High-energy-density fast-charging graphite composite material and preparation method thereof

The combination of fibrous lithium-doped porous carbon and metal oxide coated graphite material was prepared by electrospinning, which solved the problems of low specific capacity of graphite materials and low first-time efficiency of metal oxides, and achieved the improvement of high energy density fast charging performance .

CN118993057APending Publication Date: 2024-11-22SICHUAN KUNTIAN NEW ENERGY TECH CO LTD
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411202218.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-29
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

In the prior art, the low specific capacity of graphite materials, low first-time efficiency of metal oxides and high expansion limits its application in lithium-ion battery negative electrode materials.

Method used

Fibrous lithium-doped porous carbon is prepared by electrospinning a carbon source, organic lithium salt and pore-forming agent, and mixed with metal oxide and carboxymethyl cellulose lithium, and dried and reduced sintered to form a lithium/metal composite The body is coated with graphite composite material, which improves the conductivity and specific capacity of electrons and reduces the expansion of metal.

Benefits of technology

It significantly improves the first efficiency and specific capacity of graphite composite materials, reduces expansion during charging and discharging, and improves fast charging performance and cycle stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118993057A_ABST
    Figure CN118993057A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of lithium ion battery materials, and provides a high-energy-density fast-charging graphite composite material and a preparation method thereof.The preparation method comprises the following steps that S1, a carbon source, organic lithium salt and a pore forming agent are evenly mixed, and after electrostatic spinning is conducted, sintering is conducted to obtain fibrous lithium-doped porous carbon; s2, uniformly mixing lithium carboxymethyl cellulose with the solution to obtain a lithium carboxymethyl cellulose solution; and S3, uniformly mixing the lithium carboxymethyl cellulose solution, the fibrous lithium-doped porous carbon, a metal compound and graphite, drying, reducing and sintering to obtain the lithium / metal complex coated graphite composite material. Through the technical scheme, the problems of low specific capacity of the graphite material and low first efficiency and high expansion of the metal oxide of the graphite material in related technologies are solved, and the quick charging performance of the material is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of lithium ion battery materials, and in particular to a high energy density fast-charging graphite composite material and a preparation method thereof. Background Art

[0002] The current fast-charging negative electrode materials on the market mainly improve the fast-charging performance of the materials by coating soft carbon or hard carbon on the outer layer. However, since soft carbon or hard carbon itself has defects such as low initial efficiency and low specific capacity, coating on the graphite surface will reduce the initial efficiency and specific capacity. Although metal oxide materials (iron oxide, tin oxide and its metal elements, etc.) have high specific capacity and high power performance, they have the problems of large expansion when fully charged and low initial efficiency, so they cannot be used directly as negative electrode materials and need to be mixed or compounded with other substances. For example, patent application No. CN202310994541.X discloses a high first efficiency and high capacity hard carbon negative electrode material modified with a transition metal oxide. The hard carbon negative electrode material is pre-carbonized with epoxy resin, phenolic resin or a phenolic resin derivative to obtain a hard carbon precursor, and then a transition metal salt is coated on the surface of the hard carbon precursor by a hydrothermal reaction, and then the hard carbon negative electrode material is obtained by heat treatment; the first discharge efficiency, first discharge capacity and cycle stability of the hard carbon negative electrode material are low and need to be improved. Therefore, it is urgent to develop a graphite composite material with high specific capacity, high first efficiency and low full charge expansion. Summary of the invention

[0003] The present invention provides a high-energy-density fast-charging graphite composite material and a preparation method thereof, which solves the problems of low specific capacity of graphite materials and low initial efficiency and high expansion of their metal oxides in related technologies.

[0004] The technical solution of the present invention is as follows: The present invention provides a method for preparing a high energy density fast-charging graphite composite material, comprising the following steps: S1, mixing a carbon source, an organic lithium salt and a pore-forming agent uniformly, performing electrospinning, and then sintering to obtain fibrous lithium-doped porous carbon; S2, mixing the lithium carboxymethyl cellulose and the solution evenly to obtain a lithium carboxymethyl cellulose solution; S3, after uniformly mixing the lithium carboxymethyl cellulose solution, fibrous lithium-doped porous carbon, metal compound and graphite, drying and reduction sintering are performed to obtain a lithium / metal composite-coated graphite composite material.

[0005] As a further technical solution, the mass ratio of the carbon source, the organic lithium salt and the pore-forming agent in S1 is 100:5~10:5~15.

