hydrocarbon group having 1 to 6 carbon atoms include methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, tert-butyl, isobutyl, n-pentyl, sec-pentyl, tert-pentyl, isopentyl, neopentyl, 3-pentyl, cyclopentyl, n-hexyl, isohexyl, sec-hexyl, tert-hexyl, neohexyl, 2-methylpentyl, 3-methylpentyl, 1,2-dimethylbutyl, 2,2-dimethylbutyl, 1-ethylbutyl, 2-ethylbutyl, and cyclohexyl.
[0216] The organic group CL containing the chelating functional group can contain the chelating functional group, and the carbon number is 1 to 30. In addition to carbon and hydrogen, it can also contain heteroatoms such as oxygen, nitrogen, phosphorus or sulfur. The chelating functional group refers to a ligand having multiple coordination sites and a functional group that can form a chelate with a polyvalent metal ion. As the chelating functional group, it is suitable to use a chelating functional group containing aminocarboxylic acid, a chelating functional group containing aminophosphonic acid or a chelating functional group containing polyamines. Some examples of chelating functional groups containing aminocarboxylic acids include iminodiacetyl, nitrilotriacetyl, N,N-bis(2-hydroxyethyl)glycine, hydroxyethyliminodiacetyl, ethylenediaminetriacetyl, ethylenediaminetetraacetyl, 1,2-bis(2-aminophenoxy)ethanetetraacetyl, 1,2-diaminocyclohexanetetraacetyl, diethylenetriaminepentaacetyl, (2-hydroxyethyl)ethylenediaminetriacetyl, bis(2-aminoethyl)ethyleneglycoltetraacetyl, triethylenetriaminehexaacetyl, etc. Some examples of chelating functional groups containing aminophosphonic acid include aminomethylphosphonic acid, nitrilotri(methylphosphonic acid), etc. Some examples of chelating functional groups containing polyamines include polyethyleneimine, polyamidoamine dendrimer, tetrakis(2-pyridylmethyl)ethylenediamine, etc. The organic group CL containing a chelate functional group may be the above-mentioned chelate functional group alone, or a hydrocarbon group such as methyl, ethyl, or phenyl, or an ester group such as acetate, an ether group such as ethyl ether, an amide group such as benzamide, or a sulfonate group such as toluenesulfonate may be bonded to the chelate functional group.
[0217] The amount of the chelate functional group contained in the chelate polymer (I) is 0.2 to 5 mmol / g, preferably 0.5 to 5 mmol / g. When the content of the chelate functional group is within this range, heavy metal ions can be captured quickly and the amount of heavy metal ions captured is sufficient, which is preferred.
[0218] The molecular weight of the chelate polymer (I) is preferably 10,000 to 1,000,000, more preferably 50,000 to 1,000,000 in terms of weight average molecular weight. The weight average molecular weight within this range is preferred because sufficient mechanical strength can be ensured and the viscosity during processing can be adjusted to a non-problematic range.
[0219] The organic group CL containing a chelating functional group is introduced into the acidic polysaccharide or the basic polysaccharide via -A- as a spacer group. A is an organic group having 3 to 30 carbon atoms, preferably a divalent hydrocarbon group such as propylene or butylene, phenylene, or a group formed by introducing a hydroxyl group into these hydrocarbon groups. Some examples of these spacer groups include: 2-hydroxypropylene, 2,2-bis[4-(hydroxypropoxy)phenyl]propane, 1,2-bis(2-hydroxypropoxy)ethyl, or 1,3-bis(2-hydroxypropoxy)benzene, etc. In addition, the organic group used in the second embodiment of the present invention refers to a group containing heteroatoms such as oxygen, nitrogen, phosphorus, or sulfur in addition to carbon and hydrogen.
[0220] Among the chelate polymers (I), a particularly preferred chelate polymer is a chelate polymer having a structure represented by the following general formula (2).
[0221] [Chemical formula 5]
[0222]
[0223] (In the formula, A and CL have the same meanings as above. M represents a hydrogen atom or an alkali metal ion, and n represents an integer of 10 to 1000.)
[0224] The chelate polymer (I) is obtained by introducing a chelate functional group into alginic acid or alginate having excellent oxidation resistance via a covalent bond, and can capture and remove heavy metal ions even under severe conditions.
[0225] Next, the manufacturing method (I) of chelated polymer (I) is described. Manufacturing method (I) is the following method: after reacting acidic polysaccharides and / or alkaline polysaccharides with epihalohydrins and / or polyfunctional epoxy compounds having 2 to 6 epoxy groups, reacting them with a compound having an amino group and a chelating functional group, and introducing the chelating functional group into the acidic polysaccharide or the alkaline polysaccharide via a covalent bond. The initial reaction is the reaction of the hydroxyl group of the acidic polysaccharide or the amino group of the alkaline polysaccharide with epihalohydrins and / or polyfunctional epoxy compounds having 2 to 6 epoxy groups. The reaction of the amino group of the alkaline polysaccharide with epihalohydrins and / or polyfunctional epoxy compounds having 2 to 6 epoxy groups does not require the addition of a base, but in the reaction of the hydroxyl group of the acidic polysaccharide with epihalohydrins and / or polyfunctional epoxy compounds having 2 to 6 epoxy groups, a base such as sodium hydroxide needs to be added. Regarding the amount of base added, it is added in the range of 0.5 to 2 moles relative to 1 mole of hydroxyl groups of the acidic polysaccharide. This reaction can also be carried out in a heterogeneous system using alcohol or a water / alcohol mixed solvent as a solvent, but in order to ensure the uniformity of the reaction, it is preferred to dissolve the acidic polysaccharide or the alkaline polysaccharide in water for the reaction. The concentration of the polysaccharide aqueous solution is not particularly limited, but when the concentration is 0.1 to 5%, the operability is excellent and the productivity is also good, so it is preferred. Regarding the reaction temperature, in order to inhibit the hydrolysis of the polysaccharide, it is preferably reacted at a low temperature, preferably 0 to 20°C. The reaction time is preferably set according to the reaction temperature, preferably 3 hours to 24 hours.
[0226] As some examples of epihalohydrins, epichlorohydrin, epibromohydrin, epiiodohydrin and mixtures thereof can be used. In addition, as some examples of polyfunctional epoxy compounds having 2 to 6 epoxy groups, bisphenol A diglycidyl ether, bisphenol F diglycidyl ether, resorcinol diglycidyl ether, ethylene glycol diglycidyl ether, glycerol triglycidyl ether, 1,3-bis(oxiran-2-ylmethoxy)-2,2-bis[(oxiran-2-ylmethoxy)methyl]propane, etc. can be cited.
[0227] Regarding the addition amount of epihalohydrin and / or a polyfunctional epoxy compound having 2 to 6 epoxy groups, it can be added in the range of 1 to 20 moles relative to 1 mole of monosaccharide units of the polysaccharide. When acidic polysaccharides or alkaline polysaccharides are reacted with epihalohydrin and / or a polyfunctional epoxy compound having 2 to 6 epoxy groups under such conditions, chloromethyl or epoxy groups are introduced into the polysaccharide. The polysaccharide introduced with chloromethyl or epoxy groups can be recovered by dropping the reaction solution into a poor solvent for polysaccharides such as alcohol or acetone to precipitate it, or it can be used for the next reaction after removing the unreacted epihalohydrin or polyfunctional epoxy compound by heating. By reacting the chloromethyl or epoxy group introduced into the polysaccharide with the amino group in the compound having an amino group and a chelating functional group, the chelating functional group is introduced into the polysaccharide via a covalent bond. In order to suppress the hydrolysis of the polysaccharide, this reaction is also preferably reacted under mild conditions, and the reaction temperature is preferably 40 to 80°C. The reaction time is preferably set according to the reaction temperature, preferably 1 to 8 hours. Regarding the addition amount of the compound having an amino group and a chelate functional group, it can be added in the range of 1 to 20 moles relative to 1 mole of the monosaccharide unit of the polysaccharide. As specific examples of compounds having an amino group and a chelate functional group, there can be mentioned: iminodiacetic acid, nitrilotriacetic acid, ethylenediaminetetraacetic acid, N,N-bis(2-hydroxyethyl)glycine, 1,2-diaminocyclohexanetetraacetic acid, diethylenetriaminepentaacetic acid, N-(2-hydroxyethyl)ethylenediaminetriacetic acid, bis(2-aminoethyl)ethylene glycoltetraacetic acid, bis(2-aminophenyl)ethylene glycoltetraacetic acid, N-(2-hydroxyethyl)iminodiacetic acid, tetrakis(2-pyridylmethyl)ethylenediamine, triethylenetetraaminehexaacetic acid, polyethyleneimine, aminomethylphosphonic acid, aminoethylphosphonic acid, aminopropylphosphonic acid, nitrilotri(methylphosphonic acid) and their salts. These chelate compounds having an amino group can be used alone or in combination of two or more.
[0228] Next, the chelate polymer (II) according to the second embodiment of the present invention is described. The chelate polymer (II) is represented by the following general formula (3).
[0229] [Chemical formula 6]
[0230]
[0231] (In the formula, PS and X have the same meanings as above. B represents a vinyl monomer residue containing a chelating functional group and having 4 to 30 carbon atoms, D represents a vinyl monomer residue containing no chelating functional group and having 4 to 30 carbon atoms, and l and m each independently represent an integer of 10 to 500.)
[0232] In the chelate polymer (II), the chelate functional group is introduced into the graft polymer chain and bonded to the acidic polysaccharide or the basic polysaccharide via a covalent bond. The chelate functional group may be the same functional group as the above-mentioned chelate polymer (I). As the vinyl monomer residue having a chelate functional group represented by B in the general formula (3), examples include: the reaction product of the epoxy group in the vinyl monomer residue having an epoxy group such as glycidyl methacrylate and the amino group in the compound having an amino group and a chelate functional group, etc. In addition, as the vinyl monomer residue having 4 to 30 carbon atoms that does not contain a chelate functional group represented by D in the general formula (3), not only the vinyl monomer residue in which the epoxy group in the vinyl monomer residue having an epoxy group such as glycidyl methacrylate remains as it is, or the vinyl monomer residue formed by hydrolysis and ring opening, but also the vinyl monomer residue without an epoxy group may be exemplified.
[0233] The amount of the chelate functional group contained in the chelate polymer (II) is 0.2 to 5 mmol / g, preferably 0.5 to 5 mmol / g. When the content of the chelate functional group is within this range, heavy metal ions can be captured quickly and the amount of heavy metal ions captured is sufficient, which is preferred.
[0234] The molecular weight of the chelate polymer (II) is preferably 10,000 to 1,000,000, more preferably 50,000 to 1,000,000 in terms of weight average molecular weight. The weight average molecular weight within this range is preferred because sufficient mechanical strength can be ensured and the viscosity during processing can be adjusted to a non-problematic range.
[0235] Among the chelate polymers (II) according to the second embodiment of the present invention, a particularly preferred chelate polymer is a chelate polymer having a structure represented by the following general formula (4).
[0236] [Chemical formula 7]
[0237]
[0238] (In the formula, B, D, M, l, m, and n have the same meanings as above.)
[0239] The chelating polymer (II) has a structure in which a polymer having a chelating functional group is grafted onto alginic acid or alginate having excellent oxidation resistance. Since the chelating functional group is introduced into the grafted chain with high molecular mobility, the adsorption rate of heavy metal ions is fast, and trace amounts of heavy metal ions can be quickly captured and removed.
[0240] The manufacturing method of chelating polymer (II) is as follows: after graft polymerization of vinyl monomer containing epoxy group on acidic polysaccharide and / or basic polysaccharide, it is reacted with a compound having amino group and chelating functional group, and the chelating functional group is introduced into acidic polysaccharide and / or basic polysaccharide via covalent bond. As the vinyl monomer containing epoxy group, glycidyl methacrylate, glycidyl acrylate, 1-vinyl-3,4-epoxycyclohexane, allyl glycidyl ether, vinyloxyethyl glycidyl ether or their mixture can be cited. In addition, in addition to the above-mentioned vinyl monomer containing epoxy group, vinyl monomer not containing epoxy group can also be mixed and used. Examples of the vinyl monomer not containing an epoxy group include: (meth)acrylates such as methyl (meth)acrylate and ethyl (meth)acrylate; vinyl carboxylic acids or salts thereof such as (meth)acrylic acid, itaconic acid, maleic acid, fumaric acid, and vinyl benzoate; vinyl sulfonic acids or salts thereof such as vinyl sulfonic acid and styrene sulfonic acid; aromatic vinyl compounds such as styrene, vinyl toluene, vinyl pyridine, and vinyl naphthalene; dienes such as butadiene, isoprene, and chloroprene; vinyl halides such as vinyl chloride, vinylidene chloride, vinyl fluoride, vinylidene fluoride, and tetrafluoroethylene; α-olefins such as ethylene, propylene, butene, and hexene; and the like.
[0241] The initiator used for graft polymerization preferably uses a redox catalyst system. Specifically, as the oxidant, hydrogen peroxide, benzoyl peroxide, cumene hydroperoxide, etc. can be used, and as the reducing agent, divalent iron salts, thiourea dioxide, sulfites, hydrazine, etc. can be used. As preferred initiators, cerium ammonium nitrate or ammonium ferrous sulfate / hydrogen peroxide / thiourea dioxide, etc. can be mentioned.
[0242] Graft polymerization is carried out by adding a vinyl monomer to an acidic polysaccharide or alkaline polysaccharide dissolved or dispersed in water or an organic solvent, and then adding an initiator. The concentration of the acidic polysaccharide or alkaline polysaccharide is not particularly limited. When the polysaccharide is dissolved, the preferred concentration is 0.1 to 5% by weight, and when the polysaccharide is dispersed, the preferred concentration is 3 to 20% by weight. If the above concentration is used, the stirring state can be continued even if polymerization is carried out, and uniform graft polymerization can be carried out, so it is preferred. The initial concentration of the vinyl monomer is preferably 3 to 30% by weight. If the above concentration is used, it is easy to control the polymerization heat, and then it is easy to control the polymerization, so it is preferred. The polymerization temperature or polymerization time is not particularly limited either, and polymerization at 0 to 50°C for 1 to 24 hours is sufficient.
[0243] After the polymerization is completed, the unreacted monomers are removed and purified to separate the grafted polymer. Examples of the separation method include: a method of separating the grafted polymer by removing the residual monomers or solvent by heating; or a method of adding the polymerization product dropwise to a solvent that dissolves the monomers but not the grafted polymer to precipitate the grafted polymer and recover the grafted polymer.
[0244] The obtained graft polymer is dissolved or dispersed in a solvent, and a compound having an amino group and a chelating functional group is added to react with the epoxy group in the graft polymer. The reaction conditions are the same as those for the reaction of the chloromethyl or epoxy group introduced into the polysaccharide with the amino group in the compound having an amino group and a chelating functional group in the method for producing the chelating polymer (I).
[0245] The obtained chelate polymer (II) can be stored in the state of a solution or dispersion dissolved in a solvent, or can be stored in the state of being separated into a solid. As a method for separating into a solid, there can be cited: a method of removing the solvent by heating the solution or dispersion after the reaction; or a method of separating by dropping the solution or dispersion into an alcohol or acetone which is a poor solvent for the chelate polymer (II) to precipitate the polymer, etc.
[0246] The chelate polymer (I) or (II) can be added to a solution containing heavy metal ions to capture the heavy metal ions with the chelate polymer.
[0247] Hereinafter, the third aspect of the present invention will be described in detail.
[0248] A third embodiment of the present invention is a lithium ion battery electrode mixture composition, a slurry for forming a lithium ion battery electrode mixture layer containing the composition, a lithium ion battery electrode produced from the composition, and a lithium ion battery having the electrode.
[0249] In the lithium ion battery electrode mixture composition of the third embodiment of the present invention, water-insoluble or organic solvent-insoluble polymer compound particles containing chelate groups are contained in the electrode mixture containing active materials, binders and optional conductive aids. The chelate group contained in the water-insoluble or organic solvent-insoluble polymer compound particles containing chelate groups refers to a ligand having multiple coordination sites and a functional group that can form a chelate with a polyvalent metal ion. As a chelate group, a chelate group containing an aminocarboxylic acid group or an aminophosphonic acid group is suitable for use. As some examples of chelate groups containing aminocarboxylic acid groups, there can be cited: iminodiacetic acid group, nitrilotriacetic acid group, hydroxyethylglycine group, hydroxyethyliminodiacetic acid group, etc. As some examples of chelate groups containing aminophosphonic acid, there can be cited: aminomethylphosphonic acid group, nitrilotri(methylphosphonic acid) group, etc. The amount of chelate groups contained in the chelate group-containing insoluble or organic solvent-insoluble polymer compound microparticles is 0.2 to 6 mmol / g, preferably 0.5 to 5 mmol / g. When the content of the chelate groups is within this range, heavy metal ions can be captured quickly and the amount of heavy metal ions captured is sufficient, so it is preferred.
[0250] In water-insoluble polymer particles, these chelating groups can be introduced into the polymer via ionic and / or covalent bonds. On the other hand, in organic solvent-insoluble polymer particles, the chelating groups can be introduced into the polymer via ionic and / or covalent bonds, or the organic solvent-insoluble polymer and the low molecular compound having the chelating groups can be physically mixed.
[0251] The water-insoluble polymer compound in the water-insoluble polymer compound microparticles containing chelating groups refers to: synthetic polymer compounds such as vinyl polymers, polyamides, polyurethanes, polyesters, or natural polymer compounds such as polysaccharides, proteins, nucleic acids, etc., which are cross-linked by covalent bonds or ionic bonds to become water-insoluble polymer compounds; or polymer compounds with high crystallinity and polymer chains being constrained at the crystalline site to become water-insoluble polymer compounds. Among the above-mentioned water-insoluble polymer compounds, it is preferred to use polymer compounds that show stability in both oxidation resistance and reduction resistance. Specifically, it is preferred to use fluoropolymers or polysaccharides having fluorine atoms on the main chain and / or side chain, and polysaccharides are particularly preferred. Polysaccharides refer to substances having a structure in which multiple monosaccharides are linked by glycosidic bonds. Examples of polysaccharides preferably used as the polymer compound in the water-insoluble polymer compound fine particles containing chelating groups include amylose, amylopectin, dextrin, glycogen, cellulose, carboxymethyl cellulose, hydroxyalkyl cellulose, acetyl cellulose, pectin, pullulan, curdlan, chitin, chitosan, agarose, xanthan gum, guar gum, gellan gum, locust bean gum, gum arabic, tamarind gum, psyllium seed gum, carrageenan, alginic acid, alginic acid derivatives, heparin, hyaluronic acid, chondroitin sulfate, xyloglucan, glucomannan, and the like.
[0252] In the water-insoluble polymer compound, the crosslinking density is not particularly limited, but is preferably a crosslinking density of such a degree that the polymer compound does not dissolve in the solvent but swells.
[0253] The particle size of the water-insoluble or organic solvent-insoluble polymer compound microparticles containing a chelate group is preferably 0.1 to 10 μm in terms of median diameter, and more preferably 0.5 to 5 μm. When the particle size is within this range, the water-insoluble or organic solvent-insoluble polymer compound microparticles containing a chelate group in the electrode mixture layer are well dispersed, and the specific surface area is also large, so the capture efficiency of manganese ions or nickel ions is improved.
[0254] The content of the water-insoluble or organic solvent-insoluble polymer compound particles containing chelate groups in the electrode mixture is preferably 1 to 10% by mass, and more preferably 2 to 5% by mass. When the content of the water-insoluble or organic solvent-insoluble polymer compound particles containing chelate groups is within the above range, manganese ions or nickel ions can be quantitatively captured, and the active material content in the electrode mixture will not be greatly reduced, so the capacity of the battery can be maintained, so it is preferred.
[0255] As the binder used in the lithium ion battery electrode mixture composition, when using water-insoluble polymer compound fine particles containing a chelate group, a water-soluble polymer is used.
[0256] As water-soluble polymers, there can be mentioned: polysaccharides, homopolymers or copolymers of (meth) acrylic acid, homopolymers or copolymers of maleic acid and their salts, preferably neutral polysaccharides or acidic polysaccharides. As specific examples, there can be mentioned: amylose, amylopectin, carboxymethyl cellulose, guar gum, gellan gum, xanthan gum, gum arabic, alginic acid, alginic acid derivatives, agarose, carrageenan, chondroitin sulfate. More preferably, alginic acid or alginic acid derivatives are preferably used because of their excellent oxidation resistance and reduction resistance. Alginic acid derivatives refer to compounds with various substituents introduced into alginic acid, and examples thereof include: alkali metal salts of alginic acid, alginic earth metal salts of alginic acid, ammonium alginate, alginic acid esters, sulfated alginic acid, etc.
[0257] As specific examples of alginic acid or alginic acid derivatives, alginic acid, alginic acid salts, and alginic acid esters represented by the following general formula (5) are preferably used.
[0258] [Chemical formula 8]
[0259]
[0260] (In the formula, m and n are independently an integer greater than 1, R1 may be the same or different, and each represents one selected from the group consisting of hydrogen, alkali metal, alkaline earth metal, quaternary ammonium and a group represented by -R3-OH, and R3 represents a divalent hydrocarbon group having 2 to 6 carbon atoms.)
[0261] Examples of the divalent hydrocarbon group having 2 to 6 carbon atoms for R3 include ethylene, ethylidene, vinylidene, trimethylene, methylethylene, 1-methylethylidene, propenylene, tetramethylene, methyltrimethylene, dimethylethylene, 1-ethylethylidene, ethylethylene, pentamethylene, methyltetramethylene, dimethyltrimethylene, methylethylethylene, hexamethylene, cyclohexylene, and cyclohexylidene.
[0262] Alginic acid refers to the case where all R1 in formula (5) are hydrogen, alginate refers to the case where at least a part of R1 in formula (5) is an alkali metal (e.g., lithium, sodium, potassium), an alkaline earth metal (e.g., magnesium, calcium) or a quaternary ammonium (e.g., ammonium, tetramethylammonium), and alginate refers to the case where at least a part of R1 in formula (5) is a group represented by -R3-OH (R3 is a divalent hydrocarbon group having 2 to 6 carbon atoms), and this alginate can be produced by reacting alginic acid and an epoxy compound.
[0263] The ratio of mannuronic acid to guluronic acid as constituent components of alginic acid is arbitrary, and either alginic acid having a high mannuronic acid ratio which produces a soft gel or alginic acid having a high guluronic acid ratio which produces a rigid gel can be used.
[0264] The molecular weight of the polysaccharide used as the binder is preferably 10,000 to 2,000,000 in terms of weight average molecular weight. When the weight average molecular weight is within the above range, mechanical properties are good and the slurry viscosity during electrode production is also an appropriate value, which is preferred.
[0265] Sulfated polysaccharides into which sulfate groups and / or alkali metal sulfate groups are introduced are also suitable for use. The sulfate groups are introduced into the hydroxyl groups contained in the polysaccharide structure by replacing the hydrogen of the hydroxyl groups with -SO3H.
[0266] The amount of sulfate groups and / or alkali metal sulfate salt groups introduced into the polysaccharide is preferably 0.5 to 6.0 mmol / g. When the amount of sulfate groups and / or alkali metal sulfate salt groups introduced is within the above range, oxidation resistance is improved, and while maintaining the binding force to the active material, the electrolyte affinity is also excellent, so it is preferred.
[0267] An example of the polysaccharide having a sulfate group and / or an alkali metal sulfate group is an alginic acid derivative having a structure represented by the following general formula (6).
[0268] [Chemical formula 9]
[0269]
[0270] (In the formula, m and n are independently an integer greater than 1, R1 may be the same or different and each represent one selected from the group consisting of hydrogen, alkali metal, alkaline earth metal, quaternary ammonium and a group represented by -R3-O-R2, R3 represents a divalent hydrocarbon group having 2 to 6 carbon atoms, R2 may be the same or different and each represent hydrogen or -SO3M (M is hydrogen or alkali metal), and at least one of R2 is -SO3M.)
[0271] In the above general formula (6), m and n are each independently an integer greater than 1, and are preferably selected so that the weight average molecular weight of the polysaccharide having a sulfate group and / or an alkali metal sulfate group represented by the above general formula (6) is 10,000 to 2,000,000, and m and n are each independently preferably 30 to 6000.
[0272] The method for producing polysaccharides having sulfate groups and / or alkali metal sulfate groups is not particularly limited, and they can be obtained, for example, by reacting polysaccharides with a sulfating agent in an aprotic polar solvent. The reaction can be carried out in a slurry system or in a homogeneous system.
[0273] As the solvent used for the reaction, an aprotic polar solvent is preferred, and specific examples thereof include dimethyl sulfoxide, formamide, dimethylformamide, dimethylacetamide, N-methyl-2-pyrrolidone (NMP), 1,3-dimethyl-2-imidazolidinone, acetonitrile, hexamethylphosphoric acid triamide, tetramethylurea, N,N'-dimethylpropyleneurea, tetrahydrofuran, dioxane, pyridine, bipyridine, and phenanthroline.
[0274] As the polysaccharide used, those with excellent solubility in aprotic polar solvents are preferred, and examples thereof include: amylose, amylopectin, dextrin, glycogen, cellulose, carboxymethyl cellulose, hydroxyalkyl cellulose, acetyl cellulose, pectin, pullulan, curdlan, chitin, chitosan, agarose, xanthan gum, guar gum, gellan gum, locust bean gum, gum arabic, tamarind gum, psyllium seed gum, carrageenan, alginic acid, alginate, alginate ester, heparin, hyaluronic acid, chondroitin sulfate, xyloglucan, glucomannan, etc., and preferred examples thereof include: amylose, amylopectin, carboxymethyl cellulose, guar gum, gellan gum, xanthan gum, gum arabic, alginic acid, alginate, alginate ester, agarose, carrageenan, and chondroitin sulfate. More preferably, alginic acid and alginate ester can be mentioned.
[0275] The sulfating agent used is a reagent that can react with a hydroxyl group to introduce a sulfate group. Specific examples include concentrated sulfuric acid, chlorosulfonic acid, sulfur trioxide pyridine complex, sulfur trioxide trimethylamine complex, sulfur trioxide dimethylformamide complex, sulfur trioxide dimethyl sulfoxide complex, sulfur trioxide dioxane complex, etc. Among these sulfating agents, it is preferred to use a reagent that reduces the molecular weight of polysaccharides less. As a preferred sulfating agent, sulfur trioxide complex can be mentioned, and as a particularly preferred sulfating agent, sulfur trioxide pyridine complex and sulfur trioxide dimethylformamide complex can be mentioned. The amount of these sulfating agents used is not particularly limited, and it is preferably used in a range of 1 to 5 times the mole of the monosaccharide as the constituent unit of the polysaccharide. When the sulfating agent is used in this range, the amount of sulfate group introduced is large, and the molecular weight reduction of the polysaccharide can be suppressed, and a high molecular weight substance can be obtained, so it is preferred.
[0276] Other reaction conditions can be set arbitrarily, preferably the reaction temperature is selected from the range of 0°C to 100°C, the reaction time is selected from the range of 30 minutes to 12 hours, and the concentration of the polysaccharide in the reaction is selected from the range of 0.1 to 50% by mass.
[0277] There is no particular limitation on the method for separating polysaccharides having sulfate groups and / or alkali metal sulfate groups from the reaction solution after the reaction is completed. The following methods may be used: heating to remove the solvent to separate the polysaccharides having sulfate groups and / or alkali metal sulfate groups; or adding the reaction solution dropwise to a poor solvent to precipitate the polysaccharides having sulfate groups and / or alkali metal sulfate groups and filtering and recovering them.
