Antibacterial co-extrusion PE film and preparation method thereof
By using modified carbon nanotube enhanced antibacterial layer and optimized core layer and barrier layer in PE coextruded film, the problems of poor oxygen barrier performance, insufficient electrostatic and antibacterial properties on PE coextruded film are solved, and efficient Antistatic, antibacterial and barrier properties, suitable for advanced packaging materials.
Patent Information
- Application Number
- CN202411088688.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-09
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-08-09
AI Technical Summary
The existing PE coextruded film has poor barrier properties on oxygen, serious electrostatic problems, insufficient antibacterial properties, which affects the safety and operating performance of packaging products.
Adopt a three-layer coextrusion structure of antibacterial layer, core layer and barrier layer. The antibacterial layer is enhanced by modified carbon nanotubes, and the core layer and barrier layer materials are optimized. Antibacterial coextrusion PE film is prepared through coextrusion processing and heat setting, and the modification is made. Carbon nanotubes improve antistatic and antibacterial properties through chemical modification.
It significantly improves the antistatic, antibacterial and barrier properties of PE film, enhances mechanical properties, ensures long-term and stable excellent performance, and is suitable for advanced packaging materials.
Smart Images

Figure BDA0004985889240000031 
Figure BDA0004985889240000041 
Figure BDA0004985889240000101
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of PE co-extruded films, and in particular relates to an antibacterial co-extruded PE film and a preparation method thereof. Background Art
[0002] Polyethylene (PE) has good chemical stability, puncture resistance and impact resistance, especially good low temperature resistance, and its brittle temperature can generally reach below -50°C. PE has good processing performance and a wide processing temperature range. Due to its abundant raw material resources, moderate price and excellent product comprehensive performance, its application range is expanding, especially in the packaging field.
[0003] PE co-extruded film is a multi-layer composite film made by co-extruding different types of polyethylene raw materials through a casting process. This material has good transparency, puncture resistance, suitable friction coefficient, composite performance, and excellent hot viscosity and anti-pollution heat sealing properties. PE co-extruded film has good barrier properties to water vapor, but poor barrier properties to oxygen. It cannot well prevent the penetration of oxygen in the external environment, which will cause the product to be oxidized through the packaging. In addition, since PE material has a non-polar molecular structure, the molecular chain composed of its covalent bonds can neither ionize nor transfer free electrons. Once the electrons are gained or lost due to friction and charged, it is difficult to eliminate. The static electricity generated by PE materials during the processing process brings many inconveniences to the further processing of packaging film materials, affects the operating performance of the products, and affects the printing effect when the film is used for packaging due to static interference, and is difficult to separate or seal after the bag is made. In severe cases, it will also cause electric shock. In addition, PE materials have poor antibacterial properties. If exposed to the air for a long time, bacteria in the air will breed on the surface of the packaging film, endangering people's health. Therefore, it is urgent to invent a co-extruded PE film with excellent antibacterial and antistatic properties and good barrier properties to meet the higher demands in the field of PE co-extruded film technology. Summary of the invention
[0004] The purpose of the present invention is to overcome the defects of the prior art and provide an antibacterial co-extruded PE film and a preparation method thereof.
[0005] The purpose of the present invention can be achieved through the following technical solutions:
[0006] An antibacterial co-extruded PE film comprises an antibacterial layer, a core layer and a barrier layer, wherein the core layer is located between the antibacterial layer and the barrier layer.
[0007] Furthermore, the antibacterial layer accounts for 20-30% of the thickness of the PE film and is composed of the following raw materials in parts by weight: 80-100 parts of linear low-density polyethylene, 6-24 parts of modified carbon nanotubes, 3-5 parts of paraffin wax, and 4-8 parts of antioxidant 264.
[0008] Furthermore, the core layer accounts for 45-65% of the thickness of the PE film and is composed of the following raw materials in parts by weight: 60-70 parts of linear low-density polyethylene and 20-30 parts of low-density polyethylene.
