Aconitic acid mixed ester, preparation method thereof and composite material containing aconitic acid mixed ester

Through the synthesis and treatment technology of mixed aconitate mixed ester, the problem of synergistic improvement of existing aconitate in PVC is solved, and the balanced performance and wide application of PVC materials are achieved.

CN118993894APending Publication Date: 2024-11-22QINGDAO INST OF BIOENERGY & BIOPROCESS TECH CHINESE ACADEMY OF SCI

Patent Information

Application Number
CN202310575243.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-22
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

It is difficult for existing aconitate to improve plasticization and resistance in PVC at the same time, and the plasticizer itself has insufficient solvent extraction performance, which affects the toughness, stability and application range of the material.

Method used

Aconitine mixed ester, with at least two different substituents, balances the plasticization and resistance properties through synthetic methods, including esterification reaction, neutralization, bleaching and decolorization and adsorption decolorization steps to improve product purity and performance.

Benefits of technology

The balanced toughness, stability and plasticity of PVC materials are achieved, the application scope is expanded, and the extraction resistance of different solvents is improved, and the comprehensive performance of the material is enhanced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004239745910000021
    Figure BDA0004239745910000021
  • Figure BDA0004239745910000211
    Figure BDA0004239745910000211
  • Figure BDA0004239745910000221
    Figure BDA0004239745910000221
Patent Text Reader

Abstract

The invention discloses an aconitic acid mixed ester, a preparation method thereof and a composite material containing the aconitic acid mixed ester, and belongs to the technical field of preparation and application of the aconitic acid mixed ester. Three substituent groups R1, R2 and R3 of the aconitic acid mixed ester are respectively and independently selected from one of an alkyl group containing 1-5 carbon atoms, an alkyl group containing more than 6 carbon atoms, an alkyl group containing 2-5 carbon atoms and substituted by chlorine atoms and an alkyl group containing aryl, and at least two of R1, R2 and R3 are different. Three substituent groups in the aconitic acid mixed ester are at least two different, the aconitic acid mixed ester is used as a plasticizer to be added into PVC, the plasticizing performance and the tolerance performance of a product are effectively balanced, the aconitic acid mixed ester has comprehensive solvent extraction resistance, and the material has balanced toughness, stability and plasticity, so that the quality of the PVC product is improved, and the application range of the PVC product is expanded.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to an aconitic acid mixed ester and a preparation method thereof and a composite material containing the aconitic acid mixed ester, belonging to the technical field of aconitic acid mixed ester preparation and application. Background Art

[0002] Aconitate is a compound obtained by the reaction of aconitic acid and alcohols. Aconitate is used as a plasticizer in PVC products to play a plasticizing role, thereby improving the relevant properties of PVC products, such as mechanical strength, toughness, low temperature resistance and heat resistance.

[0003] However, the inventors have found that when aconitic acid single ester (i.e., the three substituents on aconitic acid are the same), when it is added to PVC products, it is often difficult to simultaneously improve the above-mentioned properties, and the tolerance of the plasticizer itself in PVC (such as volatility resistance, migration resistance, and solvent extraction resistance) is also difficult to cooperate with the plasticizing performance. For example, aconitic acid single ester containing short-chain substituents has good compatibility with PVC plastics, so the toughness and plasticity of the material are significantly improved, and the higher polarity makes it more resistant to extraction of organic solvents, but the smaller molecular weight will lead to poor thermal stability of the material and easier extraction in aqueous solution, and it is difficult to play a role for a long time; aconitic acid single ester containing long-chain substituents has a higher molecular weight so that it has good thermal stability and water resistance, but its compatibility with PVC deteriorates, and the toughness and plasticity of the material deteriorate accordingly, and the low polarity causes the material to be more easily precipitated by organic solvents.

[0004] At present, the principle of using aconitate esters to plasticize PVC in the prior art is still unclear, and the single aconitate ester used is only used to improve the plasticizing properties of PVC in a certain aspect. There is a lack of aconitate ester that can not only improve the various plasticizing properties of PVC, but also take into account the tolerance of aconitate ester itself in PVC. Summary of the invention

[0005] In order to solve the above problems, a mixed ester of aconitic acid is provided, in which at least two of the three substituents are different. When the mixed ester of aconitic acid is added to PVC as a plasticizer, the plasticizing performance and tolerance performance of the product are effectively balanced, and the mixed ester has comprehensive solvent extraction resistance, so that the material has balanced toughness, stability and plasticity, thereby improving the quality of PVC products and expanding their application range.

