Method for improving yield of titanium alloy seamless tube

By optimizing the composition of titanium alloy and combining the upsetting mode with glass lubrication technology, the problem of poor fluidity of titanium alloy seamless pipes during the extrusion process is solved, and the material yield and surface quality are significantly improved.

CN118989209AActive Publication Date: 2024-11-22CHENGDU ADVANCED METAL MATERIALS IND TECH RES INST CO LTD

Patent Information

Application Number
CN202411151770.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-21
Publication Date
2024-11-22
Estimated Expiration
2044-08-21

AI Technical Summary

Technical Problem

During the extrusion process, the existing titanium alloy seamless pipes have poor fluidity due to the high friction coefficient of the titanium alloy, which is prone to cracking or cracking, resulting in low material yield.

Method used

By optimizing the titanium alloy composition, adding transition element Cu, using commutation upsetting and diagonal upsetting switching modes to obtain titanium alloy rods with radial texture, and glass lubrication is performed before extrusion, using a new mold Perform extrusion to improve the uniformity of metal flow.

Benefits of technology

The straightness and material yield of titanium alloy seamless pipes are improved, and the surface cracking problem during the extrusion process is avoided. The extrusion pressure is small, the straightness is high, the surface quality is high, and the remaining material is small.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a method for improving the yield of a titanium alloy seamless tube, which comprises the following steps of: optimizing titanium alloy components, improving the plasticity of titanium alloy, obtaining a titanium alloy bar with a radial texture by adopting a reversing upsetting-drawing and diagonal upsetting-drawing switching mode, machining the bar to obtain a seamless tube rough blank, and carrying out hot rolling on the seamless tube rough blank to obtain the finished product of the titanium alloy seamless tube. After glass lubrication, a novel die extruder is adopted for extrusion, an extrusion die inlet arc follows a binary function formula Y = 0.04 X < 2 > + 3X + A (A is a constant), an extrusion die outlet taper angle ranges from 25 degrees to 35 degrees, the extrusion ratio ranges from 10 to 18, and the extrusion speed ranges from 90 mm / s to 120 mm / s; according to the method, the flowing uniformity of metal on the surface of the titanium alloy is improved, the problems of surface cracking and the like in the extrusion process are avoided, the extrusion force is small, the straightness is high, the surface quality is high, remaining materials are few, and the yield is high. Through the comprehensive preparation method, the surface quality and the flatness of the titanium alloy seamless tube are improved, and the yield of the seamless tube is greatly increased.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of titanium alloy processing, and in particular relates to a method for improving the yield rate of titanium alloy seamless pipes. Background Art

[0002] Titanium alloy seamless pipes have excellent mechanical properties and corrosion resistance. In recent years, they have been widely used in aerospace, ship power systems, heat exchangers for seawater desalination, water and oil pipelines for ships and offshore oil platforms, and pipe networks for municipal engineering projects on islands and reefs. The existing preparation processes for titanium alloy seamless pipes mainly include extrusion process and oblique rolling piercing-rolling process. Compared with the oblique rolling piercing process, the extrusion method was used the earliest and most mature in my country. However, during the extrusion process, due to the large friction coefficient of titanium alloy itself, the fluidity is poor, so the extruded products are easy to break or crack, resulting in a low yield rate of titanium alloy seamless pipes. Summary of the invention

[0003] In order to solve the bottleneck problem existing in the above-mentioned prior art, the present invention optimizes the composition of titanium alloy, improves the plasticity of titanium alloy, adopts the switching mode of reversing upsetting and diagonal upsetting to obtain titanium alloy rods with radial texture, and obtains seamless tube rough blanks after machining the rods. After glass lubrication, a new type of die extruder is used for extrusion, which improves the uniformity of metal flow on the surface of titanium alloy and avoids problems such as surface cracking during extrusion. The extrusion force is small, the straightness is high, the surface quality is high, the excess material is small, and the yield rate is high. Through the above-mentioned comprehensive preparation method, not only the straightness of titanium alloy seamless tubes is improved, but also the yield rate of seamless tubes is greatly improved.