[0278] As a polysaccharide having a sulfate group and / or an alkali metal sulfate salt group, a polysaccharide in which the introduced sulfate group is a regenerated type (-SO3 H) can be obtained in the initial stage of production, but at least a part of the above-mentioned regenerated type can also be ion-exchanged into an alkali metal salt type (-SO3 M' (M' represents an alkali metal (for example, lithium, sodium, potassium)). The ion exchange from the above-mentioned regenerated type to the salt type is the same as that of a general ion exchanger, and the regenerated type binder can be ion-exchanged into a salt type binder by bringing the regenerated type binder into contact with an alkali metal ion-containing solution.
[0279] The organic solvent-insoluble polymer compound in the organic solvent-insoluble polymer compound microparticles containing a chelating group refers to a synthetic polymer compound such as vinyl polymer, polyamide, polyurethane, polyester, or a polymer compound insoluble in an organic solvent due to high polarity in a natural polymer compound such as polysaccharides, proteins, nucleic acids, etc.; or a polymer compound that is cross-linked by covalent bonds or ionic bonds, thereby becoming insoluble in an organic solvent; or a polymer compound that has high crystallinity and the polymer chain is constrained at the crystalline site and becomes insoluble in an organic solvent. Among the above-mentioned organic solvent-insoluble polymer compounds, it is preferred to use a polymer compound that shows stability in both oxidation resistance and reduction resistance. Specifically, it can be cited: polycarboxylic acids such as polyacrylic acid and acidic polysaccharides, or polyhydroxy compounds such as polyvinyl alcohol and neutral polysaccharides, etc., and acidic polysaccharides are particularly preferred. Polysaccharides refer to substances having a structure in which multiple monosaccharides are linked by glycosidic bonds. Examples of polysaccharides preferably used as the polymer compound in the organic solvent-insoluble polymer compound fine particles containing chelating groups include amylose, amylopectin, dextrin, glycogen, cellulose, carboxymethyl cellulose, hydroxyalkyl cellulose, acetyl cellulose, pectin, pullulan, curdlan, chitin, chitosan, agarose, xanthan gum, guar gum, gellan gum, locust bean gum, gum arabic, tamarind gum, psyllium seed gum, carrageenan, alginic acid, alginic acid derivatives, heparin, hyaluronic acid, chondroitin sulfate, xyloglucan, and glucomannan.
[0280] In addition, as an organic solvent in an organic solvent water-insoluble polymer compound, an amide solvent is preferably used. Specific examples of amide solvents include: formamide, dimethylformamide, diethylformamide, dimethylacetamide, N-methyl-2-pyrrolidone, 1,3-dimethyl-2-imidazolidinone, hexamethylphosphoric acid triamide, tetramethylurea, N,N'-dimethylpropyleneurea, etc. Among them, as a preferred organic solvent, from the perspective of excellent solubility of the adhesive and stability for the active material, dimethylformamide, dimethylacetamide, N-methyl-2-pyrrolidone, 1,3-dimethyl-2-imidazolidinone, and N-methyl-2-pyrrolidone is particularly preferred.
[0281] As the binder used in the lithium ion battery electrode mixture composition, in the case of using the organic solvent-insoluble polymer compound particles containing the chelating group, a fluorine resin is used. As a specific example of a fluorine resin, polyvinylidene fluoride, vinylidene fluoride-hexafluoropropylene copolymer, perfluoromethyl vinyl ether-tetrafluoroethylene copolymer, polytetrafluoroethylene, fluorine rubber, etc. can be cited. Among these fluorine resins, polyvinylidene fluoride and vinylidene fluoride-hexafluoropropylene copolymer are preferably used.
[0282] Furthermore, the binder may be mixed with polyvinyl alcohol, styrene-butadiene copolymer, polyimide, polyacrylic acid, polymethacrylic acid or a salt thereof within a range not departing from the object of the third aspect of the present invention.
[0283] The active material contained in the lithium ion battery electrode mixture composition of the third embodiment of the present invention refers to a substance responsible for the electrochemical oxidation-reduction reaction in the battery, and different substances are used in the positive electrode and the negative electrode.
[0284] Examples of positive electrode active materials include: Li X CoO2、Li X NiO2、Li X MnO2、Li X Mn2O4、LiNi X Co (1-X) O2、LiNi X Mn (2-X) O4、LiMn a Ni b Co c O2 (a + b + c = 1), LiFePO4 and other lithium composite oxides. Among them, preferred are composite oxides of at least one transition metal selected from transition metals such as Co, Ni, and Mn and lithium. Specific examples include: LiCoO2, LiNiO2, LiMnO2, LiMn2 O4, LiNi X Co (1-X) O2、LiNi X Mn (2-X) O4、LiMn a Ni b Co c O2 (a+b+c=1). These lithium composite oxides may be doped with a small amount of fluorine, boron, Al, Cr, Zr, Mo, Fe and other elements, and the surface of the lithium composite oxide particles may be treated with carbon, MgO, Al2O3, SiO2 and the like.
[0285] As the negative electrode active material, there is no particular limitation as long as lithium ions can be inserted and removed, and examples thereof include natural graphite, artificial graphite, graphite, mesophase carbon microbeads (MCMB), tin and / or tin alloys, tin oxides, silicon and / or silicon alloys, silicon oxides, etc. In addition, when the negative electrode active material is an alloy, the negative electrode active material may include a material alloyed with lithium. In addition, here, as a material alloyed with lithium, examples thereof include germanium, tin, lead, zinc, magnesium, sodium, aluminum, gallium, indium, and alloys thereof.
[0286] When these active materials are in the form of particles, the average particle size is not particularly limited, but is preferably 5 μm or more and 20 μm or less.
[0287] The conductive aid included in the lithium ion battery electrode mixture composition of the third embodiment of the present invention as needed is also not particularly limited, as long as it is an electronic conductive material that does not adversely affect the battery characteristics, it can be used. Specifically, it can be cited as: conductive carbon such as Ketjen black and acetylene black; carbon materials such as natural graphite, artificial graphite, carbon whiskers, carbon nanotubes, and carbon fiber powder; metal powders and metal fibers such as Cu, Fe, Ag, Ni, Pd, Au, Pt, In, and W; or conductive metal oxides such as indium oxide and tin oxide. The amount of these conductive aids is preferably 1 to 30% by mass relative to the above-mentioned active material.
[0288] When a water-soluble polymer is used as the binder, the slurry for forming the lithium ion battery electrode mixture layer of the third embodiment of the present invention comprises the above-mentioned water-insoluble polymer compound particles containing a chelate group, a binder, an active material, a conductive auxiliary agent as required, and water. The slurry may also contain a viscosity modifier such as carboxymethyl cellulose, or a pH modifier such as an acid or an alkali as required.
[0289] On the other hand, when a fluorine resin is used as the binder, the slurry for forming the lithium ion battery electrode mixture layer comprises the organic solvent-insoluble polymer compound particles containing the chelate group, the binder, the active material, the conductive auxiliary agent as required, and the organic solvent. The slurry may also contain a viscosity modifier such as carboxymethyl cellulose, or a pH modifier such as an acid or an alkali as required.
[0290] The solid content concentration of the slurry is not particularly limited, and is preferably 20 to 80% by mass in consideration of the viscosity of the slurry, the dispersibility of the solid content, the burden on the drying process, etc. In addition, the component ratio in the slurry is preferably active material: conductive auxiliary agent: binder: water-insoluble polymer compound particles containing chelate groups or organic solvent-insoluble polymer compound particles containing chelate groups = 70 to 98: 0 to 10: 1 to 10: 1 to 10.
[0291] The method for making the above-mentioned slurry is not particularly limited, and the following examples may be mentioned: a method for making a slurry by mixing, dispersing, and dissolving a binder, an active material, a conductive aid, and water-insoluble polymer compound particles containing a chelate group or organic solvent-insoluble polymer compound particles containing a chelate group together in water or an organic solvent; first, dissolving and dispersing the binder in water or an organic solvent, then adding the active material, the conductive aid, and water-insoluble polymer compound particles containing a chelate group or organic solvent-insoluble polymer compound particles containing a chelate group to a binder solution and mixing them, thereby making a slurry; or first, mixing the active material, the conductive aid, and water-insoluble polymer compound particles containing a chelate group or organic solvent-insoluble polymer compound particles containing a chelate group, then mixing with a binder solution, etc. In addition, the mixer used to make the slurry is not particularly limited, and a mortar, a roller mill, a ball mill, a spiral mill, a vibration mill, a homogenizer, a rotation-revolution mixer, etc. can be used.
[0292] The third embodiment of the present invention is an electrode for lithium-ion batteries, which comprises the electrode mixture composition. Such an electrode for lithium-ion batteries is composed of an electrode mixture layer and a current collector obtained by coating the above-mentioned slurry on the current collector and drying it. The thickness of the electrode mixture layer composed of active material, binder, conductive auxiliary agent, water-insoluble polymer compound particles containing chelate groups or organic solvent-insoluble polymer compound particles containing chelate groups is preferably 10 to 200 μm. In order to form an electrode mixture layer of this thickness on the current collector, the unit area weight of the electrode mixture layer is preferably set to 4 to 25 mg / cm 2 . In addition, there is no particular limitation on the method for manufacturing the electrode for lithium-ion batteries, and the slurry can be coated on the current collector and dried to manufacture. There is no limitation on the method for coating the slurry, and slit coating, die coating, roller coating, dip coating, scraper coating, knife coating, wire rod coating and the like can be used. There is no particular limitation on the drying method and conditions, and a common warm air circulation dryer, reduced pressure dryer, infrared dryer, or microwave heating dryer can be used. There is no limitation on the heating temperature, and heating and drying can be performed at 50 to 150°C. Furthermore, the porous structure can be made uniform by pressurizing or pressing the electrode during or after drying.
[0293] The current collector can be any conductive body as long as the surface in contact with the electrode mixture layer shows conductivity. Examples of conductive bodies formed by the following can be given: metals such as copper, gold, aluminum, titanium, nickel, stainless steel or their alloys; conductive metal oxides such as indium oxide or tin oxide; or conductive materials such as conductive carbon. The shape of the current collector is not particularly limited, and can be in the form of foil, film, sheet, mesh, metal plate mesh, punched metal, foam, etc. The thickness of the current collector is also not particularly limited, and is preferably about 1 to 100 μm.
[0294] The lithium ion battery of the third embodiment of the present invention has the above-mentioned lithium ion battery electrode. By using the above-mentioned lithium ion battery electrode, a high-performance lithium ion battery that achieves excellent charge and discharge characteristics and extended cycle life can be provided. Lithium ion batteries are generally composed of a positive electrode, a negative electrode, a separator, a non-aqueous electrolyte, etc. The positive electrode is formed by bonding the above-mentioned positive electrode active material together with the above-mentioned conductive auxiliary agent, the above-mentioned water-insoluble polymer compound particles containing a chelating group, or the organic solvent-insoluble polymer compound particles containing a chelating group on the positive electrode current collector through the above-mentioned adhesive, and has a structure in which a positive electrode mixture layer is formed on the current collector, and the positive electrode mixture layer is composed of a positive electrode active material, an adhesive, a conductive auxiliary agent, and water-insoluble polymer compound particles containing a chelating group or organic solvent-insoluble polymer compound particles containing a chelating group. The negative electrode also has a structure similar to that of the positive electrode, and is formed by bonding the negative electrode active material, the water-insoluble polymer compound particles containing chelate groups or the organic solvent-insoluble polymer compound particles containing chelate groups, and the conductive aid as required to the negative electrode current collector through the above-mentioned binder. In addition, the water-insoluble polymer compound particles containing chelate groups or the organic solvent-insoluble polymer compound particles containing chelate groups are contained in at least one of the positive electrode and the negative electrode.
[0295] The diaphragm generally uses a porous film such as polyolefin. Since it is responsible for the shutdown function when the battery thermal runaways, it is sandwiched between the positive electrode and the negative electrode. There is no particular restriction on the diaphragm, and a known diaphragm can be used. As specific examples of diaphragms, there can be cited: a polyethylene microporous film; a polypropylene microporous film; a laminated film of a polyethylene microporous film and a polypropylene microporous film; or a non-woven fabric composed of polyester fibers, aramid fibers, glass fibers, etc.; a diaphragm coated with ceramics, aramid, or PVDF on the surface of the above-mentioned microporous film.
[0296] The non-aqueous electrolyte is formed by dissolving electrolyte salts such as LiPF4 in organic solvents such as cyclic carbonates. The battery is filled with non-aqueous electrolyte, and lithium ions move from the positive electrode to the negative electrode during charging, and move from the negative electrode to the positive electrode during discharge. The non-aqueous electrolyte is not particularly limited, and known materials can be used. As electrolyte salts, CF3SO3Li, (CF3SO2)2NLi, (CF3SO2)2CLi, LiBF4, LiB(C6H8)4, LiPF4, LiClO4, LiAsF6, LiCl, LiBr, etc. can be used. As an organic solvent for dissolving the electrolyte salt, ethylene carbonate, vinylene carbonate, propylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, 1,2-dimethoxyethane, 1,2-diethoxyethane, γ-butyrolactone, tetrahydrofuran, 1,4-dioxane, anisole, diethyl ether, sulfolane, methyl sulfolane, acetonitrile, propionitrile, butyronitrile, valeronitrile, benzonitrile, dimethylformamide, dimethyl sulfoxide, trimethyl phosphate, triethyl phosphate, etc. can be used. The concentration of the electrolyte salt in the non-aqueous electrolyte can be selected in the range of 0.1 to 5 mol / L, preferably 0.5 to 3 mol / L.
[0297] Hereinafter, the fourth aspect of the present invention will be described in detail.
[0298] A fourth aspect of the present invention is a binder for lithium ion battery electrodes, a slurry for forming a lithium ion battery electrode mixture layer containing the binder, a lithium ion battery electrode containing the binder, and a lithium ion battery having the electrode.
[0299] A binder for lithium ion battery electrodes according to a fourth aspect of the present invention contains a chelate group-containing polymer compound.
[0300] The chelating group refers to a functional group that has a ligand with multiple coordination sites and can form a chelate with a polyvalent metal ion. As the chelating group, it is suitable to use an aminocarboxylic acid chelating group or an aminophosphonic acid chelating group, or a polyamine chelating group. Some examples of aminocarboxylic acid chelating functional groups include: iminodiacetic acid group, nitrilotriacetic acid group, N,N-bis(2-hydroxyethyl)glycine group, hydroxyethyliminodiacetic acid group, ethylenediaminetriacetic acid group, ethylenediaminetetraacetic acid group, 1,2-bis(2-aminophenoxy)ethanetetraacetic acid group, 1,2-diaminocyclohexanetetraacetic acid group, diethylenetriaminepentaacetic acid group, (2-hydroxyethyl)ethylenediaminetriacetic acid group, bis(2-aminoethyl)ethyleneglycoltetraacetic acid group, triethylenetriaminehexaacetic acid group, etc. Some examples of aminophosphonic acid chelating groups include: aminomethylphosphonic acid group, nitrilotri(methylphosphonic acid), etc. Some examples of polyamine chelating groups include polyethyleneimine, polyamidoamine dendrimers, tetrakis(2-pyridylmethyl)ethylenediamine, etc. When the chelating group includes carboxylic acid or phosphonic acid, their acidic functional groups are preferably in the form of monovalent salts such as alkali metal salts or ammonium salts, because they are more easily ion-exchanged with heavy metal ions than in the form of protons.
[0301] The amount of the chelate group contained in the chelate group-containing polymer compound is 0.2 to 6 mmol / g, preferably 0.5 to 5 mmol / g. When the content of the chelate group is within this range, heavy metal ions can be captured quickly and the amount of heavy metal ions captured is sufficient, which is preferred.
[0302] The polymer compound into which the chelate group is introduced is not particularly limited, and vinyl polymers, polyamides, polyesters, polyurethanes, polysaccharides, cellulose, etc. can be used. However, it is preferably water-soluble at the time of introduction of the chelate group, and therefore, the polymer compound is preferably hydrophilic.
[0303] The molecular weight of the chelate group-containing polymer compound is 10,000 to 1,000,000, preferably 50,000 to 1,000,000, as a weight average molecular weight. The weight average molecular weight within this range is preferred because sufficient mechanical strength can be ensured and the viscosity during electrode coating can be adjusted to a non-problematic range.
[0304] The chelate group-containing polymer compound in the fourth embodiment of the present invention refers to a compound in which the chelate group is bonded to the polymer compound via a covalent bond and / or an ionic bond. In the fourth embodiment of the present invention, the chelate group is preferably bonded to the polymer compound via an ionic bond.
[0305] When the chelate group is bonded to the polymer compound via a covalent bond, an example of its structure is represented by the following general formula (1).
[0306] PS-XA-CL(1)
[0307] (In the formula, PS represents an acidic polysaccharide or a basic polysaccharide. X represents a group represented by -O- or -N(R)-, R represents a hydrogen atom or a hydrocarbon group having 1 to 6 carbon atoms. A represents an organic group having 3 to 30 carbon atoms, and CL represents an organic group having 1 to 30 carbon atoms including a chelating group.)
[0308] The general formula (1) is the same as the general formula (1) in the second embodiment of the present invention described above.
[0309] PS in the general formula (1) represents an acidic polysaccharide or an alkaline polysaccharide. Acidic polysaccharides refer to polysaccharides containing functional groups showing acidity such as carboxyl or sulfate groups. Examples of these include carboxymethyl cellulose, gellan gum, alginic acid, sulfated alginic acid, carrageenan, xanthan gum, chondroitin sulfate, heparin, hyaluronic acid, pectic acid, gum arabic, agar, tragacanth gum or their salts. Furthermore, it is also possible to mix and use with neutral polysaccharides or other water-soluble polymers within the range of not significantly reducing the amount of chelating group introduction. Among these acidic polysaccharides, alginic acid, sulfated alginic acid or their salts are preferably used because of their excellent oxidation resistance and high mechanical strength. The ratio of mannuronic acid to guluronic acid as the constituent components of alginic acid is arbitrary, and alginic acid with a high ratio of mannuronic acid that generates soft gels and alginic acid with a high ratio of guluronic acid that can obtain rigid gels can be used. On the other hand, basic polysaccharides refer to polysaccharides containing a functional group showing basicity such as an amino group, and examples of these include chitosan.
[0310] In addition, sulfated polysaccharides into which sulfate groups are introduced into the above-mentioned polysaccharides are also suitable for use in the fourth embodiment of the present invention. Sulfate groups are strongly acidic cation exchange groups that can be ion exchanged not only with alkaline salts but also with neutral salts such as NaCl or CaCl2. The introduction position of the sulfate groups is the site of the hydroxyl groups contained in the polysaccharide structure, and the introduction is carried out by replacing the hydrogen of the hydroxyl groups with -SO3H. The amount of sulfate groups introduced into the polysaccharides is preferably 0.5 to 5.0 mmol / g. When the amount of sulfate groups introduced is within the above range, the oxidation resistance can be improved while maintaining the amount of chelating group introduced, so it is preferred.
[0311] In the general formula (1), X represents a group represented by -O- or -N(R)-, and R represents a hydrogen atom or a hydrocarbon group having 1 to 6 carbon atoms. Examples of the hydrocarbon group having 1 to 6 carbon atoms include methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, tert-butyl, isobutyl, n-pentyl, sec-pentyl, tert-pentyl, isopentyl, neopentyl, 3-pentyl, cyclopentyl, n-hexyl, isohexyl, sec-hexyl, tert-hexyl, neohexyl, 2-methylpentyl, 3-methylpentyl, 1,2-dimethylbutyl, 2,2-dimethylbutyl, 1-ethylbutyl, 2-ethylbutyl, and cyclohexyl.
[0312] A in the general formula (1) is an organic group having 3 to 30 carbon atoms, preferably a divalent hydrocarbon group such as propylene, butylene, or phenylene, or a group formed by introducing a hydroxyl group into these hydrocarbon groups. Some examples of these spacer groups include 2-hydroxypropylene, 2,2-bis[4-(hydroxypropoxy)phenyl]propane, 1,2-bis(2-hydroxypropoxy)ethyl, or 1,3-bis(2-hydroxypropoxy)benzene. In addition, the organic group used in the fourth embodiment of the present invention refers to a group containing heteroatoms such as oxygen, nitrogen, phosphorus, or sulfur in addition to carbon and hydrogen.
[0313] CL in the general formula (1) only needs to contain a chelate group, has 1 to 30 carbon atoms, and may contain heteroatoms such as oxygen, nitrogen, phosphorus, or sulfur in addition to carbon and hydrogen. CL may be the above-mentioned chelate group alone, or may be bonded to a chelate group with a hydrocarbon group such as methyl, ethyl, or phenyl, an ester group such as acetate, an ether group such as ether, an amide group such as benzamide, a sulfonate group such as toluenesulfonate, or the like.
[0314] When the chelate group is bonded to the polymer compound via a covalent bond, a polymer compound having a structure represented by the following general formula (3) in which the chelate group is introduced into the graft chain can also be suitably used in the fourth aspect of the present invention.
[0315] [Chemical formula 10]
[0316]
[0317] (In the formula, PS and X have the same meanings as PS and X in the above general formula (1). B represents a vinyl monomer residue containing a chelating group and having 4 to 30 carbon atoms, D represents a vinyl monomer residue not containing a chelating group and having 4 to 30 carbon atoms, and l and m each independently represent an integer of 10 to 500.)
[0318] The general formula (3) is the same as the general formula (3) in the second embodiment of the present invention described above.
[0319] In the above general formula (3), the chelate group is introduced into the grafted polymer chain and is bonded to the acidic polysaccharide or the basic polysaccharide via a covalent bond. The chelate group may be the same group as the chelate group of the chelate group-containing polymer compound of the above general formula (1). As the vinyl monomer residue having a chelate functional group represented by B in the general formula (3), examples include: the reaction product of the epoxy group in the vinyl monomer residue having an epoxy group such as glycidyl methacrylate and the amino group in the compound having an amino group and a chelate functional group, etc. In addition, as the vinyl monomer residue having 4 to 30 carbon atoms and not containing a chelate group represented by D in the general formula (3), not only the vinyl monomer residue in which the epoxy group in the vinyl monomer residue having an epoxy group such as glycidyl methacrylate remains as it is, or the vinyl monomer residue formed by hydrolysis and ring opening, but also the vinyl monomer residue not having an epoxy group may be exemplified.
[0320] Whether the chelate group is bonded to the polymer compound via a covalent bond can be confirmed by, for example, measuring the increase in weight after the chelate group is introduced compared to that before the introduction.
[0321] On the other hand, the chelate group is bonded to the polymer compound via an ionic bond, and examples thereof include a structure in which a polymer compound having an anionic functional group is bonded to a chelate group-containing compound having a cationic functional group via an ionic bond. Examples of the anionic functional group include a carboxyl group, a sulfonic acid group, a phosphoric acid group, a phenolic hydroxyl group, and the like. Specific examples of the polymer compound having an anionic functional group include poly(acrylic acid), poly(methacrylic acid), poly(itaconic acid), poly(maleic acid), ethylene-maleic acid copolymer, isobutylene-maleic acid copolymer, methyl vinyl ether-maleic acid copolymer, styrene-maleic acid copolymer, poly(fumaric acid), poly(vinyl sulfonic acid), poly(styrene sulfonic acid), poly(2-sulfoethyl methacrylate), poly(2-sulfoethyl acrylate), poly(3-sulfopropyl methacrylate), poly(3-sulfopropyl acrylate), poly(4-sulfobutyl methacrylate), poly(4-sulfobutyl acrylate), poly(2-acrylamide-2-methylpropanesulfonic acid), poly(2-methacrylamide-2-methylpropanesulfonic acid), and vinyl polymers composed of these copolymers; and acidic polysaccharides such as carboxymethyl cellulose, gellan gum, alginic acid, sulfated alginic acid, carrageenan, xanthan gum, chondroitin sulfate, heparin, hyaluronic acid, pectic acid, gum arabic, agar, and tragacanth. These polymers can be copolymerized with other monomers within the range of oxidation resistance or reduction resistance. Among these polymer compounds, as a positive electrode binder, it is preferred to use an acidic polysaccharide with high oxidation resistance, and it is further preferred to use alginic acid or sulfated alginic acid. On the other hand, as a negative electrode binder, it is preferred to use poly (acrylic acid), poly (styrene sulfonic acid) or their copolymers, alginic acid or sulfated alginic acid with excellent reduction resistance.
[0322] On the other hand, as a compound containing a chelate group having a cationic functional group, there can be mentioned: a compound containing a chelate group including an ammonium group, a phosphonium group, a sulfonium group, etc. As a specific compound, there can be mentioned: iminodiacetic acid, nitrilotriacetic acid, ethylenediaminetetraacetic acid, N,N-bis(2-hydroxyethyl)glycine, 1,2-diaminocyclohexanetetraacetic acid, diethylenetriaminepentaacetic acid, N-(2-hydroxyethyl)ethylenediaminetriacetic acid, bis(2-aminoethyl)ethylene glycoltetraacetic acid, bis(2-aminophenyl)ethylene glycoltetraacetic acid, N-(2-hydroxyethyl)iminodiacetic acid, tetrakis(2-pyridylmethyl)ethylenediamine, triethylenetetraaminehexaacetic acid, aminomethylphosphonic acid, aminoethylphosphonic acid, aminopropylphosphonic acid, nitrilotri(methylphosphonic acid) and their salts. The acetic acid group or phosphonic acid group in the above-mentioned compound is preferably in the form of a monovalent salt such as an alkali metal salt or an ammonium salt, because it is easier to exchange ions with heavy metal ions than in the form of a proton.
[0323] The bonding of the chelate group to the polymer compound via an ionic bond can be confirmed by, for example, FT-IR measurement.
[0324] Lithium ion battery electrode adhesive can be composed only of a polymer compound containing a chelating group, and in the case of including other adhesive components, the content of the polymer compound containing a chelating group is preferably more than 10% by mass. As other adhesives, if it is an adhesive for positive electrode, fluorine resins such as polyvinylidene fluoride, vinylidene fluoride-hexafluoropropylene copolymer, perfluoromethyl vinyl ether-tetrafluoroethylene copolymer, polytetrafluoroethylene, and fluororubber can be used, if it is an adhesive for negative electrode, fluorine resins such as polyvinylidene fluoride, vinylidene fluoride-hexafluoropropylene copolymer, perfluoromethyl vinyl ether-tetrafluoroethylene copolymer, polytetrafluoroethylene, and fluororubber or hydrocarbon elastomers such as styrene-butadiene copolymer, ethylene-propylene copolymer, or polyimide can be used.
[0325] The amount of the binder comprising the chelate group-containing polymer compound is preferably 1 to 20% by mass, more preferably 3 to 10% by mass, based on the total amount of the active material, the binder, and the conductive additive.
[0326] Since the binder is flexible, it can follow the volume change of the electrode during charge and discharge, and can prevent the cracking of the electrode caused by the volume change, or the peeling and falling of the active material or the destruction of the conductive path caused by the volume change. Furthermore, the binder of the fourth embodiment of the present invention has excellent affinity with the electrolyte, so it has excellent performance as a binder for lithium ion battery electrodes, for example, it also has excellent ion conductivity; and it has excellent oxidation resistance or reduction resistance, which can ensure the stability of the electrode.
[0327] Furthermore, a chelate group is introduced into the binder, which captures manganese ions dissolved from the positive electrode active material near the positive electrode and / or negative electrode, inhibiting precipitation and accumulation on the negative electrode active material, thereby achieving excellent charge and discharge characteristics and extended cycle life.
