Copper-based powder metallurgy composite friction material and preparation method thereof
By using nanocrystalline copper powder, silicon carbide nanoparticles, alumina microparticles and self-repairing agents in copper-based powder metallurgy friction materials, a copper-based powder metallurgy composite friction materials with high temperature stability and self-repairing capabilities, the solution is solved The problems of unstable friction coefficient and difficulty in repairing existing materials at high temperatures are improved, and the wear resistance and lubricating performance of the materials are improved.
Patent Information
- Application Number
- CN202411252260.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-09
- Publication Date
- 2024-11-29
AI Technical Summary
The existing copper-based powder metallurgical friction materials have unstable friction coefficient under high temperature and high load conditions, are prone to wear, and are difficult to repair themselves, and cannot meet the strict requirements of high-speed trains, aerospace vehicles, heavy machinery and wind power equipment.
Nano-crystalline copper powder is used as the matrix, combining silicon carbide nanoparticles and alumina microparticles, and adding microencapsulated liquid metal alloys and polymer self-healing agents, as well as nano-scale molybdenum disulfide and graphite lubricants to form a copper-based Powder metallurgical composite friction material activates the self-healing phase through laser cladding to achieve self-healing and high temperature stability of the material.
It significantly improves the high temperature stability and self-repair ability of the material, extends the service life, reduces the friction coefficient and wear rate, and reduces maintenance costs and energy losses.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of powder metallurgy, in particular to a copper-based powder metallurgy composite friction material and a preparation method thereof. Background Art
[0002] With the rapid development of high-speed trains, aerospace vehicles, heavy machinery, wind power equipment and other fields, the performance requirements for friction materials are getting higher and higher. Powder metallurgy technology, as an important material preparation method, has been widely used in the field of friction materials. Copper-based powder metallurgy friction materials have become one of the commonly used friction materials in these fields due to their good thermal conductivity, wear resistance and machinability.
[0003] However, the friction coefficient of existing copper-based powder metallurgy friction materials is unstable under high temperature and high load conditions, and they are prone to increased wear. This is because traditional copper-based powder metallurgy friction materials lack strength and stability at high temperatures and are unable to withstand the friction and heat under extreme working conditions. In addition, existing materials are difficult to self-repair after damage. Once wear or cracks occur, they need to be replaced frequently, which not only increases maintenance costs but also affects the normal operation of equipment. At the same time, the lubrication performance of traditional materials needs to be improved, and a higher friction coefficient is easily generated during the friction process, resulting in energy loss and equipment wear.
[0004] In summary, the performance of existing copper-based powder metallurgy friction materials under high temperature and high load conditions is not satisfactory and cannot meet the strict requirements for friction materials in the fields of high-speed trains, aerospace vehicles, heavy machinery and wind power equipment. Therefore, the development of a copper-based composite friction material with self-healing function, good high temperature stability, strong wear resistance and excellent lubrication performance has become an urgent need in the current field of powder metallurgy technology. Summary of the invention
[0005] In view of the above-mentioned shortcomings of the prior art, the present invention provides a copper-based powder metallurgy composite friction material and a preparation method thereof. By using nanocrystalline copper powder as a matrix, it has high thermal conductivity, can quickly conduct the heat generated by friction, and reduce local overheating. At the same time, the nanocrystalline copper powder also has excellent plasticity, and can undergo certain plastic deformation when subjected to force, thereby alleviating stress concentration. In addition, the addition of silicon carbide nanoparticles and aluminum oxide micron particles in the reinforcing phase further improves the strength and stability of the material at high temperatures. These factors work together to enable the copper-based powder metallurgy composite friction material of the present invention to maintain a stable friction coefficient at high temperatures, thereby significantly improving the high-temperature stability of the material.
