Method for improving dry strength and wet strength performance of paper for daily use
By mixing microfibrillated cellulose with wet strength agent and mixing it with wood pulp slurry, environmental pollution and health risks caused by excessive amounts of wet strength agent in the prior art are solved, and a low-cost and high-performance life is achieved Paper has excellent dry and wet properties.
Patent Information
- Application Number
- CN202411341271.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-25
- Publication Date
- 2024-11-19
AI Technical Summary
When the prior art improves the dry strength and wet strength properties of domestic paper, it is often necessary to increase the amount of wet strength agent, which leads to environmental pollution and health risks. At the same time, adding a large amount of chemical reagents will increase production costs, and it is difficult to have both dry strength and strength. Wet strength performance.
By mixing microfibrillated cellulose with wet strength agent, forming a composite solution and mixing it with wood pulp slurry for dissipation, the dosage of microfibrillated cellulose and wet strength agent is controlled, and the dry and wet strength properties of domestic paper are improved.
It realizes a low-cost and low-humidity strength agent dosage of domestic paper, with high longitudinal dry tensile index and longitudinal wet tensile strength, excellent performance, longitudinal dry tensile index between 64-90N·m·g-1, longitudinal wet Tensile strength is between 160 and 270N·m-1.
Smart Images

Figure CN118979405A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of household paper, and in particular relates to a method for improving the dry strength and wet strength properties of household paper. Background Art
[0002] Tissue paper is inseparable from people's daily life. In recent years, both the production and consumption of tissue paper have been increasing year by year, indicating that people's demand for tissue paper is increasing. With the improvement of living standards, people's requirements for the quality of tissue paper, especially its strength performance, are also increasing.
[0003] Most of the daily household paper has a certain dry strength or a certain wet strength, but the household paper with both dry strength and wet strength can bring people a more comfortable feeling. The household paper with both dry strength and wet strength is relatively more attractive to consumers, stimulating consumption, and can also bring consumers a better consumption experience.
[0004] At present, the method of increasing the strength of paper is usually to increase the amount of wet strength agent. However, excessive use of wet strength agent is harmful to the environment. At the same time, the probability of organic chlorinated compounds in wet strength agent remaining in daily paper is relatively high. Long-term exposure to these harmful substances will pose a potential risk to the health of users. In addition, the strength of paper can be increased by adding a large amount of chemical reagents to improve the degree of pulp treatment, but the production cost will also increase accordingly, which is not suitable for industrial production. Summary of the invention
[0005] In view of this, the object of the present invention is to provide a method for improving the dry strength and wet strength of household paper. The method provided by the present invention uses simple materials, low cost, and a low amount of wet strength agent, and the obtained household paper has both dry strength and wet strength.
[0006] In order to solve the above technical problems, the present invention provides the following technical solutions:
[0007] The present invention provides a method for improving the dry strength and wet strength of household paper, comprising the following steps:
[0008] mixing microfibrillated cellulose, a wet strength agent and water to obtain a composite solution;
[0009] The composite solution is mixed with wood pulp slurry, and then deflaked to obtain raw pulp for household paper;
[0010] The mass of the microfibrillated cellulose in the composite solution accounts for 2% to 8% of the absolute dry mass of the wood pulp;
[0011] The mass of the wet strength agent in the composite solution accounts for 0.4-1.2% of the absolute dry mass of the wood pulp.
[0012] Preferably, the mass of the microfibrillated cellulose accounts for 0.005-0.02% of the total mass of water and the microfibrillated cellulose.
[0013] Preferably, the wet strength agent is urea-formaldehyde resin, melamine-formaldehyde resin, polyamide-polyamine-epichlorohydrin resin, polyamide-polyurea or polyethyleneimine.
[0014] Preferably, the water content of the wood pulp slurry is 70-80%.
[0015] Preferably, the beating degree of the wood pulp slurry is 20-30° SR.
[0016] Preferably, the preparation of the wood pulp slurry comprises:
[0017] The coniferous wood pulp board and the broadleaf wood pulp board are mixed, beaten and fluffed, dried and broken up, the moisture content is measured, and the pulp is refined to obtain wood pulp slurry.
[0018] Preferably, the mass ratio of the coniferous wood pulp board to the broadleaf pulp board is 5:5 to 7:3.
[0019] Preferably, the rotation speed of the deflaking is 5500-6500 rpm.
[0020] Preferably, after obtaining the pulp for daily use paper, the process further comprises papermaking and drying the pulp for daily use paper to obtain daily use paper.
[0021] Preferably, the basis weight of the household paper is 40 to 50 g / m 2 .