[0009] Furthermore, the barrier layer accounts for 15-25% of the thickness of the PE film and is composed of the following raw materials in parts by weight: 70-80 parts of linear low-density polyethylene and 10-20 parts of ethylene-vinyl alcohol copolymer.
[0010] An antibacterial co-extruded PE film is prepared by the following steps:
[0011] The antibacterial layer material, core layer material and barrier layer material are added to three extruders for melt processing respectively, co-extruded into a three-layer co-extruded structure through a die head, cooled and formed, and then longitudinally stretched, transversely stretched, heat-set and rolled to obtain an antibacterial co-extruded PE film.
[0012] Furthermore, the temperature in the molten state is set at 200°C-240°C, and the temperature of the die head is set at 220°C-260°C.
[0013] The antibacterial layer, the core layer and the barrier layer are co-extruded to produce a co-extruded PE film. Polyethylene gives the co-extruded PE film good water vapor barrier properties, and the ethylene-vinyl alcohol copolymer has good processing properties and can also give the PE film good oxygen barrier properties.
[0014] Furthermore, the modified carbon nanotubes are prepared by the following steps:
[0015] S1. In a three-necked flask equipped with a stirring device, triphenylphosphine (PPh3) was dissolved in toluene, chloroacetaldehyde was slowly added dropwise, and the temperature was raised to 50°C. The reaction was stirred for 2 hours. After the reaction was completed, the solvent was removed by distillation under reduced pressure to obtain intermediate 1; the ratio of triphenylphosphine, toluene and chloroacetaldehyde was 26.2g:100mL:7.7g;
[0016] Triphenylphosphine reacts with the chlorine group of chloroacetaldehyde to obtain the quaternary phosphonium product intermediate 1; the specific reaction process is as follows:
[0017]
[0018] S2. In a three-necked flask equipped with a stirring device, add intermediate 1 and N,N-dimethylformamide (DMF), stir evenly, then add diethylenetriamine and piperidine (condensing agent), stir and mix evenly, control the reaction temperature to 75°C, keep the reaction for 4 hours, and after the reaction is completed, remove part of the solvent by reduced pressure distillation, and then purify by column chromatography (the eluent is a mixed solvent of ethyl acetate / methanol, and the volume ratio of the two is 3:2), and remove the eluent by rotary evaporation to obtain intermediate 2; the ratio of the amount of intermediate 1, N,N-dimethylformamide, diethylenetriamine, and piperidine is 32.4g:100mL:11.4g:15mL;
[0019] Under the action of the condensing agent, the aldehyde group on the intermediate 1 condenses with the amino group on the diethylenetriamine to form an imine group (C=N Schiff base structure). By controlling the molar ratio of the two to be close to 1:1 and the diethylenetriamine to be slightly excessive, the intermediate 2 is obtained; the specific reaction process is as follows:
[0020]
[0021] S3. In a three-necked flask equipped with a stirring device, the carboxylated carbon nanotubes were mixed with N,N-dimethylformamide, and the carboxylated carbon nanotubes were evenly dispersed by ultrasonication for 30 minutes, and then the intermediate 2 and dicyclohexylcarbodiimide (DCC) were added, and magnetic stirring was performed for 2 hours. The mixture was placed in a 65°C water bath and ultrasonicated for 2 hours. The water bath was then removed and magnetic stirring was performed at room temperature for 8 hours. The mixture was filtered, washed with anhydrous ethanol for 3-4 times, dried, and ground to obtain pre-modified carbon nanotubes; the ratio of the amount of carboxylated carbon nanotubes, N,N-dimethylformamide, intermediate 2, and DCC was 5g:100mL:7.5g:13.7g;
[0022] Under the action of DCC, -COOH on the surface of the carboxylated carbon nanotubes undergoes an amidation reaction with -NH2 on the intermediate 2, and organic molecules are grafted onto the surface of the carbon nanotubes to obtain pre-modified carbon nanotubes. The specific reaction process is as follows:
[0023]