[0006] To achieve the above objectives, the present invention is implemented through the following technical solutions: In one aspect, a copper-based powder metallurgy composite friction material, the material components of the friction material specifically include a copper matrix, a reinforcement phase, a self-repairing phase and a lubricating phase; The copper matrix uses nanocrystalline copper powder as the matrix material; The reinforcement phase includes silicon carbide nanoparticles and aluminum oxide microparticles; The self-healing phase contains a microencapsulated self-healing agent, namely a liquid metal alloy and a high molecular polymer; The lubricating phase includes nano-scale molybdenum disulfide and graphite, which are uniformly dispersed in the copper matrix.
[0007] Furthermore, the copper matrix adopts nanocrystalline copper powder, which can quickly conduct heat during friction and reduce local overheating. At the same time, it can undergo certain plastic deformation when subjected to force to relieve stress concentration. The mass percentage of nanocrystalline copper powder in the material is 40%-50%.
[0008] Furthermore, the mass percentage of silicon carbide nanoparticles in the reinforcement phase is 5%-15%, and the mass percentage of aluminum oxide micron particles is 10%-15%.
[0009] Furthermore, the mass percentage of nano-scale molybdenum disulfide in the lubricating phase is 5%-10%, and the mass percentage of graphite is 5%-10%.
[0010] Furthermore, the self-healing phase selects a liquid metal alloy as a self-healing agent. The metal alloy is liquid at room temperature and is composed of gallium and indium. The alloy formed by the two is liquid at room temperature, and the liquid metal alloy is encapsulated in microcapsules. When the microcapsules are ruptured, due to its fluidity and metallic properties, the liquid metal alloy can quickly flow to the wear area and achieve self-healing by forming a metallic bond with the surrounding materials. In the copper-based powder metallurgy composite friction material, the mass percentage of the liquid metal alloy as a self-healing agent is 5%-10%.
[0011] Furthermore, the self-repairing phase selects a high molecular polymer as a self-repairing agent formed by polymerization reaction using different monomer molecules. The high molecular polymer material consists of a polyurethane main chain, a disulfide bond side chain containing a reversible chemical bond and a catalyst. When the high molecular polymer containing a reversible chemical bond is damaged, the microcapsule ruptures and releases the internal polymer to cause the reversible chemical bond to break and reorganize, flow to the damaged area, and react with the surrounding materials to form a new polymer to fill the damaged area to achieve self-repair. In the copper-based powder metallurgy composite friction material, the mass percentage of the high molecular polymer as a self-repairing agent is 5%-10%.
[0012] On the other hand, a method for preparing a copper-based powder metallurgy composite friction material is provided, wherein the specific steps of the preparation method are as follows: S1. Preparation of nanocrystalline copper powder: S1.1, ball milling: put the copper raw material into a ball mill, add grinding media, and perform ball milling at a certain speed and time to refine the copper particles to nanometer level; S1.2, Annealing stabilization: Annealing the copper powder after ball milling to eliminate the stress generated during the ball milling process, while making the crystal structure of the nanocrystalline copper powder more stable and further refining the grains; S2. Preparation of reinforcement phase particles: S2.1, powder mixing: uniformly mix silicon carbide nanometer powder and aluminum oxide micrometer powder according to mass percentage; S2.2, Chemical Vapor Deposition: The mixed powder is placed in a specific reaction furnace, and the reaction gas is introduced. Under certain temperature and pressure conditions, the reaction gas undergoes a chemical reaction on the surface of the copper powder to generate silicon carbide nanoparticles and aluminum oxide microparticles, which are evenly deposited on the surface of the copper powder; S3. Preparation of mixed powder: S3.1. Accurate weighing: accurately weigh according to the proportion of 40%-50% by mass of nanocrystalline copper powder, 10%-15% by mass of silicon carbide nanoparticles, 5%-15% by mass of aluminum oxide microparticles, 5%-10% by mass of microencapsulated self-healing agent, 5%-10% by mass of nano-scale molybdenum disulfide, and 5%-10% by mass of graphite; S3.2, fully mix: mix the weighed components for 1 hour to ensure that the components are fully dispersed and evenly distributed; S4, cold pressing: S4.1, mold pressing: the mixed powder is loaded into a mold and pressed at a pressure of 600 MPa; S4.2, Process control: During the cold pressing process, control the pressure and loading speed to make the density of the blank uniform; S5. Sintering: S5.1, atmosphere protection: the cold pressed green body is placed in a tube furnace and sintered under the protection of inert gas; S5.2, Temperature and time control: During the sintering process, the atmosphere, temperature and time are controlled to allow the various components in the material to fully diffuse and combine to form a dense copper-based composite material; S6. Surface treatment: S6.1, Laser cladding: Laser cladding is used to form a protective film on the material surface. The laser beam is focused on the material surface to melt the material surface locally. At the same time, the cladding material is sprayed into the melting area to form a metallurgical bond with the base material. S6.2. Activate the self-repairing phase: The laser power is set to 1000 W and the scanning speed is 10 mm / s. The self-repairing phase is activated through surface treatment so that it can function in time when worn.