[0022] The present invention provides a method for improving the dry strength and wet strength of household paper, comprising the following steps: mixing microfibrillated cellulose, a wet strength agent and water to obtain a composite solution; mixing the composite solution with wood pulp slurry, and performing decomposition to obtain a raw pulp for household paper; the mass of the microfibrillated cellulose in the composite solution accounts for 2% to 8% of the absolute dry mass of the wood pulp slurry; the mass of the wet strength agent in the composite solution accounts for 0.4 to 1.2% of the absolute dry mass of the wood pulp slurry. The present invention uses microfibrillated cellulose as a green adsorption carrier, which has the characteristics of high specific surface area and high free hydroxyl groups, and these characteristics can improve the retention rate of the wet strength agent on paper; after mixing the microfibrillated cellulose and the wet strength agent, they are added to the paper through the wet part in the pulp, thereby improving the dry strength and wet strength of the household paper; by controlling the amount of microfibrillated cellulose and the wet strength agent, the dry strength and wet strength of the household paper are further improved. The test results show that the longitudinal dry tensile index of the household paper prepared by the method provided by the present invention is 64 to 90 N·m·g -1 , longitudinal wet tensile strength is 160~270N·m -1 . BRIEF DESCRIPTION OF THE DRAWINGS
[0023] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.
[0024] Figure 1 is the paper performance curve of the household paper obtained in Examples 1 to 5;
[0025] Figure 2 The curves of the effect of the amount of polyamide polyepichlorohydrin resin (PAE) added on the paper properties in Comparative Examples 1 to 4 and Comparative Example 9;
[0026] Figure 3 This is a curve showing the effect of the amount of microfibrillated cellulose (MFC) added on paper properties in Comparative Examples 5 to 8 and Comparative Example 9. DETAILED DESCRIPTION
[0027] The present invention provides a method for improving the dry strength and wet strength of household paper, comprising the following steps:
[0028] mixing microfibrillated cellulose, a wet strength agent and water to obtain a composite solution;
[0029] The composite solution is mixed with wood pulp slurry, and then debonded to obtain raw pulp for household paper;
[0030] The mass of the microfibrillated cellulose in the composite solution accounts for 2% to 8% of the absolute dry mass of the wood pulp;
[0031] The mass of the wet strength agent in the composite solution accounts for 0.4-1.2% of the mass of the absolutely dry wood pulp.
[0032] In the present invention, unless otherwise specified, the raw materials and equipment used are commercially available products well known in the art.
[0033] The invention mixes microfibrillated cellulose, a wet strength agent and water to obtain a composite solution.
[0034] In the present invention, the mass of the microfibrillated cellulose accounts for 0.005-0.02% of the total mass of water and the microfibrillated cellulose, and more preferably 0.01-0.015%.
[0035] In the present invention, the wet strength agent is preferably urea-formaldehyde resin, melamine-formaldehyde resin, polyamide-polyamine-epichlorohydrin resin, polyamide-polyurea or polyethyleneimine, more preferably urea-formaldehyde resin, melamine-formaldehyde resin, polyamide-polyamine-epichlorohydrin resin or polyamide-polyurea, further preferably polyamide-polyamine-epichlorohydrin resin.
[0036] The present invention has no special requirements for the mixing, and the commonly used technical means in the art can be used. In a specific embodiment of the present invention, microfibrillated cellulose is mixed with water to obtain a microfibrillated cellulose solution, and then a wet strength agent is added. Microfibrillated cellulose is used as a carrier and an adsorbent. After the microfibrillated cellulose is diluted a hundred times, the dispersibility of the microfibrillated cellulose is improved. After the wet strength agent is added, the microfibrillated cellulose fully absorbs the wet strength agent, thereby improving the dispersibility of the wet strength agent and the retention rate of the wet strength agent on the paper.
[0037] After obtaining the composite solution, the present invention mixes the composite solution with wood pulp slurry, performs a first deflaking, and obtains raw pulp for household paper.
[0038] In the present invention, the mass of the microfibrillated cellulose in the composite solution accounts for 2-8%, preferably 3-7%, and more preferably 4-5% of the absolute dry mass of the wood pulp.
[0039] In the present invention, the mass of the wet strength agent in the composite solution accounts for 0.4-1.2% of the mass of the wood pulp absolute dry material, preferably 0.5-1%, and more preferably 0.6-0.8%. In a specific embodiment of the present invention, the mass of the wet strength agent in the composite solution accounts for 0.4%, 0.6%, 0.8%, 1% or 1.2% of the mass of the wood pulp absolute dry material.
