Negative electrode material and battery
By controlling the mass ratio and silicon grain size of crystal phase silicon in silicon elements, combined with plasma flow condensation and carbon coating treatment, the volume expansion and cycle stability of silicon-based anode material is solved, and the low lithium ion of the anode material is achieved Transmission impedance, high solid-liquid interface stability and strong long-term circulation structure stability improve battery performance.
Patent Information
- Application Number
- CN202311441600.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-10-31
- Publication Date
- 2024-12-06
AI Technical Summary
The silicon-based negative electrode material has a severe volume expansion effect during the circulation process, resulting in the material being powdered and broken, and the cycle attenuation of the battery is very fast. It is difficult for the existing technology to effectively control the average size of silicon grains to reduce volume expansion and improve cycle stability. .
By controlling the relationship between the mass ratio of crystalline silicon in silicon elements and the average size of silicon grains, the mass ratio of crystalline silicon and amorphous silicon is regulated, and plasma flow condensation process and carbon coating are used to regulate the siliceous crystal. The ratio of particle size to the mass of crystalline silicon can achieve the improvement of the overall performance of the negative electrode material.
It significantly improves the lithium ion transport impedance, solid-liquid interface stability and the stability of the crystal phase structure in long-term circulation, reduces the breakdown of negative electrode particles, improves the interface stability, and improves the electrochemical performance of negative electrode materials.
Smart Images

Figure CN119092698A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of negative electrode materials, and in particular, to a negative electrode material and a battery. Background Art
[0002] Electric new energy vehicles are the future development direction of the automobile market, and their core components are lithium-ion batteries. As the market develops, the demand for high-capacity and high-density batteries is increasing. The use of new high-specific-capacity positive and negative electrode materials is one of the important methods to improve the energy density of batteries.
[0003] More and more new materials such as metals, oxides, and metal alloys are used as active materials in negative electrode materials to continuously explore various ways to improve the energy density of batteries. Taking silicon-based negative electrode materials as an example, silicon-based negative electrode materials, as one of the above-mentioned active materials, are generally considered to be the next generation of negative electrode materials. They have ultra-high theoretical specific capacity (4200mAh / g) and low delithiation potential (<0.5V). The voltage platform of silicon is slightly higher than that of graphite. It is difficult to cause surface lithium deposition during charging, and has better safety performance. It is highly praised. However, the silicon negative electrode has a drastic volume expansion effect during the cycle process, which causes the material to pulverize and break, and the battery cycle decays quickly.
[0004] To solve this problem, the solutions commonly used in the industry include coating, secondary granulation, and control of silicon grains. However, during the heat treatment process of existing silicon-based materials, the size of silicon grains tends to grow rapidly, and single Si will cause greater volume expansion. Therefore, how to control the average size of silicon grains to reduce the volume expansion of negative electrode materials and improve the cycle stability of negative electrode materials is still an urgent problem to be solved. Summary of the invention
[0005] The present application proposes a negative electrode material and a battery, which can reduce the volume expansion of the negative electrode material and improve the cycle stability of the negative electrode material by controlling the relationship between the mass ratio of crystalline silicon in the silicon element and the average size of silicon grains.
[0006] In a first aspect, the present application provides a negative electrode material, wherein the negative electrode material contains silicon, and the silicon is at least partially present in the form of crystalline silicon;
[0007] Taking the mass content of silicon element in the negative electrode material as 100%, the mass content of crystalline silicon is A%, and the average size of silicon grains of the crystalline silicon is B nm;
[0008] The negative electrode material satisfies the following characteristics: 0.3≤A / B≤60, and 6≤A+B≤75.
[0009] In some embodiments, taking the mass content of silicon element in the negative electrode material as 100%, the mass content of crystalline silicon is A%, and the value range of A is 5-65.
[0010] In some embodiments, the negative electrode material further includes oxygen, and the average size of the silicon grains is B nm, and B≤7.
[0011] In some embodiments, the negative electrode material further includes oxygen element, and the atomic ratio of oxygen element to silicon element in the negative electrode material is x, 0<x<2.2.
[0012] In some embodiments, the negative electrode material further includes oxygen, and the component containing oxygen and silicon in the negative electrode material includes at least one of silicon oxide and silicate.
[0013] In some embodiments, the negative electrode material further includes carbon elements, and the component containing carbon elements in the negative electrode material includes at least one of amorphous carbon, graphite, graphene, carbon nanotubes and carbon fibers.
[0014] In some embodiments, the negative electrode material further includes a doping metal element, and the doping metal element is selected from at least one of Li, Mg, Cu, Ni, Fe, Cr and Zn.
[0015] In some embodiments, the doped metal element includes Mg element, and the mass content of the Mg element in the negative electrode material is 3% to 25%; and / or the average size of the silicon grains is B nm, and B≤15.
[0016] In some embodiments, the doped metal element includes Li element, and the mass content of Li element in the negative electrode material is 3% to 15%; and / or the average size of the silicon grains is B nm, and B≤10.
[0017] In some embodiments, the mass content of oxygen in the negative electrode material is 10% to 55%.
[0018] In some embodiments, the mass content of carbon in the negative electrode material is 1% to 40%.
[0019] In some embodiments, the mass content of silicon in the negative electrode material is 25% to 90%.
[0020] In some embodiments, at least a portion of the surface of the negative electrode material has a carbon layer.
[0021] In some embodiments, the particle size of the negative electrode material satisfies: D 20 -D 10 ≤4μm, D 90 -D80 ≤8μm.
[0022] In some embodiments, the specific surface area of the negative electrode material is 0.1 m 2 / g~25m 2 / g.
[0023] In some embodiments, the pH of the negative electrode material is 6-10.
[0024] In some embodiments, the true density of the negative electrode material is 2.0 g / cm 3 ~3.4g / cm 3 .
[0025] In a second aspect, the present application provides a battery, comprising the negative electrode material described in the first aspect.
[0026] The technical solution of this application has at least the following beneficial effects:
[0027] The negative electrode material provided in the present application can achieve significant improvements in lithium ion transmission impedance, solid-liquid interface stability, and stability of the crystal phase structure during long-term cycles by controlling the relationship between the mass ratio of crystalline silicon in the silicon element and the average size of silicon grains. Specifically, crystalline silicon is more structurally stable than amorphous silicon, and the peak intensity and peak position in dQ / dV change little during the battery electrode cycle. However, the direction of crystalline silicon expansion is selective, resulting in uneven expansion stress, which in turn causes the negative electrode particles to break, exposing the silicon interface to more electrolytes, triggering side reactions with the electrolyte, causing the SEI film to continue to grow and thicken, and resulting in deterioration of interface stability. The silicon element (single substance, compound) present in the amorphous state can stabilize the overall structure of the negative electrode particles and buffer the expansion deformation, reduce the breakage of the negative electrode particles and thus improve the interface stability. At the same time, amorphous materials are isotropic materials, and there is no directional selectivity in lithium insertion, and the lithium ion transfer impedance is lower. In summary, by regulating the mass proportion of crystalline silicon and the average size of silicon grains, the effects of the two parameters, silicon grain size and the mass ratio between crystalline silicon and amorphous silicon, on the electrochemical properties of the negative electrode material can be balanced, and at the same time, the negative electrode material can have low lithium ion transfer impedance, high solid-liquid interface stability, and strong long-term cyclic crystalline phase structure stability, thereby greatly improving product performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 A schematic diagram of a process for preparing a negative electrode material provided in an embodiment of the present application.