[0328] In the fourth embodiment of the present invention, the positive electrode active material is not particularly limited as long as it can insert and / or release lithium ions, and examples thereof include transition metal oxides such as CuO, Cu2O, MnO2, MoO3, V2O5, CrO3, Fe2O3, Ni2O3, and CoO3; or Li X CoO2、Li X NiO2、Li X MnO2、Li X Mn2O4、LiNi X Co (1-X) O2、LiNi a Co b A l c O2(a+b+c=1), LiNi X Mn (2-X) O4、LiMn a Ni b Co c O2(a+b+c=1), LiFePO4, LiMn X Fe (1-X) Among them, preferred are composite oxides of at least one transition metal selected from transition metals such as Co, Ni, and Mn and lithium, and specific examples thereof include: LiCoO2, LiNiO2, LiMnO2, LiMn2 O4, LiNi X Co (1-X) O2、LiNi a Co b Al c O2(a+b+c=1), LiNi X Mn (2-X) O4、LiMn a Ni b Co c O2(a+b+c=1), LiMn X Fe (1-X) These lithium composite oxides can be doped with a small amount of fluorine, boron, Al, Cr, Zr, Mo, Fe and other elements, and the surface of the lithium composite oxide particles can also be treated with carbon, MgO, Al2O3, SiO2 and the like.
[0329] In the fourth embodiment of the present invention, the negative electrode active material is not particularly limited as long as it can be inserted into and / or separated from lithium ions, and examples thereof include: lithium metal, natural graphite, artificial graphite, graphite, mesophase carbon microbeads (MCMB), tin and / or tin alloys, tin oxides, silicon and / or silicon alloys, silicon oxides, etc. In addition, when the negative electrode active material is an alloy, the negative electrode active material may contain a material alloyed with lithium. In addition, here, as a material alloyed with lithium, examples thereof include: germanium, tin, lead, zinc, magnesium, sodium, aluminum, gallium, indium, and alloys thereof.
[0330] When these active materials are in the form of particles, the average particle size is not particularly limited, but is preferably 5 μm or more and 20 μm or less.
[0331] The blending amount of these active materials is preferably 70 to 98% by mass based on the total amount of the active material, the binder, and the conductive auxiliary agent.
[0332] There are no particular restrictions on the conductive aid contained in the electrode, and any electronic conductive material that does not adversely affect the battery characteristics can be used. Specifically, conductive carbons such as Ketjen black and acetylene black; carbon materials such as natural graphite, artificial graphite, carbon whiskers, carbon nanotubes, and carbon fiber powders; metal powders and metal fibers such as Cu, Fe, Ag, Ni, Pd, Au, Pt, In, and W; or conductive metal oxides such as indium oxide and tin oxide. The amount of these conductive aids is preferably 1 to 30% by mass relative to the above-mentioned active material.
[0333] Hereinafter, the slurry for forming a lithium ion battery electrode mixture layer according to the fourth aspect of the present invention will be described in detail.
[0334] The slurry for forming the lithium ion battery electrode mixture layer of the fourth embodiment of the present invention comprises the above-mentioned binder, active material, conductive aid and water. The slurry may also contain a viscosity modifier such as carboxymethyl cellulose, or a pH modifier such as an acid or alkali as needed. The solid content concentration of the above-mentioned slurry is not particularly limited, and is preferably 20 to 80% by mass in consideration of the viscosity of the slurry, the dispersibility of the solid content, the burden on the drying process, etc. In addition, the ratio of the solid content in the above-mentioned slurry is preferably a positive electrode active material: conductive aid: binder = 70 to 98: 1 to 30: 1 to 20 in terms of mass ratio. The method for making the above-mentioned slurry is also not particularly limited, and can include: a method for making a slurry by mixing, dispersing, and dissolving the binder, active material, and conductive aid together in water; first, dissolving the binder in water, then adding the active material and conductive aid to the binder aqueous solution and mixing, thereby making a slurry; or first, mixing the active material and the conductive aid, then, mixing with the binder aqueous solution, etc. The mixer used for preparing the slurry is not particularly limited, and a mortar, a roll mill, a ball mill, a screw mill, a vibration mill, a homogenizer, a planetary mixer, or the like can be used.
[0335] Hereinafter, the lithium ion battery electrode according to the fourth aspect of the present invention will be described in detail.
[0336] The fourth embodiment of the present invention is an electrode for a lithium ion battery comprising the above-mentioned binder. The electrode for a lithium ion battery is composed of an electrode mixture layer obtained by coating the above-mentioned slurry on a current collector and drying it, and a current collector. The thickness of the electrode mixture layer composed of an active material, a binder, and a conductive additive is preferably 10 to 200 μm. In order to form an electrode mixture layer of this thickness on the current collector, the unit area weight of the electrode mixture layer is preferably set to 4 to 25 mg / cm 2 .
[0337] The above-mentioned current collector can be any conductive body as long as the surface in contact with the electrode mixture layer shows conductivity, and examples thereof include: a conductive body formed by: metals such as copper, gold, aluminum, titanium, nickel, stainless steel or their alloys; conductive metal oxides such as indium oxide or tin oxide; or conductive materials such as conductive carbon. The shape of the current collector is not particularly limited, and can be in the form of foil, film, sheet, mesh, metal plate mesh, punched metal, foam, etc. The thickness of the current collector is also not particularly limited, and is preferably about 1 to 100 μm.
[0338] There is no particular restriction on the method for manufacturing the electrode for lithium-ion batteries, and the slurry can be coated on the current collector and dried to manufacture. There is no restriction on the coating method of the slurry, and slit coating, die coating, roller coating, dip coating, scraping, knife coating, wire rod coating and the like can be used. There is no particular restriction on the drying method and conditions, and a common warm air circulation dryer, reduced pressure dryer, infrared dryer, or microwave heating dryer can be used. There is no restriction on the heating temperature, and it can be heated and dried at 50 to 150°C. Furthermore, the porous structure can also be made uniform by pressurizing and pressing the electrode during or after drying.
[0339] Hereinafter, a lithium ion battery according to a fourth aspect of the present invention will be described in detail.
[0340] The lithium ion battery of the fourth embodiment of the present invention is characterized by having the above-mentioned lithium ion battery electrode. Here, as lithium ion batteries, lithium ion primary batteries and lithium ion secondary batteries can be exemplified. By using the above-mentioned lithium ion battery electrode, a high-performance lithium ion battery with excellent charge and discharge characteristics and extended life can be provided.
[0341] Lithium-ion batteries are generally composed of a positive electrode, a negative electrode, a separator, a non-aqueous electrolyte, etc., and the representative shapes of single cells are cylindrical, square, laminated, and coin-shaped. The positive electrode is formed by bonding the above-mentioned positive electrode active material and the above-mentioned conductive aid together on the positive electrode current collector through an adhesive, and has a structure in which a positive electrode mixture layer composed of a positive electrode active material, an adhesive, and a conductive aid is formed on the current collector. The negative electrode also has a structure similar to that of the positive electrode, and is formed by bonding the following negative electrode active material and the above-mentioned conductive aid to the negative electrode current collector through an adhesive. The separator generally uses a porous film such as polyolefin, and is sandwiched between the positive and negative electrodes because it is responsible for the shutdown function when the battery thermally runs away. The non-aqueous electrolyte is formed by dissolving electrolyte salts such as LiPF4 in organic solvents such as cyclic carbonates. The battery is filled with non-aqueous electrolyte. In a primary battery, lithium ions move from the negative electrode to the positive electrode during discharge. In a secondary battery, lithium ions move from the positive electrode to the negative electrode during charge, and from the negative electrode to the positive electrode during discharge.
[0342] The non-aqueous electrolyte is not particularly limited, and known materials can be used. The non-aqueous electrolyte is formed by dissolving an electrolyte salt in an organic solvent. Examples of the electrolyte salt include CF3SO3Li, (CF3SO2)2NLi, (CF3SO2)3CLi, LiBF4, LiB(C6H5)4, LiPF6, LiClO4, LiAsF6, LiCl, LiBr, etc. As organic solvents for dissolving the electrolyte salt, examples include ethylene carbonate, vinylene carbonate, propylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, 1,2-dimethoxyethane, 1,2-diethoxyethane, γ-butyrolactone, tetrahydrofuran, 1,4-dioxane, anisole, diethyl ether, cyclopentane, methylcyclopentane, acetonitrile, propionitrile, butyronitrile, valeronitrile, benzonitrile, dimethylformamide, dimethyl sulfoxide, trimethyl phosphate, triethyl phosphate, etc. The concentration of the electrolyte salt in the non-aqueous electrolyte solution can be selected within the range of 0.1 to 5 mol / L, preferably 0.5 to 3 mol / L.
[0343] The separator is not particularly limited, and a known separator can be used. Examples of separators include: a polyethylene microporous membrane; a polypropylene microporous membrane; a laminated membrane of a polyethylene microporous membrane and a polypropylene microporous membrane; or a nonwoven fabric composed of polyester fiber, aramid fiber, glass fiber, etc.
[0344] Hereinafter, the fifth aspect of the present invention will be described in detail.
[0345] A fifth embodiment of the present invention is a composition, a binder for lithium ion battery electrodes comprising the composition, a slurry for forming a lithium ion battery electrode mixture layer comprising the composition, an electrode for a lithium ion battery comprising the composition, and a lithium ion battery having the electrode.
[0346] The composition of the fifth embodiment of the present invention is a physical mixture of a polymer compound and a chelating group-containing low-molecular compound.
[0347] The low molecular compound containing chelate group of the fifth scheme of the present invention has chelate group. Here, chelate group refers to a ligand having multiple coordination sites and a functional group that can form a chelate with a polyvalent metal ion. As a chelate group, it is suitable to use a chelate group of aminocarboxylic acid system or a chelate group of aminophosphonic acid system, and a chelate group of polyamine system. As some examples of aminocarboxylic acid chelate functional groups, it can be cited: iminodiacetic acid group, nitrilotriacetic acid group, N, N-bis (2-hydroxyethyl) glycine group, hydroxyethyliminodiacetic acid group, ethylenediaminetriacetic acid group, ethylenediaminetetraacetic acid group, 1,2-bis (2-aminophenoxy) ethanetetraacetic acid group, 1,2-diaminocyclohexanetetraacetic acid group, diethylenetriaminepentaacetic acid group, (2-hydroxyethyl) ethylenediaminetriacetic acid group, bis (2-aminoethyl) ethylene glycoltetraacetic acid group, triethylenetriaminehexaacetic acid group, etc. Some examples of aminophosphonic acid chelating groups include aminomethylphosphonic acid, nitrilotri(methylphosphonic acid), etc. Some examples of polyamine chelating groups include polyethyleneimine, polyamidoamine dendrimer, tetrakis(2-pyridylmethyl)ethylenediamine, etc. In the case where the chelating group includes carboxylic acid or phosphonic acid, their acidic functional groups are preferably in the form of monovalent salts such as alkali metal salts or ammonium salts, because they are easier to exchange ions with heavy metal ions than in the form of protons.
[0348] The chelate group-containing low-molecular compound according to the fifth embodiment of the present invention is preferably a water-soluble compound.
[0349] The molecular weight of the chelate group-containing low-molecular compound according to the fifth aspect of the present invention is preferably 10,000 or less, and more preferably 1,000 or less.
[0350] The low molecular weight compound containing chelate group of the fifth scheme of the present invention has no other restrictions as long as it has the above-mentioned chelate group. In addition, as the specific example of the low molecular weight compound containing chelate group of the fifth scheme of the present invention, it can be enumerated: formic acid, citric acid, porphyrin, polyethylene imine, iminodiacetic acid, nitrilotriacetic acid, ethylenediaminetetraacetic acid, N,N-bis(2-hydroxyethyl)glycine, 1,2-diaminocyclohexanetetraacetic acid, diethylenetriaminepentaacetic acid, N-(2-hydroxyethyl)ethylenediaminetriacetic acid, bis(2-aminoethyl)ethylene glycoltetraacetic acid, bis(2-aminophenyl)ethylene glycoltetraacetic acid, N-(2-hydroxyethyl)iminodiacetic acid, tetrakis(2-pyridylmethyl)ethylenediamine, triethylenetetraaminehexaacetic acid, aminomethylphosphonic acid, aminoethylphosphonic acid, aminopropylphosphonic acid, nitrilotri(methylphosphonic acid) and their salts.
[0351] The polymer compound of the fifth embodiment of the present invention is not particularly limited, but preferably has good affinity with the low molecular weight compound containing a chelate group, so it is preferably hydrophilic or water-soluble. In addition, the molecular weight of the polymer compound used in the fifth embodiment of the present invention is not particularly limited, and is 10,000 to 1,000,000 in terms of weight average molecular weight, preferably 50,000 to 1,000,000. When the weight average molecular weight is within this range, sufficient mechanical strength can be ensured, and the viscosity during electrode coating can be adjusted to a range without problems, so it is preferred. Specific examples of the polymer compound used in the fifth embodiment of the present invention include: poly(acrylic acid), poly(methacrylic acid), poly(itaconic acid), poly(maleic acid), ethylene-maleic acid copolymer, isobutylene-maleic acid copolymer, methyl vinyl ether-maleic acid copolymer, styrene-maleic acid copolymer, poly(fumaric acid), poly(vinyl sulfonic acid), poly(styrene sulfonic acid), poly(2-sulfoethyl methacrylate), poly(2-sulfoethyl acrylate), poly(3-sulfopropyl methacrylate ), poly(3-sulfopropyl acrylate), poly(4-sulfobutyl methacrylate), poly(4-sulfobutyl acrylate), poly(2-acrylamide-2-methylpropane sulfonic acid), poly(2-methacrylamide-2-methylpropane sulfonic acid) and vinyl polymers composed of these copolymers; acidic polysaccharides such as carboxymethyl cellulose, gellan gum, alginic acid, sulfated alginic acid, carrageenan, xanthan gum, chondroitin sulfate, heparin, hyaluronic acid, pectinic acid, gum arabic, agar, tragacanth gum and their alkali metal salts.
[0352] The “physical mixture of the polymer compound and the chelate group-containing low-molecular compound” in the composition of the fifth embodiment of the present invention means that no chemical bond such as a covalent bond or an ionic bond is generated between the polymer compound and the chelate group-containing low-molecular compound.
[0353] The blending ratio of the polymer compound and the chelate group-containing low molecular compound used in the fifth embodiment of the present invention is not particularly limited, but is preferably polymer compound: chelate group-containing low molecular compound = 100:30 to 500 in terms of weight ratio.
[0354] The physical mixing method of the chelate group-containing compound and the polymer compound is not particularly limited, and can be: a method of mixing the two in powder form; a method of dissolving the two in a solvent such as water and mixing them uniformly, removing the solvent to obtain a powder, etc.; or a method of dissolving the two in a solvent such as water and mixing them uniformly, and directly using the two.
[0355] In the composition of the fifth scheme of the present invention, the polymer compound can be one or more than two. In the case where another polymer compound (hereinafter referred to as "the second polymer compound") is included in addition to the above-mentioned polymer compound, it is preferred that the content of the above-mentioned polymer compound is 10% by mass or more, that is, the second polymer compound is 90% by mass or less. As the second polymer compound, if used for the positive electrode, fluorine resins such as polyvinylidene fluoride, vinylidene fluoride-hexafluoropropylene copolymer, perfluoromethyl vinyl ether-tetrafluoroethylene copolymer, polytetrafluoroethylene, and fluororubber can be used. If used for the negative electrode, fluorine resins such as polyvinylidene fluoride, vinylidene fluoride-hexafluoropropylene copolymer, perfluoromethyl vinyl ether-tetrafluoroethylene copolymer, polytetrafluoroethylene, and fluororubber can be used; hydrocarbon elastomers such as styrene-butadiene copolymer and ethylene-propylene copolymer; or polyimide, etc.
[0356] Hereinafter, the binder for lithium ion battery electrodes according to the fifth aspect of the present invention will be described in detail.
[0357] The composition of the fifth embodiment of the present invention can be suitably used as a binder for lithium ion battery electrodes. The amount of the binder of the fifth embodiment of the present invention is preferably 1 to 20% by mass, more preferably 3 to 10% by mass, relative to the total amount of the active material, the binder, and the conductive aid.
[0358] The adhesive of the fifth embodiment of the present invention is flexible, so it can follow the volume change of the electrode during charging and discharging, and can prevent the cracking of the electrode caused by the volume change, or the peeling and falling off of the active material or the destruction of the conductive path caused by the volume change. In addition, the adhesive of the fifth embodiment of the present invention contains many hydrophilic functional groups, so it has a high affinity with the active material and excellent coating of the active material. Furthermore, the adhesive of the fifth embodiment of the present invention has excellent affinity with the electrolyte, so it has excellent performance as an adhesive for lithium ion battery electrodes, for example, it is also excellent in ion conductivity; and it has excellent oxidation resistance or reduction resistance, which can ensure the stability of the electrode, etc.
[0359] Furthermore, a chelate group is introduced into the binder, and manganese ions dissolved from the positive electrode active material are captured by the chelate group near the positive electrode and / or the negative electrode, which can inhibit precipitation and accumulation on the negative electrode active material, thereby achieving excellent charge and discharge characteristics and extended cycle life.
[0360] In the fifth embodiment of the present invention, the positive electrode active material is not particularly limited as long as it can insert and release lithium ions, and examples thereof include transition metal oxides such as CuO, Cu2O, MnO2, MoO3, V2O5, CrO3, Fe2O3, Ni2O3, and CoO3; or Li X CoO2、Li X NiO2、LiX MnO2、Li X Mn2O4、LiNi X Co (1-X) O2、LiNi X Mn (2-X) O4、LiMn a Ni b Co c O2 (a + b + c = 1), LiFePO4 and other lithium composite oxides. Among them, preferred are composite oxides of at least one transition metal selected from transition metals such as Co, Ni, and Mn and lithium. Specific examples include: LiCoO2, LiNiO2, LiMnO2, LiMn2 O4, LiNi X Co (1-X) O2、LiNi X Mn (2-X) O4、LiMn a Ni b Co c O2 (a+b+c=1). These lithium composite oxides may be doped with a small amount of fluorine, boron, Al, Cr, Zr, Mo, Fe and other elements, and the surface of the lithium composite oxide particles may be treated with carbon, MgO, Al2O3, SiO2 and the like.
[0361] In the fifth embodiment of the present invention, the negative electrode active material is not particularly limited as long as it can be inserted into and out of lithium ions, and examples thereof include natural graphite, artificial graphite, graphite, mesophase carbon microbeads (MCMB), tin and / or tin alloys, tin oxides, silicon and / or silicon alloys, silicon oxides, etc. In addition, when the negative electrode active material is an alloy, the negative electrode active material may include a material alloyed with lithium. In addition, here, as a material alloyed with lithium, examples thereof include germanium, tin, lead, zinc, magnesium, sodium, aluminum, gallium, indium, and alloys thereof.
[0362] When these active materials are in the form of particles, the average particle size is not particularly limited, but is preferably 5 μm or more and 20 μm or less.
[0363] There are no particular restrictions on the conductive aid contained in the electrode, and any electronic conductive material that does not adversely affect the battery characteristics can be used. Specifically, conductive carbons such as Ketjen black and acetylene black; carbon materials such as natural graphite, artificial graphite, carbon whiskers, carbon nanotubes, and carbon fiber powders; metal powders and metal fibers such as Cu, Fe, Ag, Ni, Pd, Au, Pt, In, and W; or conductive metal oxides such as indium oxide and tin oxide. The amount of these conductive aids is preferably 1 to 30% by mass relative to the above-mentioned active material.
[0364] Hereinafter, the slurry for forming a lithium ion battery electrode mixture layer according to the fifth aspect of the present invention will be described in detail.
[0365] The slurry for forming the electrode mixture layer of the lithium ion battery of the fifth embodiment of the present invention comprises the above-mentioned binder, active material, conductive aid and water. The slurry may also contain a viscosity modifier such as carboxymethyl cellulose, or a pH modifier such as an acid or alkali as needed. The solid content concentration of the above-mentioned slurry is not particularly limited, and is preferably 20 to 80% by mass in consideration of the viscosity of the slurry, the dispersibility of the solid content, the burden on the drying process, etc. In addition, the ratio of the solid content in the above-mentioned slurry is preferably a positive electrode active material: conductive aid: binder = 70 to 98: 1 to 30: 1 to 20 in terms of mass ratio. The method for making the above-mentioned slurry is also not particularly limited, and can include: a method for making a slurry by mixing, dispersing, and dissolving the binder, active material, and conductive aid together in water; first, dissolving the binder in water, then adding the active material and conductive aid to the binder aqueous solution and mixing, thereby making a slurry; or first, mixing the active material and the conductive aid, then, mixing with the binder aqueous solution, etc. The mixer used for preparing the slurry is not particularly limited, and a mortar, a roll mill, a ball mill, a screw mill, a vibration mill, a homogenizer, a planetary mixer, or the like can be used.
[0366] Hereinafter, the lithium ion battery according to the fifth aspect of the present invention will be described in detail.
[0367] The fifth embodiment of the present invention is an electrode for a lithium ion battery comprising the above-mentioned binder. The electrode for a lithium ion battery is composed of an electrode mixture layer obtained by coating the above-mentioned slurry on a current collector and drying it, and a current collector. The thickness of the electrode mixture layer composed of an active material, a binder, and a conductive additive is preferably 10 to 200 μm. In order to form an electrode mixture layer of this thickness on the current collector, the unit area weight of the electrode mixture layer is preferably set to 4 to 25 mg / cm 2 .
[0368] The above-mentioned current collector can be a conductor that shows conductivity on the surface in contact with the electrode mixture layer. Examples of conductors formed by the following can be: metals such as copper, gold, aluminum, titanium, nickel, stainless steel or their alloys; conductive metal oxides such as indium oxide or tin oxide; or conductive materials such as conductive carbon. The shape of the current collector is not particularly limited, and can be in the form of foil, film, sheet, mesh, metal plate mesh, punched metal, foam, etc. The thickness of the current collector is also not particularly limited, and is preferably about 1 to 100 μm.
[0369] There is no particular limitation on the method for manufacturing the electrode for lithium-ion batteries, and the electrode can be manufactured by coating the above-mentioned slurry on the current collector and drying it. There is no limitation on the method for coating the slurry, and methods such as slit coating, die coating, roller coating, dip coating, scraping, knife coating, and wire rod coating can be used. There is no particular limitation on the drying method and conditions, and a common warm air circulation dryer, a reduced pressure dryer, an infrared dryer, or a microwave heating dryer can be used. There is no limitation on the heating temperature, and the electrode can be heated and dried at 50 to 150°C. Furthermore, the porous structure can be made uniform by pressurizing or pressing the electrode during or after drying.
[0370] The lithium ion battery of the fifth embodiment of the present invention is characterized in that it has the above-mentioned lithium ion battery electrode. By using the above-mentioned lithium ion battery electrode, a high-performance lithium ion battery that achieves excellent charge and discharge characteristics and extended cycle life can be provided. Lithium ion batteries are generally composed of a positive electrode, a negative electrode, a separator, a non-aqueous electrolyte, etc., and can be exemplified by: a laminated battery shape. The positive electrode is formed by bonding the above-mentioned positive electrode active material and the above-mentioned conductive auxiliary agent together on the positive electrode collector through an adhesive, and has a structure in which a positive electrode mixture layer composed of a positive electrode active material, an adhesive, and a conductive auxiliary agent is formed on the collector. The negative electrode also has a structure similar to that of the positive electrode, and is formed by bonding the following negative electrode active material and the above-mentioned conductive auxiliary agent to the negative electrode collector through an adhesive. The separator generally uses a porous film such as polyolefin, and is sandwiched between the positive electrode and the negative electrode because it is responsible for the shutdown function when the battery thermally runs away. The non-aqueous electrolyte is formed by dissolving an electrolyte salt such as LiP F4 in an organic solvent such as a cyclic carbonate. The battery is filled with non-aqueous electrolyte. When charging, lithium ions move from the positive electrode to the negative electrode, and when discharging, lithium ions move from the negative electrode to the positive electrode.
[0371] The non-aqueous electrolyte is not particularly limited, and known materials can be used. The non-aqueous electrolyte is formed by dissolving an electrolyte salt in an organic solvent. Examples of the electrolyte salt include CF3SO3Li, (CF3SO2)2NLi, (CF3SO2)2CLi, LiBF4, LiB(C6H8)4, LiPF4, LiClO4, LiAsF6, LiCl, and LiBr. Organic solvents for dissolving the electrolyte salt include ethylene carbonate, vinylene carbonate, propylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, 1,2-dimethoxyethane, 1,2-diethoxyethane, γ-butyrolactone, tetrahydrofuran, 1,4-dioxane, anisole, diethyl ether, cyclopentane, methyl cyclopentane, acetonitrile, propionitrile, butyronitrile, valeronitrile, benzonitrile, dimethylformamide, dimethyl sulfoxide, trimethyl phosphate, and triethyl phosphate. The concentration of the electrolyte salt in the non-aqueous electrolyte solution can be selected within the range of 0.1 to 5 mol / L, preferably 0.5 to 3 mol / L.
[0372] There is no particular limitation on the separator, and a known separator can be used. Examples of separators include: a polyethylene microporous membrane; a polypropylene microporous membrane; a laminated membrane of a polyethylene microporous membrane and a polypropylene microporous membrane; or a nonwoven fabric composed of polyester fibers, aramid fibers, glass fibers, etc.
[0373] Hereinafter, the sixth aspect of the present invention will be described in detail.
[0374] A sixth embodiment of the present invention is a composition, a binder for lithium ion battery electrodes comprising the composition, a slurry for forming a lithium ion battery electrode mixture layer comprising the composition, an electrode for a lithium ion battery comprising the composition, and a lithium ion battery having the electrode.
[0375] Hereinafter, the composition according to the sixth aspect of the present invention will be described in detail.
[0376] The composition of the sixth embodiment of the present invention is a composition comprising hydrogen ion type alginic acid and a compound containing a chelate group. Thus, in the presence of water, the hydrogen ion type alginic acid and the compound containing a chelate group form an ionic bond in water. In order to form an ionic bond between the constituent components of the composition, it is necessary to introduce at least a basic functional group into the compound containing a chelate group.
[0377] The compound containing chelate group in the sixth embodiment of the present invention is a low molecular compound having chelate group. Here, chelate group refers to a functional group that has a ligand with multiple coordination sites and can form a chelate with a polyvalent metal ion. Furthermore, the compound containing chelate group is preferably a compound having a basic functional group such as an amino group. The basic functional group described herein can include: primary amino group, secondary amino group, tertiary amino group, imino group, etc. As the chelate group, it is suitable to use a chelate group of aminocarboxylic acid system, a chelate group of aminophosphonic acid system, or a chelate group of polyamine system. Some examples of aminocarboxylic acid chelating functional groups include: iminodiacetyl, nitrilotriacetyl, N,N-bis(2-hydroxyethyl)glycine, hydroxyethyliminodiacetyl, ethylenediaminetriacetyl, ethylenediaminetetraacetyl, 1,2-bis(2-aminophenoxy)ethanetetraacetyl, 1,2-diaminocyclohexanetetraacetyl, diethylenetriaminepentaacetyl, (2-hydroxyethyl)ethylenediaminetriacetyl, bis(2-aminoethyl)ethylene glycoltetraacetyl, triethylenetriaminehexaacetyl, etc. Some examples of aminophosphonic acid chelating groups include: aminomethylphosphonic acid, nitrilotri(methylphosphonic acid), etc. Some examples of polyamine chelating groups include: polyethyleneimine, polyamidoamine dendrimer, tetrakis(2-pyridylmethyl)ethylenediamine, etc. When the chelating group comprises carboxylic acid or phosphonic acid, their acidic functional groups are preferably in the form of monovalent salts such as alkali metal salts or ammonium salts because they are more easily ion-exchanged with heavy metal ions than in the form of protons.