[0040] In the present invention, the water content of the wood pulp slurry is preferably 70-80%, more preferably 73-78%, and further preferably 75-77%. In the present invention, the beating degree of the wood pulp slurry is preferably 20-30°SR, and more preferably 23-27°SR.
[0041] In the present invention, the preparation of the wood pulp slurry preferably includes: mixing coniferous wood pulp boards and broadleaf pulp boards, beating and fluffing them, drying and breaking them up, measuring the moisture content, and refining them to obtain wood pulp slurry.
[0042] In the present invention, the mass ratio of the coniferous wood pulp board to the broadleaf pulp board is preferably 5:5 to 7:3, more preferably 5:5, 6:4 or 7:3.
[0043] The present invention has no special requirements for the mixing, and the commonly used technical means in the art can be used.
[0044] In the present invention, the beating and deflaking time is preferably 4 to 8 minutes, more preferably 5 to 6 minutes. The present invention has no special requirements for the beating and deflaking method, and the conventional means of the present invention can be used. Specifically, the wood pulp board is placed in the pulp tank of the Wally beater and water is added to perform beating and deflaking until there are no small pulp lumps.
[0045] There is no special requirement for the spin-drying in the present invention, and conventional means of the present invention can be used. In a specific embodiment of the present invention, a washing machine is used for spin-drying.
[0046] There is no special requirement for the breaking up in the present invention, and conventional means of the present invention can be used. In the specific embodiment of the present invention, a breaking up instrument is used for breaking up.
[0047] In the present invention, the method of measuring the moisture content preferably includes placing the pulp in a sealed bag and homogenizing the moisture content at 0-5° C. The purpose of measuring the moisture content is to calculate the mass of wet pulp required for subsequent refining through the solid content of the pulp.
[0048] The present invention has no special requirements for the refining, and the conventional means of the present invention can be used. In the specific embodiment of the present invention, a vertical pulping machine (PFI pulping machine) is used for refining at a gap of 0.075 mm. Refining is an operation process of treating pulp fibers suspended in water by mechanical action, so that the pulp fibers have the characteristics required for production on a papermaking machine and the produced paper can reach the expected quality. During refining, in addition to being sheared, rubbed and combed by the machine parts, the fiber cell wall also undergoes displacement, deformation and rupture, and absorbs water and swells, producing fine fibers, making the pulp soft and plastic, and also increasing the chance of the hydroxyl groups in the cellulose molecular chain to combine with the hydrogen chain, thereby improving the bonding force between the fibers.
[0049] Specifically, when performing PFI refining, according to the standard of adding 30g of absolute dry pulp and 10% pulp concentration in the instrument, the pulp dispersed evenly in the present invention is added, the moisture content of the dispersed evenly pulp is measured, and the amount of wet pulp required for 30g of absolute dry pulp and the amount of water to be added are determined based on the measured moisture content. The PFI reference standard is GB / T 29287-2012.
[0050] In the present invention, the deflaking speed is preferably 5500-6500 rpm, more preferably 5800-6200 rpm. The deflaking in the present invention is performed in a deflaker, and the deflaker is set to a certain number of revolutions, and automatically stops when the number of revolutions reaches a certain value.
[0051] In the present invention, after obtaining the pulp for daily use paper, it is preferred to further include papermaking and drying the pulp for daily use paper to obtain daily use paper. In a specific embodiment of the present invention, a dynamic paper sheet former is used for papermaking.
[0052] In the present invention, the basis weight of the household paper is preferably 40 to 50 g / m 2 , more preferably 43 to 46 g / m 2 .
[0053] The present invention has no special requirements for the drying, and conventional means of the present invention may be used, such as drying.
[0054] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution of the present invention will be clearly and completely described in conjunction with specific embodiments below. The described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Any modification, equivalent replacement, improvement, etc. made to the implementation methods of the present invention based on the technical essence and general principles of the present invention without creative work should be within the scope of protection of the present invention.
[0055] Slurry preparation
[0056] Coniferous wood pulp (name, Moon; origin, Canada; tree species, spruce) and broadleaf pulp (name, Goldfish; origin, Brazil; tree species, eucalyptus) were mixed in a mass ratio of 6:4 to obtain 360 g of mixed pulp, and the mixed pulp was soaked in 5 L of water for 4 h. The large pulp boards were torn into small pieces of 4 cm × 4 cm, and placed in the pulp tank of a Wall-e beater. 18 L of deionized water at 20°C was added for beating and fluffing (beating). After 5 minutes, the small pulp lumps were removed to obtain the fluffed pulp.
