Lithium ion secondary battery

By using low viscosity solvents in lithium-ion secondary batteries and optimizing the distribution of lithium iron phosphate particles and combining carbon nanotube conductive agents, the problems of temperature increase and performance limitation of lithium-ion batteries during fast charging are solved, and the battery is realized Efficient fast charging, long cycles and safety performance improvements.

CN118983498AActive Publication Date: 2024-11-19ZHUHAI COSMX POWER BATTERY CO LTD

Patent Information

Application Number
CN202411040356.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-19
Estimated Expiration
2044-07-31

AI Technical Summary

Technical Problem

The temperature rise of existing lithium-ion batteries during fast charging is high, resulting in limited rate performance and fast charging performance. The low electron conduction and ion conduction of lithium iron phosphate positive electrode materials limit the cycle life and safety performance of the battery.

Method used

By using low viscosity C1-C4 linear organic solvents in lithium-ion secondary batteries and controlling the particle size distribution of lithium iron phosphate primary and secondary particles, adjusting their mass proportion and solvent ratio in electrolyte, combining carbon nanometers Tube conducting agent and optimize electrolyte components to improve the transmission efficiency of lithium ions and electron conduction.

Benefits of technology

The fast charging performance improvement, extreme power improvement, cycle performance enhancement, lithium-ion secondary battery reduction, temperature rise reduction and battery expansion control are achieved, improving the overall performance and safety of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118983498A_ABST
    Figure CN118983498A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of lithium batteries, and provides a lithium ion secondary battery. The lithium ion secondary battery comprises a positive plate, a negative plate and an electrolyte, the positive plate comprises lithium iron phosphate primary particles of which the Dv50 is a1 [mu] m and lithium iron phosphate secondary particles of which the Dv50 is recorded as a2, a1lt; a2; based on the total mass of the positive electrode active material, the mass ratio of the lithium iron phosphate primary particles is w1; the electrolyte comprises a first solvent, and the first solvent comprises a C1-C4 linear organic solvent; the mass ratio of the first solvent is recorded as S1 based on the total mass of the solvent; wherein a1, w1 and S1 meet the following relational expression: # imgabs0 #, by controlling the addition amount of the first solvent, and when the Dv50 and mass ratio of the positive electrode material lithium iron phosphate primary particles meet the above conditions, the rapid charge performance of the battery can be improved, the limit power of the battery can be improved, the cycle performance and capacity retention ratio of the battery can be improved, and the temperature rise during rapid charge and the expansion of the battery can be reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of lithium batteries, and in particular to a lithium ion secondary battery. Background Art

[0002] Compared with traditional batteries, lithium-ion batteries have advantages such as high specific energy, long cycle life, no pollution, and high operating voltage, so they have been widely used in many fields such as portable electronic devices, energy storage, and automotive power. With the gradual promotion of electric vehicles, the demand for fast charging performance and safety performance of power batteries is increasing.

[0003] In order to improve the fast charging performance and safety performance of the battery, the mainstream power battery still uses lithium iron phosphate batteries, which is attributed to the higher safety performance of lithium iron phosphate batteries compared to ternary batteries. However, some inherent disadvantages of lithium iron phosphate positive electrodes, such as the low ion conductivity and electron conductivity of lithium iron phosphate positive electrode materials, make the battery temperature rise higher during fast charging, which limits the rate performance and fast charging performance. Summary of the invention

[0004] The purpose of the present invention is to overcome the above-mentioned problems existing in the prior art and provide a lithium ion secondary battery. In the lithium ion secondary battery, by using a first solvent and controlling the amount of the first solvent added, the Dv50 and mass ratio of the primary particles of lithium iron phosphate, a positive electrode material, are controlled to meet It can improve the fast charging performance of the battery, increase the battery's ultimate power, improve the battery's cycle performance and capacity retention rate, reduce lithium plating, reduce temperature rise during fast charging, and reduce battery expansion.

[0005] In order to achieve the above object, the present invention provides a lithium ion secondary battery, the lithium ion secondary battery comprising a positive electrode sheet, a negative electrode sheet and an electrolyte;

[0006] The positive electrode sheet includes a positive electrode current collector and a positive electrode active material layer disposed on at least one side of the positive electrode current collector; the positive electrode active material layer includes a positive electrode active material; the positive electrode active material includes lithium iron phosphate primary particles and lithium iron phosphate secondary particles, the Dv50 of the lithium iron phosphate primary particles is recorded as a1μm, the Dv50 of the lithium iron phosphate secondary particles is recorded as a2μm, and the Dv50 of the lithium iron phosphate secondary particles is recorded as a1 <a2;

[0007] Based on the total mass of the positive electrode active material, the mass proportion of the lithium iron phosphate primary particles is recorded as w1;

[0008] The electrolyte includes a solvent, the solvent includes a first solvent, and the first solvent includes a C1-C4 linear organic solvent; the mass proportion of the first solvent is recorded as S1 based on the total mass of the solvent;

[0009] Among them, a1, w1 and S1 satisfy the following relationship:

[0010] The present invention adopts the above technical solution to achieve the following beneficial effects:

[0011] In the lithium-ion secondary battery provided by the present invention, the linear organic solvent C1-C4 has a low viscosity. By using a low-viscosity first solvent, the transmission impedance of lithium ions in the electrolyte body and the interface between the electrolyte and the positive electrode can be reduced; at the same time, the Dv50 and mass ratio of the primary particles of lithium iron phosphate, the positive electrode material, are controlled to shorten the transmission distance of lithium ions inside the positive electrode material particles, thereby achieving rapid transmission of lithium ions in the electrolyte body, the interface between the electrolyte and the positive electrode, and the inside of the positive electrode particles, which can improve the fast charging performance of the battery, enhance the battery's ultimate power, improve the battery's cycle performance and capacity retention rate, reduce lithium plating, reduce temperature rise during fast charging, and reduce battery expansion.

[0012] The endpoints and any values ​​of the range disclosed in this article are not limited to the precise range or value, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article. Herein, in the absence of special instructions, data ranges include endpoints. BRIEF DESCRIPTION OF THE DRAWINGS

[0013] Figure 1 Shown is a schematic diagram of the structure of a square shell battery.

[0014] Figure 2 Shown are schematic diagrams of the structure of square shell batteries at different angles.

[0015] Figure 3 Shown is a schematic diagram of the cross-sectional structure of the battery shell in a square shell battery.

[0016] Figure numerals: 1-shell; 11-third side; 12-fourth side; 2-top cover; 3-positive pole; 4-negative pole; 5-liquid injection hole; 6-explosion-proof valve; 61-explosion-proof plate; 62-notched groove; 7-bottom wall. DETAILED DESCRIPTION

[0017] The specific embodiments of the present invention are described in detail below. It should be understood that the specific embodiments described herein are only used to illustrate and explain the present invention, and are not used to limit the present invention.

[0018] Unless otherwise defined, all scientific and technical terms used in the present invention have the same meanings as commonly understood by one of ordinary skill in the art to which the present invention relates.

[0019] In the present invention, the terms "battery", "lithium battery", "lithium-ion battery" and "lithium-ion secondary battery" all have the same meaning and refer to lithium-ion secondary batteries, which generally include an electrode assembly (such as a positive electrode sheet, a negative electrode sheet and a separator), a container (shell) for accommodating the electrode assembly, and an electrolyte.