[0378] The chelate group-containing compound in the sixth embodiment of the present invention is preferably a water-soluble compound. The term "water-soluble" herein means that the chelate group-containing compound can be dissolved in water at a concentration of 1% by weight or more.
[0379] The molecular weight of the chelate group-containing compound in the sixth aspect of the present invention is preferably 10,000 or less, more preferably 1,000 or less.
[0380] The compound containing chelate group in the sixth scheme of the present invention has no other restrictions as long as it has the above-mentioned chelate group. In addition, as the specific example of the compound containing chelate group of the present invention, it can be enumerated: formic acid, citric acid, porphyrin, polyethylene imine, iminodiacetic acid, nitrilotriacetic acid, ethylenediaminetetraacetic acid, N,N-bis(2-hydroxyethyl)glycine, 1,2-diaminocyclohexanetetraacetic acid, diethylenetriaminepentaacetic acid, N-(2-hydroxyethyl)ethylenediaminetriacetic acid, bis(2-aminoethyl)ethylene glycoltetraacetic acid, bis(2-aminophenyl)ethylene glycoltetraacetic acid, N-(2-hydroxyethyl)iminodiacetic acid, tetrakis(2-pyridylmethyl)ethylenediamine, triethylenetetraaminehexaacetic acid, aminomethylphosphonic acid, aminoethylphosphonic acid, aminopropylphosphonic acid, nitrilotrimethylphosphonic acid and their salts. Among the above chelate group-containing compounds, chelate group-containing compounds having a basic functional group such as an amino group or an imino group are preferred because they can form a compound in which the chelate group-containing compound is introduced into water via an ionic bond by combining with hydrogen ion type alginic acid.
[0381] The chelate group-containing compound in the sixth embodiment of the present invention is preferably a compound whose aqueous solution shows a pH of 3 to 9 when dissolved in water. When a chelate group-containing compound whose aqueous solution shows a pH of 3 to 9 is used as a component of a binder, it is preferred because the pH of an aqueous electrode mixture layer-forming slurry containing a positive electrode active material with a high nickel content can be suppressed from becoming strongly alkaline when manufacturing an electrode for a lithium ion battery, thereby preventing corrosion of the current collector. Here, the pH is a value measured when the concentration of the aqueous solution of the chelate group-containing compound is 1.0 mol / L.
[0382] Some examples of the chelate group-containing compounds showing a pH of 3 to 9 include: disodium nitrilotriacetate, disodium ethylenediaminetetraacetate, trisodium ethylenediaminetetraacetate, dipotassium ethylenediaminetetraacetate, tripotassium ethylenediaminetetraacetate, diammonium ethylenediaminetetraacetate, monocalcium ethylenediaminetetraacetate, monomagnesium ethylenediaminetetraacetate, O,O'-bis(2-aminophenyl)ethylene glycol-N,N,N',N'-tetraacetic acid tetrapotassium, N,N-bis(2-hydroxyethyl)glycine, trisodium diethylenetriaminepentaacetate, sodium gluconate, trisodium nitrilotrimethylphosphonate, disodium hydroxyethylidene diphosphonate, and the like.
[0383] The molecular weight of the hydrogen ion type alginic acid in the sixth embodiment of the present invention is preferably 10,000 to 2,000,000, more preferably 500,000 to 1,500,000 in terms of weight average molecular weight. When the weight average molecular weight is within this range, when used as a binder for lithium ion battery electrodes, it is possible to ensure that the electrode has sufficient mechanical strength and can also adjust the viscosity during electrode coating to a range without problems, so it is preferred.
[0384] The weight average molecular weight of the high molecular weight hydrogen ion type alginic acid in the sixth aspect of the present invention can be calculated by dissolving alginic acid in a buffer solution at about pH=8 and measuring it by gel permeation chromatography (GPC) and converting it into PEO.
[0385] In addition, the hydrogen ion substitution rate of the high molecular weight hydrogen ion type alginic acid in the sixth embodiment of the present invention is 80 to 99%. The hydrogen ion substitution rate described here refers to the proportion of hydrogen ions in the counter ions of the carboxyl groups in the uronic acid as a constituent of alginic acid. The above hydrogen ion substitution rate is calculated by quantifying inorganic ions such as alkali metal ions or alkaline earth metal ions or organic ions such as tetramethylammonium ions in the high molecular weight hydrogen ion type alginic acid. The hydrogen ion substitution rate in the above range means that most of the alginic acid becomes hydrogen ion type. Therefore, when the above alginic acid is used as a binder raw material, it is easy to interact with the compound containing the chelate group, thereby obtaining a preferred result.
[0386] In the sixth embodiment of the composition of the present invention, the blending ratio of hydrogen ion type alginic acid and the chelate group-containing compound is preferably such that the acidic functional groups of the hydrogen ion type alginic acid and the basic functional groups of the chelate group-containing compound are equal in amount.
[0387] In the composition of the sixth aspect of the present invention, the chelate group-containing compound is preferably blended in an amount within a range of 0.1 to 1.1 mol per mol of carboxyl groups in the high molecular weight hydrogen ion type alginic acid.
[0388] The physical mixing method of hydrogen ion type alginic acid and the compound containing chelating group is not particularly limited, and the following methods can be adopted: a method of simply mixing the two powdered forms; a method of mixing the two powdered forms while crushing them; or a method of dispersing the two in a poor solvent, mixing them uniformly, and then removing the solvent to obtain a powder.
[0389] The composition of the sixth embodiment of the present invention may contain only hydrogen ion type alginic acid and the compound containing a chelating group, or may contain other polymer compounds. In this case, the content of the hydrogen ion type alginic acid and the compound containing a chelating group is preferably 10% by mass or more relative to the total amount of the composition.
[0390] As a polymer compound different from the above-mentioned hydrogen ion type alginic acid, if used for the positive electrode, fluorine resins such as polyvinylidene fluoride, vinylidene fluoride-hexafluoropropylene copolymer, perfluoromethyl vinyl ether-tetrafluoroethylene copolymer, polytetrafluoroethylene, and fluorine rubber can be used. If used for the negative electrode, fluorine resins such as polyvinylidene fluoride, vinylidene fluoride-hexafluoropropylene copolymer, perfluoromethyl vinyl ether-tetrafluoroethylene copolymer, polytetrafluoroethylene, and fluorine rubber; hydrocarbon elastomers such as styrene-butadiene copolymer and ethylene-propylene copolymer; or polyimide, etc. can be used.
[0391] The composition of the sixth embodiment of the present invention may contain only hydrogen ion type alginic acid and a chelate group-containing compound, or may further contain a substance that functions as an active material for a lithium ion battery. Examples of the active material include the same substances as those described below.
[0392] Next, a binder for lithium ion battery electrodes according to a sixth aspect of the present invention will be described.
[0393] The composition of the sixth embodiment of the present invention can be suitably used as a binder for lithium ion battery electrodes. More specifically, by also including a compound containing a chelating group in the binder, the hydrogen ion type alginic acid forms a compound with the compound containing the chelating group, and therefore, is suitable for use as a binder for lithium ion battery electrodes that binds active materials, conductive aids, and current collectors. The compound has high toughness, excellent mechanical strength, and high adhesion to active materials, conductive aids, or current collectors, and therefore, can produce a lithium ion battery electrode without cracks or peeling or peeling.
[0394] The amount of the binder blended in the sixth aspect of the present invention is preferably 1 to 20% by mass, more preferably 2 to 10% by mass, based on the total amount of the active material, the binder, and the conductive aid.
[0395] The adhesive of the sixth embodiment of the present invention is flexible, so it can follow the volume change of the electrode during charging and discharging, and can prevent the cracking of the electrode caused by the volume change, or the peeling and falling off of the active material or the destruction of the conductive path caused by the volume change. In addition, the adhesive of the sixth embodiment of the present invention contains many hydrophilic functional groups, so it has a high affinity with the active material and excellent coating of the active material. Furthermore, the adhesive of the sixth embodiment of the present invention has excellent performance as an adhesive for lithium ion battery electrodes due to its excellent affinity with the electrolyte, for example, it also has excellent ion conductivity; and excellent oxidation resistance or reduction resistance, which can ensure the stability of the electrode, etc.
[0396] Furthermore, the binder of the sixth embodiment of the present invention has a chelating group, so the manganese ions dissolved from the positive electrode active material are captured by the chelating group near the positive electrode and / or the negative electrode, which can inhibit precipitation and accumulation on the surface of the negative electrode active material, thereby achieving excellent charge and discharge characteristics and extended cycle life.
[0397] Next, the slurry for forming a lithium ion battery electrode mixture layer according to the sixth aspect of the present invention will be described.
[0398] The slurry for forming the electrode mixture layer of the lithium ion battery of the sixth embodiment of the present invention comprises the above-mentioned binder, active material, conductive aid and water. The slurry may also contain a viscosity modifier such as carboxymethyl cellulose, or a pH modifier such as an acid or alkali as needed. The solid content concentration of the above-mentioned slurry is not particularly limited, and is preferably 20 to 80% by mass in consideration of the viscosity of the slurry, the dispersibility of the solid content, the burden on the drying process, etc. In addition, the ratio of the solid content in the above-mentioned slurry is preferably active material: conductive aid: binder = 70 to 98: 1 to 30: 1 to 20 in terms of mass ratio. The method for making the above-mentioned slurry is also not particularly limited, and can include: a method for making a slurry by mixing, dispersing, and dissolving the binder, active material, and conductive aid together in water; first, dissolving the binder in water, then adding the active material and conductive aid to the binder aqueous solution and mixing, thereby making a slurry; or first, mixing the active material and the conductive aid, then, mixing with the binder aqueous solution, etc. The mixer used for preparing the slurry is not particularly limited, and a mortar, a roll mill, a ball mill, a screw mill, a vibration mill, a homogenizer, a planetary mixer, or the like can be used.
[0399] The active material used in the sixth aspect of the present invention is a positive electrode active material when used for a positive electrode, and a negative electrode active material when used for a negative electrode.
[0400] In the sixth embodiment of the present invention, the positive electrode active material is not particularly limited as long as it can insert and / or release lithium ions, and examples thereof include transition metal oxides such as CuO, Cu2O, MnO2, MoO3, V2O5, CrO3, Fe2O3, Ni2O3, and CoO3; or Li X CoO2、Li X NiO2、Li X MnO2、Li X Mn2O4、LiNi X Co (1-X) O2、LiNi X Mn (2-X) O4、LiMn a Ni b Co cO2(a+b+c=1), LiNi 0.8 Co 0.15 Al 0.05 O2, LiFePO4, LiMn X Fe (1-X) Among them, preferred are composite oxides of at least one transition metal selected from transition metals such as Co, Ni, and Mn and lithium, and specific examples thereof include: LiCoO2, LiNiO2, LiMnO2, LiMn2 O4, LiNi X Co (1-X) O2、LiNi X Mn (2-X) O4、LiMn a Ni b Co c O2(a+b+c=1), LiNi 0.8 Co 0.15 Al 0.05 O2、Li Mn X Fe (1-X) These lithium composite oxides can be doped with a small amount of fluorine, boron, Al, Cr, Zr, Mo, Fe and other elements, and the surface of the lithium composite oxide particles can also be treated with carbon, MgO, Al2O3, SiO2 and the like.
[0401] In the sixth embodiment of the present invention, the negative electrode active material is not particularly limited as long as it can be inserted into and / or separated from lithium ions, and examples thereof include: lithium metal, natural graphite, artificial graphite, graphite, mesophase carbon microbeads (MCMB), tin and / or tin alloys, tin oxides, silicon and / or silicon alloys, silicon oxides, etc. In addition, when the negative electrode active material is an alloy, the negative electrode active material may contain a material alloyed with lithium. In addition, here, as a material alloyed with lithium, examples thereof include: germanium, tin, lead, zinc, magnesium, sodium, aluminum, gallium, indium, and alloys thereof.
[0402] When these active materials are in the form of particles, the average particle size is not particularly limited, but is preferably 5 μm or more and 20 μm or less. The amount of these active materials blended is preferably 70 to 98% by mass relative to the total amount of the active material, binder, and conductive additive.
[0403] There are no particular restrictions on the conductive aid contained in the electrode, and any electronic conductive material that does not adversely affect the battery characteristics can be used. Specifically, conductive carbons such as Ketjen black and acetylene black; carbon materials such as natural graphite, artificial graphite, carbon whiskers, carbon nanotubes, and carbon fiber powders; metal powders and metal fibers such as Cu, Fe, Ag, Ni, Pd, Au, Pt, In, and W; or conductive metal oxides such as indium oxide and tin oxide. The amount of these conductive aids is preferably 1 to 30% by mass relative to the above-mentioned active material.
[0404] Hereinafter, a lithium ion battery electrode according to a sixth aspect of the present invention will be described.
[0405] A lithium ion battery electrode according to a sixth aspect of the present invention includes an active material, a conductive auxiliary agent, and the above-mentioned binder for lithium ion battery electrodes.
[0406] The lithium-ion battery electrode is composed of an electrode mixture layer obtained by coating the slurry on a current collector and drying the slurry, and the current collector. The thickness of the electrode mixture layer composed of the active material, the binder, and the conductive additive is preferably 10 to 200 μm. In order to form an electrode mixture layer of this thickness on the current collector, the unit area weight of the electrode mixture layer is preferably set to 4 to 25 mg / cm 2 .
[0407] The above-mentioned current collector can be a conductor that shows conductivity on the surface in contact with the electrode mixture layer. Examples of conductors formed by the following can be: metals such as copper, gold, aluminum, titanium, nickel, stainless steel or their alloys; conductive metal oxides such as indium oxide or tin oxide; or conductive materials such as conductive carbon. The shape of the current collector is not particularly limited, and can be in the form of foil, film, sheet, mesh, metal plate mesh, punched metal, foam, etc. The thickness of the current collector is also not particularly limited, and is preferably about 1 to 100 μm.
[0408] There is no particular limitation on the method for manufacturing the electrode for lithium-ion batteries, and the electrode can be manufactured by coating the above-mentioned slurry on the current collector and drying it. There is no limitation on the method for coating the slurry, and methods such as slit coating, die coating, roller coating, dip coating, scraping, knife coating, and wire rod coating can be used. There is no particular limitation on the drying method and conditions, and a common warm air circulation dryer, a reduced pressure dryer, an infrared dryer, or a microwave heating dryer can be used. There is no limitation on the heating temperature, and the electrode can be heated and dried at 50 to 150°C. Furthermore, the porous structure can be made uniform by pressurizing or pressing the electrode during or after drying.
[0409] Next, a lithium ion battery according to a sixth aspect of the present invention will be described.
[0410] The lithium ion battery of the sixth embodiment of the present invention is characterized in that it has the above-mentioned lithium ion battery electrode. The lithium ion battery of the sixth embodiment of the present invention includes a lithium ion primary battery and a lithium ion secondary battery. By using the above-mentioned lithium ion battery electrode, a high-performance lithium ion battery that achieves excellent charge and discharge characteristics and extended cycle life can be provided. Lithium ion batteries are generally composed of a positive electrode, a negative electrode, a separator, a non-aqueous electrolyte, etc., and can be exemplified as: a laminated battery shape. The positive electrode is formed by bonding the above-mentioned positive electrode active material and the above-mentioned conductive auxiliary agent together on the positive electrode collector through an adhesive, and has a structure in which a positive electrode mixture layer composed of a positive electrode active material, an adhesive, and a conductive auxiliary agent is formed on the collector. The negative electrode also has a structure similar to that of the positive electrode, and is formed by bonding the following negative electrode active material and the above-mentioned conductive auxiliary agent to the negative electrode collector through an adhesive. The separator generally uses a porous film such as polyolefin, and is sandwiched between the positive electrode and the negative electrode because it is responsible for the shutdown function when the battery is thermally runaway. The non-aqueous electrolyte is formed by dissolving an electrolyte salt such as LiPF4 in an organic solvent such as a cyclic carbonate. The battery is filled with non-aqueous electrolyte. When charging, lithium ions move from the positive electrode to the negative electrode, and when discharging, lithium ions move from the negative electrode to the positive electrode.
[0411] The non-aqueous electrolyte is not particularly limited, and known materials can be used. The non-aqueous electrolyte is formed by dissolving an electrolyte salt in an organic solvent. Examples of the electrolyte salt include CF3SO3Li, (CF3SO2)2NLi, (CF3SO2)3CLi, LiBF4, LiB(C6H5)4, LiPF6, LiClO4, LiAsF6, LiCl, LiBr, etc. As organic solvents for dissolving the electrolyte salt, examples include ethylene carbonate, vinylene carbonate, propylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, 1,2-dimethoxyethane, 1,2-diethoxyethane, γ-butyrolactone, tetrahydrofuran, 1,4-dioxane, anisole, diethyl ether, cyclopentane, methylcyclopentane, acetonitrile, propionitrile, butyronitrile, valeronitrile, benzonitrile, dimethylformamide, dimethyl sulfoxide, trimethyl phosphate, triethyl phosphate, etc. The concentration of the electrolyte salt in the non-aqueous electrolyte solution can be selected within the range of 0.1 to 5 mol / L, preferably 0.5 to 3 mol / L.
[0412] There is no particular limitation on the separator, and a known separator can be used. Examples of separators include: a polyethylene microporous membrane; a polypropylene microporous membrane; a laminated membrane of a polyethylene microporous membrane and a polypropylene microporous membrane; or a nonwoven fabric composed of polyester fibers, aramid fibers, glass fibers, etc.
[0413] Hereinafter, the seventh aspect of the present invention will be described in detail.
[0414] The seventh embodiment of the present invention is high molecular weight hydrogen ion type alginic acid, a method for producing the same, a binder for lithium ion battery electrodes containing the same, a slurry for forming a lithium ion battery electrode mixture layer containing the same, an electrode for a lithium ion battery containing the same, and a lithium ion battery having the same.
[0415] Hereinafter, the high molecular weight hydrogen ion type alginic acid according to the seventh aspect of the present invention will be described in detail.
[0416] The high molecular weight hydrogen ion type alginic acid of the seventh scheme of the present invention is a linear polysaccharide composed of two uronic acids (mannuronic acid and guluronic acid), and refers to a substance in which the counter ion of the carboxyl group in the uronic acid is a hydrogen ion type. The ratio of mannuronic acid and guluronic acid as the constituent of alginic acid is arbitrary, and alginic acid with a high ratio of mannuronic acid that generates a soft gel and alginic acid with a high ratio of guluronic acid that can obtain a rigid gel can be used. In addition, the arrangement order of the two uronic acids is not particularly limited, and random or block is all OK.
[0417] The high molecular weight hydrogen ion type alginic acid of the seventh embodiment of the present invention needs to have a weight average molecular weight of 500,000 to 1,500,000. When the weight average molecular weight is within this range, the adhesive for lithium ion battery electrodes manufactured using the high molecular weight hydrogen ion type alginic acid as a raw material exhibits excellent adhesion or toughness, and exhibits preferred properties as an adhesive. In addition, since the viscosity of the slurry for forming the electrode mixture layer containing active materials, conductive additives, adhesives containing the high molecular weight hydrogen ion type alginic acid, and water for manufacturing the adhesive for lithium ion battery electrodes can be set within a range with good coating properties, the lithium ion battery electrode made from the above slurry will also become an electrode without cracks, peeling, or flaking, and can provide a battery with long life and excellent durability.
[0418] The weight average molecular weight of the high molecular weight hydrogen ion type alginic acid according to the seventh aspect of the present invention can be calculated by dissolving alginic acid in a buffer solution at about pH=8 and measuring it by gel permeation chromatography (GPC) and converting it into PEO.
[0419] In addition, the hydrogen ion substitution rate of the high molecular weight hydrogen ion type alginic acid of the seventh embodiment of the present invention is 80 to 99%. The hydrogen ion substitution rate described here refers to the proportion of hydrogen ions in the counter ions of the carboxyl groups in the uronic acid as a constituent of the alginic acid. The above hydrogen ion substitution rate is calculated by quantifying inorganic ions such as alkali metal ions or alkaline earth metal ions or organic ions such as tetramethylammonium ions in the high molecular weight hydrogen ion type alginic acid. The hydrogen ion substitution rate in the above range means that most of the alginic acid becomes hydrogen ion type. When the above alginic acid is used as a binder raw material, it is easy to interact with a compound containing a chelating group, thereby obtaining a preferred result.
[0420] Next, the method for producing hydrogen ion-type alginic acid according to the seventh aspect of the present invention will be described.
[0421] The manufacturing method of the present invention is characterized in that the alkali metal salt of alginate or alkaline earth metal salt of alginate as a raw material is dissolved in their poor solvent, and then acid is added, and the alkali metal salt of alginate or alkaline earth metal salt of alginate is not dissolved in the solvent and is dispersed in the state of contacting with acid, so that the ion exchange is hydrogen ion type. In the manufacturing method known in the past, since the alkali metal salt of alginate or alkaline earth metal salt of alginate is dissolved in water, the aqueous solution will become highly viscous even at low concentrations, and it is limited to manufacturing under low concentration conditions, and it is difficult to manufacture with good productivity at high concentrations. Therefore, the above-mentioned alginate is dispersed in a poor solvent that does not dissolve the alkali metal salt of alginate or alkaline earth metal salt of alginate, and acid is added in a heterogeneous system and an ion exchange reaction is performed to manufacture a method for hydrogen ion type alginic acid. It is found that hydrogen ion type alginic acid can be manufactured with good productivity at high concentrations. The manufacturing method of the sixth scheme of the present invention can be used not only to manufacture high molecular weight hydrogen ion type alginic acid, but also to manufacture low molecular weight hydrogen ion type alginic acid.
[0422] The poor solvent used in the above-mentioned heterogeneous reaction is not particularly limited as long as it does not dissolve the alkali metal salt of alginate and the alkaline earth metal salt of alginate. In order to promote the reaction with the acid, a poor solvent that is mutually soluble in water is preferred. Some examples of preferred poor solvents include: alcohols such as methanol, ethanol, isopropanol, and butanol; glycols such as ethylene glycol, propylene glycol, glycerol, and diethylene glycol; cyclic ethers such as tetrahydrofuran, dioxane, and trioxane; ketones such as acetone and 2-butanone, or mixed solvents of these solvents and water. In the case of using a mixed solvent of a poor solvent and water, the ratio of water in the mixed solvent is preferably 1 to 30% by mass.
[0423] The above-mentioned heterogeneous reaction is carried out in a slurry state, and the slurry concentration at this time is preferably 10 to 40% by mass. Here, the slurry concentration refers to the concentration of the alginate in the slurry.
[0424] The reaction temperature, reaction time, type or amount of acid added are not particularly limited, but mild conditions are preferably selected to inhibit the hydrolysis of alginic acid. For example, the preferred conditions are as follows: the reaction temperature is 0 to 30°C, the reaction time is 1 minute to 5 hours, the type of acid is at least one of the group consisting of hydrochloric acid, sulfuric acid, phosphoric acid, and sulfonic acid, and the amount of acid added is equivalent to 10 times the equivalent relative to the carboxyl group of alginic acid. After the reaction is completed, the high molecular weight hydrogen ion type alginic acid remains in a slurry state, so it is recovered by filtration, etc., and separated by washing and drying as needed.
[0425] Next, the binder for lithium ion battery electrodes according to the seventh aspect of the present invention will be described.
[0426] The high molecular weight hydrogen ion type alginic acid can be suitably used as a binder for lithium ion battery electrodes. More specifically, by also including a compound containing a chelating group in the binder, the high molecular weight hydrogen ion type alginic acid forms a compound with the compound containing the chelating group, and is therefore suitable for use as a binder for lithium ion battery electrodes that binds active materials, conductive aids, and current collectors. Since the compound is a high molecular weight body, it has high toughness, excellent mechanical strength, and high adhesion to active materials, conductive aids, or current collectors, so it is possible to produce a lithium ion battery electrode without cracks or peeling or peeling.
[0427] The chelate group-containing compound used in the seventh embodiment of the present invention is a compound having a chelate group. The chelate group is a functional group that is a ligand having multiple coordination sites and can form a chelate with a polyvalent metal ion.
[0428] As the chelate group, an aminocarboxylic acid-based chelate group, an aminophosphonic acid-based chelate group, or a polyamine-based chelate group is preferably used.
[0429] Some examples of aminocarboxylic acid chelating functional groups include: iminodiacetyl, nitrilotriacetyl, N,N-bis(2-hydroxyethyl)glycine, hydroxyethyliminodiacetyl, ethylenediaminetriacetyl, ethylenediaminetetraacetyl, 1,2-bis(2-aminophenoxy)ethanetetraacetyl, 1,2-diaminocyclohexanetetraacetyl, diethylenetriaminepentaacetyl, (2-hydroxyethyl)ethylenediaminetriacetyl, bis(2-aminoethyl)ethylene glycoltetraacetyl, triethylenetriaminehexaacetyl, and the like.
[0430] Some examples of aminophosphonic acid chelating groups include aminomethylphosphonic acid, nitrilotri(methylphosphonic acid), etc. Some examples of polyamine chelating groups include polyethyleneimine, polyamidoamine dendrimer, tetrakis(2-pyridylmethyl)ethylenediamine, etc.
[0431] When the chelating group comprises carboxylic acid or phosphonic acid, their acidic functional groups are preferably in the form of monovalent salts such as alkali metal salts or ammonium salts because they are more easily ion-exchanged with heavy metal ions than in the form of protons.
[0432] Some specific examples of compounds containing chelating functional groups include: iminodiacetic acid, nitrilotriacetic acid, ethylenediaminetetraacetic acid, N,N-bis(2-hydroxyethyl)glycine, 1,2-diaminocyclohexanetetraacetic acid, diethylenetriaminepentaacetic acid, N-(2-hydroxyethyl)ethylenediaminetriacetic acid, bis(2-aminoethyl)ethylene glycoltetraacetic acid, bis(2-aminophenyl)ethylene glycoltetraacetic acid, N-(2-hydroxyethyl)iminodiacetic acid, tetrakis(2-pyridylmethyl)ethylenediamine, triethylenetetraaminehexaacetic acid, aminomethylphosphonic acid, aminoethylphosphonic acid, aminopropylphosphonic acid, nitrilotri(methylphosphonic acid) and their salts. These chelating compounds having amino groups can be used alone or in combination of two or more.
[0433] The adhesive of the present invention preferably comprises a high molecular weight hydrogen ion type alginic acid and a compound containing a chelate group. In this case, the above-mentioned adhesive can use a compound made by pre-reacting the high molecular weight hydrogen ion type alginic acid and the compound containing a chelate group, or can use a composition made by simply mixing the high molecular weight hydrogen ion type alginic acid and the compound containing a chelate group. In the case of simple mixing, in fact, the high molecular weight hydrogen ion type alginic acid and the compound containing a chelate group will produce an ionic bond. For example, in order to manufacture an electrode for a lithium ion battery, when making a slurry for forming an aqueous lithium ion battery electrode mixture layer, the above-mentioned composition also includes water, so that the high molecular weight hydrogen ion type alginic acid and the compound containing a chelate group react in the system to form a compound. As an example, the compound formation reaction when using hydrogen ion type alginic acid and disodium iminodiacetic acid as a compound containing a chelate group is shown below.
[0434] [Chemical formula 11]
[0435]
[0436] The amount of the chelate group contained in the compound of the high molecular weight hydrogen ion type alginic acid and the compound containing the chelate group is 0.2 to 6 mmol / g, preferably 0.5 to 5 mmol / g. When the content of the chelate group is within this range, heavy metal ions can be captured quickly, and the heavy metal ion capture amount is also sufficient, so it is preferred.
[0437] In the above composition, the compound containing a chelating functional group is preferably blended in an amount within a range of 0.1 to 1.1 mol per mol of carboxyl groups in the high molecular weight hydrogen ion type alginic acid.