[0006] As a further technical solution, the voltage of the electrospinning in S1 is 10-30 KV, the rotation speed is 500-1000 rpm, the flow rate is 1-100 μL / min, and the time is 30-300 min.

[0007] As a further technical solution, the sintering temperature in S1 is 800-1200° C., and the sintering time is 1-6 hours.

[0008] As a further technical solution, in S1, the carbon source, the organic lithium salt and the pore-forming agent are uniformly mixed, electrospun, sintered, and activated by introducing water vapor to obtain fibrous lithium-doped porous carbon.

[0009] As a further technical solution, the activation temperature in S1 is 900-1000° C., and the activation time is 1-3 hours.

[0010] As a further technical solution, the carbon source in S1 includes one or more of phenolic resin, furfural resin, epoxy resin, glucose, sucrose, and maltose.

[0011] As a further technical solution, the organic lithium salt includes one or more of lithium acetate, lithium acetate, lithium pyruvate, and lithium stearate.

[0012] As a further technical solution, the pore-forming agent includes one or more of N-methyldiethanolamine, N-phenyldiethanolamine, N-ethyldiethanolamine, dimethylethanolamine, and diisopropanolamine.

[0013] As a further technical solution, the solution in S2 is deionized water.

[0014] As a further technical solution, the mass concentration of the lithium carboxymethyl cellulose solution in S2 is 0.5wt%~2wt%.

[0015] As a further technical solution, the metal oxide includes one or more of titanium oxide, zinc oxide, nickel oxide, niobium oxide, and tin oxide.

[0016] As a further technical solution, the graphite is artificial graphite.

[0017] As a further technical solution, the mass ratio of lithium carboxymethyl cellulose, fibrous lithium-doped porous carbon, metal compound and graphite in S3 is 0.5~2:1~5:1~3:100.

[0018] As a further technical solution, the temperature of the reduction sintering in S3 is 900-1200° C., and the time of the reduction sintering is 1-6 hours.

[0019] As a further technical solution, in S3, the carboxymethyl cellulose lithium solution, fibrous lithium-doped porous carbon, metal compound and graphite are uniformly mixed, dried, and then introduced with reducing gas for reduction sintering to obtain a lithium / metal composite-coated graphite composite material.

[0020] In the present invention, lithium carboxymethyl cellulose is carbonized to generate granular lithium-doped amorphous carbon, which is mixed with fibrous lithium-doped porous carbon to further improve the electronic conductivity during charging and discharging and reduce the expansion of the metal.

[0021] As a further technical solution, the drying is spray drying.

[0022] As a further technical solution, the reducing gas consists of hydrogen and argon.

[0023] As a further technical solution, the volume ratio of hydrogen to argon is 1-5:10.

[0024] In the present invention, the metal oxide is reduced by hydrogen to generate a metal element, thereby improving the electronic conductivity and specific capacity of the graphite composite material.

[0025] As a further technical solution, the flow rate of the reducing gas is 100 mL / min.

[0026] The present invention also provides a method for preparing a high-energy-density fast-charging graphite composite material to prepare the high-energy-density fast-charging graphite composite material.

[0027] The present invention also proposes an application of a high energy density fast-charging graphite composite material in an ion battery.

[0028] The working principle and beneficial effects of the present invention are: In the present invention, fibrous lithium-doped porous carbon prepared by electrostatic spinning from a carbon source, an organic lithium salt and a pore-forming agent is added to a graphite composite material, and a synergistic effect is produced after mixing with a metal, thereby reducing the expansion of the metal and improving the initial efficiency of the graphite composite material; utilizing the bonding performance of lithium carboxymethyl cellulose, the metal and the fibrous lithium-doped porous carbon can be uniformly coated on the surface of the artificial graphite, thereby improving the electronic conductivity during the charging and discharging process, reducing the expansion of the metal, solving the problems of low specific capacity of the graphite material, low initial efficiency and high expansion of its metal oxides, and improving the fast charging performance of the composite material. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] The present invention will be further described in detail below in conjunction with the accompanying drawings and specific embodiments.

[0030] Figure 1 The constant current ratio comparison diagram of the soft-pack batteries prepared in Examples 1-3 and Comparative Examples 1-2 is shown. DETAILED DESCRIPTION

[0031] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0032] In the following examples and comparative examples: Phenolic resin, model: CQCN700, purchased from Shandong Shengquan Chemical Co., Ltd.; Furfural resin, CAS98-01-1, was purchased from Shandong Guohua Chemical Co., Ltd.; Epoxy resin, model: SQME 2403, purchased from Shandong Shengquan Chemical Co., Ltd.; Carboxymethyl cellulose lithium, model: CMC-Li, purchased from Chongqing Lihong Fine Chemical Co., Ltd.; Artificial graphite, model: EMG-P, was purchased from Shanghai Shanshan Technology Co., Ltd.