[0020] In the present invention, the term "Dv50" refers to the particle size corresponding to when the cumulative volume particle size distribution percentage of a sample reaches 50%. Dv50 can be tested using a laser particle size analyzer.

[0021] In the present invention, the term "particle size range" means that the diameter of the lithium iron phosphate particles all fall within this range. At the same time, the present invention allows a certain error, that is, when the particle size of particles accounting for less than 5% of the total number is not within the required range, it is considered to meet the requirements, which can be measured by a transmission electron microscope (TEM).

[0022] In the present invention, the term "diameter" refers to the maximum inner straight line distance connecting two points on the surface of a lithium iron phosphate particle.

[0023] In the present invention, the term "low solvation energy" refers to a state in which the interaction between solvent molecules and ions or molecules dissolved therein in the electrolyte is weak.

[0024] In the present invention, the term "limit power" refers to the maximum power that a lithium battery can output under certain conditions, such as the power output by a lithium battery at a high rate of discharge in a short period of time when a car is started.

[0025] In the present invention, the term "low viscosity solvent" refers to a solvent having a viscosity of less than or equal to 0.5 mPa.s. The term "high viscosity solvent" refers to a solvent having a viscosity greater than 0.5 mPa.s. The test method for solvent viscosity refers to the rotation method in the national standard GB / T 10247-2008, and the viscosity is measured by a rheometer.

[0026] The present invention provides a lithium ion secondary battery, which comprises a positive electrode sheet, a negative electrode sheet and an electrolyte;

[0027] The positive electrode sheet includes a positive electrode current collector and a positive electrode active material layer disposed on at least one side of the positive electrode current collector; the positive electrode active material layer includes a positive electrode active material; the positive electrode active material includes lithium iron phosphate primary particles and lithium iron phosphate secondary particles, the Dv50 of the lithium iron phosphate primary particles is recorded as a1μm, the Dv50 of the lithium iron phosphate secondary particles is recorded as a2μm, and the Dv50 of the lithium iron phosphate secondary particles is recorded as a1 <a2;

[0028] Based on the total mass of the positive electrode active material, the mass proportion of the lithium iron phosphate primary particles is recorded as w1;

[0029] The electrolyte includes a solvent, the solvent includes a first solvent, and the first solvent includes a C1-C4 linear organic solvent; the mass proportion of the first solvent is recorded as S1 based on the total mass of the solvent;

[0030] Among them, a1, w1 and S1 satisfy the following relationship:

[0031] In the present invention, The larger the value, the better the limit power of the lithium-ion secondary battery, but it will deteriorate the battery's cycle performance or increase battery expansion; the reason may be that the larger the mass proportion of the lithium iron phosphate primary particles, the more active sites on the surface of the positive electrode sheet, which will lead to serious decomposition of the first solvent in the electrolyte and cause gas production. Therefore, it is necessary to control The cycle performance and the ultimate power of lithium batteries can be achieved in the range of 0.2-3.5. When w1 is increased, it means that more primary lithium iron phosphate particles (small particles) and fewer secondary lithium iron phosphate particles (large particles) are used as positive electrode materials. As the value of increases, the fast charging performance of the positive electrode improves, and the use of low-viscosity solvents can be reduced (reducing S1) to achieve longer battery cycle performance. Similarly, when a1 decreases, The value of increases, the Dv50 of the positive electrode material particles used is smaller, the transmission distance of lithium ions in the positive electrode solid phase becomes shorter, the fast charging performance of the positive electrode becomes better, and the use of the low-viscosity first solvent is reduced (i.e., S1 is reduced) to achieve a longer battery cycle performance. On the contrary, when w1 decreases and a1 increases, The value of decreases, the fast charging performance of the positive electrode becomes weaker, and more first solvent needs to be used, that is, the amount of the first solvent used is increased (increase S1), to reduce the transmission impedance of lithium ions at the interface. Therefore, by adjusting the Dv50 and mass proportion of the lithium iron phosphate primary particles and the mass proportion of the first solvent to meet When the lithium-ion secondary battery is charged, the battery can have a better limit power without deteriorating the fast charge cycle performance.

[0032] In general, the viscosity of the linear organic solvents C1-C4 is relatively low (viscosity ≤ 0.5 mPa.s). The present invention can reduce the transmission impedance of lithium ions in the electrolyte body and the interface between the electrolyte and the positive electrode by using a low-viscosity first solvent; at the same time, the Dv50 and mass ratio of the primary particles of the positive electrode material lithium iron phosphate are controlled to shorten the transmission distance of lithium ions inside the positive electrode material particles, thereby achieving rapid transmission of lithium ions in the electrolyte body, the interface between the electrolyte and the positive electrode, and inside the positive electrode particles, thereby improving the fast charging performance of the battery.

[0033] The positive electrode active material in the present invention includes lithium iron phosphate primary particles with a smaller Dv50 and lithium iron phosphate secondary particles with a larger Dv50, which are mixed. The large and small particles are used in combination. The lithium iron phosphate primary particles shorten the solid phase transmission distance of lithium ions from the surface of the particles to the inside of the particles, and the positive electrode fast charging performance is better; the lithium iron phosphate secondary particles can avoid the compaction density of the positive electrode particle powder being too low, resulting in a decrease in the battery energy density, so that the first lithium iron phosphate is mixed with the lithium iron phosphate secondary particles, which can take into account the fast charging performance and energy density of the battery.

[0034] In some embodiments, The value of can be, for example, 0.2, 0.3, 0.5, 0.6, 0.8, 1.0, 1.2, 1.5, 1.6, 1.8, 2.0, 2.2, 2.4, 2.5, 2.6, 2.8, 3.0, 3.2, 3.5, preferably

[0035] In some embodiments, the Dv50a1 of the lithium iron phosphate primary particles satisfies: 0.1 μm ≤ a1 ≤ 0.4 μm, for example, a1 may be 0.1 μm, 0.2 μm, 0.3 μm, or 0.4 μm. When a1, w1, and S1 satisfy When the value of a1 is adjusted to meet the above range, the smaller the Dv50 of the lithium iron phosphate primary particles, the better the kinetics, the smaller the Dv50 of the positive electrode active material (positive electrode particles), the shorter the solid phase transmission distance of lithium ions from the particle surface to the inside of the particle, the better the positive electrode fast charging performance, and the higher the capacity retention rate. However, when the Dv50 of the lithium iron phosphate primary particles is less than 0.1μm, the current positive electrode process is difficult to achieve, and it will increase the active sites on the positive electrode surface, resulting in increased battery gas production. If w1 and S1 remain unchanged, when the Dv50 of the lithium iron phosphate primary particles is greater than 0.4μm, the fast charging performance of the lithium battery will deteriorate, and the kinetics will be low, which is easy to cause lithium deposition in the battery. After lithium deposition, the capacity retention rate decreases, and it is easy to cause battery gas production.