[0029] Figure 2 This is a comparison chart of the cycle performance of the negative electrode materials provided in Example 1 and Comparative Example 1 of the present application.
[0030] Figure 3aThe software interface status of the negative electrode material of the embodiment of the present application during the XRD test is shown in FIG. Figure 1 .
[0031] Figure 3b The software interface status of the negative electrode material of the embodiment of the present application during the XRD test is shown in FIG. Figure 2 .
[0032] Figure 3c Schematic diagram 3 of the software interface status during XRD testing of the negative electrode material of an embodiment of the present application.
[0033] Figure 3d Schematic diagram 4 of the software interface status during XRD testing of the negative electrode material of an embodiment of the present application.
[0034] Figure 3e Schematic diagram 5 of the software interface status during XRD testing of the negative electrode material of an embodiment of the present application. DETAILED DESCRIPTION
[0035] The following is a preferred implementation of the embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the embodiment of the present invention. These improvements and modifications are also considered to be within the scope of protection of the embodiment of the present invention.
[0036] Specifically, the present application provides a negative electrode material, the negative electrode material contains silicon element, and the silicon element exists at least partially in the form of crystalline silicon;
[0037] Through XRD test analysis, taking the mass content of silicon element in the negative electrode material as 100%, the mass content of crystalline silicon is A%, the average size of silicon grains is B nm, and 0.3≤A / B≤60, 6≤A+B≤75.
[0038] In the above scheme, by controlling the relationship between the mass ratio of crystalline silicon in the silicon element and the average size of silicon grains, significant improvements can be achieved in lithium ion transmission impedance, solid-liquid interface stability, and stability of the crystalline structure during long-term cycles. Specifically, crystalline silicon has a more stable structure than amorphous materials, and the peak intensity and peak position in dQ / dV change little during the battery electrode cycle. However, the direction of crystalline silicon expansion is selective, resulting in uneven expansion stress, which in turn causes the negative electrode particles to break, exposing the silicon interface to more electrolytes, triggering side reactions with the electrolyte, causing the SEI film to continue to grow and thicken, and resulting in deterioration of interface stability. The silicon element (single substance, compound) present in the amorphous state can stabilize the overall structure of the negative electrode particles and buffer expansion deformation, reduce the breakage of the negative electrode particles and thus improve interface stability. At the same time, amorphous materials are isotropic materials, and there is no directional selectivity in lithium insertion, and the lithium ion transfer impedance is lower. In summary, by regulating the mass proportion of crystalline silicon and the average size of silicon grains, the effects of the two parameters, silicon grain size and the mass ratio between crystalline silicon and amorphous silicon, on the electrochemical properties of the negative electrode material can be balanced, and at the same time, the negative electrode material can have low lithium ion transfer impedance, high solid-liquid interface stability, and strong long-term cyclic crystalline phase structure stability, thereby greatly improving product performance.
[0039] Specifically, the specific value of A / B is 0.3, 0.5, 1, 5, 10, 15, 20, 25, 35, 40, 55 or 60, and the specific value of A+B is 6, 8, 10, 15, 20, 25, 35, 40, 45, 50, 55, 60, 65, 70 or 75, etc., which are not limited here. The present application controls the value of A / B and A+B, that is, controls the relationship between the two parameters of silicon grain size and the mass ratio between crystalline silicon and amorphous silicon, so as to balance the volume expansion and long cycle stability of the negative electrode material.
[0040] In some embodiments, the mass content of silicon in the negative electrode material is 100%, and the mass content of crystalline silicon is A%, and the value range of A is 5 to 65. The value range of A can be 5, 11, 21, 26, 31, 40, 50, 59, 61 or 65, etc., which are not limited here. It can be understood that when the mass content of crystalline silicon in silicon is too low, the amorphous component in silicon is too high, and the reaction activity is high. During the charge and discharge process, electrochemical sintering is prone to occur under the action of an applied voltage, so that the average size of silicon grains increases sharply, and the drastic structural changes and silicon grains of uncontrollable size jointly lead to the degradation of product cycle performance; when the mass content of crystalline silicon in silicon is too high, the charge and discharge polarization is aggravated, which leads to a decrease in product capacity, and at the same time reduces the rate performance and low temperature performance of the product. Therefore, controlling the mass content of crystalline silicon between 5% and 65% is conducive to suppressing the volume expansion effect of the negative electrode material and improving the cycle performance of the negative electrode material.
[0041] In some embodiments, the silicon grain size is B nm, and B≤7; the average size of the silicon grains can specifically be 7nm, 6.5nm, 6.0nm, 5.9nm, 5.5nm, 5.0nm, 4.5nm, 4.0nm, 3.5nm, 3nm, 2.5nm, 2nm, 1nm, etc., which are not limited here. It can be understood that when the average size of the silicon grains is too large, the expansion stress generated by the silicon grains during the lithium insertion process is uneven, which can easily cause the negative electrode material particles to break and lose electrochemical activity, thereby reducing the product cycle performance. Therefore, controlling the average size of the silicon grains within the above range is conducive to improving the uniformity of the expansion stress of the negative electrode material particles, reducing particle breakage, and allowing the negative electrode material to achieve an ideal balance in cycle performance, capacity utilization and rate performance, and obtain the best comprehensive performance.
[0042] In some embodiments, the negative electrode material further includes oxygen, and the components containing oxygen and silicon in the negative electrode material include but are not limited to at least one of silicon oxide and silicate. Silicon oxide can be represented by the general formula SiO x (0.5≤x<2). Specifically, SiO x Specifically, it can be SiO 0.5 、SiO 0.7 、SiO 0.9 、SiO、SiO 1.2 、SiO 1.5 、SiO 1.8 、SiO 1.9 Silicon oxide can be a material formed by dispersing silicon particles in SiO2, or a material having a tetrahedral structural unit, in which the silicon atom is located at the center of the tetrahedral structural unit and the silicon atom and the oxygen atom are located at the four vertices of the tetrahedral structural unit.
[0043] In some embodiments, the silicon-containing component in the negative electrode material may be elemental silicon or a silicon alloy. The elemental silicon may be amorphous silicon and / or crystalline silicon. The silicon alloy may be a silicon-lithium alloy, a silicon-magnesium alloy, a silicon-nickel alloy, or the like.
[0044] In some embodiments, the negative electrode material further includes carbon elements, and the carbon-containing component in the negative electrode material includes at least one of amorphous carbon, graphite, graphene, carbon nanotubes and carbon fibers. Amorphous carbon can be soft carbon and / or hard carbon, and graphite can be artificial graphite and / or natural graphite. It can be understood that carbon materials can improve the conductivity of silicon-based active materials. Graphite is a material with high conductivity, small volume expansion, high initial efficiency and stable cycle performance.