[0033] Example 1 A method for preparing a high energy density fast-charging graphite composite material comprises the following steps: S1. 100 g of phenolic resin, 8 g of lithium acetate and 10 g of N-methyldiethanolamine were mixed evenly, and electrospun (the voltage of the electrospinning equipment was 20 KV, the rotation speed was 800 rpm, the flow rate was 50 μL / min, and the time was 150 min), and then sintered at a temperature of 950 ° C for 3 h, and activated by passing water vapor at a temperature of 950 ° C for 2 h to obtain fibrous lithium-doped porous carbon; S2, adding 1g of lithium carboxymethyl cellulose to 99g of deionized water to prepare an aqueous solution of lithium carboxymethyl cellulose with a mass concentration of 1wt%; S3. Add 3 g of fibrous lithium-doped porous carbon to the lithium carboxymethyl cellulose aqueous solution and disperse it evenly. Then add 2 g of titanium oxide and 100 g of artificial graphite and mix them evenly. Spray dry. Heat to 1050°C and introduce a mixed gas of hydrogen and argon (the volume ratio of hydrogen to argon is 3:10, and the flow rate is 100 mL / min). Sinter for 3 hours to obtain a lithium / metal composite-coated graphite composite material.

[0034] Example 2 A method for preparing a high energy density fast-charging graphite composite material comprises the following steps: S1. 100 g furfural resin, 5 g lithium acetate and 5 g N-phenyldiethanolamine were mixed evenly, and electrospun (the voltage of the electrospinning equipment was 10 KV, the rotation speed was 500 rpm, the flow rate was 1 μL / min, and the time was 300 min), and then sintered at a temperature of 800 ° C for 6 h, and activated by passing water vapor at a temperature of 900 ° C for 3 h to obtain fibrous lithium-doped porous carbon; S2, adding 0.5g of lithium carboxymethyl cellulose to 99.5g of deionized water to prepare an aqueous solution of lithium carboxymethyl cellulose with a mass concentration of 0.5wt%; S3. Add 1g of fibrous lithium-doped porous carbon to the lithium carboxymethyl cellulose aqueous solution and disperse it evenly. Then add 1g of zinc oxide and 100g of artificial graphite and mix them evenly. Spray dry. Heat to 900°C and introduce a mixed gas of hydrogen and argon (the volume ratio of hydrogen to argon is 1:10, and the flow rate is 100mL / min). Sinter for 6h to obtain a lithium / metal composite-coated graphite composite material.

[0035] Example 3 A method for preparing a high energy density fast-charging graphite composite material comprises the following steps: S1. 100 g of epoxy resin, 10 g of lithium pyruvate and 15 g of N-ethyldiethanolamine were mixed evenly, and electrospun (the voltage of the electrospinning equipment was 30 KV, the rotation speed was 1000 rpm, the flow rate was 100 μL / min, and the time was 30 min), and then sintered at a temperature of 1200° C. for 1 h, and activated by passing water vapor at a temperature of 1000° C. for 1 h to obtain fibrous lithium-doped porous carbon; S2, adding 2 g of lithium carboxymethyl cellulose to 98 g of deionized water to prepare an aqueous solution of lithium carboxymethyl cellulose with a mass concentration of 2 wt %; S3. Add 5 g of fibrous lithium-doped porous carbon to the lithium carboxymethyl cellulose aqueous solution and disperse it evenly. Then add 3 g of nickel oxide and 100 g of artificial graphite and mix them evenly. Spray dry. Heat to 1200 ° C and pass a mixed gas of hydrogen and argon (the volume ratio of hydrogen to argon is 5:10, the flow rate is 100 mL / min) and sinter for 1 hour to obtain a lithium / metal composite coated graphite composite material.

[0036] Comparative Example 1 A method for preparing a high energy density fast-charging graphite composite material comprises the following steps: S1. 100 g of phenolic resin and 10 g of N-methyldiethanolamine were mixed evenly, spray-dried, sintered at 950° C. for 3 h, and activated by passing water vapor at 950° C. for 2 h to obtain a porous hard carbon material; S2, adding 1g of lithium carboxymethyl cellulose to 99g of deionized water to prepare an aqueous solution of lithium carboxymethyl cellulose with a mass concentration of 1wt%; S3. Add 3g of porous hard carbon material to the lithium carboxymethyl cellulose aqueous solution and disperse it evenly. Then add 2g of titanium oxide and 100g of artificial graphite and mix them evenly. Spray dry. Heat to 1050°C and pass a mixed gas of hydrogen and argon (the volume ratio of hydrogen to argon is 3:10, and the flow rate is 100mL / min). Sinter for 3h to obtain a lithium / metal composite coated graphite composite material.