[0036] In some embodiments, the Dv50 of the lithium iron phosphate secondary particles satisfies: 1μm≤a2≤2μm, for example, a2 can be 1μm, 1.1μm, 1.2μm, 1.3μm, 1.4μm, 1.5μm, 1.6μm, 1.7μm, 1.8μm, 1.9μm, 2.0μm. The smaller the Dv50 of the lithium iron phosphate secondary particles, the smaller the Dv50 of the positive electrode active material (positive electrode particles), the shorter the solid phase transmission distance of lithium ions from the surface of the particles to the inside of the particles, the better the fast charging performance, which is beneficial to improving the fast charging performance of the battery. When the Dv50 of the lithium iron phosphate secondary particles is less than 1μm, the compaction density of the positive electrode particle powder is too low, resulting in a decrease in the battery energy density, and when the Dv50 of the lithium iron phosphate secondary particles is greater than 2μm, the positive electrode lithium iron phosphate secondary particles are too large, and the transmission path of lithium ions in the second lithium iron phosphate is long, resulting in a decrease in the rate performance of the lithium battery.

[0037] In some embodiments, the particle size range of the lithium iron phosphate primary particles is 0.01 μm-1 μm, for example, it can be 0.01 μm, 0.05 μm, 0.1 μm, 0.2 μm, 0.3 μm, 0.4 μm, 0.5 μm, 0.6 μm, 0.7 μm, 0.8 μm, 0.9 μm, 1 μm. The particle size range of the lithium iron phosphate secondary particles is 1 μm-10 μm, for example, it can be 1 μm, 2 μm, 3 μm, 4 μm, 5 μm, 6 μm, 7 μm, 8 μm, 9 μm, 10 μm. When the positive electrode material particles are a mixture of lithium iron phosphate primary particles and lithium iron phosphate secondary particles, the particle size range of the lithium iron phosphate primary particles and the lithium iron phosphate secondary particles is adjusted at the same time, so that the Dv50 of the lithium iron phosphate primary particles and the lithium iron phosphate secondary particles can be within the protection scope of the present invention, thereby improving the fast charging performance of the battery and increasing the energy density of the battery.

[0038] In some embodiments, the mass proportion w1 of the lithium iron phosphate primary particles satisfies: 10%≤w1≤60%, for example, w1 can be 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, 50%, 55%, 60%, preferably 20%≤w1≤50%. As the mass proportion w1 of the lithium iron phosphate primary particles increases, the battery's ultimate power increases, but the battery's expansion also increases; if the mass proportion w1 of the lithium iron phosphate primary particles is too small, it is easy to cause lithium deposition in the battery. When a1, w1 and S1 meet When the value of w1 is adjusted to meet the above range, it can avoid that w1 is too large, resulting in a low compaction density of the positive electrode sheet, which leads to a decrease in the energy density of the battery, thereby improving the energy density of the battery; and avoid that w1 is too large, resulting in an increase in surface active sites, which leads to serious decomposition of the electrolyte and gas production, thereby reducing the expansion of the battery; it can also avoid that w1 is too small and cannot effectively shorten the solid phase transmission distance of lithium ions, thereby improving the fast charging performance of the battery and reducing lithium plating.

[0039] Test method for detecting the mass ratio of lithium iron phosphate primary particles in the battery: The volume fraction of lithium iron phosphate primary particles and lithium iron phosphate secondary particles can be obtained by testing with a Malvern laser particle size analyzer. For lithium iron phosphate materials, the chemical structure and crystal density are the same, mass = volume * density, the density is the same, the mass ratio = volume ratio, and the volume ratio is the mass ratio.

[0040] In some embodiments, if the positive electrode active material includes only lithium iron phosphate primary particles and lithium iron phosphate secondary particles, the mass ratio of the lithium iron phosphate secondary particles is 1-w1.

[0041] In some embodiments, the mass proportion S1 of the first solvent satisfies: 10%≤S1≤90%, for example, S1 can be 10%, 20%, 30%, 40%, 50%, 60%, 70%, 80%, 90%, more preferably 20%≤S1≤70%. The more low-viscosity first solvent there is, the smaller the impedance of lithium ion transmission in the electrolyte liquid phase, the lower the solvation energy of the first solvent, and the lithium ion interface transmission impedance can be reduced. When a1, w1 and S1 meet When the value of S1 is adjusted to meet the above range, the impedance of lithium ion migration in the electrolyte body and the transmission impedance of lithium ions at the interface can be reduced, further improving the fast charging performance of the battery; at the same time, avoid using too much S1, which will result in less high-viscosity solvent, causing the interface generated by the electrolyte at the negative electrode to be unstable, resulting in continuous decomposition of the electrolyte, increased gas production, and a higher battery expansion rate.

[0042] In some embodiments, the viscosity of the first solvent is ≤0.5 mPa.s, and the first solvent includes at least one or more of ethyl acetate EA (0.426 mPa.s), methyl acetate MA (0.364 mPa.s), methyl formate MF (0.328 mPa.s), ethylene glycol dimethyl ester (0.46 mPa.s), dimethanol formal DMM (0.33 mPa.s), and acetonitrile AN (0.35 mPa.s), preferably ethyl acetate.

[0043] In some embodiments, the solvent further comprises a second solvent, the second solvent comprises a C1-C10 cyclic organic solvent and / or a linear organic solvent having a carbon number greater than 4, and the viscosity of the second solvent is greater than 0.5 mPa.s. When the present invention uses a low-viscosity first solvent, and when the lithium iron phosphate primary particles and the lithium iron phosphate secondary particles are mixed and used, the solvent is adjusted to include a high-viscosity second solvent, which can make the interface generated by the electrolyte at the negative electrode more stable, reduce the decomposition and gas production of the electrolyte, and reduce the expansion of the battery.

[0044] In some embodiments, the second solvent includes at least one or more of ethylene carbonate EC (1.9 mPa.s 40°C), propylene carbonate PC (2.53 mPa.s), butylene carbonate BC (3.2 mPa.s), γ-butyrolactone (1.73 mPa.s), diethyl carbonate DEC (0.748 mPa.s), ethyl methyl carbonate EMC (0.65 mPa.s), dimethyl carbonate DMC (0.58 mPa.s), propyl propionate PP (0.68 mPa.s), and ethyl propionate EP (0.502 mPa.s).

[0045] In some embodiments, the positive electrode active material layer further comprises a conductive agent; the conductive agent comprises carbon nanotubes, and the aspect ratio of the carbon nanotubes is recorded as a3. Although the present invention uses a low-viscosity first solvent and a mixture of lithium iron phosphate primary particles and lithium iron phosphate secondary particles, a1, w1 and S1 meet When the positive electrode material is charged, the lithium ions can be quickly transferred between the interface and the solid phase of the positive electrode particles, but the improvement effect on the electronic conduction of the positive electrode material particles is not obvious. The electrochemical system still needs fast electron transfer to achieve rapid energy conversion of the battery system. In order to further improve the electronic conduction of the positive electrode material and reduce the bulk impedance of the battery, the present invention also adds a carbon nanotube conductive agent to the positive electrode active material layer. Carbon nanotubes include multi-walled carbon nanotubes and / or single-walled carbon nanotubes.