[0438] The above-mentioned lithium ion battery electrode adhesive can use only a compound of a high molecular weight hydrogen ion type alginic acid and a compound containing a chelating group, or it can include other adhesive components. In this case, the content of the adhesive composed of the above-mentioned compound is preferably more than 10% by mass. As other adhesives, if it is an adhesive for the positive electrode, fluorine resins such as polyvinylidene fluoride, vinylidene fluoride-hexafluoropropylene copolymer, perfluoromethyl vinyl ether-tetrafluoroethylene copolymer, polytetrafluoroethylene, and fluororubber can be used. If it is an adhesive for the negative electrode, fluorine resins such as polyvinylidene fluoride, vinylidene fluoride-hexafluoropropylene copolymer, perfluoromethyl vinyl ether-tetrafluoroethylene copolymer, polytetrafluoroethylene, and fluororubber can be used; hydrocarbon elastomers such as styrene-butadiene copolymer and ethylene-propylene copolymer; or polyimide, etc.
[0439] Next, the slurry for forming a lithium ion battery mixture layer according to the seventh aspect of the present invention will be described.
[0440] The slurry for forming the lithium ion battery electrode mixture layer of the seventh embodiment of the present invention comprises the above-mentioned binder, active material, conductive aid and water. The slurry may also contain a viscosity modifier such as carboxymethyl cellulose, or a pH modifier such as an acid or alkali as needed. The solid content concentration of the above-mentioned slurry is not particularly limited, and is preferably 20 to 80% by mass in consideration of the viscosity of the slurry, the dispersibility of the solid content, the burden on the drying process, etc. In addition, the ratio of the solid content in the above-mentioned slurry is preferably active material: conductive aid: binder = 70 to 98: 1 to 30: 1 to 20 in terms of mass ratio. The method for making the above-mentioned slurry is also not particularly limited, and can include: a method for making a slurry by mixing, dispersing, and dissolving the binder, active material, and conductive aid together in water; first, dissolving the binder in water, then adding the active material and conductive aid to the binder aqueous solution and mixing, thereby making a slurry; or first, mixing the active material and the conductive aid, then, mixing with the binder aqueous solution, etc. The mixer used for preparing the slurry is not particularly limited, and a mortar, a roll mill, a ball mill, a screw mill, a vibration mill, a homogenizer, a planetary mixer, or the like can be used.
[0441] The active material used in the seventh aspect of the present invention is a positive electrode active material when the electrode is a positive electrode, and a negative electrode active material when the electrode is a negative electrode.
[0442] The positive electrode active material used in the sixth embodiment of the present invention is not particularly limited as long as it can insert lithium ions in a primary battery, and is not particularly limited as long as it can insert and remove lithium ions in a secondary battery, and examples thereof include transition metal oxides such as CuO, Cu2O, MnO2, MoO3, V2O5, CrO3, Fe2O3, Ni2O3, and CoO3; or Li X CoO2、Li X NiO2、Li X MnO2、Li X Mn2O4、LiNi X Co (1-X) O2、LiNi X Mn (2-X) O4、LiMn a Ni b Co c O2(a+b+c=1), LiFePO4, LiMn (1-X) Fe X PO4 and other lithium composite oxides. Among them, as the active material of the primary battery, MnO2 is preferred, and as the active material of the secondary battery, a composite oxide of at least one transition metal selected from transition metals such as Co, Ni, and Mn and lithium is preferred. As specific examples, LiCoO2, LiNiO2, LiMnO2, LiMn2 O4, LiNi X Co (1-X) O2、LiNi X Mn (2-X) O4、Li Mn a Ni b Co c O2(a+b+c=1), LiFePO4, LiMn (1-X) Fe X These lithium composite oxides can be doped with a small amount of fluorine, boron, Al, Cr, Zr, Mo, Fe and other elements, and the surface of the lithium composite oxide particles can also be treated with carbon, MgO, Al2O3, SiO2 and the like.
[0443] For the negative electrode active material used in the seventh embodiment of the present invention, if it is a primary battery, as long as the lithium ions can be separated, there is no particular restriction. If it is a secondary battery, as long as the lithium ions can be inserted and separated, there is no particular restriction. For example, lithium metal, natural graphite, artificial graphite, graphite, mesophase carbon microbeads (MCMB), tin and / or tin alloys, tin oxides, silicon and / or silicon alloys, silicon oxides, etc. can be cited. In addition, when the negative electrode active material is an alloy, the negative electrode active material can contain a material that is alloyed with lithium. In addition, here, as a material that is alloyed with lithium, for example, germanium, tin, lead, zinc, magnesium, sodium, aluminum, gallium, indium and their alloys can be cited.
[0444] When these active materials are in the form of particles, the average particle size is not particularly limited, but is preferably 5 μm or more and 20 μm or less. The amount of these active materials blended is preferably 70 to 98% by mass relative to the total amount of the active material, binder, and conductive additive.
[0445] There are no particular restrictions on the conductive aid contained in the electrode, and any electronic conductive material that does not adversely affect the battery characteristics can be used. Specifically, conductive carbons such as Ketjen black and acetylene black; carbon materials such as natural graphite, artificial graphite, carbon whiskers, carbon nanotubes, and carbon fiber powders; metal powders and metal fibers such as Cu, Fe, Ag, Ni, Pd, Au, Pt, In, and W; or conductive metal oxides such as indium oxide and tin oxide. The amount of these conductive aids is preferably 1 to 30% by mass relative to the total amount of the active material, binder, and conductive aid.
[0446] Next, the lithium ion battery electrode according to the seventh aspect of the present invention will be described.
[0447] A lithium ion battery electrode according to a seventh aspect of the present invention comprises an active material, a conductive auxiliary agent, and the above-mentioned binder for lithium ion battery electrodes.
[0448] The lithium-ion battery electrode is composed of an electrode mixture layer obtained by coating the slurry on a current collector and drying the slurry, and the current collector. The thickness of the electrode mixture layer composed of the active material, the binder, and the conductive additive is preferably 10 to 200 μm. In order to form an electrode mixture layer of this thickness on the current collector, the unit area weight of the electrode mixture layer is preferably set to 4 to 25 mg / cm 2 .
[0449] The current collector can be any conductive body as long as the surface in contact with the electrode mixture layer shows conductivity. Examples of conductive bodies formed by the following can be given: metals such as copper, gold, aluminum, titanium, nickel, stainless steel or their alloys; conductive metal oxides such as indium oxide or tin oxide; or conductive materials such as conductive carbon. The shape of the current collector is not particularly limited, and can be in the form of foil, film, sheet, mesh, metal plate mesh, punched metal, foam, etc. The thickness of the current collector is also not particularly limited, and is preferably about 1 to 100 μm.
[0450] There is no particular restriction on the method for manufacturing the electrode for lithium-ion batteries, and the slurry can be coated on the current collector and dried to manufacture. There is no restriction on the coating method of the slurry, and it can be coated by using slit coating, die coating, roller coating, dip coating, scraping, knife coating, wire rod coating and the like. There is no particular restriction on the drying method and conditions, and a common warm air circulation dryer, reduced pressure dryer, infrared dryer, or microwave heating dryer can be used. There is no restriction on the heating temperature, and it can be heated and dried at 50 to 150°C. Furthermore, the porous structure can also be made uniform by pressurizing and pressing the electrode during or after drying.
[0451] Next, a lithium ion battery according to a seventh aspect of the present invention will be described.
[0452] The lithium ion battery of the seventh embodiment of the present invention is characterized in that it has the above-mentioned lithium ion battery electrode. The lithium ion battery of the present invention can be a primary battery or a secondary battery. By using the above-mentioned lithium ion battery electrode, a high-performance lithium ion battery can be provided, which achieves excellent charge and discharge characteristics and achieves an extension of the cycle life in the case of a secondary battery. Lithium ion batteries are generally composed of a positive electrode, a negative electrode, a separator, a non-aqueous electrolyte, etc., and can be exemplified by: a laminated battery shape. The positive electrode is formed by bonding the above-mentioned positive electrode active material and the above-mentioned conductive auxiliary agent together on the positive electrode collector by a binder, and has a structure in which a positive electrode mixture layer composed of a positive electrode active material, a binder, and a conductive auxiliary agent is formed on the collector. The negative electrode also has a structure similar to that of the positive electrode, and is formed by bonding the following negative electrode active material and the above-mentioned conductive auxiliary agent to the negative electrode collector by a binder. The separator generally uses a porous film such as polyolefin, and is sandwiched between the positive electrode and the negative electrode because it is responsible for the shutdown function when the battery is thermally runaway. Non-aqueous electrolytes are electrolyte salts such as LiPF4 dissolved in organic solvents such as cyclic carbonates. The battery is filled with non-aqueous electrolytes. In secondary batteries, lithium ions move from the positive electrode to the negative electrode during charging, and from the negative electrode to the positive electrode during discharge.
[0453] The non-aqueous electrolyte is not particularly limited, and known materials can be used. The non-aqueous electrolyte is formed by dissolving an electrolyte salt in an organic solvent. Examples of the electrolyte salt include CF3SO3Li, (CF3SO2)2NLi, (CF3SO2)2CLi, LiBF4, LiB(C6H8)4, LiPF4, LiClO4, LiAsF6, LiCl, and LiBr. Organic solvents for dissolving the electrolyte salt include ethylene carbonate, vinylene carbonate, propylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, 1,2-dimethoxyethane, 1,2-diethoxyethane, γ-butyrolactone, tetrahydrofuran, 1,4-dioxane, anisole, diethyl ether, cyclopentane, methyl cyclopentane, acetonitrile, propionitrile, butyronitrile, valeronitrile, benzonitrile, dimethylformamide, dimethyl sulfoxide, trimethyl phosphate, and triethyl phosphate. The concentration of the electrolyte salt in the non-aqueous electrolyte solution can be selected within the range of 0.1 to 5 mol / L, preferably 0.5 to 3 mol / L.
[0454] There is no particular limitation on the separator, and a known separator can be used. Examples of separators include: a polyethylene microporous membrane; a polypropylene microporous membrane; a laminated membrane of a polyethylene microporous membrane and a polypropylene microporous membrane; or a nonwoven fabric composed of polyester fibers, aramid fibers, glass fibers, etc.
[0455] Example
[0456] Hereinafter, the present invention will be described in more detail based on Examples, but the present invention is not limited to these Examples.
[0457] (Example of the first aspect of the present invention)
[0458] (Reference Example 1-1) Production of Sulfated Alginic Acid
[0459] Under stirring, 3.0 g (monosaccharide unit is 17 mmol) of H-type alginate (manufactured by KIMICA Co., Ltd., trade name KIMICA ACID G) was gradually added in small amounts to 150 ml of dimethyl sulfoxide (hereinafter referred to as "DMSO") to make it uniformly dispersed. Next, 6.75 g (42.5 mmol) of sulfur trioxide pyridine complex was added under stirring, and the temperature was raised after it was evenly dispersed, and the reaction was carried out at 40°C for 8 hours. Alginate dissolves as the reaction proceeds, and a uniform solution is formed at the end of the reaction. After the reaction is completed, the reaction solution is added dropwise to ethanol, and the precipitated product is captured with a glass filter, washed with ethanol, and dried under reduced pressure at room temperature to separate the product. The separation yield is 5.8 g, and the sulfur content obtained by elemental analysis is 12.5% by mass, and the weight average molecular weight determined by gel permeation chromatography (GPC) is 85,000. The sulfate content calculated based on the sulfur content is 3.9 mmol / g.
[0460] (Example 1-1)
[0461] Under stirring, 1.0 g (monosaccharide unit is 5.7 mmol) of hydrogen ion type alginic acid (manufactured by KIMICA Co., Ltd., trade name KIMICA ACID G) was gradually added in small amounts to 100 ml of pure water to make a white paste-like uniform dispersion. Next, 2.72 g (5.7 mmol) of bis(2-aminoethyl) glycol tetraacetic acid (manufactured by Tokyo Chemical Industry, hereinafter referred to as "BAPTA") and 0.93 g (22.8 mmol) of sodium hydroxide (manufactured by Tokyo Chemical Industry) were dissolved in 20 ml of pure water and added dropwise to the above-mentioned alginic acid dispersion. The dispersion gradually becomes transparent with the addition, and after the addition is completed, it becomes a transparent and viscous brown aqueous solution. The aqueous solution was stirred at room temperature for 1 hour, and then added dropwise to 4 L of acetone to generate a precipitate. The precipitate obtained was recovered by filtration, and then washed with acetone and separated by drying under reduced pressure. The isolated yield was 3.9 g, and the nitrogen content determined by elemental analysis was 4.6% by mass. The chelating functional group content calculated from the nitrogen content was 3.3 mmol / g. The product was easily soluble in water.
[0462] In order to confirm that the chelating functional groups were introduced into the alginic acid, the FT-IR spectra before and after the reaction were compared. Figure 1 and Figure 2 The hydrogen ion form of alginate before the reaction was 1740 cm -1 The stretching vibration absorption of the carbonyl group of the carboxylic acid was observed at 1740 cm -1 The absorption at 1600 cm -1 New absorption derived from stretching vibration of the carbonyl group of carboxylate was observed at 147°, which showed that alginic acid and BAPTA were bonded via ionic bonds.
[0463] The molecular weight of the chelate polymer was measured by aqueous GPC and the weight average molecular weight was 350,000.
[0464] <Evaluation of heavy metal ion capture ability>
[0465] In order to evaluate the heavy metal ion capture ability of the chelate polymer, the following determination was performed. 0.1 g of the above-mentioned chelate polymer was dissolved in 20 ml of pure water, and 1.9 g of lithium manganate (trial production by our company, crystal structure: spinel, hereinafter referred to as "LMO") was added to prepare a slurry. After the obtained slurry was concentrated with an evaporator, it was dried under reduced pressure at 80°C to remove water to obtain a mixture of the chelate polymer and LMO. 1.0 g was taken from the above mixture, placed in a TEFLON (registered trademark) container, and sealed after drying under reduced pressure at 120°C for 4 hours. The sealed TEFLON (registered trademark) container was opened in a glove box, and an electrolyte (Kishida Chemical, a solution obtained by dissolving 1 mol / L of LiPF6 in a mixed solvent of ethylene carbonate: dimethyl carbonate = 1:2) was added. After 15 ml, it was sealed again and heated at 85°C for 4 hours. After the heating was completed, the TEFLON (registered trademark) container was opened in the glove box, filtered using a syringe filter, and the filtrate was collected. The obtained filtrate was subjected to acid decomposition, and manganese ions were quantified by ICP-MS. As a result, the concentration of manganese ions was less than 1 ppm, confirming that the manganese ions eluted from the LMO by heating were captured by the chelate polymer.
[0466] (Example 1-2)
[0467] Use 1.1g (5.7mmol) of disodium iminodiacetic acid monohydrate (Fuji Film Wako Pure Chemical Industries, Ltd.) to replace BAPTA and sodium hydroxide, except that, by the same operation as Example 1-1, manufacture chelate polymer. Separation yield is 1.9g, and the nitrogen content tried to be obtained by elemental analysis is 3.7% by mass %, and the chelate functional group content calculated according to the nitrogen content is 2.6mmol / g, and it is soluble in water.
[0468] In order to confirm that the chelating functional groups were introduced into the alginic acid, the FT-IR spectra before and after the reaction were compared. The hydrogen ion-type alginic acid before the reaction had a peak at 1740 cm -1 The stretching vibration absorption of the carbonyl group of the carboxylic acid was observed at 1740 cm -1 The absorption at 1620cm -1 New absorption derived from the stretching vibration of the carbonyl group of the carboxylate was observed at 40°C. This shows that alginic acid and iminodiacetic acid are bonded via an ionic bond.
[0469] The molecular weight of the chelate polymer was measured by aqueous GPC and the weight average molecular weight was 320,000.
[0470] <Evaluation of heavy metal ion capture ability>
[0471] The heavy metal ion capturing ability of the chelate polymer produced in Example 1-2 was evaluated by the same method as in Example 1-1. The manganese ion concentration in the filtrate was less than 1 ppm, and it was confirmed that the manganese ions eluted from the LMO by heating were captured by the chelate polymer.
[0472] (Example 1-3)
[0473] Use tetrasodium ethylenediaminetetraacetate (Tokyo Chemical Industry, hereinafter referred to as " EDTA ") 2.37g (5.7mmol) to replace BAPTA and sodium hydroxide, in addition, by the operation identical with embodiment 1-1, manufacture chelated polymer.Separation yield is 2.4g, and the nitrogen content that tries to be achieved by ultimate analysis is 3.9% by mass %, and the chelate functional group content that calculates according to nitrogen content is 1.4mmol / g, is soluble in water.
[0474] In order to confirm that the chelating functional groups were introduced into the alginic acid, the FT-IR spectra before and after the reaction were compared. The hydrogen ion-type alginic acid before the reaction had a peak at 1740 cm -1 The stretching vibration absorption of the carbonyl group of the carboxylic acid was observed at 1740 cm -1 The absorption at 1600 cm -1 New absorption derived from the stretching vibration of the carbonyl group of the carboxylate was observed at 140°C, which showed that alginic acid and EDTA were bonded via ionic bonds.
[0475] The molecular weight of the chelate polymer was measured by aqueous GPC and the weight average molecular weight was 380,000.
[0476] <Evaluation of heavy metal ion capture ability>
[0477] The heavy metal ion capturing ability of the chelate polymer produced in Example 1-3 was evaluated by the same method as in Example 1-1. The concentration of manganese ions in the filtrate was less than 1 ppm, and it was confirmed that the manganese ions eluted from the LMO by heating were captured by the chelate polymer.
[0478] (Examples 1-4)
[0479] Use aminomethylphosphonic acid (Tokyo Chemical Industry, hereinafter referred to as "AMP") 0.63g (5.7mmol) and sodium hydroxide (Tokyo Chemical Industry) 0.46g (11.4mmol) to replace BAPTA and sodium hydroxide, in addition, by the operation identical with embodiment 1-1, manufacture chelated polymer.Separation yield is 1.7g, and the nitrogen content that tries to be achieved by ultimate analysis is 2.8% by mass %, and the chelate functional group content that calculates according to nitrogen content is 2.0mmol / g, and is soluble in water.
[0480] In order to confirm that the chelating functional groups were introduced into the alginic acid, the FT-IR spectra before and after the reaction were compared. The hydrogen ion-type alginic acid before the reaction had a peak at 1740 cm -1 The stretching vibration absorption of the carbonyl group of the carboxylic acid was observed at 1740 cm -1 The absorption at 1630cm -1 New absorption derived from the stretching vibration of the carbonyl group of the carboxylate was observed at 147°, which showed that alginic acid and AMP were bonded via ionic bonds.
[0481] The molecular weight of the chelate polymer was measured by aqueous GPC and the weight average molecular weight was 300,000.
[0482] <Evaluation of heavy metal ion capture ability>
[0483] The heavy metal ion capturing ability of the chelate polymer produced in Example 1-4 was evaluated by the same method as in Example 1-1. The manganese ion concentration in the filtrate was less than 1 ppm, and it was confirmed that the manganese ions eluted from the LMO by heating were captured by the chelate polymer.
[0484] (Examples 1-5)
[0485] Use 2.6ml (5.7mmol) of 50% aqueous solution of nitrilotri(methylphosphonic acid) (Tokyo Chemical Industry, hereinafter referred to as "NTMP") and 1.37g (34.2mmol) of sodium hydroxide (Tokyo Chemical Industry) to replace BAPTA and sodium hydroxide, in addition, manufacture chelated polymer by the same operation as Example 1-1. The separation yield is 3.3g, and the nitrogen content tried to be achieved by elemental analysis is 1.8% by mass %, and the chelate functional group content calculated according to the nitrogen content is 1.3mmol / g, which is soluble in water.
[0486] In order to confirm that the chelating functional groups were introduced into the alginic acid, the FT-IR spectra before and after the reaction were compared. The hydrogen ion-type alginic acid before the reaction had a peak at 1740 cm -1 The stretching vibration absorption of the carbonyl group of the carboxylic acid was observed at 1740 cm -1 The absorption at 1640cm -1 New absorption derived from the stretching vibration of the carbonyl group of the carboxylate was observed at 140°C, which showed that alginic acid and NTMP were bonded via ionic bonds.
[0487] The molecular weight of the chelate polymer was measured by aqueous GPC and the weight average molecular weight was 350,000.
[0488] <Evaluation of heavy metal ion capture ability>
[0489] The heavy metal ion capturing ability of the chelate polymer produced in Example 1-5 was evaluated by the same method as in Example 1-1. The manganese ion concentration in the filtrate was less than 1 ppm, and it was confirmed that the manganese ions eluted from the LMO by heating were captured by the chelate polymer.
[0490] (Examples 1-6)
[0491] 1.5 g of sulfated alginic acid (5.7 mmol of monosaccharide unit) prepared in Reference Example 1-1 was used to replace hydrogen ion type alginic acid; 2.2 g (11.4 mmol) of disodium iminodiacetic acid monohydrate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was used to replace BAPTA and sodium hydroxide. In addition, the chelate polymer was prepared by the same operation as in Example 1-1. The separation yield was 3.0 g, the nitrogen content obtained by elemental analysis was 5.4% by mass, and the chelate functional group content calculated based on the nitrogen content was 3.9 mmol / g, and it was easily soluble in water.
[0492] In order to confirm that the chelating functional groups were introduced into the alginic acid, the FT-IR spectra before and after the reaction were compared. -1 The stretching vibration absorption of the carbonyl group of the carboxylic acid was observed at 1730 cm -1 The absorption at 1620cm -1 New absorption derived from stretching vibration of the carbonyl group of the carboxylate was observed at 40°C, which showed that the sulfated alginic acid and iminodiacetic acid were bonded via ionic bonds.
[0493] The molecular weight of the chelate polymer was measured by aqueous GPC and the weight average molecular weight was 88,000.
[0494] <Evaluation of heavy metal ion capture ability>
[0495] The heavy metal ion capturing ability of the chelate polymer produced in Example 1-6 was evaluated by the same method as in Example 1-1. The manganese ion concentration in the filtrate was less than 1 ppm, and it was confirmed that the manganese ions eluted from the LMO by heating were captured by the chelate polymer.
[0496] (Examples 1-7)
[0497] 1.0 g (carboxyl group: 13.9 mmol) of polyacrylic acid (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., average molecular weight: 1,000,000) was used to replace hydrogen ion type alginic acid; 2.7 g (14 mmol) of disodium iminodiacetic acid monohydrate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was used to replace BAPTA and sodium hydroxide. The chelate polymer was manufactured by the same operation as in Example 1-1. The separation yield was 2.6 g, the nitrogen content obtained by elemental analysis was 6.1% by mass, and the chelate functional group content calculated based on the nitrogen content was 4.4 mmol / g, and it was easily soluble in water.
[0498] In order to confirm that the chelating functional group was introduced into the polyacrylic acid, the FT-IR spectra before and after the reaction were compared. -1 The stretching vibration absorption of the carbonyl group of the carboxylic acid was observed at 1710 cm -1 The absorption at 1570cm -1 New absorption derived from stretching vibration of the carbonyl group of the carboxylate was observed at 40°C. This shows that polyacrylic acid and iminodiacetic acid are bonded via ionic bonds.
[0499] The molecular weight of the chelate polymer was measured by aqueous GPC and the weight average molecular weight was 340,000.
[0500] <Evaluation of heavy metal ion capture ability>
[0501] The heavy metal ion capturing ability of the chelate polymer produced in Example 1-7 was evaluated by the same method as in Example 1-1. The concentration of manganese ions in the filtrate was less than 1 ppm, and it was confirmed that the manganese ions eluted from the LMO by heating were captured by the chelate polymer.
[0502] (Example 1-8)
[0503] 300 ml of n-decane (manufactured by Fujifilm Wako Pure Chemicals) was placed in a 1L separable flask equipped with a full zone stirring blade, and 37.1 g of sorbitan monooleate (manufactured by Fujifilm Wako Pure Chemicals) was added and dissolved under stirring, and the system was cooled to 5°C. Next, 60 g (monosaccharide unit is 341 mmol) of hydrogen ion type alginic acid (manufactured by KIMICA Co., Ltd., trade name KIMICA ACID SA) was gradually added in small amounts under stirring to prepare a light brown uniform dispersion. On the other hand, 79.0 g (375 mmol) of disodium iminodiacetic acid hydrate (manufactured by Tokyo Chemical Industry) was dissolved in 220 ml of pure water and slowly added dropwise to the above alginic acid dispersion over 1 hour. The dispersion formed a w / o emulsion as the dropwise addition was performed, and it became a light brown milky state when the dropwise addition was completed. After stirring the aqueous solution at 5°C for 1 hour, 4 L of acetone was added dropwise to generate a precipitate. The precipitate obtained was recovered by filtration, washed with acetone, and then separated by drying under reduced pressure. The isolated yield was 130.2 g. The nitrogen content determined by elemental analysis was 4.2% by mass. The chelating functional group content calculated from the nitrogen content was 3.0 mmol / g. The product was easily soluble in water.
[0504] In order to confirm that the chelating functional groups were introduced into the alginic acid, the FT-IR spectra before and after the reaction were compared. The hydrogen ion-type alginic acid before the reaction had a peak at 1740 cm -1 The stretching vibration absorption of the carbonyl group of the carboxylic acid was observed at 1740 cm -1 The absorption at 1620cm -1 New absorption derived from stretching vibration of the carbonyl group of carboxylate was observed at 40°C, which showed that alginic acid and disodium iminodiacetic acid were bonded via ionic bonds.
[0505] The molecular weight of the chelate polymer was measured by aqueous GPC and the weight average molecular weight was 160,000.
[0506] <Evaluation of heavy metal ion capture ability>
[0507] The heavy metal ion capturing ability of the chelate polymer produced in Example 1-8 was evaluated by the same method as in Example 1-1. The concentration of manganese ions in the filtrate was less than 1 ppm, and it was confirmed that the manganese ions eluted from the LMO by heating were captured by the chelate polymer.
[0508] (Examples 1-9)
[0509] Soybean oil (Fuji Film Wako Pure Chemicals) 300ml was used to replace n-decane; sorbitan monooleate was not used, except that the chelated polymer was manufactured by the same operation as in Example 1-8. The separation yield was 138.4g, and the nitrogen content obtained by elemental analysis was 3.3% by mass %, and the chelate functional group content calculated according to the nitrogen content was 2.4mmol / g, which was soluble in water.
[0510] In order to confirm that the chelating functional groups were introduced into the alginic acid, the FT-IR spectra before and after the reaction were compared. The hydrogen ion-type alginic acid before the reaction had a peak at 1740 cm -1 The stretching vibration absorption of the carbonyl group of the carboxylic acid was observed at 1740 cm -1 The absorption at 1620cm -1 New absorption derived from stretching vibration of the carbonyl group of carboxylate was observed at 40°C, which showed that alginic acid and disodium iminodiacetic acid were bonded via ionic bonds.
[0511] The molecular weight of the chelate polymer was measured by aqueous GPC and the weight average molecular weight was 160,000.
[0512] <Evaluation of heavy metal ion capture ability>
[0513] The heavy metal ion capturing ability of the chelate polymer produced in Example 1-9 was evaluated by the same method as in Example 1-1. The concentration of manganese ions in the filtrate was less than 1 ppm, and it was confirmed that the manganese ions eluted from the LMO by heating were captured by the chelate polymer.
[0514] (Examples 1-10)
[0515] The addition amount of hydrogen ion type alginic acid was set to 30g (monosaccharide unit was 171mmol); 71.1g (171mmol) of tetrasodium ethylenediaminetetraacetic acid dihydrate (manufactured by Tokyo Chemical Industry) was used to replace disodium iminodiacetic acid, and in addition, the chelated polymer was manufactured by the same operation as in Example 1-8. The separation yield was 95.0g, and the nitrogen content obtained by elemental analysis was 5.0% by mass %, and the chelate functional group content calculated according to the nitrogen content was 3.5mmol / g, and it was easily soluble in water.