[0004] In order to achieve the above-mentioned object of the invention, the present invention provides a method for improving the yield rate of titanium alloy seamless pipes, the method comprising the following steps:

[0005] ① The raw materials are mixed and pressed into a plurality of electrode blocks, and the plurality of electrode blocks are welded to obtain a consumable electrode, and a transition element Cu is added, wherein the mass content of the Cu element is 3% to 7%; the plasticity of the alloy is improved by adding the transition element Cu.

[0006] ② The consumable electrode obtained in step ① is smelted 2 to 3 times in a vacuum consumable arc furnace to obtain a titanium alloy ingot.

[0007] ③ The titanium alloy ingot obtained in step ② is kept at 880℃~1100℃ for 4~5h, and then subjected to 6 fires of upsetting and rolling to form titanium alloy bars. The upsetting adopts the switching mode of xyz reversing upsetting and diagonal reversing upsetting; xyz reversing upsetting adopts three-pier and three-drawing, and diagonal reversing upsetting adopts four-pier and four-drawing, and the deformation of each fire is 40%~50%; after the first fire of xyz reversing upsetting, the second fire is diagonal reversing upsetting, and so on, that is, after each xyz reversing upsetting, it is replaced with diagonal reversing upsetting, and the two upsetting modes are operated alternately, and the last fire is drawn and rolled into bars. This forging method can significantly improve the uniformity of the forged bar structure, reduce the segregation of Cu elements, and improve the subsequent extrusion pass rate and surface quality.

[0008] ④ The bar obtained in step ③ is subjected to no less than two rounds of fine forging, and the fine forged bar is annealed at an annealing temperature of [T-(120-200)]°C for 1-2 hours, wherein T is the phase transition point temperature in °C. After annealing and straightening, the bar is subjected to polishing and drilling to obtain a titanium alloy seamless pipe rough blank.

[0009] ⑤Heat the titanium alloy seamless tube rough blank obtained in step ④ at a heating temperature of [T β -(50~80)]℃, where T β is the phase transition point temperature, in degrees Celsius; then glass lubricant is applied to the inner and outer surfaces of the tube.

[0010] ⑥ The lubricated seamless tube obtained in step ⑤ is extruded by a horizontal extruder, and the arc of the extrusion die entrance follows the binary function formula Y = 0.04X 2 +3X+A (A is a constant), the extrusion die outlet cone angle is 25°~35°; the extrusion ratio is 10~18, and the extrusion speed is 90~120mm / s.

[0011] ⑦ The seamless pipe obtained in step ⑥ is vacuum annealed, straightened, pickled and then put into storage.

[0012] Compared with the prior art, the present invention has the following beneficial effects:

[0013] The present invention optimizes the composition of titanium alloy, improves the plasticity of titanium alloy, adopts the switching mode of reversing upsetting and diagonal upsetting to obtain titanium alloy rods with radial texture, obtains seamless tube rough blanks after machining, and uses a new die extruder for extrusion after glass lubrication, thereby improving the uniformity of metal flow on the surface of titanium alloy, avoiding problems such as surface cracking during extrusion, and having small extrusion force, high straightness, high surface quality, little excess material, and high yield rate. Through the above comprehensive preparation method, not only the surface quality and straightness of titanium alloy seamless tubes are improved, but also the yield rate of seamless tubes is greatly improved. DETAILED DESCRIPTION

[0014] The present invention is further described below in conjunction with specific examples, but the present invention is not limited in any way. To avoid redundant description, the raw materials in the following examples are all commercially available products unless otherwise specified, and the methods used are all conventional methods unless otherwise specified.