[0046] In some embodiments, the aspect ratio a3 of the carbon nanotubes, the mass proportion w2 of the carbon nanotubes, and the mass proportion S1 of the first solvent satisfy the relationship: 0.4≤a3*w2*S1≤8, for example, 0.4, 0.5, 0.6, 0.8, 1.0, 2.0, 3.0, 4.0, 5.0, 6.0, 7.0, 8.0, preferably 0.5≤a3*w2*S1≤6. When a1, w1, and S1 satisfy When a3, w2 and S1 are adjusted to meet 0.4≤a3*w2*S1≤8, the battery has a lower body impedance reduction and excellent limit power, and can meet the battery's long cycle at a high rate. The larger the a3*w2*S1 value, the faster the charge is transferred in the positive current collector and the positive electrode membrane, and the faster the charge is transferred in the lithium ion electrolyte liquid phase, which improves the fast charging performance of the lithium ion battery. In the formula 0.4≤a3*w2*S1≤8, when the aspect ratio a3 of the carbon nanotubes is increased, the amount of carbon nanotubes used w2 is increased, that is, the a3*w2 value increases, the conductivity of the positive electrode sheet is better; increasing the amount of low viscosity solvent used, that is, increasing S1, can reduce the transmission impedance of lithium ions in the electrolyte liquid phase, thereby reducing the body impedance of the battery. When the conductivity of the positive electrode sheet is good, that is, a3*w2 is large, it is necessary to reduce the use of S1 to prevent the electrolyte from oxidizing and producing gas at the positive electrode, causing battery failure.

[0047] In some embodiments, the aspect ratio a3 of the carbon nanotubes satisfies: 200≤a3≤1500, for example, a3 can be 200, 300, 400, 500, 600, 700, 800, 900, 1000, 1100, 1200, 1300, 1400, 1500, more preferably 500≤a3≤1000. The larger the aspect ratio of the carbon nanotubes, the stronger the conductivity. When carbon nanotubes with a larger aspect ratio are used, the conductivity of the positive electrode is better. However, if the aspect ratio of the carbon nanotubes is too large, more active sites will be exposed, which makes it easier to react with components in the electrolyte, resulting in serious gas generation of the electrolyte. When a1, w1 and S1 meet When a3, w2 and S1 satisfy 0.4≤a3*w2*S1≤8, and then adjust the carbon nanotube aspect ratio a3 within the above range, the conductivity of the positive electrode can be improved, the ion conduction of the positive electrode material particles can be improved, and at the same time, the battery gas production caused by the excessive aspect ratio of the carbon nanotubes can be avoided, thereby reducing battery expansion.

[0048] In some embodiments, the mass proportion w2 of the carbon nanotubes satisfies: 0.1%≤w2≤2%, for example, w2 can be 0.1%, 0.2%, 0.4%, 0.5%, 0.6%, 0.8%, 1.0%, 1.2%, 1.4%, 1.5%, 1.6%, 1.8%, 2.0%, more preferably 0.2%≤w2≤1%. When the carbon nanotube content is low, the ion conductivity of the positive electrode material particles is not improved well, and the fast charging performance of the battery deteriorates; the more carbon nanotubes, the better the conductivity of the positive electrode, and the lower the body impedance of the battery, but excessive use will cause the electrolyte to decompose on the carbon nanotubes, resulting in electrolyte consumption and capacity decay. When a1, w1 and S1 satisfy When a3, w2 and S1 satisfy 0.4≤a3*w2*S1≤8, and then adjust the mass proportion w2 of the carbon nanotubes to be within the above range, the electronic conduction performance of the positive electrode material particles can be better, and the body impedance of the battery can be lower, thereby further improving the fast charging performance of the battery and reducing the gas production and expansion of the battery.

[0049] Although the present invention uses a low-viscosity first solvent and mixes lithium iron phosphate primary particles and lithium iron phosphate secondary particles, a1, w1 and S1 meet When the positive electrode material is used, the lithium ions can be quickly transferred between the interface and the solid phase of the positive electrode particles, but the improvement effect on the electronic conduction of the positive electrode material particles is not obvious. The electrochemical system still needs fast electron transfer to achieve rapid energy conversion of the battery system. In order to further improve the electronic conduction of the positive electrode material and reduce the bulk impedance of the battery, the present invention also provides a carbon layer on the surface of at least one side of the positive electrode current collector.

[0050] In some embodiments, a carbon layer is disposed on the surface of at least one side of the positive electrode current collector, and the positive electrode active material layer is disposed on the surface of the carbon layer and / or the surface of the positive electrode current collector. For example, carbon layers are disposed on the surfaces of opposite sides of the positive electrode current collector, and the positive electrode active material layer is disposed on the surface of the carbon layer away from the positive electrode current collector; or, a carbon layer is disposed on the surface of one side of the positive electrode current collector, and the positive electrode active material layer is disposed on the surface of the carbon layer away from the positive electrode current collector, and the positive electrode active material layer is also disposed on the surface of the positive electrode current collector where no carbon layer is disposed.

[0051] In some embodiments, the thickness of the carbon layer is denoted as a4 μm, and a4 satisfies: 0.2≤a4≤2, for example, a4 can be 0.2, 0.3, 0.5, 0.6, 0.8, 1.0, 1.2, 1.4, 1.5, 1.6, 1.8, 2.0, and more preferably 0.5≤a4≤1.5. The thicker the carbon layer, the better the contact between the positive electrode current collector and the positive electrode active material layer, the stronger the electron conductivity, the smaller the impedance of the positive electrode sheet, and the stronger the fast charging capability of the battery; but when the carbon layer is too thick, the mass proportion of the positive electrode current collector will increase, and the energy density of the battery will decrease. At the same time, if there are more carbon layers, they will be oxidized at the positive electrode to generate carbon dioxide, causing the battery to swell and fail. When a1, w1 and S1 satisfy When a carbon layer is provided on the surface of the current collector and the thickness of the carbon layer is adjusted within the above range, the positive electrode sheet can have better electronic conductivity and lower impedance, thereby further improving the fast charging performance of the battery, while reducing the energy density loss of the battery and reducing gas expansion of the battery.

[0052] Furthermore, the present invention provides a carbon layer on the surface of the positive electrode current collector and uses a carbon nanotube conductive agent to solve the problem of low electronic conductivity of lithium iron phosphate positive electrode materials. When used in combination with a low-viscosity first solvent, the charge transfer speed of the liquid phase can be increased, thereby reducing the body impedance of the battery and solving the temperature rise problem.

[0053] When a1, w1 and S1 satisfy When a3, w2 and S1 satisfy 0.4≤a3*w2*S1≤8, the battery can have better ultimate power and fast charging performance, but the interface generated by the electrolyte at the negative electrode is unstable, resulting in continuous decomposition of the electrolyte, affecting the long cycle performance of the battery. In order to meet the long cycle performance of the battery, it is necessary to design the additives in the electrolyte.

[0054] The design scheme of additives in the electrolyte is as follows:

[0055] In some embodiments, the electrolyte further includes a first additive; the mass proportion of the first additive is recorded as b1 based on the total mass of the electrolyte, and b1 satisfies: 0.1%≤b1≤8%, for example, b1 can be 0.1%, 0.2%, 0.4%, 0.5%, 0.8%, 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, preferably 2%≤b1≤5%. When the first additive is less, the negative electrode interface is not stable enough and the battery performance decreases. When the first additive is more, it will cause the viscosity of the electrolyte to decrease and the battery impedance to increase. When a1, w1 and S1 satisfy When a3, w2 and S1 satisfy 0.4≤a3*w2*S1≤8, adding the first additive to the electrolyte and adjusting the mass proportion of the first additive to the above range can improve the stability of the battery negative electrode interface, reduce the battery impedance, and thereby improve the battery cycle performance and capacity retention rate.

[0056] In some embodiments, the first additive includes one or more of vinylene carbonate VC, vinyl vinyl carbonate VEC, fluoroethylene carbonate FEC, vinyl sulfate, ethylene sulfite, fluorobenzene, thiophene, and 2-fluorothiophene.