[0045] In some embodiments, the negative electrode material also includes oxygen element, and the atomic ratio of oxygen element to silicon element in the negative electrode material is x, 0<x<2.2, specifically it can be 0.1, 0.2, 0.5, 0.8, 0.9, 1, 1.2, 1.5, 1.8, 1.9, 2.1, 2.185, etc., or it can be other values within the above range.
[0046] In some embodiments, the negative electrode material further includes a doped metal element, and the doped metal element is selected from at least one of Li, Mg, Cu, Ni, Fe, Cr and Zn. In the element distribution spectrum obtained by scanning the SEM section of the negative electrode material particles by X-ray, the distribution surface of Si, O and the doped metal element is in a uniform dispersion state. In the negative electrode material, Si, O and the doped metal element are evenly distributed in the particles, which can effectively reduce the infiltration of air and other components into the particles and cause the active components to fail. The structure and properties will not deteriorate during long-term storage, and it is very suitable for lithium-ion batteries. The uniformly dispersed distribution state of the metal elements is conducive to the expansion and contraction of the negative electrode material at the same level at all places during the lithium insertion and extraction process, and there will be no stress weak points caused by excessive local expansion. The doped metal can also improve the conductivity of the negative electrode material and enhance the structural strength of the negative electrode material, so that the material performance is better.
[0047] In some embodiments, the negative electrode material also includes doped metal elements, the doped metal elements include Mg element, and the mass content of Mg element in the negative electrode material is 3% to 25%; specifically, it can be 3%, 5%, 8%, 10%, 12%, 14%, 18%, 20%, 23%, 24% or 25%, etc., or it can be other values within the above range.
[0048] In some embodiments, when the negative electrode material further includes a doped metal element, and the doped metal element includes a Mg element, the silicon grain size in the negative electrode material is B nm, and B≤15; the average size of the silicon grains can be 15nm, 12nm, 10nm, 9nm, 7nm, 6.0nm, 5.5nm, 5.0nm, 4.5nm, 4.0nm, 3nm, 2nm, 1nm, etc., which are not limited here. It can be understood that the negative electrode material can specifically include MgSiO3 and Mg2SiO4. When the metal M is magnesium, the Si crystallite size can be reduced and the expansion of the material can be reduced.
[0049] In some embodiments, the negative electrode material further includes doped metal elements, the doped metal elements include Li element, and the mass content of Li element in the negative electrode material is 3% to 15%; specifically, it can be 3%, 5%, 8%, 9%, 10%, 12%, 13%, 14% or 15%, etc., or it can be other values within the above range.
[0050] In some embodiments, when the negative electrode material further includes a doped metal element, and the doped metal element includes a Li element, the size of the silicon grains in the negative electrode material is B nm, and B≤10; the average size of the silicon grains can be 10nm, 9nm, 7nm, 6.0nm, 5.5nm, 5.0nm, 4.5nm, 4.0nm, 3nm, 2nm, 1nm, etc., which are not limited here. It can be understood that the silicon grain size in the negative electrode material is ≤10nm, which is conducive to the dispersed distribution of silicon grains, can effectively reduce the volume expansion of silicon, and improve the cycle performance.
[0051] In some embodiments, the mass content of oxygen in the negative electrode material is 10% to 55%, specifically 10%, 12%, 15%, 20%, 25%, 30%, 35%, 40%, 45% or 55%, etc., and of course it can also be other values within the above range, which is not limited here.
[0052] In some embodiments, at least part of the surface of the negative electrode material has a carbon layer. It is understandable that the carbon layer on the surface of the negative electrode material can reduce the repeated formation of the SEI film and cause the material particles to break, which is beneficial to improving the cycle performance of the negative electrode material and reducing the volume expansion caused by the formation of the SEI film.
[0053] In some embodiments, the active material (silicon and / or silicon oxide material, etc.) is dispersed in the carbon material, and the carbon material constructs a conductive network for the active material, which overcomes the disadvantage of poor conductivity of the active material (such as silicon oxide), and is beneficial to the capacity and cycle stability of silicon oxide. In some embodiments, the mass content of the carbon element in the negative electrode material is 1% to 40%; specifically, it can be 2%, 5%, 8%, 10%, 12%, 15%, 18%, 20%, 25%, 28%, 35% or 40%, etc., and of course, it can also be other values within the above range, which are not limited here.
[0054] In some embodiments, the mass content of silicon in the negative electrode material is 25% to 90%; specifically, it can be 25%, 30%, 40%, 50%, 55%, 60%, 65%, 70%, 85%, 88% or 90%, etc., and of course, it can also be other values within the above range, which are not limited here. Preferably, the mass content of silicon in the negative electrode material is 40% to 60%.
[0055] In some embodiments, in the negative electrode material, the active material and the carbon material are dispersed with each other in the form of particles.
[0056] In some embodiments, at least a portion of the surface of the negative electrode material has a carbon layer.
[0057] In some embodiments, the pH value of the negative electrode material is 6-10, specifically 6, 7, 8, 8.5, 9, 9.5 or 10, etc., which are not limited here. Preferably, the pH value of the negative electrode material is 7-10.
[0058] In some embodiments, the specific surface area of the negative electrode material is 0.1 m 2 / g~25m 2 / g, specifically 0.1m 2 / g, 1.0m 2 / g, 1.5m 2 / g, 1.8m 2 / g, 2.0m 2 / g, 2.5m 2 / g, 3.0m 2 / g, 3.6m 2 / g, 4.0m 2 / g, 5m 2 / g, 5.5m 2 / g, 6.0m 2 / g, 7.0m 2 / g, 8.0m 2 / g, 8.5m 2 / g, 10.0m 2 / g, 12.0m 2 / g, 15.0m 2 / g, 18.0m 2 / g or 25m 2 / g, but is not limited to the listed values, and other values not listed in the numerical range are also applicable. It can be understood that the smaller the specific surface area, the better. Too large a specific surface area is likely to lead to the formation of SEI film, consume too much irreversible lithium salt, and reduce the initial efficiency of the battery. Considering the cost of the preparation process, preferably, the specific surface area of the negative electrode material is 1m 2 / g~10m 2 / g.
[0059] In some embodiments, the true density of the negative electrode material is 2.0 g / cm 3 ~3.4g / cm 3 , specifically 2.0 g / cm 3 , 2.2g / cm 3 , 2.4g / cm 3 , 2.6g / cm 3 , 2.8g / cm 3 , 2.9g / cm 3 、3.0g / cm 3 、3.2g / cm 3 or 3.4m 2 / g, and other values not listed in this numerical range are also applicable. Controlling the true density within the above range is beneficial to improving the energy density and rate performance of the negative electrode material.