[0013] Furthermore, in the preparation process of the S1 nanocrystalline copper powder, high-purity copper powder is placed in a ball mill, grinding media is added, and ball milling is performed under the protection of inert gas argon. The ball milling time is 24 hours and the ball milling speed is 200 rpm. After the ball milling is completed, the copper powder is annealed at a temperature of 600°C and a holding time of 2 hours to eliminate internal stress and further refine the grains.
[0014] Furthermore, the S2.2 chemical vapor deposition deposits reinforcement phase particles on the surface of the pretreated nanocrystalline copper powder. The deposition process is carried out at 600° C., the reaction time is 1 hour, and the gas flow rate is controlled at 50 sccm to make the particles evenly distributed on the surface of the copper powder.
[0015] Furthermore, the S5 sintering is performed under argon protection, heated at a heating rate of 5°C / min, heated to 1100°C and then kept warm for 2 hours to form a dense copper-based composite material.
[0016] Compared with the known public technology, the technical solution provided by the present invention has the following beneficial effects: 1. The present invention introduces microencapsulated self-healing agents, namely liquid metal alloys and high molecular polymers. When the surface of the material is worn, the microcapsules rupture and release the self-healing agents to fill the worn areas, thereby realizing the self-healing function of the material. This self-healing ability can effectively extend the service life of the material and reduce the maintenance frequency and cost of the equipment. At the same time, the lubricating phase composed of nano-scale molybdenum disulfide and graphite reduces the friction coefficient, reduces the occurrence of wear, and further cooperates with the self-healing phase to extend the service life of the material.
[0017] 2. The present invention adopts nanocrystalline copper powder as the matrix, which has high thermal conductivity and can quickly conduct the heat generated by friction to reduce local overheating. At the same time, the nanocrystalline copper powder also has excellent plasticity and can undergo certain plastic deformation when subjected to force, thereby alleviating stress concentration. The addition of silicon carbide nanoparticles and aluminum oxide micron particles in the reinforcing phase further improves the strength and stability of the material at high temperatures. These factors work together to enable the copper-based powder metallurgy composite friction material of the present invention to maintain a stable friction coefficient at high temperatures, significantly improving the high-temperature stability of the material. DETAILED DESCRIPTION
[0018] In order to make the purpose, technical solution and advantages of the present invention clearer, the technical solution in the present invention is described clearly and completely. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0019] The present invention will be further described below in conjunction with the embodiments. Embodiment 1
[0020] This embodiment describes in detail a specific process of a method for preparing a copper-based powder metallurgy composite friction material, and displays in detail specific preparation parameters and performance test data to verify the stability and self-healing properties of the invention.
[0021] Preparation of nanocrystalline copper powder: High-purity copper powder is placed in a ball mill, grinding media is added, and ball milling is performed at a ball milling speed of 200 rpm for 24 hours under the protection of inert gas argon to refine the copper particles to the nanometer level. After ball milling, the copper powder is annealed at 600°C for 2 hours to eliminate the stress generated during the ball milling process, while making the crystal structure of the nanocrystalline copper powder more stable and further refining the grains.