[0057] In some embodiments, the electrolyte further includes a second additive; the mass proportion of the second additive is recorded as b2 based on the total mass of the electrolyte; b1, b2 and S1 satisfy the relationship: Preferably, the mass proportion b2 of the second additive satisfies: 0.1%≤b2≤4%, more preferably 0.5%≤b2≤3%. When the second additive is less, the battery capacity will decay rapidly during the fast charge cycle. When the second additive is more, the battery impedance will increase, the battery power limit will deteriorate, the battery dynamics will be poor, and the battery lithium deposition and cycle dive will occur. When a1, w1 and S1 meet When a3, w2 and S1 satisfy 0.4≤a3*w2*S1≤8, adding the second additive to the electrolyte and adjusting the mass proportion of the second additive to the above range can improve the battery's kinetic performance, reduce the battery impedance, improve the battery's limit power, improve the battery's cycle performance, and reduce lithium plating.

[0058] In some embodiments, the second additive includes: one or more of tri(trimethylsilyl)phosphate TMSP, tri(trimethylsilyl)borate TMSB, vinyl sulfate DTD, methylene disulfonate MMDS, 1,3-propane sultone PS, lithium difluorophosphate LiPO2F2, lithium bis(oxalatoborate) LiBOB, lithium difluorooxalatoborate LiODFB, lithium difluorobis(oxalatophosphate) LiODFP, and lithium tetrafluoroborate LiBF4, preferably DTD+LiPO2F2.

[0059] When a1, w1 and S1 satisfy When a3, w2 and S1 satisfy 0.4≤a3*w2*S1≤8, the battery can have better ultimate power and fast charging performance. However, in order to meet the long cycle performance of the battery, the electrolyte lithium salt in the electrolyte needs to be designed to meet the long cycle performance of the battery.

[0060] The design scheme of electrolyte lithium salt in the electrolyte is as follows:

[0061] In some embodiments, the electrolyte further includes an electrolyte lithium salt; the mass proportion of the electrolyte lithium salt is recorded as b3 based on the total mass of the electrolyte, and b3 satisfies: 8%≤b3≤20%, for example, b3 can be 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, 20%. When b3 is too small, the electrolyte lithium salt content is too low, which will result in low conductivity of the electrolyte and poor cycle performance of the battery; when b3 is too large, that is, the electrolyte lithium salt content is too high, anions and cations in the electrolyte combine, and the ionic conductivity decreases, which is not conducive to improving the fast charging performance of the battery. When a1, w1 and S1 satisfy When a3, w2 and S1 satisfy 0.4≤a3*w2*S1≤8, when the electrolyte lithium salt content is adjusted within the above range, while improving the battery fast charging performance and maximum power, it is also beneficial to improve the conductivity of the electrolyte, improve the long cycle performance of the battery, and improve the battery capacity retention rate.

[0062] In some embodiments, the electrolyte lithium salt includes lithium bis(fluorosulfonyl)imide LiFSI and lithium hexafluorophosphate LiPF6. Preferably, the mass ratio of lithium bis(fluorosulfonyl)imide to lithium hexafluorophosphate is w3, and S1 and w3 satisfy: 0.02≤S1*w3≤3, more preferably 0.2≤S1*w3≤0.5. Preferably, w3 satisfies: 0.01≤w3≤2, for example, w3 can be 0.01, 0.1, 0.2, 0.3, 0.5, 0.6, 0.8, 1.0, 1.2, 1.4, 1.5, 1.6, 1.8, 2.0, preferably 0.3≤w3≤1.

[0063] When the electrolyte lithium salt content of the electrolyte is determined, when the LiFSI content increases, that is, w3 increases, the ionic conductivity of the electrolyte increases. When w3 is too large, it will lead to too little LiPF6, which cannot stabilize the negative electrode interface and cannot passivate the positive electrode current collector. When the LiFSI content decreases, that is, w3 decreases, the conductivity of the electrolyte decreases, resulting in insufficient electrolyte kinetics, and in severe cases, causing rapid lithium deposition in the battery. When a1, w1 and S1 meet When S1 and w3 are adjusted to satisfy 0.1≤S1*w3≤1 and w3 is adjusted within the above range, when S1 decreases, w3 can be increased, that is, the relative content of LiFSI can be increased to improve the conductivity, so as to meet the fast charging cycle; when S1 increases, the interface is not stable enough, and the fast charging cycle of the battery will deteriorate. Reducing w3, that is, increasing the relative content of LiPF6 can generate a more stable interface and improve the cycle performance of the battery.

[0064] According to the above formula, the lithium-ion secondary battery of the present invention has good fast-charge cycle performance and good limit power, but the battery body will overheat during fast charging, the diaphragm will shrink at high temperature, and there is a safety hazard of battery short circuit. Therefore, in order to improve the safety performance of the battery, the present invention also designs that the battery also includes a battery shell, which can quickly conduct heat to prevent heat accumulation.

[0065] The design of the battery housing is as follows.

[0066] The battery housing satisfies at least one of the following conditions, and preferably satisfies all of the following conditions:

[0067] (i) the shell thickness d1 of the largest side surface of the battery shell satisfies: 0.2 mm ≤ d1 ≤ 3 mm, for example, d1 can be 0.2 mm, 0.4 mm, 0.5 mm, 0.6 mm, 0.8 mm, 1.0 mm, 1.2 mm, 1.5 mm, 1.6 mm, 1.8 mm, 2.0 mm, 2.2 mm, 2.5 mm, 2.8 mm, 3 mm;

[0068] (ii) The thickness d2 of the battery shell satisfies: 20mm≤d2≤60mm. The thickness d2 of the battery shell refers to the shell thickness of the side surfaces of the battery shell with smaller areas except for the side surface with the largest area. For example, d2 can be 20mm, 25mm, 30mm, 35mm, 40mm, 45mm, 50mm, 55mm, 58mm, 60mm, 70mm, 80mm, 90mm, or 100mm.

[0069] (iii) the width d3 of the battery housing satisfies: 50 mm ≤ d3 ≤ 400 mm, for example, d3 can be 50 mm, 100 mm, 120 mm, 140 mm, 160 mm, 180 mm, 200 mm, 220 mm, 240 mm, 260 mm, 280 mm, 300 mm, 320 mm, 350 mm, 380 mm, or 400 mm;

[0070] (iv) The height d4 of the battery shell satisfies: 50 mm≤d4≤400 mm. For example, d4 can be 50 mm, 70 mm, 90 mm, 100 mm, 120 mm, 140 mm, 160 mm, 180 mm, 200 mm, 220 mm, 250 mm, 280 mm, 300 mm, 320 mm, 350 mm, 380 mm, or 400 mm.

[0071] The smaller the shell thickness d1 of the largest side of the battery shell, the faster the heat diffuses from the inside of the battery to the outside, preventing heat accumulation, which is beneficial to reducing the temperature rise of the battery during fast charging; the larger the thickness d2 of the battery shell, the greater the heat accumulation of the battery and the higher the temperature rise; the larger the battery shell width d3 and the battery shell height d4, the larger the battery shell area, the faster the heat transfer and the smaller the temperature rise. When a1, w1 and S1 meet When the parameters of the battery casing are adjusted within the above range, heat can be quickly conducted to prevent heat accumulation, which is beneficial to reducing the temperature rise of the battery during fast charging, reducing safety problems caused by battery overheating, and improving the safety performance of the battery.