[0057] The deflated pulp is dried, placed in a disperser, put into a sealed bag, and placed in a refrigerator to evenly distribute the moisture. The moisture content of the dispersed pulp is measured to be 65%. The dispersed pulp is refined with a vertical beater, water is added, and the pulp is ground to 26°SR with a gap of 0.075 mm to obtain a wood pulp slurry with a moisture content of 75%, which is set aside.
[0058] Example 1
[0059] Weigh microfibrillated cellulose (MFC) according to 2% of the absolute dry matter of wood pulp slurry, disperse MFC with deionized water to obtain 0.01wt% MFC solution. Add polyamide polyepichlorohydrin resin (PAE) to the 0.01wt% MFC solution, with the absolute dry matter of PAE accounting for 0.4% of the absolute dry matter of wood pulp slurry, to obtain a PAE-MFC composite solution. Mix the pulp and the PAE-MFC composite solution in a deflaker and deflake for 6000r, transfer to the slurry barrel of a dynamic paper former and mix and stir for 2 minutes to obtain a pulp for household paper. The obtained pulp for household paper is made into several pieces with a quantitative of 45g / m 2 The daily tissue paper is dried into shape and stored.
[0060] Example 2
[0061] MFC was weighed at 2% of the absolute dry weight of the wood pulp slurry, and PAE was weighed at 0.6% of the absolute dry weight of the wood pulp slurry. Other conditions were the same as those in Example 1.
[0062] Example 3
[0063] MFC was weighed at 2% of the absolute dry weight of the wood pulp slurry, and PAE was weighed at 0.8% of the absolute dry weight of the wood pulp slurry. Other conditions were the same as those in Example 1.
[0064] Example 4
[0065] MFC was weighed at 2% of the absolute dry weight of the wood pulp slurry, and PAE was weighed at 1% of the absolute dry weight of the wood pulp slurry. Other conditions were the same as those in Example 1.
[0066] Example 5
[0067] MFC was weighed at 2% of the absolute dry weight of the wood pulp slurry, and PAE was weighed at 1.2% of the absolute dry weight of the wood pulp slurry. Other conditions were the same as those in Example 1.
[0068] Comparative Example 1
[0069] PAE absolute dry material was weighed at 0.3% of the absolute dry material of wood pulp, and no MFC was added. Other conditions were the same as those in Example 1.
[0070] Comparative Example 2
[0071] PAE absolute dry material was weighed at 0.6% of the absolute dry material of wood pulp, and no MFC was added. Other conditions were the same as those in Example 1.
[0072] Comparative Example 3
[0073] PAE absolute dry material was weighed at 0.9% of the absolute dry material of wood pulp, and no MFC was added. Other conditions were the same as those in Example 1.
[0074] Comparative Example 4
[0075] PAE absolute dry material was weighed at 1.2% of the absolute dry material of wood pulp, and no MFC was added. Other conditions were the same as those in Example 1.
[0076] Comparative Example 5
[0077] MFC was weighed according to 2% of the absolute dry weight of wood pulp, without adding PAE, and other conditions were the same as those in Example 1
[0078] Comparative Example 6
[0079] MFC was weighed according to 4% of the absolute dry weight of wood pulp, without adding PAE, and other conditions were the same as those in Example 1.
[0080] Comparative Example 7
[0081] MFC was weighed according to 6% of the absolute dry weight of wood pulp, without adding PAE, and other conditions were the same as those in Example 1.
[0082] Comparative Example 8
[0083] MFC was weighed according to 8% of the absolute dry weight of wood pulp, without adding PAE, and other conditions were the same as those in Example 1.
[0084] Comparative Example 9
[0085] No microfibrillated cellulose and PAE were added, and other conditions were the same as those in Example 1.
[0086] The dry strength and wet strength of the household paper obtained in Examples 1 to 5 and Comparative Examples 1 to 3, 6, and 8 to 9 were tested with reference to GB / T 12914-2018 and QB / T 4508-2023, and the test results are shown in Table 1.
[0087] Table 1 Test results of dry strength and wet strength of household paper prepared in Examples 1 to 5 and Comparative Examples 1 to 3, 6, 8 to 9
[0088]
[0089] As can be seen from Table 1, the longitudinal dry tensile strength and longitudinal wet tensile strength of the household paper prepared by the present invention are excellent. If microfibrillated cellulose and PAE are not added, the longitudinal dry tensile index of the obtained paper is 30.5 N·m·g -1 , longitudinal wet tensile strength index is 100N·m -1 , the dry strength and wet strength of the paper are poor. If only microfibrillated cellulose or PAE is added, although the dry strength and wet strength of the paper are increased, the increase is not much. If microfibrillated cellulose and PAE are added at the same time, the longitudinal dry tensile index of the paper is between 64 and 90 N·m·g -1 , longitudinal wet tensile strength is 160~270N·m -1 When the dosage of microfibrillated cellulose stock solution is 2% of the absolute dry matter of wood pulp slurry and the absolute dry matter of PAE accounts for 1.2% of the absolute dry matter of wood pulp slurry, the dry strength and wet strength of the obtained household paper are the largest.