[0022] Preparation of reinforcing phase particles: Silicon carbide nanoparticles and aluminum oxide micron powders are uniformly mixed, and the mixed powders are placed in a specific reactor. Reaction gas is introduced at 600°C for 1 hour. The gas flow rate is controlled at 50 sccm to allow the reaction gas to react chemically on the surface of the copper powder to generate silicon carbide nanoparticles and aluminum oxide micron particles, which are uniformly deposited on the surface of the copper powder.
[0023] Preparation of mixed powder: Accurately weigh the components according to the proportion of 45% by mass of nanocrystalline copper powder, 10% by mass of silicon carbide nanoparticles, 10% by mass of aluminum oxide microparticles, 8% by mass of microencapsulated self-healing agent, 8% by mass of nano-scale molybdenum disulfide, and 8% by mass of graphite, and mix the weighed components for 1 hour to ensure that the components are fully dispersed and evenly distributed.
[0024] Cold pressing: The mixed powder is loaded into the mold and pressed at a pressure of 600MPa. During the cold pressing process, the pressure and loading speed are controlled to ensure the density and uniformity of the blank.
[0025] Sintering: The cold-pressed green body is placed in a tubular furnace and sintered under the protection of argon. It is heated to 1100°C at a heating rate of 5°C / min and kept warm for 2 hours to allow the components in the material to fully diffuse and combine to form a dense copper-based composite material.
[0026] Surface treatment: Laser cladding is used to form a protective film on the material surface. The laser beam is focused on the material surface to locally melt the material surface. At the same time, the cladding material is sprayed into the melting area to form a metallurgical bond with the base material. The laser power is set to 1000W and the scanning speed is 10mm / s. The self-repairing phase is activated through surface treatment so that it can play a role in time when worn.
[0027] Performance test: The test results of the materials obtained in this example are shown in the attached table 1. Embodiment 2
[0028] Preparation of nanocrystalline copper powder: High-purity copper powder is placed in a ball mill, grinding media is added, and ball milling is performed at a ball milling speed of 250 rpm for 24 hours under the protection of inert gas argon to refine the copper particles to the nanometer level. After ball milling, the copper powder is annealed at 600°C for 2 hours to eliminate the stress generated during the ball milling process, while making the crystal structure of the nanocrystalline copper powder more stable and further refining the grains.
[0029] Preparation of reinforcing phase particles: Silicon carbide nanoparticles and aluminum oxide micron powders are uniformly mixed, and the mixed powders are placed in a specific reactor. Reaction gas is introduced at 600°C for 1 hour. The gas flow rate is controlled at 50 sccm to allow the reaction gas to react chemically on the surface of the copper powder to generate silicon carbide nanoparticles and aluminum oxide micron particles, which are uniformly deposited on the surface of the copper powder.
[0030] Preparation of mixed powder: Accurately weigh the components according to the proportion of 50% by mass of nanocrystalline copper powder, 15% by mass of silicon carbide nanoparticles, 15% by mass of aluminum oxide microparticles, 7% by mass of microencapsulated self-healing agent, 7% by mass of nano-scale molybdenum disulfide, and 7% by mass of graphite, and mix the weighed components for 1 hour to ensure that the components are fully dispersed and evenly distributed.
[0031] Cold pressing: The mixed powder is loaded into the mold and pressed at a pressure of 650MPa. During the cold pressing process, the pressure and loading speed are controlled to ensure the density and uniformity of the blank.
[0032] Sintering: The cold-pressed green body is placed in a tubular furnace and sintered under the protection of argon. It is heated to 1150°C at a heating rate of 5°C / min and kept warm for 2.5 hours to allow the components in the material to fully diffuse and combine to form a dense copper-based composite material.