[0072] In some embodiments, d1 and S1 satisfy: 0.4≤d1 / S1≤20, for example, the ratio can be 0.2, 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20. The larger the ratio of d1 / S1, the larger d1, when S1 remains unchanged, the slower heat dissipation of the battery causes greater expansion of the battery; when d1 remains unchanged, the smaller S1, the poor improvement effect of lithium ion transmission impedance in the electrolyte liquid phase, affecting the fast charging performance of the battery; and a too large ratio of d1 / S1 will affect the energy density of the battery. When a1, w1 and S1 satisfy When d1 and S1 are adjusted to meet the above conditions, the fast charging performance of the battery can be improved, the battery expansion can be reduced, and excessive loss of battery energy density can be avoided.

[0073] In some embodiments, Figure 1 and Figure 2 As shown, the battery housing includes a shell 1, and the shell 1 includes a first side surface and a second side surface that are relatively arranged along the X-axis direction (i.e., the length direction of the shell), the first side surface is, for example, a top cover 2, and the second side surface is, for example, a bottom wall 7. A positive pole 3 and a negative pole 4 are relatively arranged at both ends of the top cover 2 along the first direction of the shell 1, and a liquid injection hole 5 is also arranged on the top cover 2, and the liquid injection hole 5 is arranged between the positive pole 3 and the negative pole 4. An explosion-proof valve 6 is arranged at the central part of the bottom wall 7, and the explosion-proof valve 6 can also be arranged on other side walls of the shell 1. The number of explosion-proof valves 6 can be selected and adjusted according to the gas production and voltage conditions of the battery. When at least two explosion-proof valves 6 are provided, they can be arranged on the bottom wall 7 and other side walls.

[0074] In some embodiments, Figure 1 , Figure 3 As shown, the shell 1 is surrounded by six rectangular surfaces, wherein along the Y-axis direction, two oppositely disposed rectangular surfaces with the largest area are recorded as the third side surface 11 and the fourth side surface 12, the shell thickness of the third side surface 11 and the fourth side surface 12 are both d1, and the shell thickness of the remaining side surfaces is d2, d1 being smaller than d2. The distance of the shell 1 along the Y-axis direction is recorded as the width of the shell, denoted by d3; the distance of the shell 1 along the Z-axis direction is recorded as the height of the shell, denoted by d4.

[0075] The lithium-ion secondary battery of the present invention has good fast-charge cycle performance and good limit power according to the above formula, but the battery body will overheat during fast charging, and the diaphragm will shrink at high temperature, which may cause the battery to short-circuit. In order to further enhance the safety performance of the battery and use a safer diaphragm, the present invention also designs the structure and strength of the diaphragm to reduce the shrinkage of the diaphragm and avoid battery short-circuit.

[0076] The design of the diaphragm is as follows:

[0077] In some embodiments, the battery further comprises a diaphragm, the diaphragm comprising a base film, a glue layer and a ceramic layer; the ceramic layer is disposed on the surface of at least one side of the base film; the glue layer is disposed on the surface of at least one side of the base film, or is disposed on the surface of the ceramic layer away from the base film. For example, the structure of the diaphragm can be glue layer + ceramic + base film, glue layer + ceramic + base film + glue layer, glue layer + ceramic + base film + ceramic + glue layer. When a1, w1 and S1 satisfy When the structure of the diaphragm is adjusted within the above range, the structural stability of the diaphragm can be improved, and the thermal shrinkage of the diaphragm can be reduced, thereby reducing the risk of short circuit in the battery and improving the safety performance of the battery.

[0078] In some embodiments, the base film includes at least one of polyethylene PE, polypropylene PP, polyethylene terephthalate, polyimide, PE and PP composite structure. And / or, the ceramic layer includes one or more of aluminum oxide Al2O3, aluminum hydroxide, magnesium oxide, aluminum oxide, zirconium oxide, titanium oxide and silicon oxide. And / or, the adhesive layer is a conventional spray-coated adhesive layer, for example, including one or more of polyvinylidene fluoride, vinylidene fluoride-hexafluoropropylene copolymer, polyacrylic acid resin, polymethyl acrylate, butyl acrylate-acrylonitrile copolymer, polyacrylonitrile, ethylene-acrylic acid copolymer, polyethyl acrylate or sodium carboxymethyl cellulose.

[0079] In some embodiments, the lithium-ion secondary battery may be a power lithium battery, a consumer lithium battery, or an energy storage lithium battery.

[0080] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0081] Unless otherwise specified, the materials and reagents used in the following examples can be obtained from commercial sources.

[0082] The batteries of the examples and comparative examples of the present invention were prepared according to the following preparation method, and the differences from Example A1 are shown below.

[0083] Example A1

[0084] (1) Preparation of positive electrode sheet

[0085] Lithium iron phosphate powder, polyvinylidene fluoride, acetylene black and carbon nanotubes (aspect ratio a3 is 706) with different ternary materials are put into a vacuum mixer according to a mass ratio of 96:2:1.5:0.5, and N-methylpyrrolidone (NMP) is added. They are fully mixed under the action of the vacuum mixer until a uniform and fluid positive electrode slurry is formed, in which the solid content is 55wt%; the above positive electrode slurry is evenly coated on a carbon-coated aluminum foil with a thickness of 12μm (the thickness a4 of the carbon layer is 1μm), with a double-sided surface density of 22mg / cm2, dried, rolled, slit and punched to obtain a positive electrode sheet.

[0086] (2) Preparation of negative electrode sheet

[0087] Graphite, styrene-butadiene rubber, sodium carboxymethyl cellulose and acetylene black are put into a vacuum mixer in a mass ratio of 96.5:1:1:1.5, deionized water is added, and they are fully mixed under the action of the vacuum mixer to finally form a uniform and fluid negative electrode slurry with a solid content of 45wt%. The negative electrode slurry is evenly coated on a copper foil with a thickness of 6μm, dried, rolled and die-cut to obtain a negative electrode sheet.

[0088] (3) Preparation of electrolyte

[0089] In an argon glove box with a water content of <0.1ppm and an oxygen content of <0.1ppm, ethylene carbonate (EC), ethyl methyl carbonate (EMC) and ethyl acetate (EA) are mixed evenly in a mass ratio of 3:2:5, and fully dried lithium hexafluorophosphate (LiPF6) and bis(fluorosulfonyl)imide lithium salt LiFSI are added thereto for stirring and dissolution. The mass of LiPF6 and LiFSI added is 10% and 5% of the total mass of the electrolyte. 2% of vinylene carbonate VC based on the total mass of the electrolyte is added, 2% of fluoroethylene carbonate FEC based on the total mass of the electrolyte is added, 1.0% of vinyl sulfate DTD based on the total mass of the electrolyte is added, and 1.0% of lithium difluorophosphate LiPO2F2 based on the total mass of the electrolyte is added. The mixture is stirred evenly, and the electrolyte is obtained after passing the physical property test.

[0090] (4) Preparation of batteries

[0091] The positive electrode sheet obtained in step (1), the negative electrode sheet obtained in step (2) and the diaphragm (the structure of the diaphragm is glue layer + ceramic + base film + glue layer, the glue coating layer is PVDF, and the positive electrode side of the diaphragm contains ceramic Al2O3) are wound to obtain a bare battery cell; the bare battery cell is welded with a pole ear and placed in a battery casing, and the electrolyte prepared in step (3) is injected into the dried and qualified battery cell, and a battery is obtained after standing, aging, formation, exhaust, aging, sorting and other processes.