[0060] In some embodiments, the particle size of the negative electrode material satisfies: D 20 -D 10 ≤4μm, D 90 -D 80 ≤8μm; D 20 -D 10 Specifically, it can be 1 μm, 1.5 μm, 2 μm, 2.5 μm, 3.5 μm, or 4 μm, etc. 90 -D 80 Specifically, it can be 1μm, 1.5μm, 2μm, 2.5μm, 3.5μm, 5μm, 5.5μm, 6μm, 6.5μm or 8μm, etc., which are not limited here. It can be understood that when the particle size of the negative electrode material deviates from the above range, it means that the overall particle size distribution of the product is shifted toward the direction of large particle size. Large particle size particles are more fragile in long cycles and are more likely to break and deactivate, affecting the electrochemical performance of the product; when D 20 -D 10 Not meeting the requirements and D 90 -D 80 When the requirements are met, the overall particle size distribution of the product shifts toward the direction of small particle size. Small particle size particles have a larger specific surface area, so they have a higher reaction activity with the electrolyte and are not easy to generate a stable SEI, which affects the long-term cycle performance and high-temperature storage performance of the product. Therefore, controlling the particle size of the negative electrode material within the above range is conducive to improving the rate performance, long-cycle stability and high-temperature storage performance of the negative electrode material.
[0061] The present application also provides a method for preparing a negative electrode material, such as Figure 1 As shown, the method includes the following steps S10 to S20:
[0062] S10, heating and gasifying a raw material mixture containing silicon and oxygen elements in a vacuum state to form vapor, transporting the vapor to a plasma flow for plasma reaction, and condensing to obtain a precursor;
[0063] S20, carbon-coating the precursor, and heat-treating the carbon-coated product at 800° C. to 1100° C. to obtain a negative electrode material. Wherein, based on the mass content of silicon element in the negative electrode material being 100%, the mass content of crystalline silicon is A%, the average size of silicon grains is B nm, and 0.3≤A / B≤60, 6≤A+B≤75.
[0064] The present application provides a method for preparing a negative electrode material. The vapor formed after the raw material mixture is heated and gasified is transported to a plasma flow for a plasma reaction. The plasma has the characteristics of low temperature and high energy level. The precursor vapor condenses and settles in the plasma to generate uniformly distributed silicon microcrystalline seeds without affecting the amorphous state of the entire substance. When such seeds exist in the precursor, the silicon grain size in the aforementioned S20 process can be promoted to grow rapidly, and the mass proportion of crystalline silicon that is out of control due to excessive heat treatment time can be reduced. The plasma condensation process is used to obtain seeds, and high-temperature heat treatment is used to regulate the crystallization state. The two aspects of 0.3≤A / B≤60 and 6≤A+B≤75 can be achieved. That is, by controlling the relationship between the mass proportion of crystalline silicon in the silicon element and the average size of silicon grains, the negative electrode material obtains the best comprehensive performance.
[0065] The following is a detailed introduction to this program:
[0066] S100, heating and gasifying a raw material mixture containing silicon and oxygen in a vacuum state to form vapor, transporting the vapor to a plasma flow for plasma reaction, and condensing to obtain a precursor.
[0067] In some embodiments, the raw material mixture includes Si, SiO y Mixture of SiO2 and SiO y At least one of a mixture of Si and Si, and a mixture of Si and SiO2, wherein 0<y<2.
[0068] In some embodiments, the raw material mixture further includes a doping metal element, and the doping metal element is selected from at least one of Li, Mg, Cu, Ni, Fe, Cr and Zn; the doping metal element can be added to the raw material mixture in the form of a metal element, a metal oxide, etc.
[0069] In some embodiments, the doping metal element is selected from Mg and / or Li.
[0070] In some embodiments, the pressure in the vacuum state is 1.333×10 -1 Pa~1.333×10 -6 Pa, specifically 1.333×10 -1 Pa, 1.333×10 -2 Pa, 1.333×10 -3 Pa, 1.333×10 -4 Pa, 1.333×10 -5 Pa or 1.333×10 -6 Pa, etc., are not limited here.
[0071] In some embodiments, the temperature of heating and gasification is 1000° C. to 1800° C., specifically 1000° C., 1050° C., 1100° C., 1200° C., 1250° C., 1300° C., 1350° C., 1400° C., 150° C., 1600° C., 1700° C. or 1800° C. It is understandable that the above temperature is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0072] In some embodiments, the gas source of the plasma flow includes at least one of argon, hydrogen, neon, and helium.
[0073] In some embodiments, the RF power of the plasma generating device is 10 kW to 100 kW; specifically, it can be 10 kW, 20 kW, 30 kW, 40 kW, 50 kW, 60 kW, 70 kW, 80 kW, 90 kW, 100 kW, etc., which is not limited here.
[0074] In some embodiments, the raw material mixture also includes a doping metal element, the doping metal includes Li, and the molar ratio of Si to Li in the raw material mixture is (1-50):1; specifically, it can be 1:1, 5:1, 10:1, 15:1, 20:1, 25:1, 30:1, 40:1 or 50:1, etc., which is not limited here.
[0075] In some embodiments, the raw material mixture also includes a doped metal element, the doped metal includes Mg, and the molar ratio of Si to Mg in the raw material mixture is (5-50):1; specifically, it can be 5:1, 10:1, 15:1, 20:1, 25:1, 30:1, 40:1 or 50:1, etc., which is not limited here.
[0076] In some embodiments, the cooling is performed by cooling with a protective gas, and the protective gas includes at least one of nitrogen, argon, neon, krypton, and helium.
[0077] In some embodiments, the method further comprises crushing the condensed precursor so that the particle size D of the precursor is 50 The particle size D of the precursor is 0.1 μm to 25 μm. 50 Specifically, it can be 0.1μm, 0.3μm, 0.4μm, 0.5μm, 1μm, 2μm, 3μm, 4μm, 6μm, 10μm, 12μm, 15μm, 20μm or 25μm, etc., which is not limited here.
[0078] S20, carbon-coating the precursor, and heat-treating the carbon-coated product at 800° C. to 1100° C. to obtain a negative electrode material.
[0079] In one embodiment, the carbon coating treatment is at least one of solid phase carbon coating, liquid phase carbon coating and gas phase carbon coating. In the present application, the carbon coating treatment is low temperature coating, which can effectively inhibit the increase of silicon grain size.
[0080] Specifically, the steps of the carbon coating treatment specifically include: heating the precursor obtained by the cooling treatment, introducing a protective gas and a carbon source gas, and thermally cracking the carbon source gas to obtain a carbon coating product.
[0081] In some embodiments, the carbon source gas used for gas-phase carbon coating includes hydrocarbons.
[0082] In some embodiments, the carbon source gas includes at least one of methane, acetylene, ethylene, ethane, propane, propylene, propyne, acetone, and benzene.
[0083] In some embodiments, the chemical vapor deposition device includes at least one of a rotary chemical vapor deposition reactor, a plasma enhanced chemical vapor deposition reactor, a chemical vapor deposition tube furnace, and a fluidized bed. Specifically, the chemical vapor deposition device is at least one of a rotary furnace and a box furnace.