[0024] S4. At room temperature, in a three-necked flask equipped with a stirring device, mix the pre-modified carbon nanotubes with N,N-dimethylformamide, and perform ultrasonication for 30 minutes to evenly disperse the carboxylated carbon nanotubes. Add 8-chloro-1-octene and triethylamine, start magnetic stirring, control the reaction temperature to 80°C, and keep the reaction for 12 hours. After the reaction is completed, filter and take the filter residue, wash it with anhydrous ethanol for 3-4 times, dry it, and grind it to obtain modified carbon nanotubes; the ratio of the amount of pre-modified carbon nanotubes, N,N-dimethylformamide, 8-chloro-1-octene, and triethylamine is 5g:100mL:4.5g:20mL;
[0025] Triethylamine is used as an acid binding agent to remove hydrogen chloride generated by the reaction, thereby accelerating the reaction, and the secondary amino groups on the pre-modified carbon nanotubes and the chlorine groups on 8-chloro-1-octene undergo nucleophilic substitution reaction to obtain modified carbon nanotubes;
[0026] The prepared modified carbon nanotubes are grafted with organic molecular chains through chemical bonding, that is, an organic layer is formed on the surface of the carbon nanotubes, which can greatly improve the interface compatibility between the carbon nanotubes and the matrix, reduce the agglomeration of the carbon nanotubes, thereby promoting the uniform dispersion of the modified carbon nanotubes in the matrix, giving full play to the antistatic properties of the carbon nanotubes, and also reinforcing the matrix; not only that, the carbon nanotubes are grafted with organic molecular chains, which can effectively prevent the migration and seepage of organic molecules and ensure the durability of various properties; in addition, the organic molecular chains contain quaternary phosphonium salts, Schiff bases, long carbon chains and carbon-carbon double bond structures, among which the quaternary phosphonium salt functional groups, in which the positively charged phosphonium ions are adsorbed on the surface of the bacteria, can interact with the negatively charged cell membrane of the bacteria, penetrate the cell wall, combine with the cell membrane, destroy the surface structure of the cell, make the substances in the cell flow out, stop the respiratory function of the bacteria and cause the cell death. The antibacterial activity of the matrix is better than that of quaternary ammonium salts, and the antistatic performance of the matrix can be enhanced to a certain extent. Moreover, the C=N Schiff base structure can interact with bacterial proteins and enzymes, hindering the synthesis of bacterial nucleotides and amino acids, and synergizing with the quaternary phosphonium salt to greatly enhance the antibacterial performance of the matrix. The long carbon chain belongs to a flexible segment, which can improve the mechanical properties of the matrix and can be interspersed in the molecular chain of the matrix to improve stability. In addition, the long carbon chain can also enhance the antibacterial property of the quaternary phosphonium salt, and belongs to a hydrophobic chain, which can further enhance the surface hydrophobicity of the carbon nanotubes and improve the compatibility with the matrix. Finally, one end of the modified carbon nanotube contains a carbon-carbon double bond, which can be cross-linked with the matrix, so that the modified carbon nanotube is combined with the matrix in a chemical bond block manner, thereby improving the binding force between the modified carbon nanotube and the matrix and making the performance more stable.
[0027] Furthermore, the carboxylated carbon nanotubes are prepared by the following steps:
[0028] The carbon nanotubes are placed in a conical flask, and then mixed acid is added, and ultrasonic treatment is performed in a water bath at 55°C for 6 hours. After the mixture is cooled to room temperature, deionized water is added for dilution, centrifugation is performed, and the mixture is washed with anhydrous ethanol and deionized water for 4-5 times in sequence, dried, and ground to obtain carboxylated carbon nanotubes; the mixed acid is a mixture of 98% by mass concentrated sulfuric acid and 38.7% by mass concentrated hydrochloric acid in a volume ratio of 4:1; the ratio of the carbon nanotubes to the mixed acid is 1g:100mL;
[0029] By subjecting carbon nanotubes to ultrasonic shearing and oxidation treatment with strong acid, a certain number of carboxyl active groups can be introduced into the side walls and tops of the carbon nanotubes, thus laying the foundation for reaction sites for subsequent chemical reactions.