[0516] In order to confirm that the chelating functional groups were introduced into the alginic acid, the FT-IR spectra before and after the reaction were compared. The hydrogen ion-type alginic acid before the reaction had a peak at 1740 cm -1 The stretching vibration absorption of the carbonyl group of the carboxylic acid was observed at 1740 cm -1 The absorption at 1600 cm -1 New absorption derived from the stretching vibration of the carbonyl group of the carboxylate was observed at 140°C, which showed that alginic acid and EDTA were bonded via ionic bonds.
[0517] The molecular weight of the chelate polymer was measured by aqueous GPC and the weight average molecular weight was 180,000.
[0518] <Evaluation of heavy metal ion capture ability>
[0519] The heavy metal ion capturing ability of the chelate polymer produced in Example 1-10 was evaluated by the same method as in Example 1-1. The concentration of manganese ions in the filtrate was less than 1 ppm, and it was confirmed that the manganese ions eluted from the LMO by heating were captured by the chelate polymer.
[0520] (Example 1-11)
[0521] The amount of hydrogen ion type alginic acid added was set to 30g (monosaccharide unit was 171mmol); 300ml of hexadecane (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was used instead of n-decane; 100.5g (171mmol) of 50% aqueous solution of NTMP (manufactured by Tokyo Chemical Industry Co., Ltd.) and 109.0g (1363mmol) of 50% aqueous solution of sodium hydroxide (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) were used instead of disodium iminodiacetic acid aqueous solution; the reaction temperature was set to 20°C. In addition, the chelate polymer was manufactured by the same operation as in Example 1-8. The separation yield was 118.3g, the nitrogen content obtained by elemental analysis was 2.3% by mass, and the chelate functional group content calculated based on the nitrogen content was 1.6mmol / g, and it was easily soluble in water.
[0522] In order to confirm that the chelating functional groups were introduced into the alginic acid, the FT-IR spectra before and after the reaction were compared. The hydrogen ion-type alginic acid before the reaction had a peak at 1740 cm -1 The stretching vibration absorption of the carbonyl group of the carboxylic acid was observed at 1740 cm -1 The absorption at 1640cm -1 New absorption derived from the stretching vibration of the carbonyl group of the carboxylate was observed at 140°C, which showed that alginic acid and NTMP were bonded via ionic bonds.
[0523] The molecular weight of the chelate polymer was measured by aqueous GPC and the weight average molecular weight was 180,000.
[0524] <Evaluation of heavy metal ion capture ability>
[0525] The heavy metal ion capturing ability of the chelate polymer produced in Example 1-11 was evaluated by the same method as in Example 1-1. The manganese ion concentration in the filtrate was less than 1 ppm, and it was confirmed that the manganese ions eluted from the LMO by heating were captured by the chelate polymer.
[0526] (Comparative Example 1-1)
[0527] <Evaluation of heavy metal ion capture ability>
[0528] The elution behavior of manganese ions was evaluated using only LMO without using a chelating polymer under the same conditions as in Example 1-1. The concentration of manganese ions in the filtrate was 15 ppm, which was a higher value than that in the example.
[0529] (Comparative Example 1-2)
[0530] Sodium alginate (KIMICA Co., Ltd., trade name ALGITEX LL) 1.0g (monosaccharide unit is 5.0mmol) is used to replace hydrogen ion type alginic acid; iminodiacetic acid (Tokyo Chemical Industry) 1.5g (11.4mmol) is used to replace BAPTA and sodium hydroxide. In addition, the chelated polymer is manufactured by the same operation as Example 1-1. The separation yield is 2.0g, and the nitrogen content obtained by elemental analysis is 2.9% by mass, and the chelated functional group content calculated according to the nitrogen content is 2.1mmol / g, which is a value lower than that of the embodiment. It can be considered that since the anionic polymer used is a sodium salt, an ionic bond cannot be formed between the anionic polymer and the chelated compound, and the chelated functional group content in the product is reduced. In addition, the weight average molecular weight obtained by GPC measurement is 300,000.
[0531] <Evaluation of heavy metal ion capture ability>
[0532] The heavy metal ion capturing ability of the product obtained in Comparative Example 1-2 was evaluated by the same method as Example 1-1. The manganese ion concentration in the filtrate was 12 ppm, which was higher than that of the Example. The manganese ion capturing ability of the product of Comparative Example 1-2 was lower than that of the chelating polymer of the Example.
[0533] (Comparative Examples 1-3)
[0534] <Evaluation of heavy metal ion capture ability>
[0535] The heavy metal ion capture ability of sodium alginate alone in Comparative Example 1-2 was evaluated by the same method as in Example 1-1. The concentration of manganese ions in the filtrate was 14 ppm, which was a higher value than that in Example 1-1. It can be seen that the manganese ion capture ability of sodium alginate alone was lower than that of the chelating polymer in Example 1-2.
[0536] (Comparative Examples 1-4)
[0537] <Evaluation of heavy metal ion capture ability>
[0538] The heavy metal ion capture ability of the sulfated alginic acid alone produced in Reference Example 1-1 was evaluated by the same method as in Example 1-1. The concentration of manganese ions in the filtrate was 11 ppm, which was a higher value than that of the Example. It can be seen that the manganese ion capture ability of the sulfated alginic acid alone was lower than that of the chelating polymer in the Example.
[0539] (Example of the second aspect of the present invention)
[0540] (Example 2-1)
[0541] <Production of Chelate Polymer (I)>
[0542] [Chemical formula 12]
[0543]
[0544] Under stirring, 0.50 g (monosaccharide unit is 2.5 mmol) of sodium alginate (manufactured by Qingdao Polyocean Algae Group Co., Ltd., weight average molecular weight 1,300,000) was gradually added to 50 ml of pure water in small amounts to make a viscous uniform solution. Next, 0.10 g (2.5 mmol) of sodium hydroxide (manufactured by Tokyo Chemical Industry) was added to dissolve it, and then 3.10 g (50 mmol) of epichlorohydrin (manufactured by Tokyo Chemical Industry) was added, and the mixture was reacted at 20°C for 6 hours. The reacted solution was added dropwise to 2 L of ethanol to form a precipitate, which was recovered by filtration, washed with ethanol, and separated by vacuum drying. The separation yield was 0.43 g, which was easily soluble in water. 0.30 g of the above reaction product was weighed and dissolved in 100 ml of pure water. Next, 8.4 g (43 mmol) of disodium iminodiacetic acid monohydrate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was added to dissolve it, and the mixture was reacted at 80°C for 2 hours. The aqueous solution after the reaction was purified by ultrafiltration membrane (manufactured by Pall, Japan, molecular weight cutoff 1000) to remove excess iminodiacetic acid. The purified aqueous solution was added dropwise to acetone to precipitate the polymer, which was filtered, recovered, and separated by drying under reduced pressure. The separation yield was 0.33 g, which was soluble in water and had a weight average molecular weight of 370,000 as measured by aqueous GPC. The nitrogen content was 2.2% by weight, and the iminodiacetic acid group content calculated based on the nitrogen content was 1.6 mmol / g.
[0545] <Evaluation of heavy metal ion capture ability>
[0546] In order to evaluate the heavy metal ion capture ability of the chelate polymer, the following determination was performed. 0.1 g of the above-mentioned chelate polymer was dissolved in 20 ml of pure water, and 1.9 g of lithium manganate (trial production of our company, hereinafter referred to as "LMO") was added to prepare a slurry. After the obtained slurry was concentrated with an evaporator, it was dried under reduced pressure at 80 ° C to remove water to obtain a mixture of the chelate polymer and LMO. 1.0 g was taken from the above mixture, put into a TEFLON (registered trademark) container, and sealed after drying under reduced pressure at 120 ° C for 4 hours. The sealed TEFLON (registered trademark) container was opened in a glove box, and an electrolyte (Kishida Chemical, a solution obtained by dissolving 1 mol / L of LiPF6 in a mixed solvent of ethylene carbonate: dimethyl carbonate = 1:2) was added. After 15 ml, it was sealed again and heated at 85 ° C for 4 hours. After the heating was completed, the TEFLON (registered trademark) container was opened in the glove box, filtered using a syringe filter, and the filtrate was collected. The obtained filtrate was subjected to acid decomposition, and manganese ions were quantified by ICP-MS. As a result, the concentration of manganese ions was less than 1 ppm, confirming that the manganese ions eluted from the LMO by heating were captured by the chelate polymer.
[0547] (Example 2-2)
[0548] <Production of Chelate Polymer (II)>
[0549] [Chemical formula 13]
[0550]
[0551] Under stirring, 2.25 g (monosaccharide unit: 12.7 mmol) of hydrogen ion alginic acid (KIMICA ACID G, manufactured by KIMICA Co., Ltd.) was gradually added in small amounts to 150 ml of pure water to prepare a white dispersion. Next, 4.86 g (34.2 mmol) of glycidyl methacrylate (manufactured by Tokyo Chemical Industry) was added and uniformly dispersed, and then 0.16 g (0.3 mmol) of ammonium cerium (IV) nitrate (manufactured by Aldrich) was added and polymerized at 55°C for 5 hours. The solution after polymerization was added dropwise to 2 L of methanol to generate a precipitate, which was recovered by filtration, washed with methanol, and separated by vacuum drying. The separation yield was 7.15 g, and the yield was 100% by weight. 2.25 g of the graft polymer thus obtained was dispersed in 40 ml of a dioxane / water (4 / 6) mixed solvent, and 16.8 g (86 mmol) of disodium iminodiacetic acid monohydrate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was added, and the temperature was raised to 80°C and reacted for 6 hours. After the reaction, dioxane was evaporated and pure water was added to make the volume 250 ml. After adjusting the pH to 3, the mixture was stirred at room temperature for 48 hours. At the end of the reaction, the polymer became insoluble in water, so it was recovered by filtration, washed with water and methanol in turn, and dried under reduced pressure. The yield was 3.1 g, and the chelating functional group content calculated based on the nitrogen content was 2.2 mmol / g. When comparing the IR spectra before and after the reaction, the reaction with disodium iminodiacetic acid resulted in a peak at 1260 cm -1 The absorption of the epoxy group at 1600 cm -1 The carbonyl absorption derived from disodium iminodiacetic acid increased, thereby confirming the progress of the reaction.
[0552] <Evaluation of heavy metal ion capture ability>
[0553] The heavy metal ion capture ability was evaluated by the same method as in Example 2-1 using 0.1 g of the chelate polymer pulverized product (D50 = 2.9 μm) produced in Example 2-2 instead of 0.1 g of the chelate polymer produced in Example 2-1. The concentration of manganese ions in the filtrate was less than 1 ppm, confirming that the manganese ions dissolved from the LMO due to heating were captured by the chelate polymer.
[0554] (Example 2-3)
[0555] <Production of Chelate Polymer (I)>
[0556] [Chemical formula 14]
[0557]
[0558] Under stirring, 5.0 g (monosaccharide unit is 22 mmol) of chitosan (Aldrich, weight average molecular weight 350,000) is gradually added in small amounts to a mixed solvent of 50 ml of pure water and 50 ml of ethanol to prepare a dispersion. Next, 10.0 g (164 mmol) of epichlorohydrin (Tokyo Chemical) is added, heated and reacted under reflux for 2 hours. After the reaction, the dispersion is added dropwise to 2 L of ethanol, stirred, and the precipitate is recovered by filtration, then washed with ethanol and dried under reduced pressure. The separation yield is 6.2 g. 0.8 g of the above reaction product is weighed and dispersed in 100 ml of pure water. Next, 16.8 g (86 mmol) of disodium iminodiacetic acid monohydrate (Fujifilm Wako Pure Chemical Industries, Ltd.) is added and reacted at 80°C for 6 hours. The dispersion after the reaction is filtered, washed with pure water, and separated by drying under reduced pressure. The isolated yield was 0.9 g, which was insoluble in water and had a nitrogen content of 6.1% by weight. The iminodiacetic acid group content calculated from the nitrogen content was 4.4 mmol / g.
[0559] <Evaluation of heavy metal ion capture ability>
[0560] The chelate polymer powder (D50 = 3.6 μm) 0.1 g and sodium alginate (manufactured by Qingdao Poly Ocean Algae Group Co., Ltd., weight average molecular weight 1,300,000) 0.1 g prepared in Example 2-3 were used to replace the chelate polymer 0.1 g prepared in Example 2-1; the amount of LMO added was changed from 1.9 g to 1.8 g, and the heavy metal ion capture ability was evaluated by the same method as in Example 2-1. The concentration of manganese ions in the filtrate was less than 1 ppm, confirming that the manganese ions dissolved from the LMO due to heating were captured by the chelate polymer.
[0561] (Example 2-4)
[0562] <Production of Chelate Polymer (I)>
[0563] [Chemical formula 55]
[0564]
[0565] 28.6 g (164 mmol) of ethylene glycol diglycidyl ether (produced by Tokyo Chemical Industry) was used instead of epichlorohydrin, and the same operation reaction as in Example 2-3 was carried out. The yield of the epoxy-modified chitosan obtained was 8.0 g. 0.8 g of the above epoxy-modified chitosan was used to react with sodium iminodiacetate by the same operation as in Example 2-3. The separation yield was 0.9 g, insoluble in water, and the nitrogen content was 2.8% by weight. The iminodiacetate content calculated based on the nitrogen content was 2.2 mmol / g. The nitrogen content obtained by elemental analysis was 2.8% by mass, and the chelating functional group content calculated based on the nitrogen content was 2.0 mmol / g, and it was insoluble in water.
[0566] <Evaluation of heavy metal ion capture ability>
[0567] The chelate polymer pulverized product (D50=5.6 μm) 0.1 g manufactured in Example 2-4 was used to replace the chelate polymer pulverized product manufactured in Example 2-3. In addition, the heavy metal ion capture ability was evaluated by the same method as in Example 2-3. The concentration of manganese ions in the filtrate was 3 ppm, confirming that the manganese ions dissolved from LMO due to heating were captured by the chelate polymer.
[0568] (Comparative Example 2-1)
[0569] <Evaluation of heavy metal ion capture ability>
[0570] The elution behavior of manganese ions was evaluated using only LMO without using a chelating polymer under the same conditions as in Example 2-1. The concentration of manganese ions in the filtrate was 15 ppm, which was a higher value than that in the example.
[0571] (Comparative Example 2-2)
[0572] <Evaluation of heavy metal ion capture ability>
[0573] The elution behavior of manganese ions was evaluated by the same method as in Example 2-1 except that 0.1 g of sodium alginate (manufactured by Qingdao Poly Ocean Algae Industry Group Co., Ltd., weight average molecular weight 1,300,000) was used instead of the chelate polymer manufactured in Example 2-1. The concentration of manganese ions in the filtrate was 14 ppm, which was a higher value than that in Example 2-1.
[0574] (Example of the third aspect of the present invention)
[0575] <Production of water-insoluble polymer compound microparticles containing chelate groups>
[0576] (Reference Example 3-1) Introduction of chelating groups into alginate graft polymer and its pulverization
[0577] Under stirring, 2.25 g (monosaccharide unit is 12.7 mmol) of acid-type alginic acid (manufactured by KIMICA Co., Ltd., trade name KIMICA ACID G) was gradually added in small amounts to 150 ml of pure water to make it uniformly dispersed. Next, 4.86 g (34.2 mmol) of glycidyl methacrylate (manufactured by Tokyo Chemical Industry) was added under stirring, and stirring was continued overnight under a nitrogen flow. Next, 0.162 g (0.297 mmol) of ammonium cerium (IV) nitrate (manufactured by Aldrich) was dissolved in 7.5 ml of 1 mol / L nitric acid (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.), and added to the above-mentioned aqueous dispersion via a syringe. After the addition, the system was heated and polymerized at 55°C for 5 hours. After the polymerization was completed, the obtained emulsion was added dropwise to methanol, and the precipitated product was captured with a glass filter, washed with methanol, and then dried under reduced pressure at 40°C to separate the grafted polymer. The yield was 7.15 g, and the yield was 100%. Next, 6.0 g of the obtained graft polymer was dispersed in a mixed solvent consisting of 180 ml of pure water and 120 ml of dioxane, 50.4 g (258 mmol) of disodium iminodiacetic acid monohydrate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was added, the temperature was raised, and the mixture was reacted at 80°C for 6 hours. After the reaction was completed, dioxane was removed from the obtained dispersion by evaporation, 300 ml of pure water was added, the pH was adjusted to 3 with sulfuric acid, and then stirred at room temperature for 48 hours. After the stirring was completed, lithium hydroxide (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was added to adjust the pH to 7, the dispersion was filtered, and the solid was recovered. The recovered solid was washed with ethanol and separated by drying under reduced pressure. The yield was 9.3 g, and the amount of iminodiacetic acid group introduced was 2.2 mmol / g calculated from the nitrogen content. The obtained alginic acid graft polymer with iminodiacetic acid group introduced was pulverized using a jet mill (Nano Jetmizer NJ-50C model manufactured by Aisin Nano Technology). The median diameter after crushing was 2.9 μm.
[0578] (Reference Example 3-2) Introduction of chelating groups into chitosan and its pulverization
[0579] 5.0 g of chitosan (manufactured by Aldrich, deacetylation rate of 75% or more, molecular weight 300,000) was dispersed in a mixed solvent of 50 ml of pure water and 50 ml of ethanol, and 10.0 g (164 mmol) of epichlorohydrin (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was added and heated, and the mixture was reacted under reflux for 2 hours. The obtained emulsion was added dropwise to ethanol, and the precipitate was recovered, washed with ethanol, and dried under reduced pressure. The yield of the product was 6.2 g, and the yield was 89%. 4.8 g of the product was separated and dispersed in 600 ml of pure water. 100.8 g (516 mmol) of disodium iminodiacetic acid monohydrate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was added, the temperature was raised, and the mixture was reacted at 80°C for 6 hours. After the reaction was completed, the solid was recovered by filtration, washed with pure water, and separated by drying under reduced pressure. The yield was 5.5 g, and the amount of iminodiacetic acid group introduced calculated from the nitrogen content was 4.4 mmol / g. The obtained chitosan into which iminodiacetic acid groups were introduced was pulverized using a jet mill (Nano Jetmizer NJ-50C manufactured by Aisin NanoTechnology). The median diameter after pulverization was 4.8 μm.
[0580] (Reference Example 3-3) Pulverization of cellulose having iminodiacetate groups introduced therein
[0581] After drying under reduced pressure, Chelist Fiber IRY-HW (manufactured by Chelist Co., Ltd.), which is cellulose into which iminodiacetate groups are introduced, was measured for nitrogen content, and the amount of iminodiacetate groups introduced was calculated. The amount of iminodiacetate groups introduced was 2.1 mmol / g. The obtained cellulose into which iminodiacetate groups are introduced was pulverized using a jet mill (Nano Jetmizer NJ-50C manufactured by Aisin Nano Technology). The median diameter after pulverization was 2.1 μm.
[0582] <Production of organic solvent-insoluble polymer compound microparticles containing a chelate group>
[0583] (Reference Example 3-4) Preparation of sodium alginate having chelating groups introduced therein and its pulverization
[0584] Under stirring, 10.0 g (monosaccharide unit is 50 mmol) of sodium alginate (manufactured by Qingdao Polyocean Algae Group Co., Ltd., weight average molecular weight 1,300,000) was gradually added to 1000 ml of pure water in small amounts to make a viscous uniform solution. Next, 2.0 g (50 mmol) of sodium hydroxide (manufactured by Tokyo Chemical Industry) was added and dissolved, and then 62.0 g (1.0 mol) of epichlorohydrin (manufactured by Tokyo Chemical Industry) was added, and the mixture was reacted at 20°C for 6 hours. The reacted solution was added dropwise to 4 L of ethanol to form a precipitate, which was recovered by filtration, washed with ethanol, and separated by vacuum drying. The separation yield was 8.6 g, which was easily soluble in water. 6.0 g of the above reaction product was weighed and dissolved in 600 ml of pure water. Next, 168 g (860 mmol) of disodium iminodiacetic acid monohydrate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was added and dissolved, and the mixture was reacted at 80°C for 2 hours. The aqueous solution after the reaction was purified by ultrafiltration membrane (made by Pall, Japan, molecular weight cutoff 1000) to remove excess disodium iminodiacetic acid. The purified aqueous solution was added dropwise to acetone to precipitate the polymer, filtered, recovered, and separated by drying under reduced pressure. The separation yield was 6.6 g, which was soluble in water, and the weight average molecular weight measured by aqueous GPC was 370,000. The nitrogen content was 2.2% by weight, and the iminodiacetic acid content calculated based on the nitrogen content was 1.6 mmol / g. The obtained sodium alginate introduced with iminodiacetic acid groups was crushed using a jet mill (Nano Jetmizer NJ-50C made by Aisin Nano Technology). The median diameter after crushing was 4.2 μm.
[0585] (Reference Example 3-5) Preparation and pulverization of a sodium alginate / disodium iminodiacetic acid mixture
[0586] Under stirring, 10 g (monosaccharide unit is 50 mmol) of sodium alginate (manufactured by KIMICA Co., Ltd., trade name ALGITEX L) was gradually added to 500 ml of pure water in small amounts to obtain a viscous uniform solution. Next, 9.8 g (50 mmol) of disodium iminodiacetic acid monohydrate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was added to the above-mentioned sodium alginate aqueous solution to dissolve it and prepare a uniform solution. After the aqueous solution was stirred at room temperature for 1 hour, it was added dropwise to 4 L of acetone to generate a precipitate. The obtained precipitate was recovered by filtration, washed with acetone, and separated by drying under reduced pressure. The separation yield was 17.5 g, and the nitrogen content obtained by elemental analysis was 4.1% by mass. The chelating functional group content calculated based on the nitrogen content was 2.9 mmol / g, which was easily soluble in water. The obtained sodium alginate / disodium iminodiacetic acid mixture was crushed using an air flow mill (Nano Jetmizer NJ-50C manufactured by Aisin Nano Technology). The median diameter after crushing was 3.7 μm.
[0587] <Manufacturing of laminated batteries>
[0588] (Example 3-1)
[0589] A positive electrode slurry was prepared from the following materials to produce a positive electrode.
[0590] Positive electrode active material: lithium manganese oxide (LMO: trial production by our company, LiMn2 O4) 91 parts by mass
[0591] Conductive aid: 3 parts by mass of acetylene black (AB: Li-400 manufactured by Denka Corporation)
[0592] Water-insoluble polymer compound microparticles containing chelating groups: 3 parts by mass of an alginate graft polymer into which iminodiacetic acid groups have been introduced (Reference Example 3-1)
[0593] Binder: Sodium alginate (ALGITEX L manufactured by KIMICA Co., Ltd.) 3 parts by mass
[0594] Dissolve 3 parts by mass of sodium alginate in water to prepare an aqueous solution. Add 91 parts by mass of LMO, 3 parts by mass of AB and the alginate graft polymer with iminodiacetic acid groups introduced in Reference Example 3-1 to the aqueous solution, add water while stirring with a planetary mixer to prepare a positive electrode slurry. Apply the slurry on aluminum foil with a coater, dry at 80°C and nitrogen under normal pressure for 24 hours, and then dry under reduced pressure at 120°C for 4 hours, roll-press, and make a positive electrode. The capacity per unit area is 1.45 mAh / cm 2 .
[0595] Next, a negative electrode slurry was prepared from the following materials to produce a negative electrode.
[0596] Negative electrode active material: 95 parts by mass of blocky artificial graphite (Gr: MAG-D manufactured by Showa Denko Materials Co., Ltd.)
[0597] Binder: 5 parts by mass of polyvinylidene fluoride (PVDF: Solef 5130 manufactured by Solvay)
[0598] 5 parts by mass of the above PVDF were dissolved in N-methyl-2-pyrrolidone (NMP), 95 parts by mass of Gr were added to the solution, and NMP was added while stirring with a planetary mixer to prepare a negative electrode slurry. The slurry was coated on a copper foil with a film applicator, dried at 80°C under nitrogen for 24 hours, and then dried under reduced pressure at 150°C for 4 hours, and rolled to make a negative electrode. The capacity per unit area is 1.74 mAh / cm 2 , the AC ratio is 1.20.
[0599] Using the positive electrode and negative electrode obtained as above, a laminated battery is made as follows. That is, vinylene carbonate is added to a mixed solvent of ethylene carbonate / diethyl carbonate (1 / 1) to make it 1% by mass, and then, lithium hexafluorophosphate is dissolved to make it 1 mol / L to make an electrolyte. The diaphragm uses a polyethylene microporous film (Senior system) coated with aluminum oxide on one side. Then, the above-mentioned positive electrode and negative electrode are stacked on both sides of the diaphragm, and the electrolyte is injected to make a laminated battery.
[0600] (Example 3-2)
[0601] A positive electrode slurry was prepared from the following materials, and a positive electrode was produced by the same method as in Example 3-1.
[0602] Positive electrode active material: lithium manganese oxide (LMO: trial production by our company, LiMn2 O4) 94 parts by mass
[0603] Conductive aid: 3 parts by mass of acetylene black (AB: Li-400 manufactured by Denka Corporation)
[0604] Binder: Sodium alginate (ALGITEX L manufactured by KIMICA Co., Ltd.) 3 parts by mass
[0605] The capacity per unit area is 1.50 mAh / cm 2 .
[0606] Next, a negative electrode slurry was prepared from the following materials to produce a negative electrode.
[0607] Negative electrode active material: 94 parts by mass of blocky artificial graphite (Gr: MAG-D manufactured by Showa Denko Materials Co., Ltd.)
[0608] Water-insoluble polymer compound microparticles containing chelating groups: 3 parts by mass of an alginate graft polymer into which iminodiacetic acid groups have been introduced (Reference Example 3-1)
[0609] Binder: Sodium alginate (ALGITEX L manufactured by KIMICA Corporation) 1.5 parts by mass
[0610] Binder: 1.5 parts by mass of styrene-butadiene rubber (SBR: TRD2001 manufactured by JSR)
[0611] 1.5 parts by mass of the above sodium alginate was dissolved in water to prepare an aqueous solution. 94 parts by mass of Gr, 3 parts by mass of the alginate graft polymer with iminodiacetic acid groups introduced in Reference Example 3-1, and 1.5 parts by mass of SBR were added to the aqueous solution, and water was added while stirring with a planetary mixer to prepare a negative electrode slurry. The negative electrode was prepared using the same method as in Example 3-1 using the slurry. The capacity per unit area was 1.80 mAh / cm 2, AC ratio was 1.20. Using the positive electrode and negative electrode obtained as above, a laminated battery was prepared in the same manner as in Example 3-1.
[0612] (Example 3-3)
[0613] The positive electrode and the negative electrode were prepared by the same operation as in Example 3-2 except that the chitosan introduced with iminodiacetic acid groups prepared in Reference Example 3-2 was added to the negative electrode instead of the alginate graft polymer introduced with iminodiacetic acid groups prepared in Reference Example 3-1. The capacity per unit area of the positive electrode was 1.50 mAh / cm 2 The unit area capacity of the negative electrode is 1.80 mAh / cm 2 , AC ratio was 1.20. Using the positive electrode and negative electrode obtained as above, a laminated battery was prepared in the same manner as in Example 3-1.