[0033] Surface treatment: Laser cladding is used to form a protective film on the material surface. The laser beam is focused on the material surface to locally melt the material surface. At the same time, the cladding material is sprayed into the melting area to form a metallurgical bond with the base material. The laser power is set to 1200W and the scanning speed is 12mm / s. The self-repairing phase is activated through surface treatment so that it can play a role in time when worn.
[0034] Performance test: The test results of the materials obtained in this example are shown in the attached table 1. Embodiment 3
[0035] Preparation of nanocrystalline copper powder: High-purity copper powder is placed in a ball mill, grinding media is added, and ball milling is performed at a ball milling speed of 180 rpm for 18 hours under the protection of inert gas argon to refine the copper particles to the nanometer level. After ball milling, the copper powder is annealed at 550°C for 1.5 hours to eliminate the stress generated during the ball milling process, while making the crystal structure of the nanocrystalline copper powder more stable and further refining the grains.
[0036] Preparation of reinforcing phase particles: Silicon carbide nanoparticles and aluminum oxide micron powders are uniformly mixed, and the mixed powders are placed in a specific reactor. Reaction gas is introduced at 600°C for 1 hour. The gas flow rate is controlled at 50 sccm to allow the reaction gas to react chemically on the surface of the copper powder to generate silicon carbide nanoparticles and aluminum oxide micron particles, which are uniformly deposited on the surface of the copper powder.
[0037] Preparation of mixed powder: accurately weigh the components according to the proportion of 40% by mass of nanocrystalline copper powder, 12% by mass of silicon carbide nanoparticles, 12% by mass of aluminum oxide microparticles, 9% by mass of microencapsulated self-healing agent, 9% by mass of nano-scale molybdenum disulfide, and 9% by mass of graphite, and mix the weighed components for 1 hour to ensure that the components are fully dispersed and evenly distributed.
[0038] Cold pressing: The mixed powder is loaded into the mold and pressed at a pressure of 550MPa. During the cold pressing process, the pressure and loading speed are controlled to ensure the density and uniformity of the blank.
[0039] Sintering: The cold-pressed green body is placed in a tubular furnace and sintered under the protection of argon. It is heated to 1050°C at a heating rate of 5°C / min and kept warm for 1.5 hours to allow the components in the material to fully diffuse and combine to form a dense copper-based composite material.
[0040] Surface treatment: Laser cladding is used to form a protective film on the material surface. The laser beam is focused on the material surface to locally melt the material surface. At the same time, the cladding material is sprayed into the melting area to form a metallurgical bond with the base material. The laser power is set to 800W and the scanning speed is 8mm / s. The self-repairing phase is activated through surface treatment so that it can play a role in time when worn.
[0041] Performance test: The test results of the materials obtained in this example are shown in the attached table 1. Embodiment 4
[0042] Preparation of nanocrystalline copper powder: High-purity copper powder is placed in a ball mill, grinding media is added, and ball milling is performed at a ball milling speed of 220 rpm for 20 hours under the protection of inert gas argon to refine the copper particles to the nanometer level. After ball milling, the copper powder is annealed at 600°C for 2 hours to eliminate the stress generated during the ball milling process, while making the crystal structure of the nanocrystalline copper powder more stable and further refining the grains.
[0043] Preparation of reinforcing phase particles: Silicon carbide nanoparticles and aluminum oxide micron powders are uniformly mixed, and the mixed powders are placed in a specific reactor. Reaction gas is introduced at 580°C for 2 hours. The gas flow rate is controlled at 50 sccm to allow the reaction gas to react chemically on the surface of the copper powder to generate silicon carbide nanoparticles and aluminum oxide micron particles, which are uniformly deposited on the surface of the copper powder.
[0044] Preparation of mixed powder: accurately weigh the components according to the proportion of 48% by mass of nanocrystalline copper powder, 14% by mass of silicon carbide nanoparticles, 14% by mass of aluminum oxide microparticles, 6% by mass of microencapsulated self-healing agent, 6% by mass of nano-scale molybdenum disulfide, and 6% by mass of graphite, and mix the weighed components for 1 hour to ensure that the components are fully dispersed and evenly distributed.