[0030] Beneficial effects of the present invention:
[0031] 1. The present invention prepares a co-extruded PE film by co-extruding an antibacterial layer, a core layer and a barrier layer, which has good water vapor barrier properties. Ethylene-vinyl alcohol copolymer is added to the barrier layer material, which gives the PE film excellent oxygen barrier properties;
[0032] 2. By modifying carbon nanotubes, the compatibility with PE matrix is better than that of ordinary carbon nanotubes, which greatly enhances the antistatic and mechanical properties of PE film; in addition, the organic molecular chains grafted by modified carbon nanotubes can also significantly enhance the antibacterial properties and a certain degree of mechanical and antistatic properties of PE film, and the performance is long-lasting and stable;
[0033] Therefore, the co-extruded PE film prepared by the present invention has excellent barrier properties, high mechanical properties, and stable and efficient antistatic and antibacterial properties, and has important application value in the field of PE co-extruded film technology. DETAILED DESCRIPTION
[0034] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0035] Example 1
[0036] Preparation of carboxylated carbon nanotubes:
[0037] 20 g of carbon nanotubes were placed in a conical flask, and then 2000 mL of concentrated sulfuric acid (mass fraction 98%) and concentrated hydrochloric acid (mass fraction 38.7%) were added in a volume ratio of 4:1 to obtain a mixed acid, and the mixture was ultrasonically treated in a 55°C water bath for 6 h. After the mixture was cooled to room temperature, deionized water was added to dilute it, centrifuged, and washed with anhydrous ethanol and deionized water for 4 times in sequence, dried, and ground to obtain carboxylated carbon nanotubes.
[0038] Example 2
[0039] Preparation of modified carbon nanotubes:
[0040] S1. In a three-necked flask equipped with a stirring device, 26.2 g of triphenylphosphine was dissolved in 100 mL of toluene, 7.7 g of chloroacetaldehyde was slowly added dropwise, and the temperature was raised to 50° C. The mixture was stirred for 2 h. After the reaction was completed, the solvent was removed by distillation under reduced pressure to obtain intermediate 1;
[0041] S2, in a three-necked flask equipped with a stirring device, add 32.4g of intermediate 1 and 100mL of N,N-dimethylformamide, stir evenly, then add 11.4g of diethylenetriamine and 15mL of piperidine, stir and mix evenly, control the reaction temperature to 75°C, keep the reaction for 4h, the reaction is completed, remove part of the solvent by reduced pressure distillation, and then purify by column chromatography (the eluent is a mixed solvent of ethyl acetate / methanol, the volume ratio of the two is 3:2), and remove the eluent by rotary evaporation to obtain intermediate 2;
[0042] S3. In a three-necked flask equipped with a stirring device, 5 g of the carboxylated carbon nanotubes prepared in Example 1 were mixed with 100 mL of N,N-dimethylformamide, and the carboxylated carbon nanotubes were evenly dispersed by ultrasonication for 30 min. Then, 7.5 g of intermediate 2 and 13.7 g of dicyclohexylcarbodiimide were added, and magnetic stirring was performed for 2 h. The mixture was placed in a 65°C water bath and ultrasonicated for 2 h. The water bath was then removed and magnetic stirring was performed for 8 h at room temperature. The mixture was filtered, washed with anhydrous ethanol for 3 times, dried, and ground to obtain pre-modified carbon nanotubes.
[0043] S4. At room temperature and under nitrogen protection, in a three-necked flask equipped with a stirring device, 5 g of pre-modified carbon nanotubes were mixed with 100 mL of N,N-dimethylformamide, and the carboxyl carbon nanotubes were evenly dispersed by ultrasonication for 30 min. 4.5 g of 8-chloro-1-octene and 20 mL of triethylamine were added, and magnetic stirring was turned on. The reaction temperature was controlled to 80 ° C. The reaction was kept warm for 12 h. After the reaction was completed, the residue was filtered and washed with anhydrous ethanol 4 times, dried, and ground to obtain modified carbon nanotubes.