[0015] Example 1

[0016] A method for improving the yield rate of titanium alloy seamless pipes, producing TA18 titanium alloy seamless pipes with a specification of Φ48×12mm, the specific process flow is:

[0017] ① The raw materials are mixed to press a plurality of electrode blocks, the plurality of electrode blocks are welded to obtain a consumable electrode, and a transition element Cu is added; the mass content of the Cu element is 3%.

[0018] ② The consumable electrode obtained in step ① is smelted twice in a vacuum consumable arc furnace to obtain a titanium alloy ingot; the ingot specification is Φ550mm.

[0019] ③ The titanium alloy ingot obtained in step ② is kept at 880°C for 5h, and subjected to 6 fires of upsetting and rounding to form a titanium alloy bar (machining). The upsetting and drawing adopts the switching mode of xyz reversing upsetting and diagonal reversing upsetting and drawing; odd-numbered fires of reversing upsetting and drawing (three upsetting and three drawing) → even-numbered fires of diagonal upsetting and drawing (four upsetting and four drawing), and the last fire (sixth fire) is upsetting and forging (drawing and lengthening and rounding).

[0020] ④ The bar obtained in step ③ is subjected to no less than two rounds of fine forging, and the fine forged bar (Φ150mm bar) is annealed (750℃ / 2h), and after annealing and straightening, it is polished and drilled to Φ130*Φ30mm to obtain a titanium alloy seamless pipe rough blank.

[0021] ⑤Heat the titanium alloy seamless tube rough blank obtained in step ④ at a heating temperature of [T β -(50~80)]℃, where T β is the phase transition point temperature; then the glass lubricant is applied to the inner and outer surfaces of the tube.

[0022] ⑥ The lubricated seamless tube obtained in step ⑤ is extruded by a horizontal extruder with an extrusion force of 20 N, an extrusion ratio of 12.5, and an extrusion speed of 100 mm / s to obtain a Φ48×12 mm seamless tube.

[0023] ⑦ The seamless pipe obtained in step ⑥ is vacuum annealed, straightened, pickled and then put into storage; the annealing temperature is 700°C and the insulation time is 2h.

[0024] The TA18 titanium alloy seamless tube prepared in Example 1 has a smooth outer surface, a straightness of 4 mm / m, and a yield rate of 97%.

[0025] Example 2

[0026] A method for improving the yield rate of titanium alloy seamless pipes, producing TA18 titanium alloy seamless pipes with a specification of Φ48×12mm, the specific process flow is:

[0027] ① The raw materials are mixed to press a plurality of electrode blocks, the plurality of electrode blocks are welded to obtain a consumable electrode, and a transition element Cu is added; the mass content of the Cu element is 7%.

[0028] ② The consumable electrode obtained in step ① is smelted three times in a vacuum consumable arc furnace to obtain a titanium alloy ingot; the ingot specification is Φ550mm.

[0029] ③ The titanium alloy ingot obtained in step ② is kept at 1100℃ for 4h, and subjected to 6 fires of upsetting and rolling into titanium alloy bars (machining). The upsetting and drawing adopts the switching mode of xyz reversing upsetting and diagonal reversing upsetting and drawing; odd-numbered fires of reversing upsetting and drawing (three upsetting and three drawing) → even-numbered fires of diagonal upsetting and drawing (four upsetting and four drawing), and the last fire (sixth fire) is upsetting and forging (drawing and lengthening and rolling).

[0030] ④ The bar obtained in step ③ is subjected to no less than two rounds of fine forging, and the fine forged bar (Φ150mm bar) is annealed (750℃ / 2h), and after annealing and straightening, it is polished and drilled to Φ130*Φ30mm to obtain a titanium alloy seamless pipe rough blank.

[0031] ⑤Heat the titanium alloy seamless tube rough blank obtained in step ④ at a heating temperature of [T β -(50~80)]℃, where T β is the phase transition point temperature; then the glass lubricant is applied to the inner and outer surfaces of the tube.