[0084] In some embodiments, the temperature of thermal cracking is 600°C-800°C, and the time of thermal cracking is 2h-20h. The temperature of thermal cracking can be 600°C, 620°C, 650°C, 680°C, 700°C, 750°C or 800°C, etc., which is not limited here. The time of thermal cracking can be 2h, 3h, 4h, 6h, 8h, 10h, 12h, 15h or 20h, etc., which is not limited here.
[0085] In some embodiments, the carbon source gas is introduced under a protective gas.
[0086] In some embodiments, the protective gas includes at least one of nitrogen, helium, neon, argon, krypton, and xenon.
[0087] In some embodiments, the step of carbon coating treatment specifically includes: carbonizing a mixture obtained by mixing the precursor obtained by cooling treatment with a solid carbon source to obtain a negative electrode material.
[0088] In some embodiments, the solid carbon source includes at least one of sugars, esters, hydrocarbons, organic acids and high molecular polymers, and can specifically be at least one of polyvinyl chloride, polyvinyl butyral, polyacrylonitrile, polyacrylic acid, polyethylene glycol, polypyrrole, polyaniline, sucrose, glucose, maltose, citric acid, asphalt, furfural resin, epoxy resin and phenolic resin.
[0089] In some embodiments, the cooling product and the carbon source can be mixed by VC mixing, fusion, ball milling, three-dimensional mixing, fluidized bed mixing, etc.
[0090] In some embodiments, the mass ratio of the solid carbon source to the precursor is 5:(5-95).
[0091] In some embodiments, the temperature of the carbonization treatment is 500°C-800°C, and the time of the carbonization treatment is 2h-20h. The temperature of the carbonization treatment can be 500°C, 530°C, 580°C, 600°C, 620°C, 650°C, 680°C, 700°C, 750°C or 800°C, etc., which is not limited here. The time of thermal cracking can be 2h, 3h, 4h, 6h, 8h, 10h, 12h, 15h or 20h, etc., which is not limited here.
[0092] In some embodiments, the equipment used for solid phase carbon coating is at least one of a rotary kiln, a box furnace, a roller kiln, a tunnel kiln, and a push plate kiln.
[0093] In some embodiments, the protective gas may be at least one of nitrogen, argon, helium, neon, krypton, and xenon.
[0094] The liquid phase carbon coating process specifically comprises mixing the cooled product with the carbon source uniformly, then placing it in a furnace, introducing a protective gas, and heat treating the mixture so that the carbon source is cracked and coated on the surface of the cooled product.
[0095] In some embodiments, the carbon source used for liquid carbon coating is an organic carbon source, specifically low-temperature liquid asphalt, furfuryl alcohol, glycidyl methacrylate, triethylene glycol dimethacrylate, and the like.
[0096] In some embodiments, the protective gas may be at least one of nitrogen, argon, helium, neon, krypton, and xenon.
[0097] In some embodiments, when the carbon-coated product is placed at 800° C. to 1100° C. for heat treatment, the heat treatment holding time is 0.5 h to 18 h to obtain a negative electrode material.
[0098] In some embodiments, the temperature of the heat treatment may be 800°C, 850°C, 900°C, 950°C, 1000°C, 1050°C or 1100°C, etc., which is not limited herein.
[0099] In some embodiments, the holding time of the heat treatment is 0.5h to 18h, specifically 0.5h, 1h, 2h, 3h, 4h, 6h, 8h, 10h, 12h, 16h or 18h, etc., which are not limited here. Preferably, the holding time of the heat treatment is 3h to 8h. The maximum temperature treatment holding time during heat treatment is defined as the time when the temperature measured by the heat treatment equipment reaches the maximum temperature of the heat treatment within the range of ±10°C. The text related to the high temperature heat treatment time in the following text refers to this concept and will not be repeated. An embodiment of the present invention also provides a lithium ion battery, using the negative electrode material provided by the above embodiment of the present invention or the negative electrode material prepared by the method for preparing the negative electrode material provided by the above embodiment of the present invention. The lithium ion battery provided by the embodiment of the present invention has the advantages of excellent rate performance and low expansion.
[0100] Test method:
[0101] 1) Particle size of negative electrode material:
[0102] The particle size test method refers to GB / T 19077-2016. It can be conveniently measured using a laser particle size analyzer, such as the Mastersizer 3000 laser particle size analyzer from Malvern Instruments Ltd., UK.
[0103] 2) Testing method for specific surface area of negative electrode material:
[0104] Under constant temperature and low temperature, after measuring the adsorption amount of gas on the solid surface at different relative pressures, the monolayer adsorption amount of the sample is obtained based on the Brownauer-Etter-Taylor adsorption theory and its formula (BET formula), thereby calculating the specific surface area of the material.
[0105] 3) pH test of negative electrode material:
[0106] Take 10 g of negative electrode material, add 10 g of water, stir for 30 min, and then measure the pH value using a pH meter.
[0107] 4) Test of the mass content of carbon element in negative electrode material:
[0108] Thermogravimetric analysis was used to measure the mass content of amorphous carbon.
[0109] 5) Test of the mass content of oxygen in negative electrode materials:
[0110] Use an oxygen, nitrogen and hydrogen analyzer to test the oxygen content.
[0111] 6) Test method for the mass content of doped metal elements in negative electrode materials:
[0112] The negative electrode material was burned at 750°C in an oxygen-containing atmosphere to constant weight, and then dissolved with a mixed acid consisting of concentrated HF, concentrated HCl, and concentrated HNO3 until the solution no longer produced bubbles. The mixed acid was then added in double the amount. When the solution still had no bubbles, the digestion solution of the negative electrode material was obtained by solid separation. The mass content of the doped metal elements in the digestion solution was tested by electrically coupled plasma atomic emission spectroscopy.
[0113] 7) Test method for average size of silicon grains in negative electrode materials:
[0114] The negative electrode material was tested using an X-ray diffraction analysis device model TD3600 produced by Dandong Tongda, and the data was processed using X'Pert HighScore Plus software. The parameters in the Strip K-Alpha2 project were set as follows: K-A1 / K-A2Intensity ratio was 0.5, wavelength ratio corr was 0, and Strip K-Alpha2 was smoothed with a smooth degree parameter of 1. After the software automatically searched for peaks, the angle range was set to 27.5-29.5. After using automatic fitting, the half-peak width and peak position of the Si characteristic peak at about 28° were read from the Peak List, and the average size of silicon grains was calculated by substituting the Scherrer formula.
[0115] 8) Test method for mass content of crystalline silicon in negative electrode materials
[0116] 4.5g of the negative electrode material of each embodiment and comparative example was taken respectively, and mixed evenly with 0.5g of magnesium oxide (analytical grade) sealed and preserved to ensure no deterioration, and the sampling was accurate to 0.1mg, and the mixture was manually ground and mixed using an agate mortar. It was necessary to grind the small fragments that may exist in the magnesium oxide powder with slight force. The grinding time was recommended to be 15-20min, and the white powder could not be seen visually, and there was no upper limit on the time. The X-ray diffraction analysis equipment model TD3600 produced by Dandong Tongda was used for testing, and the test parameters were as follows:
[0117] Divergence slit DS / ° 1.0 Scanning range / ° 10~90 Anti-scatter slit SS / ° 1.0 Scan Step / ° 0.02 Receiving slit SS / mm 0.4 Scan Mode Step Scan Voltage / kV 40 Integration time per step / s 2 Current / mA 40 Scan time / min 2:13'20"
[0118] The above X-ray diffraction (XRD) data were processed using Jade 6.0 software. The data processing flow and parameter settings are as follows. Right-click the BG icon in the main toolbar. Figure 3a Set the background parameters as shown and click "Apply". The red dot obtained indicates the set background point.