[0045] Cold pressing: The mixed powder is loaded into the mold and pressed at a pressure of 580MPa. During the cold pressing process, the pressure and loading speed are controlled to ensure the density and uniformity of the blank.
[0046] Sintering: The cold-pressed green body is placed in a tubular furnace and sintered under the protection of argon. It is heated to 1080°C at a heating rate of 5°C / min and kept warm for 2 hours to allow the components in the material to fully diffuse and combine to form a dense copper-based composite material.
[0047] Surface treatment: Laser cladding is used to form a protective film on the material surface. The laser beam is focused on the material surface to locally melt the material surface. At the same time, the cladding material is sprayed into the melting area to form a metallurgical bond with the base material. The laser power is set to 1000W and the scanning speed is 10mm / s. The self-repairing phase is activated through surface treatment so that it can play a role in time when worn.
[0048] Performance test: The test results of the materials obtained in this example are shown in the attached table 1. Embodiment 5
[0049] Preparation of nanocrystalline copper powder: High-purity copper powder is placed in a ball mill, grinding media is added, and ball milling is performed at a ball milling speed of 210 rpm for 22 hours under the protection of inert gas argon to refine the copper particles to the nanometer level. After ball milling, the copper powder is annealed at 620°C for 2.2 hours to eliminate the stress generated during the ball milling process, while making the crystal structure of the nanocrystalline copper powder more stable and further refining the grains.
[0050] Preparation of reinforcing phase particles: Silicon carbide nanoparticles and aluminum oxide micron powders are uniformly mixed, and the mixed powders are placed in a specific reactor. Reaction gas is introduced at 600°C for 1 hour. The gas flow rate is controlled at 50 sccm to allow the reaction gas to react chemically on the surface of the copper powder to generate silicon carbide nanoparticles and aluminum oxide micron particles, which are uniformly deposited on the surface of the copper powder.
[0051] Preparation of mixed powder: Accurately weigh the components according to the proportion of 40% by mass of nanocrystalline copper powder, 10% by mass of silicon carbide nanoparticles, 10% by mass of aluminum oxide microparticles, 5% by mass of microencapsulated self-healing agent, 10% by mass of nano-scale molybdenum disulfide, and 10% by mass of graphite, and mix the weighed components for 1 hour to ensure that the components are fully dispersed and evenly distributed.
[0052] Cold pressing: The mixed powder is loaded into the mold and pressed at a pressure of 620MPa. During the cold pressing process, the pressure and loading speed are controlled to ensure the density and uniformity of the blank.
[0053] Sintering: The cold-pressed green body is placed in a tubular furnace and sintered under the protection of argon. It is heated to 1120°C at a heating rate of 5°C / min and kept warm for 2.2 hours to allow the components in the material to fully diffuse and combine to form a dense copper-based composite material.
[0054] Surface treatment: Laser cladding is used to form a protective film on the material surface. The laser beam is focused on the material surface to locally melt the material surface. At the same time, the cladding material is sprayed into the melting area to form a metallurgical bond with the base material. The laser power is set to 1100W and the scanning speed is 11mm / s. The self-repairing phase is activated through surface treatment so that it can play a role in time when worn.
[0055] Performance test: The test results of the materials obtained in this example are shown in the attached table 1.
[0056] Comparative Example:
[0057] The preparation of nanocrystalline copper powder is the same as in Example 1; Nanocrystalline copper powder is directly mixed, pressed and sintered with a lubricating phase (nano-grade molybdenum disulfide 5%, graphite 5%) without adding a reinforcing phase or a self-healing phase.
[0058] Performance test: The test results of the materials obtained in this comparative example are shown in the attached table 1.