[0090] Figure 1 The paper performance curves of the household paper obtained in Examples 1 to 5 are shown in FIG. Figure 1 It can be seen that the household paper prepared by the present invention has excellent longitudinal dry tensile strength, longitudinal wet tensile strength and transverse tensile strength. As the proportion of PAE in the PAE-MFC composite solution increases, the performance of the paper is also improved. However, if the amount of PAE added is further increased, the strength of the paper is not greatly improved and the cost will increase, which does not meet the actual requirements. At the same time, the continued addition of MFC will block the pores of the paper and make the paper airtight.
[0091] Figure 2 The following is a curve showing the effect of the amount of polyamide polyepichlorohydrin resin (PAE) added on paper properties in Comparative Examples 1 to 4 and Comparative Example 9. Figure 2It can be seen that as the amount of PAE added increases, the transverse tensile strength and longitudinal wet tensile strength of the prepared paper gradually increase, and the longitudinal tensile index first increases and then decreases. This shows that PAE wet strength agent is mainly used to improve the wet strength of paper, and also has a promoting effect on dry strength. However, the more the amount is used, the better the dry strength of the paper is. Experiments show that when the amount added reaches a certain amount, continuing to increase the amount does not have a better effect on the performance of the paper.
[0092] Figure 3 The curves of the effect of the amount of microfibrillated cellulose (MFC) added on the paper properties in Comparative Examples 5 to 8 and Comparative Example 9 are shown in FIG. Figure 3 It can be seen that as the amount of MFC added increases, the transverse tensile strength, longitudinal wet tensile strength and longitudinal tensile index of the prepared paper gradually increase. This shows that the addition of MFC will make the connection between fibers tighter and strengthen the connection between fibers through hydrogen bonds, thereby improving the strength of the paper. The pores of fiber pulp are also conducive to the retention of MFC, so MFC is suitable as a reinforcing agent and retention aid. However, it is worth noting that excessive use of MFC will block the pores of the paper, leading to a series of problems such as airtightness. Therefore, the present invention controls the amount of MFC added to 2% to 8% of the absolute dry mass of the wood pulp slurry.
[0093] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for improving the dry strength and wet strength of household paper, characterized in that: The following steps are involved: mixing microfibrillated cellulose, a wet strength agent and water to obtain a composite solution; The composite solution is mixed with wood pulp slurry, and then deflaked to obtain raw pulp for household paper; The mass of the microfibrillated cellulose in the composite solution accounts for 2% to 8% of the absolute dry mass of the wood pulp; The mass of the wet strength agent in the composite solution accounts for 0.4-1.2% of the absolute dry mass of the wood pulp.
2. The method according to claim 1, characterized in that The mass of the microfibrillated cellulose accounts for 0.005-0.02% of the total mass of water and the microfibrillated cellulose.
3. The method according to claim 1, characterized in that The wet strength agent is urea-formaldehyde resin, melamine-formaldehyde resin, polyamide-polyamine-epichlorohydrin resin, polyamide-polyurea or polyethyleneimine.
4. The method according to claim 1, characterized in that: The water content of the wood pulp slurry is 70-80%.
5. The method according to claim 1, characterized in that The beating degree of the wood pulp slurry is 20-30°SR.
6. The method according to claim 1, characterized in that The preparation of the wood pulp slurry comprises: The coniferous wood pulp board and the broadleaf wood pulp board are mixed, beaten and fluffed, dried and broken up, the moisture content is measured, and the pulp is refined to obtain wood pulp slurry.
7. The method according to claim 6, characterized in that The mass ratio of the coniferous wood pulp board to the broadleaf pulp board is 5:5 to 7:
3.
8. The method according to claim 1, characterized in that The rotation speed of the delamination is 5500-6500 rpm.
9. The method according to claim 1, characterized in that: After obtaining the raw pulp for daily use paper, the method further includes papermaking and drying the raw pulp for daily use paper to obtain daily use paper.
10. The method according to claim 9, characterized in that The basis weight of the daily paper is 40 to 50 g / m 2 .
Citation Information
Patent Citations
A method to form a web comprising fibers
CN109983176A
Absorbent paper products having unique physical strength properties
CN110139961A
Paper base material, preparation method thereof and flexible paper-based packaging body
CN117904893A