[0119] Click the BE button in the middle toolbar to delete or add background points on the graph. On the graph, use the left mouse button to add background points and the right mouse button to delete background points. Delete all background points above the background line to make the background line the lowest. Click "Remove" in the background parameter setting dialog box to deduct the background.
[0120] according to Figure 3b Set the smoothing parameters as shown below to complete the smoothing operation. Figure 3c Set the peak search parameters as shown, click "Apply", select all the check boxes on the left, and click "OK".
[0121] like Figure 3d As shown in the above phase analysis window, right-click in the upper toolbar icon, and click on the possible elements in the pop-up periodic table. After selecting the possible elements in the above periodic table, click "OK". Click on the toolbar icon, then only the phases related to the selected element will remain in the phase analysis window, making it convenient for phase retrieval and analysis.
[0122] In such Figure 3e In the Phase Analysis window, select the appropriate PDF card based on the sample conditions, elemental composition, peak matching degree and other factors. Click the check box in front of the selected card and the card will be selected.
[0123] Note: Phase selection principle
[0124] When other factors are the same, give priority to cards with low FOM values and J values of C or +. Be sure to choose cards with RIR values, otherwise quantitative calculations cannot be performed.
[0125] When processing the same data multiple times, testing the same sample multiple times, or testing the same series of samples multiple times, try to choose the same PDF card. Even if you cannot choose the same PDF card, you must choose a card with the same or similar RIR value to ensure the consistency of the calculation results.
[0126] If you cannot find a known card in the window list, you can enter the card number in the input window and press Enter, and the corresponding card will be added to the window list. After the crystal phase is determined, return to the main window of the software. For different phases, select the appropriate angle range for fitting. Generally, a phase only needs to fit its strongest peak, but if the peak to be fitted overlaps with other peaks, it should be fitted together with the overlapping peaks to reasonably separate the peaks.
[0127] After selecting the range, right-click icon, and click the "Refine" button three times in the pop-up dialog box. After the strongest peaks of all phases are fitted, proceed to the next step.
[0128] Click the "Option" button in the taskbar and select "Easy Quantitative Analysis" in the drop-down box. In the pop-up quantitative calculation window, first select the internal standard phase to be added, fill in the amount of internal standard added (mass percentage) and check the "Internal Standard" checkbox.
[0129] Then check each phase one by one, pay attention to the peak checkboxes marked with angles on the left side of the window (as shown above), and only check one of the strongest peaks (or other peaks selected for calculation) for each phase, and uncheck the remaining peaks to avoid calculation errors. Click the "Calc RIR" button in the toolbar above the window, and then click the "Calc Wt%" button, and the calculation is complete. Then click the "Show Graph" button to display the calculation results.
[0130] Wherein, "Wt(n)%" represents the mass percentage content of each crystalline phase after deducting the internal standard, and reads the mass percentage content of the Si phase; "Others+Amorphous" represents the sum of the contents of unidentified crystalline phases and amorphous phases, and represents the amorphous phase content in this method.
[0131] The number in brackets after each crystalline phase content value represents the calculation error. This method requires that the error value does not exceed 10% of the corresponding crystalline phase content value (except for amorphous phase and low-content crystalline phase).
[0132] Repeated calculation: Since the fitting operation is greatly affected by human factors, it also has a great impact on the final calculation results. Therefore, each sample is calculated three times according to the above steps, and the relative standard deviation (RSD) of the three calculations is required to be ≤10% to reduce the impact of human factors. After manually deducting the background, smoothing the curve, patrolling the peak to confirm the crystal phase, and fitting the data, the strongest peak of each phase is used as the standard for calculation to obtain the composition ratio of all crystal phases and amorphous phases. Then, the proportion of silicon crystal phase in the total sample is confirmed as above, and the percentage is converted into a decimal count and set as M. Si .
[0133] Calculation Method of the Mass Ratio of Crystalline Silicon The carbon content of the negative electrode materials of each embodiment and comparative example was tested using the aforementioned test method, and the decimals were counted and set to M C The negative electrode materials of each embodiment and comparative example were tested for oxygen content using the aforementioned test method, with decimal counts set as M O The total content of each metal element in the negative electrode materials of each embodiment and comparative example was tested using the aforementioned test method, and the decimals were counted and set as M M In summary, the mass ratio of crystalline silicon = M Si / (1-M C -M O -MM ).
[0134] 9) Cycle performance and rate test
[0135] The prepared negative electrode material is mixed with graphite (artificial graphite S360 series) in a ratio of 10:90, and then mixed with sodium carboxymethyl cellulose CMC, binder styrene-butadiene rubber SBR, conductive agent Super-P, and conductive agent KS-6 in a mass ratio of 92:2:2:4 to form a slurry, which is coated on a copper foil, and vacuum dried and rolled to prepare a negative electrode sheet; the counter electrode is a lithium sheet, and a 1 mol / L LiPF6 / ethylene carbonate + dimethyl carbonate + methyl ethyl carbonate (v / v=1:1:1) electrolyte and a Celgard2400 separator are assembled into a button battery.
[0136] The cycle performance test uses a 30mA current to perform constant current charge and discharge experiments, and the charge and discharge voltage is limited to 0-1.5V. The LAND battery test system of Wuhan Jinnuo Electronics Co., Ltd. is used for testing. At room temperature, the button battery is cycled at 0.1C, 0.2C, and 0.5C for one cycle, and then charged and discharged at 1C for 47 cycles. The capacity of the 50th week is divided by the capacity of the first week to obtain the product's 50-week cycle capacity retention rate. The 0.1C capacity divided by the 1C capacity is used to evaluate the product rate performance.
[0137] The negative electrode materials prepared in each embodiment and comparative example are used as negative electrode precursors. The mass ratio of precursor, conductive agent (Super P) and binder (CMC+SBR) in the electrode sheet coating is 92:4:4. The counter electrode is a lithium sheet. A 1 mol / L LiPF6 / EC+DMC+EMC (v / v=1:1:1) electrolyte and Celgard2400 diaphragm are used to assemble button cells. The first cycle charge and discharge test is carried out with this battery. The charge and discharge system is
[0138] Charging: 0.1C to 10mV CC, 0.02C to 5mV CC; Discharging: 0.1C to 1.5V CC.
[0139] The following is a further description of the embodiments of the present invention in multiple embodiments. The embodiments of the present invention are not limited to the following specific embodiments. The embodiments can be appropriately modified within the scope of the unchanged main rights.