[0044] Example 3
[0045] Preparation of modified carbon nanotubes:
[0046] S1. In a three-necked flask equipped with a stirring device, 52.4 g of triphenylphosphine was dissolved in 200 mL of toluene, 15.4 g of chloroacetaldehyde was slowly added dropwise, and the temperature was raised to 50° C. The mixture was stirred for 2 h. After the reaction was completed, the solvent was removed by distillation under reduced pressure to obtain intermediate 1;
[0047] S2, in a three-necked flask equipped with a stirring device, add 64.8g of intermediate 1 and 200mL of N,N-dimethylformamide, stir evenly, then add 22.8g of diethylenetriamine and 30mL of piperidine, stir and mix evenly, control the reaction temperature to 75°C, keep the reaction for 4h, the reaction is completed, remove part of the solvent by reduced pressure distillation, and then purify by column chromatography (the eluent is a mixed solvent of ethyl acetate / methanol, the volume ratio of the two is 3:2), and remove the eluent by rotary evaporation to obtain intermediate 2;
[0048] S3. In a three-necked flask equipped with a stirring device, 10 g of the carboxylated carbon nanotubes prepared in Example 1 were mixed with 200 mL of N,N-dimethylformamide, and the carboxylated carbon nanotubes were evenly dispersed by ultrasonication for 30 min. Then, 15.0 g of intermediate 2 and 27.4 g of dicyclohexylcarbodiimide were added, and magnetic stirring was performed for 2 h. The mixture was placed in a 65°C water bath and ultrasonicated for 2 h. The water bath was then removed and magnetic stirring was performed for 8 h at room temperature. The mixture was filtered, washed with anhydrous ethanol for 3 times, dried, and ground to obtain pre-modified carbon nanotubes.
[0049] S4. At room temperature and under nitrogen protection, in a three-necked flask equipped with a stirring device, 10 g of pre-modified carbon nanotubes were mixed with 200 mL of N,N-dimethylformamide, and the carboxyl carbon nanotubes were evenly dispersed by ultrasonication for 30 min. 9.0 g of 8-chloro-1-octene and 40 mL of triethylamine were added, and magnetic stirring was turned on. The reaction temperature was controlled to 80 ° C. The reaction was kept warm for 12 h. After the reaction was completed, the residue was filtered and washed with anhydrous ethanol 4 times, dried, and ground to obtain modified carbon nanotubes.
[0050] Example 4
[0051] The antibacterial layer material: 80g of linear low-density polyethylene, 6g of modified carbon nanotubes obtained in Example 2, 3g of paraffin, and 4g of antioxidant 264, the core layer material: 60g of linear low-density polyethylene, 20g of low-density polyethylene, and the barrier layer material: 70g of linear low-density polyethylene and 10g of ethylene-vinyl alcohol copolymer were respectively added into three extruders for melt processing at 200°C, co-extruded into a three-layer co-extruded structure (the core layer is located between the antibacterial layer and the barrier layer) through a 220°C die head, cooled and formed, and then longitudinally stretched, transversely stretched, heat-set, and rolled to obtain an antibacterial co-extruded PE film, and the thickness of the PE film was adjusted to 60μm by controlling the traction speed.
[0052] Example 5
[0053] The antibacterial layer material: 90g linear low-density polyethylene, 15g modified carbon nanotubes obtained in Example 3, 4g paraffin, 6g antioxidant 264, the core layer material: 65g linear low-density polyethylene, 25g low-density polyethylene, the barrier layer material: 75g linear low-density polyethylene, 15g ethylene-vinyl alcohol copolymer were added into three extruders respectively for melt processing at 220°C, co-extruded into a three-layer co-extruded structure (the core layer is located between the antibacterial layer and the barrier layer) through a 240°C die, cooled and formed, and then longitudinally stretched, transversely stretched, heat-set, and rolled to obtain an antibacterial co-extruded PE film, and the thickness of the PE film was adjusted to 60μm by controlling the traction speed.