[0059] Performance test description: Friction coefficient (×10^-7cm³ / J): The friction coefficient of the material under a specific load and speed is measured by simulating the friction test under actual working conditions; Wear rate (MPa): The wear rate is calculated by measuring the mass loss of the material during the friction process; Compressive strength (MPa): The maximum bearing capacity of the material when compressed to failure is measured by a standard pressure test method; Thermal conductivity (W / mK): The thermal conductivity of the material is measured using the laser flash method to evaluate its thermal management capabilities; Self-healing effect evaluation: The self-healing effect of the material is evaluated through a repair test after simulating wear, which is divided into four levels: "none", "good", "excellent" and "excellent".
[0060] Table 1, Performance test results of copper-based powder metallurgy composite friction materials: Example Embodiment 1 Embodiment 2 Embodiment 3 Embodiment 4 Embodiment 5 Comparative Example Friction coefficient 0.27 0.26 0.28 0.25 0.24 0.32 Wear rate 0.85 0.78 0.90 0.75 0.70 1.20 Compressive strength 650 680 620 700 720 400 Thermal conductivity 180 190 175 195 200 120 Self-repair effect evaluation good excellent good excellent Excellent none
[0061] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. Such modifications or replacements will not cause the essence of the corresponding technical solutions to deviate from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A copper-based powder metallurgy composite friction material, characterized in that: The material components of the friction material specifically include a copper matrix, a reinforcement phase, a self-repairing phase and a lubricating phase; The copper matrix uses nanocrystalline copper powder as the matrix material; The reinforcement phase includes silicon carbide nanoparticles and aluminum oxide microparticles; The self-healing phase contains a microencapsulated self-healing agent, namely a liquid metal alloy and a high molecular polymer; The lubricating phase includes nano-scale molybdenum disulfide and graphite, which are uniformly dispersed in the copper matrix.
2. The copper-based powder metallurgy composite friction material according to claim 1, characterized in that: The copper matrix adopts nanocrystalline copper powder, which can quickly conduct heat during friction and reduce local overheating. At the same time, it can undergo certain plastic deformation when subjected to force to relieve stress concentration. The mass percentage of nanocrystalline copper powder in the material is 40%-50%.
3. The copper-based powder metallurgy composite friction material according to claim 1, characterized in that: The mass percentage of silicon carbide nanoparticles in the reinforcement phase is 5%-15%, and the mass percentage of aluminum oxide micron particles is 10%-15%.
4. The copper-based powder metallurgy composite friction material according to claim 1, characterized in that: The mass percentage of nano-scale molybdenum disulfide in the lubricating phase is 5%-10%, and the mass percentage of graphite is 5%-10%.
5. The copper-based powder metallurgy composite friction material according to claim 4, characterized in that: The self-healing phase selects a liquid metal alloy as a self-healing agent, which is a metal alloy that is liquid at room temperature and is composed of gallium and indium. The alloy formed by the two is liquid at room temperature, and the liquid metal alloy is encapsulated in a microcapsule. When the microcapsule is broken, due to its fluidity and metallic properties, the liquid metal alloy can quickly flow to the wear area and achieve self-healing by forming a metal-to-metal bond with the surrounding materials. In the copper-based powder metallurgy composite friction material, the mass percentage of the liquid metal alloy as a self-healing agent is 5%-10%.
6. The copper-based powder metallurgy composite friction material according to claim 4, characterized in that: The self-repairing phase selects a high molecular polymer as a self-repairing agent and is formed by polymerization reaction using different monomer molecules. The high molecular polymer material consists of a polyurethane main chain, a disulfide bond side chain containing a reversible chemical bond and a catalyst. When the high molecular polymer containing a reversible chemical bond is damaged, the microcapsule ruptures and releases the internal polymer to cause the reversible chemical bond to break and recombine, flow to the damaged area, and undergo polymerization reaction by combining with the surrounding materials to form a new polymer, which fills the damaged area to achieve self-repair. In the copper-based powder metallurgy composite friction material, the mass percentage of the high molecular polymer as a self-repairing agent is 5%-10%.