[0032] ⑥ The lubricated seamless tube obtained in step ⑤ is extruded by a horizontal extruder with an extrusion force of 18N, an extrusion ratio of 12.5, and an extrusion speed of 100mm / s to obtain a Φ48×12mm seamless tube.

[0033] ⑦ The seamless pipe obtained in step ⑥ is vacuum annealed, straightened, pickled and then put into storage; the annealing temperature is 700°C and the insulation time is 2h.

[0034] The TA18 titanium alloy seamless tube obtained in Example 2 has a smooth outer surface, a straightness of 3 mm / m, and a yield rate of 98%.

[0035] For any technician familiar with the art, without departing from the scope of the technical solution of the present invention, the technical content disclosed above can be used to make many possible changes and modifications to the technical solution of the present invention, or modified into equivalent embodiments with equivalent changes. Therefore, any simple modification, equivalent change and modification made to the above embodiments according to the technical essence of the present invention without departing from the content of the technical solution of the present invention should still fall within the scope of protection of the technical solution of the present invention.

Claims

1. A method for improving the yield rate of titanium alloy seamless pipes. It is characterized in that The method comprises the following steps: ① The raw materials are mixed and pressed into multiple electrode blocks, and the multiple electrode blocks are welded to obtain consumable electrodes, and the transition element Cu is added; ② The consumable electrode obtained in step ① is melted 2 to 3 times in a vacuum consumable arc furnace to obtain a titanium alloy ingot; ③ The titanium alloy ingot obtained in step ② is kept at 880° C. to 1100° C. for 4 to 5 hours, and subjected to 6 rounds of upsetting and rolling to form a titanium alloy bar, wherein the upsetting adopts a switching mode of xyz reversing upsetting and diagonal reversing upsetting; ④ The bar obtained in step ③ is subjected to no less than two rounds of fine forging, the fine forged bar is annealed, and after annealing and straightening, it is subjected to lathing and drilling to obtain a titanium alloy seamless pipe rough blank; ⑤Heat the titanium alloy seamless pipe rough blank obtained in step ④ at a heating temperature of T β -(50~80)℃, where T β is the phase transition point temperature; then the glass lubricant is applied to the inner and outer surfaces of the tube blank; ⑥ The lubricated seamless tube obtained in step ⑤ is extruded by a horizontal extruder, and the arc of the extrusion die entrance follows the binary function formula Y = 0.04X 2 +3X+A, extrusion die outlet cone angle 25°~35°; extrusion ratio 10~18, extrusion speed 90~120mm / s; ⑦ The seamless pipe obtained in step ⑥ is vacuum annealed, straightened, pickled and then put into storage.

2. The method according to claim 1, It is characterized in that In step ①, the mass content of the Cu element is 3% to 7%.

3. The method according to claim 2, It is characterized in that In step ③, the xyz reversing upsetting and drawing adopts three upsetting and three drawing, and the diagonal reversing upsetting and drawing adopts four upsetting and four drawing, and the deformation amount per fire is 40% to 50%.

4. The method according to claim 3, It is characterized in that Step ③ The two upsetting modes are operated alternately, and each time the xyz reversing upsetting is replaced by the diagonal reversing upsetting.

5. The method according to claim 4, It is characterized in that The annealing temperature in step ④ is [T-(120-200)]°C, and the holding time is 1-2h, wherein T is the phase transition point temperature.

Citation Information

Patent Citations

  • Preparation method of titanium alloy seamless pipe

    CN112439806A

  • Method for increasing shrinkage strain ratio of TA18 titanium alloy seamless tube and TA18 titanium alloy seamless tube

    CN116656994A

  • Weak-texture TA18 titanium alloy bar and preparation method thereof

    CN116770116A

  • Titanium alloy seamless tube and preparation method thereof

    CN117358778A

  • Smelting and forging method for titanium alloy with low component range

    CN117551904A

Cited By

  • Preparation method of TA15 titanium alloy cold-rolled pipe

    CN117564728A