[0140] Example 1
[0141] A method for preparing a negative electrode material comprises the following steps:
[0142] (1) Take a mixture of silicon and silicon dioxide, place it in a reaction chamber, and evacuate it to a vacuum degree of less than 1*10 -4Pa, heated to 1100℃, vapor formed by gasification; in the vacuum deposition chamber, helium is used to generate plasma flow at RF power of 30kW, the vapor is transported to the plasma flow for plasma reaction, and the condensed and collected solid is crushed to D 50 =12μm precursor.
[0143] (2) The precursor was carbon-coated at 700°C for 6 hours using a CVD method, and the carbon-coated product was heat-treated at 1100°C for 1 hour to obtain a negative electrode material.
[0144] The parameters of the negative electrode materials are detailed in Table 1.
[0145] Example 2
[0146] A method for preparing a negative electrode material comprises the following steps:
[0147] (1) Take a mixture of silicon, silicon dioxide and magnesium oxide, place it in a reaction chamber, and evacuate it to a vacuum degree of less than 1*10 -4 Pa, heated to 1100℃, vapor is formed, and helium is used in the vacuum deposition chamber to generate plasma flow at RF power of 30kW. The vapor is transported to the plasma flow for plasma reaction, and the solid collected by condensation is crushed into D 50 =12μm precursor.
[0148] (2) The precursor was carbon-coated at 700°C for 6 hours using a CVD method, and the carbon-coated product was heat-treated at 900°C for 1 hour to obtain a negative electrode material.
[0149] The parameters of the negative electrode materials are detailed in Table 1.
[0150] Example 3
[0151] A method for preparing a negative electrode material comprises the following steps:
[0152] (1) Take a mixture of silicon, silicon dioxide and magnesium metal, place it in a reaction chamber, and evacuate it to a vacuum degree of less than 1*10 -4 Pa, heated to 1100℃, vapor is formed, and helium is used in the vacuum deposition chamber to generate plasma flow at RF power of 20kW. The vapor is transported to the plasma flow for plasma reaction, and the solid collected by condensation is crushed into D 50 =12μm precursor.
[0153] (2) The precursor was carbon-coated at 700°C for 6 hours using a CVD method, and the carbon-coated product was heat-treated at 920°C for 2 hours to obtain a negative electrode material.
[0154] The other parameters of the negative electrode materials are shown in Table 1.
[0155] Example 4
[0156] A method for preparing a negative electrode material comprises the following steps:
[0157] (1) Take a mixture of silicon, silicon dioxide and metallic lithium, place it in a reaction chamber, and evacuate it to a vacuum degree of less than 1*10 -4 Pa, heated to 1300℃, vapor is formed, and helium is used in the vacuum deposition chamber to generate plasma flow at 20kW RF power. The vapor is transported to the plasma flow for plasma reaction, and the solid collected by condensation is crushed into D 50 =6μm precursor.
[0158] (2) The precursor was carbon-coated at 700°C for 6 hours using a CVD method, and the carbon-coated product was heat-treated at 950°C for 1 hour to obtain a negative electrode material.
[0159] The other parameters of the negative electrode materials are shown in Table 1.
[0160] Example 5
[0161] A method for preparing a negative electrode material comprises the following steps:
[0162] (1) Take a mixture of silicon and silicon dioxide, place it in a reaction chamber, and evacuate it to a vacuum degree of less than 1*10 -4 Pa, heated to 1200℃, vaporized to form a plasma flow using helium at a radio frequency power of 90kW in a vacuum deposition chamber, the vapor is transported to the plasma flow for plasma reaction, and the condensed and collected solids are crushed to D 50 =5μm precursor.
[0163] (2) The precursor was carbon-coated at 800°C for 6 hours using a CVD method, and the carbon-coated product was heat-treated at 1000°C for 8 hours to obtain a negative electrode material.
[0164] The other parameters of the negative electrode materials are shown in Table 1.
[0165] Example 6
[0166] The difference from Example 1 is that the carbon-coated product is heat-treated at 1100° C. for 18 hours.
[0167] Example 7
[0168] The difference from Example 1 is that the carbon-coated product is heat treated at 800° C. for 2 hours.
[0169] Example 8
[0170] A method for preparing a negative electrode material comprises the following steps:
[0171] (1) Take a mixture of silicon, silicon dioxide and metallic lithium, place it in a reaction chamber, and evacuate it to a vacuum degree of less than 1*10 -4 Pa, heated to 1300℃, vapor is formed, and helium is used in the vacuum deposition chamber to generate plasma flow at 20kW RF power. The vapor is transported to the plasma flow for plasma reaction, and the solid collected by condensation is crushed into D 50 =6μm precursor.
[0172] (2) The precursor was carbon-coated at 550°C for 1 hour using a CVD method, and the carbon-coated product was heat-treated at 950°C for 1 hour to obtain a negative electrode material.
[0173] Other parameters of negative electrode materials are shown in Table 1
[0174] Example 9
[0175] The difference from Example 1 is that the particle size of the negative electrode material is D20-D10=5.1 μm, and D90-D80=9.5 μm.
[0176] Comparative Example 1
[0177] A method for preparing a negative electrode material comprises the following steps:
[0178] (1) Take a mixture of silicon and silicon dioxide, place it in a reaction chamber, and evacuate it to a vacuum degree of less than 1*10 -4 Pa, heated to 1200℃, vaporized to form steam, condensed and collected solids, crushed to D 50 =5μm composite.
[0179] (2) The composite was carbon-coated at 800° C. using a CVD method, and the carbon-coated product was heat-treated at 1000° C. for 8 hours to obtain a negative electrode material.
[0180] The parameters of the negative electrode materials are detailed in Table 1.
[0181] Comparative Example 2
[0182] A method for preparing a negative electrode material comprises the following steps:
[0183] (1) Take a mixture of silicon and silicon dioxide, place it in a reaction chamber, and evacuate it to a vacuum degree of less than 1*10 -4 Pa, heated to 1200 ° C, neon gas was used in the vacuum deposition chamber to generate plasma flow at a radio frequency power of 5 kW, the vapor was transported into the plasma flow for plasma reaction, and the condensed and collected solids were crushed into D 50 =5μm composite.
[0184] (2) The composite was carbon-coated at 900° C. using a CVD method, and the carbon-coated product was heat-treated at 1200° C. for 20 hours to obtain a negative electrode material.
[0185] The other parameters of the negative electrode materials are shown in Table 1.
[0186] Comparative Example 3
[0187] A method for preparing a negative electrode material comprises the following steps:
[0188] (1) Take a mixture of silicon and silicon dioxide, place it in a reaction chamber, and evacuate it to a vacuum degree of less than 1*10 -4 Pa, heated to 1200℃, vaporized to form steam, condensed and collected solids, crushed to D 50 =5μm composite.
[0189] (2) The composite was carbon-coated at 700°C by CVD method, and the carbon-coated product was heat-treated at 400°C for 24 hours to obtain a negative electrode material; the parameters of the negative electrode material are detailed in Table 1.
[0190] Comparative Example 4
[0191] The difference from Example 1 is that the carbon-coated product is heat-treated at 1400° C. for 8 hours.