[0614] (Example 3-4)
[0615] The positive electrode and negative electrode were prepared by the same operation as in Example 3-1, except that the cellulose with iminodiacetate groups introduced in Reference Example 3-3 was added to the positive electrode instead of the alginate graft polymer with iminodiacetate groups introduced in Reference Example 3-1. The capacity per unit area of the positive electrode was 1.48 mAh / cm 2 The unit area capacity of the negative electrode is 1.74 mAh / cm 2 , AC ratio was 1.18. Using the positive electrode and negative electrode obtained as above, a laminated battery was prepared in the same manner as in Example 3-1.
[0616] (Example 3-5)
[0617] A laminated battery was prepared by the same method as in Example 3-1 using the positive electrode prepared in Example 3-1 and the negative electrode prepared in Example 3-2. The unit area capacity of the positive electrode was 1.45 mAh / cm 2 The unit area capacity of the negative electrode is 1.80 mAh / cm 2 , AC ratio was 1.24. Using the positive electrode and negative electrode obtained as above, a laminated battery was prepared in the same manner as in Example 3-1.
[0618] (Example 3-6)
[0619] A positive electrode slurry was prepared from the following materials to produce a positive electrode.
[0620] Positive electrode active material: lithium manganese oxide (LMO: our company's trial production LiMn2 O4) 91 parts by mass
[0621] Organic solvent-insoluble polymer compound microparticles containing a chelating group: 3 parts by mass of an alginate graft polymer into which iminodiacetic acid groups have been introduced (Reference Example 3-1)
[0622] Conductive aid: 3 parts by mass of acetylene black (AB: Li-400 manufactured by Denka Corporation)
[0623] Binder: 3 parts by mass of polyvinylidene fluoride (PVDF: Solef 5130 manufactured by Solvay)
[0624] 3 parts by mass of the above PVDF were dissolved in N-methyl-2-pyrrolidone (NMP), and 91 parts by mass of LMO, 3 parts by mass of alginate graft polymer introduced with iminodiacetic acid groups produced in Reference Example 3-1, and 3 parts by mass of AB were added to the solution. While adding NMP, stirring was performed with a planetary mixer to prepare a slurry for the positive electrode. The slurry was applied on an aluminum foil with a coater, dried at 80°C under nitrogen at normal pressure for 24 hours, and then dried under reduced pressure at 150°C for 4 hours, and roll-pressed to prepare a positive electrode. On the other hand, a negative electrode was prepared by the same operation as in Example 3-1. The capacity per unit area of the positive electrode is 1.45 mAh / cm 2 The unit area capacity of the negative electrode is 1.74 mAh / cm 2 , AC ratio was 1.20. Using the positive electrode and negative electrode obtained as above, a laminated battery was prepared in the same manner as in Example 3-1.
[0625] (Example 3-7)
[0626] The positive electrode and negative electrode were prepared by the same operation as in Example 3-6 except that the sodium alginate with chelating groups introduced in Reference Example 3-4 was added to the positive electrode instead of the alginate graft polymer with iminodiacetic acid groups introduced in Reference Example 3-1. The positive electrode and negative electrode were prepared by the same operation as in Example 3-6. The unit area capacity of the positive electrode was 1.46 mAh / cm 2 The unit area capacity of the negative electrode is 1.74 mAh / cm 2 , AC ratio was 1.19. Using the positive electrode and negative electrode obtained as above, a laminated battery was prepared in the same manner as in Example 3-1.
[0627] (Example 3-8)
[0628] The sodium alginate / disodium iminodiacetate mixture prepared in Reference Example 3-5 was added to the positive electrode instead of the alginate grafted polymer with iminodiacetate groups prepared in Reference Example 3-1; PVDF was used as the positive electrode binder instead of sodium alginate. The positive electrode and negative electrode were prepared by the same operation as in Example 3-1. The unit area capacity of the positive electrode was 1.47 mAh / cm 2 The unit area capacity of the negative electrode is 1.74 mAh / cm2 , AC ratio was 1.18. Using the positive electrode and negative electrode obtained as above, a laminated battery was prepared in the same manner as in Example 3-1.
[0629] (Comparative Example 3-1)
[0630] A positive electrode slurry was prepared from the following materials, and a positive electrode was produced by the same method as in Example 3-1.
[0631] Positive electrode active material: lithium manganese oxide (LMO: trial production by our company, LiMn2 O4) 94 parts by mass
[0632] Conductive aid: 3 parts by mass of acetylene black (AB: Li-400 manufactured by Denka Corporation)
[0633] Binder: Sodium alginate (ALGITEX L manufactured by KIMICA Co., Ltd.) 3 parts by mass
[0634] The capacity per unit area is 1.50 mAh / cm 2 .
[0635] Next, the negative electrode was prepared in the same manner as in Example 3-1. The capacity per unit area was 1.80 mAh / cm 2 , AC ratio was 1.20. Using the positive electrode and negative electrode prepared as above, a laminated battery was prepared in the same manner as in Example 3-1.
[0636] (Comparative Example 3-2)
[0637] A positive electrode slurry was prepared from the following materials to produce a positive electrode.
[0638] Positive electrode active material: lithium manganese oxide (LMO: trial production by our company, LiMn2 O4) 94 parts by mass
[0639] Conductive aid: 3 parts by mass of acetylene black (AB: Li-400 manufactured by Denka Corporation)
[0640] Binder: 3 parts by mass of polyvinylidene fluoride (PVDF: Solef 5130 manufactured by Solvay)
[0641] 3 parts by mass of the above PVDF were dissolved in N-methyl-2-pyrrolidone (NMP), 94 parts by mass of LMO and 3 parts by mass of AB were added to the solution, and NMP was added while stirring with a planetary mixer to prepare a positive electrode slurry. The slurry was coated on aluminum foil with a coater, dried at 80°C and nitrogen for 24 hours under normal pressure, and then dried at 150°C under reduced pressure for 4 hours, and rolled to make a positive electrode. The capacity per unit area is 1.52 mAh / cm 2Next, the negative electrode was prepared by the same method as in Example 3-1. The capacity per unit area was 1.82 mAh / cm 2 , AC ratio was 1.20. Using the positive electrode and negative electrode prepared as above, a laminated battery was prepared in the same manner as in Example 3-1.
[0642] <Charge and discharge characteristics evaluation>
[0643] Using the laminated batteries obtained in Examples 3-1 to 3-8 and Comparative Examples 3-1 and 3-2, the charge and discharge characteristics were evaluated under the following conditions.
[0644] Charging: Constant current constant voltage (CCCV mode)
[0645] Discharge: Constant current (CC mode)
[0646] Potential range: 3.0~4.2V
[0647] C rate: 1C
[0648] Temperature: 60℃
[0649] Under the above conditions, charge and discharge were performed for 100 cycles. The results are shown in Table 1. It can be seen that by adding water-insoluble polymer compound particles containing chelate groups or organic solvent-insoluble polymer compound particles containing chelate groups to the positive electrode and / or the negative electrode, the capacity retention rate shows a higher value than that of the comparative example, and the cycle characteristics are improved.
[0650] [Table 1]
[0651]
[0652] (Example of the fourth aspect of the present invention)
[0653] <Production of chelate group-containing polymer compound>
[0654] (Reference Example 4-1) Production of Alginic Acid Introduced with Iminodiacetic Acid Groups by Covalent Bond
[0655] Under stirring, 0.50 g (monosaccharide unit is 2.5 mmol) of sodium alginate (manufactured by Qingdao Polyocean Algae Group Co., Ltd., weight average molecular weight 1,300,000) was gradually added to 50 ml of pure water in small amounts to make a viscous uniform solution. Next, 0.10 g (2.5 mmol) of sodium hydroxide (manufactured by Tokyo Chemical Industry) was added and dissolved, and then 3.10 g (50 mmol) of epichlorohydrin (manufactured by Tokyo Chemical Industry) was added, and the mixture was reacted at 20°C for 6 hours. The reacted solution was added dropwise to 2 L of ethanol to form a precipitate, which was recovered by filtration, washed with ethanol, and separated by vacuum drying. The separation yield was 0.43 g, which was easily soluble in water. 0.30 g of the above reaction product was weighed and dissolved in 100 ml of pure water. Next, 8.4 g (43 mmol) of disodium iminodiacetic acid monohydrate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was added and dissolved, and the mixture was reacted at 80°C for 2 hours. The reacted aqueous solution was purified for 24 hours by ultrafiltration membrane (made by Pall, Japan, molecular weight cut-off 1000) to remove excess iminodiacetic acid. The purified aqueous solution was added dropwise to acetone to precipitate the polymer, filtered, recovered, and separated by drying under reduced pressure. The separation yield was 0.33 g, which was soluble in water, and the weight average molecular weight measured by aqueous GPC was 370,000. The nitrogen content was 2.2% by weight, and the chelating group content calculated based on the nitrogen content was 1.6 mmol / g.
[0656] (Reference Example 4-2) Production of Alginic Acid Introduced with Disodium Iminodiacetic Acid Groups by Ionic Bonding
[0657] Under stirring, 1.0 g (monosaccharide unit is 5.7 mmol) of hydrogen ion type alginic acid (manufactured by KIMICA Co., Ltd., trade name KIMICA ACID G) was gradually added in small amounts to 100 ml of pure water to make a white paste-like uniform dispersion. Next, 1.1 g (5.7 mmol) of disodium iminodiacetic acid monohydrate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was directly added to the above-mentioned alginic acid dispersion and stirred. The dispersion gradually becomes transparent as it is added, and after the addition is completed, it becomes a transparent and viscous aqueous solution. The aqueous solution was stirred at room temperature for 1 hour, and then added dropwise to 4 L of acetone to generate a precipitate. The precipitate obtained was recovered by filtration, then washed with acetone, and separated by drying under reduced pressure. The separation yield was 1.9 g, and the nitrogen content obtained by elemental analysis was 3.7% by mass, and the chelate group content calculated based on the nitrogen content was 2.6 mmol / g, which was easily soluble in water. In order to confirm that a chelate group was introduced into the alginic acid, the FT-IR spectra before and after the reaction were compared. The hydrogen ion form of alginate before the reaction was 1740 cm -1 The stretching vibration absorption of the carbonyl group of the carboxylic acid was observed at 1740 cm -1 The absorption at 1620cm -1New absorption originating from the stretching vibration of the carbonyl group of the carboxylate was observed. It can be seen that alginic acid and iminodiacetic acid are bonded via ionic bonds. Next, the molecular weight of the polymer compound containing the chelate group was measured by aqueous GPC. The weight average molecular weight was 320,000.
[0658] (Reference Example 4-3) Production of alginic acid into which nitrilotri(methylenephosphonic acid sodium) groups are introduced through ionic bonds. The amount of hydrogen ion-type alginic acid added is set to 2.0 g (monosaccharide unit is 11.4 mmol); 5.2 ml (11.4 mmol) of 50% aqueous solution of nitrilotri(methylenephosphonic acid) (produced by Tokyo Chemical Industry) and 68.4 ml (68.4 mmol) of 1N aqueous sodium hydroxide solution (produced by Fujifilm Wako Pure Chemical Industries, Ltd.) are used instead of disodium iminodiacetic acid monohydrate. Apart from this, alginic acid into which chelating groups are introduced is produced by the same operation as Reference Example 4-2. The separation yield is 6.7 g, and the nitrogen content determined by elemental analysis is 1.8% by mass. The chelating group content calculated based on the nitrogen content is 1.3 mmol / g, and it is easily soluble in water. In order to confirm that chelating groups are introduced into alginic acid, the FT-IR spectra before and after the reaction are compared. The hydrogen ion-type alginic acid before the reaction has a wavelength of 1740 cm -1 The stretching vibration absorption of the carbonyl group of the carboxylic acid was observed at 1740 cm -1 The absorption at 1620cm -1 New absorption originating from the stretching vibration of the carbonyl group of the carboxylate was observed. It can be seen that alginic acid and iminodiacetic acid are bonded via ionic bonds. Next, the molecular weight of the polymer compound containing the chelate group was measured by aqueous GPC. The weight average molecular weight was 350,000.
[0659] <Manufacturing of laminated batteries>
[0660] (Example 4-1)
[0661] A positive electrode slurry was prepared from the following materials to produce a positive electrode.
[0662] Positive electrode active material: lithium manganese oxide (LMO: our company's trial production LiMn2 O4, crystal phase: spinel) 94 parts by mass
[0663] Conductive aid: 3 parts by mass of acetylene black (AB: Li-400 manufactured by Denka Corporation)
[0664] Binder: 3 parts by weight of chelate-containing alginic acid (reference example 4-1)
[0665] 3 parts by mass of the chelate group-containing alginic acid prepared in Reference Example 4-1 were dissolved in water to prepare an aqueous solution. 94 parts by mass of LMO and 3 parts by mass of AB were added to the aqueous solution, and water was added while stirring with a planetary mixer to prepare a positive electrode slurry. The slurry was coated on an aluminum foil with a film applicator, dried at 80°C under nitrogen for 24 hours, and then dried under reduced pressure at 120°C for 4 hours to prepare a positive electrode. The capacity per unit area was 1.50 mAh / cm 2 In addition, the prepared positive electrode was wound into a cylinder with a diameter of 8 mm, and the appearance of the positive electrode was observed. The appearance of the positive electrode was good, and no cracks in the electrode mixture layer, peeling from the current collector, or falling off were observed.
[0666] Next, a negative electrode slurry was prepared from the following materials to produce a negative electrode.
[0667] Negative electrode active material: 95 parts by mass of blocky artificial graphite (Gr: MAG-D manufactured by Showa Denko Materials Co., Ltd.)
[0668] Binder: 5 parts by mass of polyvinylidene fluoride (PVDF: Solef 5130 manufactured by Solvay)
[0669] 5 parts by mass of the above PVDF were dissolved in N-methyl-2-pyrrolidone (NMP), 95 parts by mass of Gr were added to the solution, and NMP was added while stirring with a planetary mixer to prepare a negative electrode slurry. The slurry was applied to a copper foil with an applicator, dried at 80°C under nitrogen at normal pressure for 24 hours, and then dried under reduced pressure at 150°C for 4 hours to prepare a negative electrode. The capacity per unit area was 1.80 mAh / cm, and the AC ratio was 1.20.
[0670] Using the positive electrode and negative electrode obtained as above, a laminated battery is prepared as follows. That is, vinylene carbonate is added to a mixed solvent of ethylene carbonate / diethyl carbonate (1 / 1) to make it 1% by mass, and then lithium hexafluorophosphate is dissolved to make it 1 mol / L to prepare an electrolyte, and a polyethylene microporous film (made by Senior) coated with aluminum oxide on one side is used as a separator. Then, the positive electrode and the negative electrode are stacked on both sides of the separator, and the electrolyte is injected to prepare a laminated battery.
[0671] (Example 4-2)
[0672] A laminate battery was prepared by the same operation as in Example 4-1 except that the chelate group-containing polymer compound obtained in Reference Example 4-2 was used as the positive electrode binder.
[0673] (Example 4-3)
[0674] A laminate battery was prepared by the same operation as in Example 4-1 except that the chelate group-containing polymer compound obtained in Reference Example 4-3 was used as the positive electrode binder.
[0675] (Comparative Example 4-1)
[0676] A laminated battery was produced by the same operation as in Example 4-1 except that PVDF (Solef 5130 manufactured by Solvay) was used as the positive electrode binder and NMP was used as the solvent to produce a positive electrode slurry.
[0677] <Charge and discharge characteristics evaluation>
[0678] Using the laminated batteries obtained in Examples 4-1 to 4-3 and Comparative Example 4-1, the charge and discharge characteristics were evaluated under the following conditions.
[0679] Charging: Constant current constant voltage (CCCV mode)
[0680] Discharge: Constant current (CC mode)
[0681] Potential range: 3.0~4.2V
[0682] C rate: 1C
[0683] Temperature: 60℃
[0684] Under the above conditions, charge and discharge were performed 100 times. The results are shown in Figure 3 . Figure 3 It is a graph showing the charge and discharge cycle characteristics of the laminated battery obtained in Example 4-1, Example 4-2, and Comparative Example 4-1, showing the change of discharge capacity with the number of cycles. From the results, it can be seen that in the system of Example 4-1 and Example 4-2 in which the polymer compound containing a chelate group of the present invention is used as an adhesive, even if the number of cycles increases, the reduction of discharge capacity is small, and stable charge and discharge can be performed, while in the system of Comparative Example 4-1 in which PVDF is used as an adhesive, the discharge capacity decreases as the number of cycles increases. In addition, the capacity retention rate of the discharge capacity after 100 cycles is 88.4% in Example 4-1, 86.2% in Example 4-2, and 81.3% in Comparative Example 4-1. In addition, the charge and discharge cycle characteristics of the laminated battery of Example 4-3 are also good, and the capacity retention rate of the discharge capacity after 100 cycles is 88.6% in Example 4-3.
[0685] <Manufacturing of positive electrode>
[0686] (Example 4-4)
[0687] NCM523 (produced by Toyoshima Seisakusho Co., Ltd.) as a lithium composite oxide was used instead of LMO as the positive electrode active material; the composition of the positive electrode mixture layer was changed to active material: AB: binder = 94:4:2, and the positive electrode was prepared by the same operation as in Example 4-1. The obtained positive electrode was wound on a cylinder with a diameter of 8 mm, and the appearance of the positive electrode was observed. The appearance of the positive electrode was good, and no cracks in the electrode mixture layer, peeling from the current collector, or falling off were observed.
[0688] (Example 4-5)
[0689] Electrolytic manganese dioxide (EMD: manufactured by Tosoh Corporation) was used as the positive electrode active material instead of LMO; the composition of the positive electrode mixture layer was changed to active material: AB: binder = 93:3:4, and the positive electrode was prepared by the same operation as in Example 4-1. The obtained positive electrode was wound on a cylinder with a diameter of 8 mm, and the appearance of the positive electrode was observed. The appearance of the positive electrode was good, and no cracks, peeling from the current collector, or falling off of the electrode mixture layer were observed.
[0690] <Accelerated degradation test of positive electrode active material>
[0691] (Example 4-6)
[0692] 0.05g of the chelate-containing polymer compound manufactured in Reference Example 4-1 was dissolved in 20ml of pure water, and then 0.95g of LMO was added and stirred to make a slurry. After heating the slurry and removing the water with an evaporator, the obtained mixture was crushed with a mortar and dried under reduced pressure at 120°C to completely remove the water. In a glove box, 15ml of electrolyte (1MLiPF6, EC / DMC=1 / 2, manufactured by KISHIDA CHEMICAL) was added to the mixture and sealed, and heated at 85°C for 4 days. After the heat treatment, the electrolyte was recovered by filtration, and the amount of Mn in the electrolyte was measured, and the result was less than 1ppm. This shows that the Mn ions dissolved from LMO are captured by the polymer compound containing the chelate group. It can be considered that the high capacity retention rate of the laminated battery to which the polymer compound containing the chelate group is added is the result of suppressing the accumulation of Mn to the negative electrode.
[0693] (Example 4-7)
[0694] The accelerated degradation test was conducted under the same conditions and operations as in Example 4-6 except that 0.25 g of the chelate group-containing polymer compound prepared in Reference Example 4-2 was used instead of 0.05 g of the chelate group-containing polymer compound prepared in Reference Example 4-1; 4.75 g of NCM523 was used instead of 0.95 g of LMO; and the heating treatment days were changed from 4 days to 18 days. The Mn and Ni contents in the electrolyte after the heating treatment were both less than 1 ppm.
[0695] (Example 4-8)
[0696] 0.25 g of the polymer compound containing a chelate group produced in Reference Example 4-2 was used instead of 0.05 g of the polymer compound containing a chelate group produced in Reference Example 4-1; 4.75 g of EMD was used instead of 0.95 g of LMO; 1 M LiClO4, PC / DME = 1 / 1 (produced by Toyama Pharmaceutical Industries) was used for the electrolyte; the heating treatment conditions were changed from 85°C × 4 days to 80°C × 30 days, and the accelerated degradation test was performed under the same conditions and operations as Example 4-6. The amount of Mn in the electrolyte after the heating treatment was less than 1 ppm.
[0697] (Comparative Example 4-2)
[0698] The accelerated degradation test was conducted under the same conditions and operation as in Example 4-6 except that no chelate group-containing polymer compound was added and 1.0 g of LMO was used. The amount of Mn in the electrolyte after the heat treatment was 14 ppm, and dissolution of Mn was observed.
[0699] (Comparative Example 4-3)
[0700] The accelerated degradation test was conducted under the same conditions and operation as in Example 4-7 except that no chelate group-containing polymer compound was added and 5.0 g of NCM523 was used. The amounts of Mn and Ni in the electrolyte after the heat treatment were 1 ppm and 28 ppm, respectively, and dissolution of Mn and Ni was observed.
[0701] (Comparative Example 4-4)
[0702] The accelerated degradation test was conducted under the same conditions and operation as in Example 4-8 except that no chelate group-containing polymer compound was added and 5.0 g of EMD was used. The amount of Mn in the electrolyte after the heat treatment was 28 ppm, and dissolution of Mn was observed.
[0703] (Example of the fifth aspect of the present invention)
[0704] <Production of a composition comprising a polymer compound and a chelate group-containing low molecular weight compound>
[0705] (Example 5-1) Preparation of a Composition of Sodium Alginate and Sodium Nitrilotri(Methylenephosphonate)
[0706] Under stirring, 2.0 g (monosaccharide unit is 10 mmol) of sodium alginate (manufactured by Qingdao Polyocean Algae Group Co., Ltd., weight average molecular weight 1,300,000) was gradually added to 100 ml of pure water in small amounts to make a viscous uniform solution. Next, 4.6 ml (10 mmol) of nitrilotri(methylenephosphonic acid) (manufactured by Tokyo Chemical Industry, 50% aqueous solution) and 60 ml (60 mmol) of 1N sodium hydroxide aqueous solution (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) were mixed under ice cooling, and the obtained mixed solution was added to the above-mentioned sodium hydroxide aqueous solution. After adding, after mixing at room temperature for 1 hour, the mixed solution was added dropwise to 2 L of acetone to generate a precipitate, which was recovered by filtration, washed with acetone, and separated after drying under reduced pressure. The separation yield was 6.4 g, and the nitrogen content of the obtained mixture was 1.8% by weight, and the chelate group content calculated based on the nitrogen content was 1.3 mmol / g. The composition calculated from the nitrogen content was as follows: 220 parts by weight of nitrilotri(methylenephosphonic acid) relative to 100 parts by weight of sodium alginate.
[0707] (Example 5-2) Preparation of a Composition of Sodium Alginate and Disodium Iminodiacetic Acid
[0708] A physical mixture of sodium alginate and disodium iminodiacetate was prepared by the same method as in Example 5-1 except that 2.0 g (10 mmol) of disodium iminodiacetate monohydrate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was used instead of 4.6 ml (10 mmol) of nitrilotri(methylenephosphonic acid) (manufactured by Tokyo Chemical Industry, 50% aqueous solution) and 60 ml (60 mmol) of 1N aqueous sodium hydroxide solution (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.). The separation yield was 3.9 g, and the nitrogen content of the obtained mixture was 3.3% by weight. The chelate group content calculated from the nitrogen content was 2.4 mmol / g. The composition calculated from the nitrogen content was as follows: 70 parts by weight of disodium iminodiacetate relative to 100 parts by weight of sodium alginate.
[0709] <Manufacturing of laminated batteries>
[0710] (Example 5-3)
[0711] A positive electrode slurry was prepared from the following materials to produce a positive electrode.
[0712] Positive electrode active material: lithium manganese oxide (LMO: our company's trial production LiMn2 O4, crystal phase: spinel) 94 parts by mass
[0713] Conductive aid: 3 parts by mass of acetylene black (AB: Li-400 manufactured by Denka Corporation)
[0714] Binder: 3 parts by mass of a physical mixture of sodium alginate and sodium nitrilotri(methylenephosphonate) prepared in Example 5-1
[0715] 3 parts by mass of the binder prepared in Example 5-1 were dissolved in water to prepare an aqueous solution. 94 parts by mass of LMO and 3 parts by mass of AB were added to the aqueous solution, and water was added while stirring with a planetary mixer to prepare a positive electrode slurry. The slurry was applied to an aluminum foil with a coater, dried at 80°C under nitrogen at normal pressure for 24 hours, and then dried under reduced pressure at 120°C for 4 hours to prepare a positive electrode. The capacity per unit area was 1.50 mAh / cm 2 .
[0716] Next, a negative electrode slurry was prepared from the following materials to produce a negative electrode.
[0717] Negative electrode active material: 95 parts by mass of blocky artificial graphite (Gr: MAG-D manufactured by Showa Denko Materials Co., Ltd.)
[0718] Binder: 5 parts by mass of polyvinylidene fluoride (PVDF: Solef 5130 manufactured by Solvay)
[0719] 5 parts by mass of the above PVDF were dissolved in N-methyl-2-pyrrolidone (NMP), 95 parts by mass of Gr were added to the solution, and NMP was added while stirring with a planetary mixer to prepare a negative electrode slurry. The slurry was coated on a copper foil with a film applicator, dried at 80°C under nitrogen for 24 hours, and then dried under reduced pressure at 150°C for 4 hours to prepare a negative electrode. The capacity per unit area is 1.80 mAh / cm 2 , the AC ratio is 1.20.
[0720] Using the positive electrode and negative electrode obtained as above, a laminated battery is prepared as follows. That is, vinylene carbonate is added to a mixed solvent of ethylene carbonate / diethyl carbonate (1 / 1) to make it 1% by mass, and then lithium hexafluorophosphate is dissolved to make it 1 mol / L to prepare an electrolyte, and a polyethylene microporous film (made by Senior) coated with aluminum oxide on one side is used as a separator. Then, the positive electrode and the negative electrode are stacked on both sides of the separator, and the electrolyte is injected to prepare a laminated battery.
[0721] (Example 5-4)
[0722] A laminated battery was prepared by the same operation as in Example 5-3 except that the physical mixture of sodium alginate and disodium iminodiacetate produced in Example 5-2 was used as a positive electrode binder.
[0723] (Comparative Example 5-1)
[0724] A laminated battery was produced by the same operation as in Example 5-3 except that PVDF (Solef 5130 manufactured by Solvay) was used as the positive electrode binder and NMP was used as the solvent to produce a positive electrode slurry.
[0725] <Charge and discharge characteristics evaluation>
[0726] Using the laminated batteries obtained in Examples 5-3 and 5-4 and Comparative Example 5-1, the charge and discharge characteristics were evaluated under the following conditions.
[0727] Charging: Constant current constant voltage (CCCV mode)
[0728] Discharge: Constant current (CC mode)
[0729] Potential range: 3.0~4.2V
[0730] C rate: 1C
[0731] Temperature: 60℃
[0732] Under the above conditions, charge and discharge were performed for 100 cycles. In the systems of Example 5-3 and Example 5-4, in which the physical mixture of the polymer compound of the present invention and the low molecular compound containing a chelating group was used as an adhesive, the discharge capacity decreased less even if the number of cycles increased, and stable charge and discharge could be performed. However, in the system of Comparative Example 5-1, in which PVDF was used as an adhesive, it was observed that the discharge capacity decreased as the number of cycles increased. The capacity retention rate of the discharge capacity after 100 cycles was 88.9% in Example 5-3, 89.0% in Example 5-4, and 81.3% in Comparative Example 5-1.