[0037] Comparative Example 2 The only difference between this comparative example and Example 1 is that titanium oxide is not added in step S3.

[0038] Experimental example 1. Button battery test The lithium / metal composite-coated graphite composite materials prepared in Examples 1 to 3 and the graphite composite negative electrode materials of Comparative Examples 1 to 2 were assembled into button batteries according to the following method: Add binder, conductive agent and solvent to the negative electrode material, stir and mix to make negative electrode slurry, apply the negative electrode slurry on copper foil, dry, roll and cut to make negative electrode sheet. The binder is polyvinylidene fluoride, the conductive agent is SP conductive agent, the solvent is NMP, and the weight ratio of negative electrode material, SP conductive agent, polyvinylidene fluoride and NMP is 95:1:4:220. Use metal lithium sheet as counter electrode, polyethylene (PE) film, polypropylene (PP) film or polyethylene propylene (PEP) composite film as separator, and LiPF 6 / EC+DEC(LiPF 6 The concentration of EC was 1.3 mol / L, the volume ratio of EC and DEC was 1:1) as the electrolyte, and the battery was assembled in an argon-filled glove box.

[0039] The button cells were installed on the Wuhan Blue Electric CT2001A battery tester, and charged and discharged at a rate of 0.1C. The charge and discharge voltage range was 0.005V to 2.0V, and the first discharge capacity and first discharge efficiency were measured. The 2C rate discharge capacity was tested, and the rate performance (2C / 0.1C) and cycle performance (0.1C / 0.1C, 100 weeks) were calculated.

[0040] The specific surface area and particle size of the above negative electrode materials were tested in accordance with the national standard GB / T 24533-2019 "Graphite Negative Electrode Materials for Lithium-ion Batteries"; the powder conductivity was tested by a four-probe tester; the powder OI value was tested by XRD equipment, and the test results are shown in Table 1: Table 1 Performance test results of button batteries prepared in Examples 1 to 3 and Comparative Examples 1 to 2

[0041] As can be seen from Table 1, the discharge specific capacity, first efficiency and powder conductivity of the graphite composite negative electrode materials prepared in Examples 1 to 3 are significantly better than those in Comparative Examples 1 to 2; the reason may be that the surface of the graphite material is coated with fibrous lithium-doped porous carbon, which reduces its irreversible capacity and improves its ionic conductivity, improves the first efficiency and reduces polarization; and doped with metal oxides with high specific capacity to improve the specific capacity of the material; and the low expansion characteristics of the outer porous carbon are used to improve the cycle performance of the composite material.

[0042] 2. Soft pack battery test The negative electrode was prepared by using the graphite composite negative electrode materials prepared in Examples 1 to 3 and Comparative Examples 1 to 2, respectively, and the ternary material (LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O 2 ) as the positive electrode material to prepare the positive electrode, with LiPF 6 (The solvent is EC+DEC, the volume ratio is 1:1, and the concentration is 1.3 mol / L) as the electrolyte and celegard2400 as the separator to prepare a 2Ah soft-pack battery.

[0043] When preparing the negative electrode, a binder, a conductive agent, and a solvent are added to the negative electrode material, stirred and mixed to form a negative electrode slurry, and the negative electrode slurry is coated on a copper foil, dried, rolled, and cut to form a negative electrode sheet. The binder is LA132 binder, the conductive agent is SP conductive agent, the solvent is double distilled water, and the weight ratio of the negative electrode material, SP conductive agent, LA132 binder and double distilled water is 95:1:4:220.

[0044] When preparing the positive electrode, a binder, a conductive agent, and a solvent are added to the positive electrode material, and the mixture is stirred and mixed to form a positive electrode slurry. The positive electrode slurry is coated on an aluminum foil, dried, rolled, and cut to form a positive electrode sheet. The binder is PVDF, the conductive agent is SP, and the solvent is N-methylpyrrolidone. The weight ratio of the positive electrode material, the conductive agent, the binder, and the solvent is 93:3:4:140.