[0192] The negative electrode materials obtained in the examples and comparative examples were subjected to performance tests. The results of the above performance tests are shown in Table 1:
[0193] Table 1. Summary of performance test results
[0194]
[0195] According to the data in Table 1, by controlling the relationship between the mass ratio of crystalline silicon in silicon and the average size of silicon grains, significant improvements can be achieved in lithium ion transmission impedance, solid-liquid interface stability, and long-term cycle crystal phase structure stability. Specifically, crystalline silicon is more structurally stable than amorphous materials, and the peak intensity and peak position in dQ / dv change little during the cycle, but the direction of crystalline silicon expansion is selective, resulting in uneven expansion stress, which in turn causes the negative electrode particles to break and expose more silicon interfaces, triggering side reactions with the electrolyte, causing the SEI film to grow and thicken continuously, resulting in deterioration of interface stability; silicon elements (single substance, compound) in the amorphous state can stabilize the overall structure of the negative electrode particles, buffer expansion deformation, reduce the breakage of negative electrode particles, and improve interface stability. At the same time, amorphous materials are isotropic materials, and there is no directional selectivity in lithium insertion, and the lithium ion transmission impedance is lower; in summary, by regulating the mass ratio of crystalline silicon and the average size of silicon grains, the negative electrode products can simultaneously have low lithium ion transmission impedance, high solid-liquid interface stability, and strong long-term cycle crystal phase structure stability, greatly improving the overall performance of the product.
[0196] The mass content of crystalline silicon in Example 7 is lower than that in Example 1. This is because the temperature of the carbonized coating product is relatively low and the time is too short during the heat treatment process. Therefore, a part of the silicon element does not form crystalline silicon, which causes a slight decrease in the cycle performance of the negative electrode material.
[0197] The negative electrode material prepared in Example 9 has a particle size deviation from D 20 -D 10 ≤4μm, D 90 -D 80 In the range of ≤8μm, the particle size distribution of the negative electrode material shifts toward the larger particle size as a whole. Large particle sizes are more fragile and more likely to break and deactivate during long cycles, affecting the electrochemical performance of the product. Therefore, the cycle performance of the negative electrode material is reduced.
[0198] During the preparation of the composite in Comparative Example 1, steam was not input into the plasma flow for plasma reaction. After the inducing effect of the seed crystal was lost, the mass content of crystalline silicon decreased significantly. Although the first-cycle reversible capacity of the negative electrode material increased, its cycle performance decreased significantly and the rate performance also decreased.
[0199] In Comparative Example 2, the heat treatment temperature is too high and the treatment time is too long, resulting in a significant increase in the mass content of crystalline silicon beyond the expected range. The size of the silicon particles will also increase, resulting in an imbalance in the ratio of amorphous silicon to crystalline silicon, which can easily lead to excessive local expansion stress in the negative electrode material, resulting in a decrease in the rate performance and cycle performance of the negative electrode material.
[0200] In Comparative Example 3, plasma was not used to manufacture seed crystals and the carbonization temperature was too low. After a long period of carbonization, the silicon grains were difficult to grow, causing the mass content of crystalline silicon to increase significantly beyond the expected range, causing A / B to exceed the required range, resulting in deterioration of product performance.
[0201] In Comparative Example 4, the carbonization temperature of the semi-finished product containing seed crystals was too high, resulting in rapid growth of silicon grains. Although the mass content of crystalline silicon did not exceed expectations, the product expansion stress was still out of control, leading to performance degradation.
[0202] Although the present application is disclosed as above with preferred embodiments, it is not intended to limit the claims. Any technical personnel in this field may make several possible changes and modifications without departing from the concept of the present application. Therefore, the scope of protection of the present application shall be based on the scope defined by the claims of the present application.
Claims
1. A negative electrode material, characterized in that: The negative electrode material contains silicon, and the silicon is at least partially present in the form of crystalline silicon; Taking the mass content of silicon element in the negative electrode material as 100%, the mass content of crystalline silicon is A%, and the average size of silicon grains of the crystalline silicon is B nm; The negative electrode material satisfies the following characteristics: 0.3≤A / B≤60, and 6≤A+B≤75.
2. The negative electrode material according to claim 1, characterized in that Taking the mass content of silicon element in the negative electrode material as 100%, the mass content of crystalline silicon is A%, and the value range of A is 5-65.
3. The negative electrode material according to claim 1, characterized in that The average size of the silicon grains is B nm, and B≤7.
4. The negative electrode material according to claim 1, characterized in that Meet at least one of the following characteristics: (1) The negative electrode material further includes an oxygen element, and the atomic ratio of the oxygen element to the silicon element in the negative electrode material is x, 0<x<2.2; (2) The negative electrode material further includes oxygen, and the component containing oxygen and silicon in the negative electrode material includes at least one of silicon oxide and silicate; (3) The negative electrode material further includes carbon element, and the component containing the carbon element in the negative electrode material includes at least one of amorphous carbon, graphite, graphene, carbon nanotubes and carbon fibers.
5. The negative electrode material according to claim 1, characterized in that The negative electrode material further includes a doped metal element, and the doped metal element is selected from at least one of Li, Mg, Cu, Ni, Fe, Cr and Zn.
6. The negative electrode material according to claim 5, characterized in that The doped metal element includes Mg element, and the mass content of the Mg element in the negative electrode material is 3% to 25%; and / or the average size of the silicon grains is B nm, and B≤15.
7. The negative electrode material according to claim 5, characterized in that The doped metal element comprises Li element, and the mass content of Li element in the negative electrode material is 3% to 15%; and / or the average size of the silicon grains is B nm, and B≤10.
8. The negative electrode material according to claim 1, characterized in that Meet at least one of the following characteristics: (1) The mass content of oxygen in the negative electrode material is 10% to 55%; (2) The mass content of carbon in the negative electrode material is 1% to 40%; (3) The mass content of silicon in the negative electrode material is 25% to 90%.
9. The negative electrode material according to any one of claims 1 to 8, characterized in that Meet at least one of the following characteristics: (1) At least part of the surface of the negative electrode material has a carbon layer; (2) The particle size of the negative electrode material satisfies: D 20 -D 10 ≤4μm, D 90 -D 80 ≤8μm; (3) The specific surface area of the negative electrode material is 0.1 m 2 / g~25m 2 / g; (4) The pH of the negative electrode material is 6 to 10; (5) The true density of the negative electrode material is 2.0 g / cm 3 ~3.4g / cm 3 .
10. A battery, characterized in that: The negative electrode material comprises the negative electrode material as claimed in any one of claims 1 to 9.
Citation Information
Patent Citations
Compound material of anode fit for producing secondary battery and its produced battery
CN101064367A
Connecting material for solid oxide fuel cell, manufacturing method thereof, and solid oxide fuel cell comprising same
CN112204781A
Silicon compound negative electrode material, preparation method thereof and lithium ion battery
CN112563476A
Negative electrode plate and lithium ion battery
CN113130869A
Composite silicon material and lithium ion battery
CN113130870A