[0092] (5) Test battery

[0093] Electrochemical performance test: The electrochemical performance test is carried out using the following test methods using a Blue Electric charge and discharge test cabinet:

[0094] (1) Fast charging cycle performance test

[0095] Fast charge cycle performance test: At 25°C, use a vernier caliper to measure the thickness d1 of the battery before the cycle, charge the divided battery to 3.65V at 1C constant current and constant voltage, with a cut-off current of 0.05C, and then discharge it to 2.5V at 1C constant current, and record the initial discharge capacity C0. Then charge the battery to 20% SOC at 1C, then charge it to 80% SOC at 5C, and finally charge it to 100% SOC at 1C constant current and constant voltage, with a cut-off current of 0.05C, and then discharge it to 2.5V at 1C constant current, and repeat this cycle. After 1000 cycles of charge and discharge, calculate the capacity retention rate at the 1000th week, and record the battery thermal thickness d2 at the same time. The calculation formula is as follows:

[0096] 1000th cycle capacity retention rate (%) = (1000th cycle discharge capacity / first cycle discharge capacity) × 100%.

[0097] The battery expansion rate at the 1000th cycle (%) = (battery thickness d2 at the 1000th cycle / battery thickness d1 before the cycle) × 100%.

[0098] (2) Extreme power test

[0099] At 25°C, charge the divided battery to 3.65V at 1C constant current and constant voltage, with a cut-off current of 0.05C, and then discharge it to 2.5V at 1C constant current, and record the initial discharge capacity C0. Discharge the battery to 50% SOC at 1C, record the battery body temperature T0 after standing for 4 hours, and then discharge the battery to the lower limit voltage of 2.5V at a rate of 10C, record the discharge time and the maximum temperature T1 during the discharge process, and calculate the temperature rise T1-T0. The longer the discharge time, the better the limit power.

[0100] (3) Battery lithium deposition judgment

[0101] At 25°C, charge the divided battery to 3.65V at 1C constant current and constant voltage, with a cut-off current of 0.05C, and then discharge it to 2.5V at 1C constant current, and record the initial discharge capacity C0. Then charge the battery to 20% SOC at 1C, then charge it to 80% SOC at 6C, and finally charge it to 100% SOC at 1C constant current and constant voltage, with a cut-off current of 0.05C, and then discharge it to 2.5V at 1C constant current, and cycle it 20 times. After that, charge the battery to 20% SOC at 1C, then charge it to 80% SOC at 6C, and then charge it to 100% SOC at 1C constant current and constant voltage to reach a fully charged state. Finally, dissect the fully charged battery in a dry room to observe whether there is lithium deposition on the surface, and judge it as no lithium deposition, slight lithium deposition, lithium deposition, or severe lithium deposition.

[0102] The Example A group, the Example B group and the Example C group and the Comparative Examples N1-N4 groups were carried out with reference to the Example A1, and the differences are shown in Table 1, and the performance test data are recorded in Table 2. Among them, the Dv50 (a1) of the lithium iron phosphate primary particles was changed in the Example A group, the Dv50 (a2) of the lithium iron phosphate secondary particles was changed in the Example B group, the mass proportion w1 of the lithium iron phosphate primary particles was changed in the Example C group, the mass proportion S1 of the first solvent was changed in the Example D group, and the same amount of MA was substituted for EA in the Example D4. The Dv50 of the lithium iron phosphate primary particles was changed in the Comparative Examples N1 and N2, the mass proportion of the lithium iron phosphate primary particles was changed in the Comparative Example N3, and the mass proportion of the first solvent was changed in the Comparative Example N4.

[0103] Table 1

[0104]

[0105]

[0106] Table 2

[0107]

[0108]

[0109] As can be seen from Table 2, the present invention uses a low-viscosity first solvent and controls the amount of the first solvent added, while controlling the Dv50 and mass ratio of the positive electrode material lithium iron phosphate primary particles to meet When the battery is charged, the battery fast charging performance can be improved, the battery limit power can be increased, the battery cycle performance and capacity retention rate can be improved, the temperature rise during fast charging can be reduced, and the battery expansion can be reduced. In Example D4, the MA viscosity is lower, the battery limit power is better, and the expansion rate is increased.

[0110] The Example E group, the Example F group and the Example G group were carried out with reference to the Example A1, and the specific differences are shown in Table 3, and the performance test data are recorded in Table 4. Among them, in the Example E group, the aspect ratio of the carbon nanotubes was changed by a3; in the Example F group, the mass proportion of the carbon nanotubes was changed by w2; and in the Example G group, the thickness of the carbon layer was changed by a4.

[0111] Table 3

[0112]

[0113] Table 4

[0114]

[0115]

[0116] As can be seen from Table 4, the results of Example E group show that the longer the aspect ratio of carbon nanotubes, the better the conductivity and the better the kinetics, but too large an aspect ratio will expose more active sites, the electrolyte will produce serious gas, and the battery expansion rate will be higher. The results of Example F group show that as the use of carbon nanotubes increases, the limit power discharge time increases, but the electrolyte gas production will also increase, and the battery expansion rate will be higher. The results of Example G group show that as the thickness of the carbon layer increases, the limit power discharge time increases, but the gas production will also increase, and the battery expansion rate is higher.

[0117] The Example H Group, the Example I Group, the Example J Group, the Example K Group, the Example L Group and the Example M Group were carried out with reference to the Example A1, and the specific differences are shown in Table 5, and the performance test data are recorded in Table 6. In the Example H Group, the mass proportion of the first additive was changed by b1; in the Example I Group, the type of the first additive was changed, wherein the first additive was not added in Example I3; in the Example J Group, the mass proportion of the second additive was changed by b2, wherein the second additive was not added in Example J4; and in the Example K Group, the type of the second additive was changed. In the Example L Group, the content of the lithium salt was changed by b3. In the Example M Group, the mass ratio of LiFSI to LiPF6 was changed by w3 in Examples M1-M4; in Example M5, only LiFSI was present, and in Example M6, only LiPF6 was present.

[0118] Table 5

[0119]

[0120]

[0121] Table 6

[0122]

[0123]

[0124] It can be seen from Table 6 that in the Example H group, the content of the first additive increases, the limit power discharge time is shortened, the capacity retention rate increases, and the battery expansion is reduced. In the Example I group, VC+VEC will cause the battery impedance to increase and the limit power to decrease, but it can reduce the battery expansion. In the Example J group, the second additive content increases, the battery impedance increases, the limit power decreases, the kinetics deteriorates, and the capacity retention rate decreases. Too much increase in the second additive content will cause lithium precipitation and cycle diving. In the Example L group, an increase in the lithium salt content will cause a decrease in the limit power, and a decrease in the lithium salt content will reduce the cycle capacity retention rate. In the Example M group, LiFSI increases, the limit power of the battery increases, and the battery expansion will also increase.

[0125] The Example O Group and the Example P Group were carried out with reference to the Example A1, and the main differences are shown in Table 7.

[0126] Table 7

[0127]

[0128] It can be seen from Table 7 that when d1 and S1 satisfy 0.4≤d1 / S1≤20, the battery expansion can be reduced.