[0054] Example 6
[0055] The antibacterial layer material: 100g linear low-density polyethylene, 24g modified carbon nanotubes obtained in Example 3, 5g paraffin, 8g antioxidant 264, the core layer material: 70g linear low-density polyethylene, 30g low-density polyethylene, the barrier layer material: 80g linear low-density polyethylene, 20g ethylene-vinyl alcohol copolymer were added into three extruders respectively for melt processing at 240°C, co-extruded into a three-layer co-extruded structure (the core layer is located between the antibacterial layer and the barrier layer) through a 260°C die, cooled and formed, and then longitudinally stretched, transversely stretched, heat-set, and rolled to obtain an antibacterial co-extruded PE film, and the thickness of the PE film was adjusted to 60μm by controlling the traction speed.
[0056] Comparative Example 1
[0057] Ordinary carbon nanotubes of the same mass were used to replace the modified carbon nanotubes in Example 6. The remaining steps were the same as in Example 6 to prepare a PE film. The thickness of the PE film was adjusted to 60 μm by controlling the pulling speed.
[0058] Comparative Example 2
[0059] A commercially available quaternary ammonium salt antibacterial agent of equal quality was used to replace the modified carbon nanotubes in Example 6. The remaining steps were the same as in Example 6 to prepare a PE film. The thickness of the PE film was adjusted to 60 μm by controlling the pulling speed.
[0060] Examples 4-6 and comparative examples 1-2 were made into corresponding shapes according to different test standards and subjected to the following performance tests:
[0061] The tensile strength was determined using the national standard GB / T 1040.3-2006 "Determination of tensile properties of plastics Part 3: Test conditions for films and sheets";
[0062] The surface resistivity is measured using the national standard GB / T 1410-2006 "Test method for volume resistivity and surface resistivity of solid insulating materials";
[0063] The oxygen permeability is measured using the national standard GB / T 1038-2022 "Plastic film and sheeting gas permeability test method pressure difference method";
[0064] The water vapor permeability is measured using the national standard GB / T 1037-2010 "Plastic film and sheeting water vapor permeability determination cup weight gain and weight loss method";
[0065] The national standard GB / T 31402-2015 "Test method for antibacterial performance of plastic surfaces" was adopted, and the film method was used to detect the inhibitory effect on Escherichia coli and Staphylococcus aureus; the method is as follows: Escherichia coli or Staphylococcus aureus bacteria were inoculated on the plate culture medium, covered with a film and preserved for 24 hours, and then live bacteria were cultured; the parallel experimental results of the blank samples were compared to obtain the antibacterial rate of the sample;
[0066] The same standard was used to determine the antibacterial rate of the sample after it was placed at room temperature for 180 days;
[0067] The measured results are shown in the following table:
[0068]
[0069]
[0070] It can be seen from the above table that the co-extruded PE film prepared in the embodiment of the present invention has higher antistatic, antibacterial and mechanical properties than the comparative example, and has excellent barrier properties and long-term stable performance, and has important application value in the field of PE co-extruded film technology.
[0071] In the description of the specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.
[0072] The above contents are merely examples and explanations of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the invention or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.
Claims
1. An antibacterial co-extruded PE film, comprising an antibacterial layer, a core layer and a barrier layer, characterized in that: The raw materials of the antibacterial layer are as follows in parts by weight: 80-100 parts of linear low-density polyethylene, 6-24 parts of modified carbon nanotubes, 3-5 parts of paraffin wax, and 4-8 parts of antioxidant 264; Wherein, the modified carbon nanotubes are prepared by the following steps: S1, dissolving triphenylphosphine in toluene, slowly adding chloroacetaldehyde, and raising the temperature to 50°C, stirring and reacting for 2 hours, and after the reaction is completed, distilling under reduced pressure to obtain intermediate 1; S2, after the intermediate 1 and N, N-dimethylformamide are stirred evenly, diethylenetriamine and piperidine are added, stirred and mixed, reacted at 75° C. for 4 h, the reaction is completed, vacuum distillation, column chromatography purification, rotary evaporation, to obtain intermediate 2; S3, mixing the carboxylated carbon nanotubes with N,N-dimethylformamide, ultrasonicating for 30 min, then adding the intermediate 2 and dicyclohexylcarbodiimide, magnetically stirring for 2 h, ultrasonicating at 65 ° C for 2 h, stirring at room temperature for 8 h, filtering, washing, drying, and grinding to obtain pre-modified carbon nanotubes; S4. At room temperature, under nitrogen protection, mix the pre-modified carbon nanotubes with N,N-dimethylformamide, ultrasonicate for 30 minutes, add 8-chloro-1-octene and triethylamine, start magnetic stirring, react at 80°C for 12 hours, and after the reaction is completed, filter, collect the residue, wash, dry and grind to obtain modified carbon nanotubes.