[0045] (1) Rate performance test The soft-pack battery prepared by using the graphite negative electrode material in Examples 1 to 3 and Comparative Examples 1 to 2 was subjected to rate performance test: the charge and discharge voltage range was 2.8 to 4.2 V, the test temperature was 25±3.0°C, and the battery was charged at 1.0C, 2.0C, 3.0C, and 5.0C, and discharged at 1.0C. The constant current ratio of the battery under different charging modes was tested, and the results are shown in Table 2: Table 2 Test results of rate performance of soft-pack batteries in Examples 1 to 3 and Comparative Examples 1 to 2

[0046] From Table 2 and Figure 1It can be seen that the rate charging performance of the soft-pack battery prepared by the present invention is significantly better than that of the comparative example, and the charging time is shorter, indicating that the composite negative electrode material of the present invention has good fast charging performance. The reason may be that the example material has high powder conductivity and high specific surface area, which improves the constant current ratio of the material.

[0047] (2) Cyclic performance test The soft-pack batteries made of the graphite negative electrode materials in Examples 1 to 3 and Comparative Examples 1 to 2 were subjected to the following experiment: 500 charge and discharge cycles were performed in sequence at a charge and discharge rate of 2C / 2C and a voltage range of 2.8 to 4.2V to test their capacity retention rate and initial charge DCR. The results are shown in Table 3: Table 3 Cyclic performance test of soft pack batteries prepared in Examples 1 to 3 and Comparative Examples 1 to 2

[0048] It can be seen from Table 3 that the cycle performance of the lithium ion batteries prepared with the composite negative electrode materials prepared in Examples 1 to 3 of the present invention is better than that in Comparative Examples 1 to 2. The reason is that the surface of the graphite material is coated with fibrous lithium-doped porous carbon, which increases the insertion and extraction rate of lithium ions during the charge and discharge process, reduces its irreversible capacity loss, and improves the cycle performance.

[0049] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing a high energy density fast-charging graphite composite material, characterized in that: The following steps are involved: S1, mixing a carbon source, an organic lithium salt and a pore-forming agent uniformly, performing electrospinning, and then sintering to obtain fibrous lithium-doped porous carbon; S2, mixing the lithium carboxymethyl cellulose and the solution evenly to obtain a lithium carboxymethyl cellulose solution; S3, after uniformly mixing the lithium carboxymethyl cellulose solution, fibrous lithium-doped porous carbon, metal compound and graphite, drying and reduction sintering are performed to obtain a lithium / metal composite-coated graphite composite material.

2. The method for preparing a high energy density fast-charging graphite composite material according to claim 1, characterized in that: The mass ratio of the carbon source, the organic lithium salt and the pore-forming agent in S1 is 100:5-10:5-15.

3. The method for preparing a high energy density fast-charging graphite composite material according to claim 1, characterized in that: The voltage of the electrospinning in S1 is 10-30 KV, the rotation speed is 500-1000 rpm, the flow rate is 1-100 μL / min, and the time is 30-300 min.

4. The method for preparing a high energy density fast-charging graphite composite material according to claim 1, characterized in that: The sintering temperature in S1 is 800-1200° C., and the sintering time is 1-6 hours.

5. The method for preparing a high energy density fast-charging graphite composite material according to claim 1, characterized in that: The carbon source in S1 includes one or more of phenolic resin, furfural resin, epoxy resin, glucose, sucrose, and maltose.

6. The method for preparing a high energy density fast-charging graphite composite material according to claim 1, characterized in that: The organic lithium salt includes one or more of lithium acetate, lithium acetate, lithium pyruvate, and lithium stearate.

7. The method for preparing a high energy density fast-charging graphite composite material according to claim 1, characterized in that: The mass ratio of lithium carboxymethyl cellulose, fibrous lithium-doped porous carbon, metal compound and graphite in S3 is 0.5-2:1-5:1-3:

100.

8. The method for preparing a high energy density fast-charging graphite composite material according to claim 1, characterized in that: The reduction sintering temperature in S3 is 900-1200° C., the reduction sintering time is 1-6 hours, and the reduction sintering is performed using a reducing gas in S3. The reducing gas is a mixture of hydrogen and argon in a volume ratio of 1-5:

10.

9. A high energy density fast charging graphite composite material prepared according to the preparation method of a high energy density fast charging graphite composite material according to any one of claims 1 to 8.

10. Use of the high energy density fast charging graphite composite material as claimed in claim 9 in ion batteries.

Citation Information

Cited By

  • Graphite composite material, preparation method thereof and application of graphite composite material in lithium ion battery

    CN119852375A

  • Graphite composite negative electrode active material and preparation method and application thereof

    CN119864407A