[0006] According to one aspect of the present application, a mixed ester of aconitic acid is provided, and the structural formula of the mixed ester of aconitic acid is as follows:

[0007]

[0008] Wherein, R1, R2, and R3 are independently selected from an alkyl group containing 1 to 5 carbon atoms, an alkyl group containing 6 or more carbon atoms, an alkyl group containing 2 to 5 carbon atoms and substituted by chlorine atoms, or an alkyl group containing an aromatic group, and at least two of R1, R2, and R3 are different.

[0009] The above-mentioned aconitic acid mixed ester is a mixture of aconitic acid complex esters, and at least two of R1, R2, and R3 of the aconitic acid complex esters are different, which can make a single aconitic acid ester carry different substituents, thereby coordinating the tolerance of the aconitic acid ester itself and the plasticizing performance of PVC, thereby improving the quality of PVC products and expanding the application range of PVC products.

[0010] Optionally, at least one of R1, R2, and R3 is selected from an alkyl group having 1 to 5 carbon atoms, and at least one is selected from an alkyl group having 6 or more carbon atoms.

[0011] Since the shorter the alkyl chain of the substituent in the aconitate, the greater the proportion of polar ester groups, the better the compatibility with PVC, the longer the alkyl chain, the better the flexibility, the better the lubricity between PVC molecular chains, and theoretically the better the plasticizing effect. However, the present application found that if the alkyl chain is blindly short, the plasticizer can only be embedded in the PVC molecular chain but cannot shield the strong interaction between the PVC molecular chains (poor shielding effect), so the plasticizing effect may not be good, and if the substituted alkyl chain is blindly long, the proportion of polar ester groups is getting smaller and smaller, and the compatibility with PVC is poor. Even if it has a large steric hindrance to shield the interaction with PVC, it cannot be embedded in the PVC molecular chain due to poor compatibility (poor solvent effect), and it is difficult to dissolve the "connection point" between the PVC molecular chains, and the plasticizing effect will also decrease. The aconitic acid mixed ester contains a short-chain alkyl group with 1 to 5 carbon atoms, which increases the polarity of the aconitic acid mixed ester and improves its organic solvent extraction resistance in PVC plastics, and has good compatibility with PVC. It also contains a long-chain alkyl group with more than 6 carbon atoms, which can improve its volatility resistance, migration resistance and water solvent extraction resistance in PVC. The short-chain alkyl group and the long-chain alkyl group work together to obtain an aconitic acid mixed ester that can improve various plasticizing properties of PVC and take into account the tolerance of the aconitic acid ester itself in PVC, and can also improve its extraction resistance in different solvents.

[0012] Optionally, at least one of R1, R2, and R3 is selected from butyl, and at least one is selected from isooctyl;

[0013] Preferably, two of R1, R2 and R3 are selected from butyl and one is selected from isooctyl, or two of R1, R2 and R3 are selected from isooctyl and one is selected from butyl.

[0014] Butyl itself has a certain steric hindrance that can effectively shield the interaction between PVC molecular chains. When it is in the aconitate structure, because of the small number of alkyl groups, the polarity of aconitate is large, and good compatibility with PVC is obtained. Butyl has a stronger shielding effect than shorter alkyl groups and a better compatibility effect than longer alkyl groups. Therefore, butyl aconitate has the best plasticizing effect. However, in addition to the plasticizing effect, the material also needs better stability. Isooctyl (2-ethylhexyl) itself has a larger molecular chain, good thermal stability, and has a branched chain, which is more difficult to migrate to the outside world. Therefore, the combination of butyl and isooctyl can make the aconitate material have both plasticizing and stabilizing properties, and by adjusting the ratio of butyl and isooctyl, the focus of the aconitate plasticizer can be further adjusted, such as more efficient plasticization or longer-lasting stability.