[0129] The Example Q group was carried out with reference to the Example A1, wherein the structure of the diaphragm in the Example Q1 was glue layer + ceramic + base film + ceramic + glue layer; and the structure of the diaphragm in the Example Q2 was glue layer + base film + ceramic + glue layer. The performance test is recorded in Table 8.

[0130] Table 8

[0131]

[0132] It can be seen from Table 8 that the structural change of the diaphragm will affect the expansion rate of the battery, and the fast charging performance will be slightly better when there is no ceramic layer.

[0133] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A lithium ion secondary battery, characterized in that: The lithium-ion secondary battery comprises a positive electrode sheet, a negative electrode sheet and an electrolyte; The positive electrode sheet includes a positive electrode current collector and a positive electrode active material layer disposed on at least one side of the positive electrode current collector; the positive electrode active material layer includes a positive electrode active material; the positive electrode active material includes lithium iron phosphate primary particles and lithium iron phosphate secondary particles, the Dv50 of the lithium iron phosphate primary particles is recorded as a1μm, the Dv50 of the lithium iron phosphate secondary particles is recorded as a2μm, and the Dv50 of the lithium iron phosphate secondary particles is recorded as a1 <a2; Based on the total mass of the positive electrode active material, the mass proportion of the lithium iron phosphate primary particles is recorded as w1; The electrolyte includes a solvent, the solvent includes a first solvent, and the first solvent includes a C1-C4 linear organic solvent; the mass proportion of the first solvent is recorded as S1 based on the total mass of the solvent; Among them, a1, w1 and S1 satisfy the following relationship:

2. The lithium ion secondary battery according to claim 1, characterized in that: a1, w1 and S1 satisfy the following relationship: Preferably, the Dv50 of the lithium iron phosphate primary particles satisfies: 0.1 μm ≤ a1 ≤ 0.4 μm; and / or, the Dv50 of the lithium iron phosphate secondary particles satisfies: 1 μm ≤ a2 ≤ 2 μm; Preferably, the particle size of the lithium iron phosphate primary particles is in the range of 0.01 μm to 1 μm; and / or the particle size of the lithium iron phosphate secondary particles is in the range of 1 μm to 10 μm.

3. The lithium ion secondary battery according to claim 1, characterized in that: The mass proportion w1 of the lithium iron phosphate primary particles satisfies: 10%≤w1≤60%, preferably 20%≤w1≤50%; And / or, the mass proportion S1 of the first solvent satisfies: 10%≤S1≤90%, preferably 20%≤S1≤70%.

4. The lithium ion secondary battery according to claim 1, characterized in that: The solvent further includes a second solvent, wherein the second solvent includes a C1-C10 cyclic organic solvent and / or a linear organic solvent having a carbon number greater than 4; Preferably, the viscosity of the first solvent is ≤0.5 mPa.s, and the first solvent comprises at least one or more of ethyl acetate, methyl acetate, methyl formate, ethylene glycol dimethyl ester, dimethanol formal, and acetonitrile, more preferably ethyl acetate; Preferably, the viscosity of the second solvent is >0.5 mPa.s, and the second solvent includes at least one or more of ethylene carbonate, propylene carbonate, butylene carbonate, γ-butyrolactone, diethyl carbonate, ethyl methyl carbonate, dimethyl carbonate, propyl propionate, and ethyl propionate.

5. The lithium ion secondary battery according to claim 1, characterized in that: The positive electrode active material layer further includes a conductive agent; the conductive agent includes carbon nanotubes, and the aspect ratio of the carbon nanotubes is denoted as a3; Preferably, the mass proportion of the carbon nanotubes is recorded as w2 based on the total mass of the positive electrode active material; Among them, a3, w2 and S1 satisfy the relationship: 0.4≤a3*w2*S1≤8.

6. The lithium ion secondary battery according to claim 5, characterized in that: a3, w2 and S1 satisfy the relationship: 0.5≤a3*w2*S1≤6; And / or, the aspect ratio a3 of the carbon nanotubes satisfies: 200≤a3≤1500, preferably 500≤a3≤1000; And / or, the mass proportion w2 of the carbon nanotubes satisfies: 0.1%≤w2≤2%, preferably 0.2%≤w2≤1%.

7. The lithium ion secondary battery according to any one of claims 1 to 6, characterized in that: A carbon layer is disposed on at least one side of the positive electrode current collector, and the positive electrode active material layer is disposed on the surface of the carbon layer and / or the surface of the positive electrode current collector; Preferably, the thickness of the carbon layer is denoted as a4 μm, and a4 satisfies: 0.2≤a4≤2, more preferably 0.5≤a4≤1.

5.

8. The lithium ion secondary battery according to any one of claims 1 to 6, characterized in that: The electrolyte further includes a first additive; based on the total mass of the electrolyte, the mass proportion of the first additive is denoted as b1, and b1 satisfies: 0.1%≤b1≤8%, preferably 2%≤b1≤5%; Preferably, the first additive includes one or more of vinylene carbonate, vinyl ethylene carbonate, fluoroethylene carbonate, vinyl sulfate, ethylene sulfite, fluorobenzene, thiophene, and 2-fluorothiophene.

9. The lithium ion secondary battery according to claim 8, characterized in that: The electrolyte further includes a second additive; the mass proportion of the second additive is recorded as b2 based on the total mass of the electrolyte; b1, b2 and S1 satisfy the relationship: Preferably, the mass proportion b2 of the second additive satisfies: 0.1%≤b2≤4%, more preferably 0.5%≤b2≤3%; Preferably, the second additive includes one or more of tris(trimethylsilyl)phosphate, tris(trimethylsilyl)borate, vinyl sulfate, methylene disulfonate, 1,3-propane sultone, lithium difluorophosphate, lithium bis(oxalatoborate), lithium difluorooxalatoborate, lithium difluorobis(oxalatophosphate), and lithium tetrafluoroborate.

10. The lithium ion secondary battery according to claim 1, characterized in that: The lithium-ion secondary battery also includes a battery housing; Preferably, the battery housing satisfies at least one of the following conditions: (i) The shell thickness d1 of the largest side of the battery shell satisfies: 0.2 mm ≤ d1 ≤ 3 mm; (ii) The thickness d2 of the battery casing satisfies: 20 mm ≤ d2 ≤ 100 mm; (iii) The width d3 of the battery housing satisfies: 50 mm ≤ d3 ≤ 400 mm; (iv) The height d4 of the battery case satisfies: 50 mm ≤ d4 ≤ 400 mm.

Citation Information

Patent Citations

  • Low-temperature lithium iron phosphate battery and preparation method thereof

    CN109802094A

  • Quick-charging type high-energy-density lithium ion battery

    CN111600066A

  • Lithium secondary battery and preparation method thereof

    CN116826165A

  • High-energy-density fast-charging lithium iron phosphate battery and preparation method thereof

    CN117117337A

  • Cell, battery pack, and electricity-consumption device

    US20240128513A1

Cited By

  • Lithium ion battery and electric device

    CN119994147A

  • Lithium secondary battery, positive electrode active material, preparation method of positive electrode active material, and electric device

    CN120015902A

  • Lithium secondary battery and electrical device

    WO2026166217A1

  • Battery, battery apparatus and electric device

    WO2026179393A1

  • Lithium-ion battery cell, lithium-ion battery and electric device

    WO2026184251A1