[0733] (Example of the sixth aspect of the present invention)
[0734] <Production of a composition comprising a polymer compound and a chelate group-containing compound>
[0735] (Example 6-1) Preparation of a composition of hydrogen ion-type alginic acid and trisodium nitrilotrimethylphosphonate
[0736] Under stirring, 250 g (monosaccharide unit is 1.07 mol) of sodium alginate (made by Shandong Jiejing Co., Ltd., with a water content of 15% and a weight average molecular weight of 1,100,000) was gradually added to 440 ml of ethanol (made by Fujifilm Wako Pure Chemical Industries, Ltd.) to prepare a brown dispersion. Next, 192 g (1.89 mol) of 35% hydrochloric acid (made by Fujifilm Wako Pure Chemical Industries, Ltd.) was diluted with 188 g of pure water and added to the above dispersion, and reacted at 8°C for 2 hours. During the reaction, the dispersion state was maintained, and the slurry concentration was 26%. After the reaction was completed, the slurry was filtered, and the obtained solid component was redispersed in 4 L of pure water. After stirring for 1 hour, it was filtered and separated, and dried under reduced pressure at 80°C. The yield of the obtained hydrogen ion-type alginate was 149 g, the weight average molecular weight was 620,000, the sodium content was 0.91%, and the hydrogen ion substitution rate obtained based on the sodium content was 93.0%. 1.8 g of the hydrogen ion type alginic acid (monosaccharide unit: 10 mmol) prepared as above and 3.2 g (10 mmol) of trisodium nitrilotrimethylphosphonate (manufactured by Tongren Chemical Research Institute) were mixed in a mortar to prepare a composition. The nitrogen content of the obtained mixture was 2.8% by weight, and the chelate group content calculated from the nitrogen content was 2.0 mmol / g. In addition, the pH of the trisodium nitrilotrimethylphosphonate aqueous solution was 4.0.
[0737] (Example 6-2) Preparation of a Composition of Hydrogen Ion Alginic Acid and Disodium Iminodiacetic Acid
[0738] 1.8 g of hydrogen ion type alginic acid (monosaccharide unit: 10 mmol) prepared in Example 6-1 and 2.0 g (10 mmol) of disodium iminodiacetate monohydrate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) were mixed in a mortar to prepare a composition. The nitrogen content of the obtained mixture was 4.0% by weight, and the chelate group content calculated from the nitrogen content was 2.8 mmol / g. In addition, the pH of the disodium iminodiacetate aqueous solution was 11.0.
[0739] (Example 6-3) Preparation of a Composition of Hydrogen Ion Alginic Acid and Disodium Ethylenediaminetetraacetate
[0740] 1.8 g of hydrogen ion type alginic acid (monosaccharide unit: 10 mmol) prepared in Example 6-1 and 3.7 g (10 mmol) of disodium ethylenediaminetetraacetic acid dihydrate (manufactured by Tongren Chemical Research Institute) were mixed in a mortar to prepare a composition. The nitrogen content of the obtained mixture was 5.1% by weight, and the chelate group content calculated from the nitrogen content was 1.8 mmol / g. In addition, the pH of the disodium ethylenediaminetetraacetic acid aqueous solution was 4.2.
[0741] <Manufacturing of laminated batteries>
[0742] (Example 6-4)
[0743] A positive electrode slurry was prepared from the following materials to produce a positive electrode.
[0744] Positive electrode active material: lithium manganese oxide (LMO: our company's trial production of LiMn2 O4, crystal phase: spinel) 94 parts by weight
[0745] Conductive aid: 3 parts by weight of acetylene black (AB: Li-400 manufactured by Denka Corporation)
[0746] Binder: 3 parts by weight of the composition of hydrogen ion type alginic acid and trisodium nitrilotrimethylphosphonate prepared in Example 6-1
[0747] 3 parts by weight of the binder prepared in Example 6-1 were dissolved in water to prepare an aqueous solution. 94 parts by weight of LMO and 3 parts by weight of AB were added to the aqueous solution, and water was added while stirring with a planetary mixer to prepare a positive electrode slurry. The slurry was applied to an aluminum foil with a coater, dried at 80°C under nitrogen for 24 hours, and then dried under reduced pressure at 120°C for 4 hours to prepare a positive electrode. The capacity per unit area was 1.50 mAh / cm 2 .
[0748] Next, a negative electrode slurry was prepared from the following materials to produce a negative electrode.
[0749] Negative electrode active material: 95 parts by weight of blocky artificial graphite (Gr: MAG-D manufactured by Showa Denko Materials Co., Ltd.)
[0750] Binder: 5 parts by weight of polyvinylidene fluoride (PVDF: Solef 5130 manufactured by Solvay)
[0751] 5 parts by weight of the above PVDF was dissolved in N-methyl-2-pyrrolidone (NMP), 95 parts by weight of Gr was added to the solution, and NMP was added while stirring with a planetary mixer to prepare a negative electrode slurry. The slurry was coated on a copper foil with a film applicator, dried at 80°C under nitrogen for 24 hours, and then dried under reduced pressure at 150°C for 4 hours to prepare a negative electrode. The capacity per unit area is 1.80 mAh / cm 2 , the AC ratio is 1.20.
[0752] Using the positive electrode and negative electrode obtained as above, a laminated battery is prepared as follows. That is, vinylene carbonate is added to a mixed solvent of ethylene carbonate / diethyl carbonate (1 / 1) to make it 1% by weight, and then lithium hexafluorophosphate is dissolved to make it 1 mol / L to prepare an electrolyte, and a polyethylene microporous film (made by Senior) coated with aluminum oxide on one side is used as a separator. Then, the positive electrode and the negative electrode are stacked on both sides of the separator, and the electrolyte is injected to prepare a laminated battery.
[0753] (Example 6-5)
[0754] A laminated battery was produced by the same operation as in Example 6-4 except that the composition of hydrogen ion type alginic acid and disodium iminodiacetic acid produced in Example 6-2 was used as a positive electrode binder.
[0755] (Example 6-6)
[0756] A laminated battery was produced by the same operation as in Example 6-4 except that the composition of hydrogen ion type alginic acid and disodium ethylenediaminetetraacetate produced in Example 6-3 was used as a positive electrode binder.
[0757] (Comparative Example 6-1)
[0758] A laminated battery was produced by the same operation as in Example 6-4 except that PVDF (Solef 5130 manufactured by Solvay) was used as the positive electrode binder and NMP was used as the solvent to produce a positive electrode slurry.
[0759] (Comparative Example 6-2)
[0760] A composition prepared by mixing 2.3 g (monosaccharide unit: 10 mmol) of sodium alginate (manufactured by Shandong Jiejing Co., Ltd., water content: 15%, weight average molecular weight: 1,100,000) and 2.0 g (10 mmol) of disodium iminodiacetic acid monohydrate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) in a mortar was used as a binder for the positive electrode. Except for this, a laminated battery was prepared by the same operation as in Example 6-4.
[0761] <Charge and discharge characteristics evaluation>
[0762] Using the laminated batteries obtained in Examples 6-4, 6-5, and 6-6 and Comparative Examples 6-1 and 6-2, the charge and discharge characteristics were evaluated under the following conditions.
[0763] Charging: Constant current constant voltage (CCCV mode)
[0764] Discharge: Constant current (CC mode)
[0765] Potential range: 3.0~4.2V
[0766] C rate: 1C
[0767] Temperature: 60℃
[0768] Under the above conditions, charge and discharge were performed for 100 cycles. In the laminated batteries of Examples 6-4, 6-5, and 6-6, in which the composition of the hydrogen ion type alginic acid and the amino-containing chelate group-containing compound of the present invention is used as a binder, the discharge capacity decreases less even if the number of cycles increases, and stable charge and discharge can be performed. However, in the system of Comparative Example 6-1 in which PVDF is used as a binder, it is observed that the discharge capacity decreases as the number of cycles increases. The capacity retention rate of the discharge capacity after 100 cycles is 90.9% in Example 6-4, 89.5% in Example 6-5, 89.3% in Example 6-6, and 81.3% in Comparative Example 6-1.
[0769] On the other hand, in Comparative Example 6-2 in which a composition of sodium alginate and disodium iminodiacetic acid, in which the binder does not form an ionic bond, was used as a binder, the capacity retention rate of the discharge capacity after 100 cycles was 89.0%, showing a good capacity retention rate, but gas was generated during the cycle test and the laminated battery expanded significantly.
[0770] <Evaluation of the corrosion status of the current collector>
[0771] (Example 6-7)
[0772] The positive electrode slurry was manufactured by the same method as in Example 6-4, except that NCM523 (manufactured by Toyoshima Seisakusho), which is lithium nickel cobalt manganese oxide, was used as an active material instead of lithium manganese oxide (LMO: LiMn2O4 produced by our company on a trial basis, crystal phase: spinel). The pH of the slurry was 9.0. Although the positive electrode active material with a high nickel content was made into an aqueous slurry, the strong alkalinity of the slurry was suppressed by using the composition of Example 6-1 as a binder. The slurry was applied to an aluminum foil by the same method as in Example 6-4 and dried to manufacture a positive electrode. After being left at room temperature for 7 days, the obtained positive electrode mixture layer was peeled off, and the corrosion state of the aluminum foil was confirmed, and no corrosion of the aluminum foil was observed.
[0773] (Examples 6-8)
[0774] NCM523 (produced by Toyoshima Seisakusho) which is lithium nickel cobalt manganese oxide was used as an active material instead of lithium manganese oxide (LMO: our company's trial production LiMn2 O4, crystal phase: spinel); the composition of Example 6-3 was used as a binder, and the positive electrode slurry was manufactured by the same method as Example 6-4 except that it was used as a binder. The pH of the slurry was 9.4. Although the positive electrode active material with a high nickel content was made into an aqueous slurry, the strong alkalinity of the slurry was suppressed by using the composition of Example 6-3 as a binder. The slurry was applied to aluminum foil by the same method as Example 6-4 and dried to manufacture a positive electrode. After being left at room temperature for 7 days, the obtained positive electrode mixture layer was peeled off, and the corrosion state of the aluminum foil was confirmed, and no corrosion of the aluminum foil was observed.
[0775] (Comparative Example 6-3)
[0776] NCM523 (produced by Toyoshima Seisakusho) which is lithium nickel cobalt manganese oxide was used as an active material instead of lithium manganese oxide (LMO: our company's trial production of LiMn2 O4, crystal phase: spinel); sodium alginate (produced by Shandong Jiejing Co., Ltd., with a water content of 15%, a weight average molecular weight of 1,100,000) was used as a binder. The positive electrode slurry was manufactured by the same method as Example 6-4. The pH of the slurry was 11.2. When the positive electrode active material with a high nickel content is made into an aqueous slurry, the slurry becomes strongly alkaline. The slurry was applied to an aluminum foil by the same method as Example 6-4 and dried to manufacture a positive electrode. After being left at room temperature for 7 days, the obtained positive electrode mixture layer was peeled off and the corrosion state of the aluminum foil was confirmed. As a result, corrosion of the aluminum foil was observed.
[0777] (Embodiment of the Seventh Aspect of the Present Invention)
[0778] (Example 7-1)
[0779] <Production of high molecular weight hydrogen ion type alginic acid>
[0780] Under stirring, 250 g (monosaccharide unit is 1.07 mol) of sodium alginate (manufactured by Shandong Jiejing Co., Ltd., water content 15%, weight average molecular weight 1,100,000) was gradually added to 440 ml of ethanol (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) to prepare a brown dispersion. Next, 192 g (1.89 mol) of 35% hydrochloric acid (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was diluted with 188 g of pure water and added to the above dispersion, and reacted at 8°C for 2 hours. During the reaction, the dispersion state was maintained, and the slurry concentration was 26%. After the reaction was completed, the slurry was filtered, and the obtained solid component was redispersed in 4 L of pure water. After stirring for 1 hour, it was filtered and separated, and dried under reduced pressure at 80°C. The yield of the obtained high molecular weight hydrogen ion type alginate was 149 g, the weight average molecular weight was 620,000, the sodium content was 0.91%, and the hydrogen ion substitution rate obtained based on the sodium content was 93.0%. The weight average molecular weight was measured by dissolving a sample in a 0.1 M phosphate buffer solution (pH=8.0) and using GPC (PEO conversion).
[0781] <Evaluation of heavy metal ion capture ability>
[0782] In order to evaluate the heavy metal ion capture ability of the adhesive composed of high molecular weight hydrogen ion type alginic acid and a compound containing a chelating group, the following measurement was performed. 0.05 g of the high molecular weight hydrogen ion type alginic acid manufactured in Example 7-1 and 0.06 g of disodium iminodiacetic acid hydrate (manufactured by Tokyo Chemical Industry) were dissolved in 20 ml of pure water, and 1.9 g of lithium manganate (trial production by our company, crystal structure: spinel, hereinafter referred to as "LMO") was added to prepare a slurry. After the obtained slurry was concentrated with an evaporator, it was dried under reduced pressure at 80°C to remove water to obtain a mixture of an adhesive composed of high molecular weight hydrogen ion type alginic acid and a compound containing a chelating group and LMO. 1.0 g was taken from the above mixture, placed in a TEFLON (registered trademark) container, and sealed after being dried under reduced pressure at 120°C for 4 hours. The sealed TEFLON (registered trademark) container was opened in the glove box, and 15 ml of electrolyte (made by KISHIDA CHEMICAL, a solution obtained by dissolving 1 mol / L of LiPF6 in a mixed solvent of ethylene carbonate: dimethyl carbonate = 1:2) was added, and then sealed again and heated at 85°C for 4 hours. After the heating was completed, the TEFLON (registered trademark) container was opened in the glove box, filtered using a syringe filter, and the filtrate was collected. The obtained filtrate was acid-decomposed, and the manganese ions were quantified by ICP-MS. As a result, the concentration of manganese ions was less than 1 ppm, confirming that the manganese ions dissolved from LMO due to heating were captured.
[0783] <Manufacturing of laminated batteries>
[0784] A positive electrode slurry was prepared from the following materials to produce a positive electrode.
[0785] Positive electrode active material: lithium manganese oxide (LMO: our company's trial production LiMn2 O4, crystal phase: spinel) 94 parts by mass
[0786] Conductive aid: 3 parts by mass of acetylene black (AB: Li-400 manufactured by Denka Corporation)
[0787] Binder: 3 parts by mass of a 1:1.2 mixture (mass ratio) of high molecular weight hydrogen ion type alginic acid produced in Example 7-1 and disodium iminodiacetic acid hydrate (produced by Tokyo Chemical Industry)
[0788] 3 parts by mass of the above binder was dissolved in water to prepare an aqueous solution. 94 parts by mass of LMO and 3 parts by mass of AB were added to the aqueous solution, and water was added while stirring with a planetary mixer to prepare a positive electrode slurry. The slurry was applied to an aluminum foil with a coater, dried at 80°C under nitrogen for 24 hours, and then dried under reduced pressure at 120°C for 4 hours to prepare a positive electrode. The capacity per unit area was 1.50 mAh / cm 2 .
[0789] Next, a negative electrode slurry was prepared from the following materials to produce a negative electrode.
[0790] Negative electrode active material: 95 parts by mass of blocky artificial graphite (Gr: MAG-D manufactured by Showa Denko Materials Co., Ltd.)
[0791] Binder: 5 parts by mass of polyvinylidene fluoride (PVDF: Solef 5130 manufactured by Solvay)
[0792] 5 parts by mass of the above PVDF were dissolved in N-methyl-2-pyrrolidone (NMP), 95 parts by mass of Gr were added to the solution, and NMP was added while stirring with a planetary mixer to prepare a negative electrode slurry. The slurry was coated on a copper foil with a film applicator, dried at 80°C under nitrogen for 24 hours, and then dried under reduced pressure at 150°C for 4 hours to prepare a negative electrode. The capacity per unit area is 1.80 mAh / cm 2 , the AC ratio is 1.20.
[0793] Using the positive electrode and negative electrode obtained as above, a laminated battery is prepared as follows. That is, vinylene carbonate is added to a mixed solvent of ethylene carbonate / diethyl carbonate (1 / 1) to make it 1% by mass, and then lithium hexafluorophosphate is dissolved to make it 1 mol / L to prepare an electrolyte, and a polyethylene microporous film (made by Senior) coated with aluminum oxide on one side is used as a separator. Then, the positive electrode and the negative electrode are stacked on both sides of the separator, and the electrolyte is injected to prepare a laminated battery.
[0794] <Charge and discharge characteristics evaluation>
[0795] Using the laminated battery obtained in Example 7-1, the charge and discharge characteristics were evaluated under the following conditions.
[0796] Charging: Constant current constant voltage (CCCV mode)
[0797] Discharge: Constant current (CC mode)
[0798] Potential range: 3.0~4.2V
[0799] C rate: 1C
[0800] Temperature: 60℃
[0801] Under the above conditions, charge and discharge were performed for 100 cycles. The capacity retention rate of the discharge capacity after 100 cycles was 89.3%, indicating good cycle characteristics.
[0802] (Example 7-2)
[0803] <Production of high molecular weight hydrogen ion type alginic acid>
[0804] Sodium alginate (B-8, weight average molecular weight 780,000) manufactured by KIMICA Co., Ltd. was used instead of sodium alginate manufactured by Shandong Jiejing Co., Ltd.; except that the reaction time was set to 1 hour, high molecular weight hydrogen ion type alginic acid was manufactured by the same operation as in Example 7-1. The yield of the obtained high molecular weight hydrogen ion type alginic acid was 164 g, the weight average molecular weight was 520,000, the sodium content was 2.01%, and the hydrogen ion substitution rate obtained based on the sodium content was 84.3%.
[0805] <Evaluation of heavy metal ion capture ability>
[0806] The heavy metal ion capture ability of the mixture of high molecular weight hydrogen ion type alginic acid and sodium iminodiacetic acid hydrate (mass ratio of 1:1.2) produced in Example 7-2 was evaluated by the same method as Example 7-1. The concentration of manganese ions in the filtrate was less than 1 ppm, confirming that the manganese ions eluted from LMO by heating were captured.
[0807] <Manufacturing of laminated batteries>
[0808] A positive electrode slurry was prepared by the same operation as in Example 7-1, except that a 1:1.2 mixture (mass ratio) of high molecular weight hydrogen ion type alginic acid and disodium iminodiacetic acid hydrate (produced by Tokyo Chemical Industry) produced in Example 7-2 was used as a binder.
[0809] In addition, a negative electrode was also produced by the same operation as in Example 7-1, and a laminated battery was also produced by the same operation as in Example 7-1.
[0810] <Charge and discharge characteristics evaluation>
[0811] Using the laminated battery obtained in Example 7-2, the charge and discharge characteristics were evaluated under the same conditions as in Example 7-1. The capacity retention rate of the discharge capacity after 100 cycles was 87.1% in Example 7-1, indicating good cycle characteristics.
[0812] (Comparative Example 7-1)
[0813] <Production of high molecular weight hydrogen ion type alginic acid>
[0814] 440 ml of pure water was used instead of 440 ml of ethanol, and 250 g of sodium alginate (manufactured by Shandong Jiejing Company, with a water content of 15% and a weight average molecular weight of 1,100,000) (monosaccharide unit is 1.07 mol) was gradually added in small amounts under stirring. At the stage when about 20 g of sodium alginate was added, the system became highly viscous and could not be stirred, and subsequent operations could not be continued. It can be seen from this that when sodium alginate ions are exchanged for hydrogen ion-type alginic acid in a homogeneous system, viscosity restrictions will occur, and operations under high concentration conditions cannot be performed, and operations under low concentration conditions are limited.
[0815] (Comparative Example 7-2)
[0816] <Hydrogen ion type alginic acid>
[0817] As commercially available hydrogen ion alginic acid, hydrogen ion alginic acid (KIMICA ACIDSA) produced by KIMICA Co., Ltd. was obtained. The weight average molecular weight was 60,000, the sodium content was 0.40%, and the hydrogen ion substitution rate calculated from the sodium content was 96.9%.
[0818] <Evaluation of heavy metal ion capture ability>
[0819] The heavy metal ion capture capacity of the mixture of the commercially available hydrogen ion type alginic acid and sodium iminodiacetic acid hydrate (mass ratio of 1:1.2) was evaluated by the same method as in Example 7-1. The concentration of manganese ions in the filtrate was less than 1 ppm, confirming that the manganese ions eluted from the LMO by heating were captured.
[0820] <Manufacturing of laminated batteries>
[0821] A 1:1.2 mixture (mass ratio) of commercially available hydrogen ion alginic acid and disodium iminodiacetic acid hydrate (manufactured by Tokyo Chemical Industry) obtained in Comparative Example 7-2 was used as a binder. A positive electrode slurry was prepared by the same operation as in Example 7-1 to produce a positive electrode. In the obtained positive electrode, the electrode mixture layer was partially peeled off from the current collector, and a laminated battery could not be produced.
[0822] While the invention has been described in detail and with reference to specific embodiments thereof, it will be apparent to one skilled in the art that various changes and modifications can be made therein without departing from the spirit and scope of the invention.
[0823] In addition, the entire contents of the following patent documents including specifications, claims, drawings, and abstracts are incorporated herein as the disclosure of the specification of the present invention.
[0824] Japanese Patent Application No. 2022-015789 filed on February 3, 2022
[0825] Japanese Patent Application No. 2022-018051 filed on February 8, 2022
[0826] Japanese Patent Application No. 2022-028082 filed on February 25, 2022
[0827] Japanese Patent Application No. 2022-028083 filed on February 25, 2022
[0828] Japanese Patent Application No. 2022-108026 filed on July 4, 2022
[0829] Japanese Patent Application No. 2022-108027 filed on July 4, 2022
[0830] Japanese Patent Application No. 2022-162036 filed on October 7, 2022
[0831] Japanese Patent Application No. 2022-203600 filed on December 20, 2022
[0832] Japanese Patent Application No. 2022-203601 filed on December 20, 2022
[0833] Japanese Patent Application No. 2023-003811 filed on January 13, 2023
[0834] Industrial Applicability
[0835] In summary, according to the present invention, a water-soluble chelate polymer can be provided which can rapidly capture a trace amount of heavy metal ions and reduce the amount of heavy metal ions to below the ppm level in a short period of time.
Claims
1. A water-soluble chelate polymer, which is formed by bonding an anionic polymer having a carboxyl group, a sulfonic acid group and / or a sulfate group and a chelate functional group having a cationic functional group via an ionic bond, in, The water-soluble chelating polymer contains 0.2 to 6 mmol / g of chelating functional groups and has a weight average molecular weight of 30,000 to 1,000,000.
2. The water-soluble chelating polymer according to claim 1, in, The anionic polymer is an acidic polysaccharide.
3. The water-soluble chelating polymer according to claim 1, in, The chelating functional group is an aminocarboxylic acid group or an aminophosphonic acid group.
4. A method for producing a water-soluble chelating polymer, in, An anionic polymer having carboxyl groups, sulfonic acid groups and / or sulfate groups is brought into contact with an acid to convert the carboxyl groups, sulfonic acid groups and / or sulfate groups into hydrogen ion forms, and then brought into contact with a chelate functional group-containing compound having an amino group to introduce a chelate functional group into the anionic polymer.
5. The method for producing a water-soluble chelate polymer according to claim 4, It is characterized in that An anionic polymer having a hydrogen ion type carboxyl group, sulfonic acid group and / or sulfate group is dispersed in a hydrophobic solvent, a chelating functional group-containing compound having an amino group is dissolved in water, and the two are mixed to prepare a water-in-oil emulsion and introduce a chelating functional group into the anionic polymer.
6. A method for capturing heavy metal ions, in, The water-soluble chelate polymer according to claim 1 is added to a solution containing heavy metal ions to capture the heavy metal ions with the chelate polymer.
7. A chelate polymer having a structure represented by the following general formula (1), comprising 0.2 to 5 mmol / g of a chelate functional group, PS-XA-CL(1) In the formula, PS represents an acidic polysaccharide or a basic polysaccharide, X represents a group represented by -O- or -N(R)-, R represents a hydrogen atom or a hydrocarbon group having 1 to 6 carbon atoms, A represents an organic group having 3 to 30 carbon atoms, and CL represents an organic group having 1 to 30 carbon atoms containing a chelating functional group.
8. The chelate polymer according to claim 7, having a structure represented by the following general formula (2): [Chemical formula 1] In the formula, A and CL have the same meanings as above, M represents a hydrogen atom or an alkali metal ion, and n represents an integer of 10 to 1000.
9. A method for producing a chelated polymer according to claim 7, in, After the acidic polysaccharide and / or the basic polysaccharide is reacted with an epihalohydrin and / or a polyfunctional epoxy compound having 2 to 6 epoxy groups, it is reacted with a compound having an amino group and a chelating functional group.
10. A chelate polymer having a structure represented by the following general formula (3), comprising 0.2 to 5 mmol / g of a chelate functional group, [Chemical formula 2] In the formula, PS and X represent the same meanings as above, B represents a vinyl monomer residue containing a chelating functional group and having 4 to 30 carbon atoms, D represents a vinyl monomer residue not containing a chelating functional group and having 4 to 30 carbon atoms, and l and m each independently represent an integer of 10 to 500.
11. The chelate polymer according to claim 10, having a structure represented by the following general formula (4): [Chemical formula 3] In the formula, B, D, M, l, m, and n have the same meanings as above.
12. A method for producing a chelating polymer according to claim 10, in, After graft-polymerizing an epoxy group-containing vinyl monomer onto an acidic polysaccharide and / or a basic polysaccharide, the monomer is reacted with a compound having an amino group and a chelating functional group.
13. A method for capturing heavy metal ions, in, The chelate polymer according to any one of claims 7, 8, 10 and 11 is added to a solution containing heavy metal ions to capture the heavy metal ions with the chelate polymer.
14. A lithium ion battery electrode composition, in, The electrode mixture including an active material, a binder and, if necessary, a conductive auxiliary agent contains water-insoluble polymer compound fine particles containing a chelate group, and the binder is a water-soluble polymer.
15. The lithium ion battery electrode composition according to claim 14, in, The water-insoluble polymer compound particles containing chelate groups are water-insoluble polysaccharide particles containing chelate groups.
16. The lithium ion battery electrode composition according to claim 14 or 15, in, The water-soluble polymer is a polysaccharide, a homopolymer or copolymer of (meth)acrylic acid, a homopolymer or copolymer of maleic acid, or a salt thereof.
17. A lithium ion battery electrode composition, in, The electrode mixture including an active material, a binder and, if necessary, a conductive auxiliary agent contains organic solvent-insoluble polymer compound fine particles containing a chelate group, and the binder is a fluorine-based resin.
18. The lithium ion battery electrode composition according to claim 17, in, The organic solvent-insoluble polymer compound particles containing chelating groups are organic solvent-insoluble polysaccharide particles containing chelating groups.
19. A binder for lithium ion battery electrodes, in, In lithium-ion batteries, the binder that binds the active material, the conductive aid, and the current collector contains a polymer compound containing a chelate group.
20. The adhesive according to claim 19, in, The chelate group in the chelate group-containing polymer compound is bonded to the polymer compound via a covalent bond and / or an ionic bond.
21. A composition comprising a high molecular weight compound and a low molecular weight compound containing a chelating group.
22. The composition according to claim 21, in, The polymer compound is a water-soluble polymer compound, and the low-molecular compound containing a chelating group is a water-soluble compound.
23. A composition comprising hydrogen ion-type alginic acid and a compound containing a chelating group.
24. The composition according to claim 23, in, The chelate group-containing compound is a compound containing at least one basic functional group selected from the group consisting of a primary amino group, a secondary amino group, a tertiary amino group, or an imino group.
25. The composition according to claim 23 or 24, in, The chelate group-containing compound is a compound whose aqueous solution has a pH of 3 to 9 when dissolved in water.
26. A high molecular weight hydrogen ion type alginic acid having a weight average molecular weight of 500,000 to 1,500,000 and a hydrogen ion substitution rate of 80 to 99%.
27. A method for producing hydrogen ion type alginic acid, in, At least one of an alkali metal alginate or an alkaline earth metal alginate is dispersed in a poor solvent thereof, and then an acid is added to exchange ions of at least one of the alkali metal alginate or an alkaline earth metal alginate into a hydrogen ion form in a dispersed state.
Citation Information