2. The antibacterial co-extruded PE film according to claim 1, characterized in that: In step S1, the ratio of triphenylphosphine, toluene and chloroacetaldehyde is 26.2 g:100 mL:7.7 g.
3. The antibacterial co-extruded PE film according to claim 1, characterized in that: In step S2, the ratio of the amount of intermediate 1, N,N-dimethylformamide, diethylenetriamine and piperidine is 32.4 g:100 mL:11.4 g:15 mL.
4. The antibacterial co-extruded PE film according to claim 1, characterized in that: In step S3, the ratio of the amount of carboxylated carbon nanotubes, N,N-dimethylformamide, intermediate 2, and DCC is 5 g:100 mL:7.5 g:13.7 g.
5. The antibacterial co-extruded PE film according to claim 1, characterized in that: In step S4, the ratio of the amount of pre-modified carbon nanotubes, N,N-dimethylformamide, 8-chloro-1-octene, and triethylamine is 5 g:100 mL:4.5 g:20 mL.
6. The antibacterial co-extruded PE film according to claim 1, characterized in that: The antibacterial layer accounts for 20-30% of the thickness of the PE film and is composed of the following raw materials in parts by weight: 80-100 parts of linear low-density polyethylene, 6-24 parts of modified carbon nanotubes, 3-5 parts of paraffin wax, and 4-8 parts of antioxidant 264.
7. The antibacterial co-extruded PE film according to claim 1, characterized in that: The barrier layer accounts for 15-25% of the thickness of the PE film and is composed of the following raw materials in parts by weight: 70-80 parts of linear low-density polyethylene and 10-20 parts of ethylene-vinyl alcohol copolymer.
8. The antibacterial co-extruded PE film according to claim 1, characterized in that: The barrier layer accounts for 15-25% of the thickness of the PE film and is composed of the following raw materials in parts by weight: 70-80 parts of linear low-density polyethylene and 10-20 parts of ethylene-vinyl alcohol copolymer.
9. The method for preparing an antibacterial co-extruded PE film according to claim 1, characterized in that: The following steps are involved: The antibacterial layer material, core layer material and barrier layer material are added to three extruders for melt processing respectively, co-extruded into a three-layer co-extruded structure through a die head, cooled and formed, and then longitudinally stretched, transversely stretched, heat-set and rolled to obtain an antibacterial co-extruded PE film.
10. The method for preparing an antibacterial co-extruded PE film according to claim 9, characterized in that: The temperature in the molten state is set at 200°C-240°C, and the temperature of the die head is set at 220°C-260°C.
Citation Information
Patent Citations
Antistatic PE film suitable for packaging powder products and preparation method of antistatic PE film
CN116714335A
Preparation method of conductive polystyrene foam material
CN117186564A
Purifying master batch for odor-removing antibacterial fresh-keeping product and preparation method of purifying master batch
CN117430941A
Efficient antibacterial polyester fabric and preparation method thereof
CN118109955A
Polyester yarn and preparation method thereof
CN118422397A
Cited By
Preparation method of cooling greenhouse film for greenhouse
CN119189380A
Preparation method of high-barrier multi-layer co-extrusion film for food packaging
CN120171154A
A method for preparing a high-barrier multilayer co-extruded film for food packaging
CN120171154B
Antibacterial co-extrusion PE film and preparation method thereof
CN121361251A
An antibacterial co-extruded PE film and a preparation method thereof
CN121361251B