7. A method for preparing a copper-based powder metallurgy composite friction material, characterized in that: The specific steps of the preparation method are: S1. Preparation of nanocrystalline copper powder: S1.1, ball milling: put the copper raw material into a ball mill, add grinding media, and perform ball milling at a certain speed and time to refine the copper particles to nanometer level; S1.2, Annealing stabilization: Annealing the copper powder after ball milling to eliminate the stress generated during the ball milling process, while making the crystal structure of the nanocrystalline copper powder more stable and further refining the grains; S2. Preparation of reinforcement phase particles: S2.1, powder mixing: uniformly mix silicon carbide nanometer powder and aluminum oxide micrometer powder according to mass percentage; S2.2, Chemical Vapor Deposition: The mixed powder is placed in a specific reaction furnace, and the reaction gas is introduced. Under certain temperature and pressure conditions, the reaction gas undergoes a chemical reaction on the surface of the copper powder to generate silicon carbide nanoparticles and aluminum oxide microparticles, which are evenly deposited on the surface of the copper powder; S3. Preparation of mixed powder: S3.
1. Accurate weighing: accurately weigh according to the proportion of 40%-50% by mass of nanocrystalline copper powder, 10%-15% by mass of silicon carbide nanoparticles, 5%-15% by mass of aluminum oxide microparticles, 5%-10% by mass of microencapsulated self-healing agent, 5%-10% by mass of nano-scale molybdenum disulfide, and 5%-10% by mass of graphite; S3.2, fully mix: mix the weighed components for 1 hour to ensure that the components are fully dispersed and evenly distributed; S4, cold pressing: S4.1, mold pressing: the mixed powder is loaded into a mold and pressed at a pressure of 600 MPa; S4.2, Process control: During the cold pressing process, control the pressure and loading speed to make the density of the blank uniform; S5. Sintering: S5.1, atmosphere protection: the cold pressed green body is placed in a tube furnace and sintered under the protection of inert gas; S5.2, Temperature and time control: During the sintering process, the atmosphere, temperature and time are controlled to allow the various components in the material to fully diffuse and combine to form a dense copper-based composite material; S6. Surface treatment: S6.1, Laser cladding: Laser cladding is used to form a protective film on the material surface. The laser beam is focused on the material surface to melt the material surface locally. At the same time, the cladding material is sprayed into the melting area to form a metallurgical bond with the base material. S6.
2. Activate the self-repairing phase: The laser power is set to 1000 W and the scanning speed is 10 mm / s. The self-repairing phase is activated through surface treatment so that it can function in time when worn.
8. The method for preparing a copper-based powder metallurgy composite friction material according to claim 7, characterized in that: In the preparation process of the S1 nanocrystalline copper powder, high-purity copper powder is placed in a ball mill, grinding media is added, and ball milling is performed under the protection of inert gas argon. The ball milling time is 24 hours and the ball milling speed is 200 rpm. After the ball milling is completed, the copper powder is annealed at 600°C for 2 hours to eliminate internal stress and further refine the grains.
9. The method for preparing a copper-based powder metallurgy composite friction material according to claim 7, characterized in that: The S2.2 chemical vapor deposition deposits reinforcement phase particles on the surface of the pretreated nanocrystalline copper powder. The deposition process is carried out at 600° C., the reaction time is 1 hour, and the gas flow rate is controlled at 50 sccm to ensure that the particles are evenly distributed on the surface of the copper powder.
10. The method for preparing a copper-based powder metallurgy composite friction material according to claim 7, characterized in that: The S5 sintering is performed under argon protection, with heating at a heating rate of 5° C. / min, and then heated to 1100° C. and kept warm for 2 hours to form a dense copper-based composite material.
Citation Information
Cited By
Powder metallurgy friction material and preparation method thereof
CN120095140A
Powder metallurgical friction material and method for its production
CN120095140B
Nano-alloy composite material for self-repairing surface of metal friction pair and preparation method and application of nano-alloy composite material