[0015] Optionally, at least one of R1, R2 and R3 is selected from an alkyl group containing 1 to 3 carbon atoms, and at least one is selected from an alkyl group containing an aromatic group.

[0016] When at least one of R1, R2, and R3 is selected from an alkyl group containing 1 to 3 carbon atoms, the substituted alkyl chain itself is very easy to volatilize and migrate. At this time, even if other substituents are introduced with long chains containing more than 6 carbon atoms, it is difficult to change the limitations of the short-chain alkyl group. By introducing aromatic alkyl groups into the molecular structure, the benzene rings contained therein have a large steric hindrance, which can make up for the insufficient spatial shielding effect and poor heat resistance of short-chain esters. The above-mentioned mixed esters of aconitic acid have good plasticity, volatility resistance, migration resistance and heat resistance.

[0017] Optionally, at least one of R1, R2, and R3 is selected from an alkyl group having more than 10 carbon atoms, and at least one is selected from an alkyl group having 2-5 carbon atoms and substituted by a chlorine atom.

[0018] When at least one of R1, R2, and R3 is selected from an alkyl group containing more than 10 carbon atoms, the substituted alkyl chain itself is difficult to be compatible with PVC, and even the introduction of a short chain cannot effectively improve it. Therefore, the introduction of an alkyl group substituted by Cl can make the molecule of the aconitic acid mixed ester contain a Cl atom, and the Cl atom can have a strong dipole moment with the H on PVC, thereby increasing the compatibility with PVC and achieving the purpose of enhancing the interaction.

[0019] According to another aspect of the present application, a method for preparing the mixed esters of aconitic acid described in any one of the above items is provided, comprising the following steps:

[0020] S1: mixing the aconitic acid obtained by fermentation with alcohols, and performing an esterification reaction under a catalyst to obtain a mixed solution containing aconitic acid ester;

[0021] S2: neutralizing the mixed solution containing aconitate with an alkali solution, separating the liquids to obtain an organic phase A, then bleaching and decolorizing the organic phase A, washing, and separating the liquids to obtain an organic phase B;

[0022] S3: performing a desolventizing treatment on the organic phase B to obtain a purified product;

[0023] S4: adding a decolorizing agent to the purified product for adsorption decolorization, and filtering to obtain the aconitic acid mixed ester;

[0024] The alcohol is selected from at least two of an alkyl alcohol having 1 to 5 carbon atoms, an alkyl alcohol having 6 or more carbon atoms, an alkyl alcohol having 2 to 5 carbon atoms and substituted by chlorine atoms, and an alkyl alcohol containing an aromatic group.

[0025] Optionally, the alkyl alcohol containing 1 to 5 carbon atoms is selected from at least one of methanol, ethanol, 2-methoxyethanol, 2-ethoxyethanol, propanol, isopropanol, n-butanol, isobutanol and tert-butanol;

[0026] The alkyl alcohol containing 6 or more carbon atoms is selected from at least one of n-pentanol, isopentanol, tert-pentanol, 2-methylpentanol, 2-methyl-2-pentanol, 2-methyl-3-pentanol, 3-ethyl-3-pentanol, 4-methyl-1-pentanol, 4-methyl-2-pentanol, n-hexanol, 2-hexanol, 3-hexanol, 2-ethylhexanol, 3,5,5-trimethylhexanol, n-heptanol, 2-heptanol, 3-heptanol, 2-methylheptanol, 4-methyl-3-heptanol, 3-propylheptanol, 2,6-dimethyl-4-heptanol, n-octanol, 2-octanol, n-nonanol, 2-nonanol, 3-nonanol, 5-ethyl-2-nonanol, 2,6,8-trimethyl-4-nonanol, n-decanol, isodecanol, undecanol, and dodecanol;

[0027] The alkyl alcohol containing 2 to 5 carbon atoms and substituted by chlorine atoms is selected from at least one of chloroethanol, 1-chloro-2-propanol, 3-chloro-1-propanol and 2-chloro-1-propanol;

[0028] The aromatic group-containing alkyl alcohol is at least one selected from benzyl alcohol and phenylethyl alcohol.

[0029] The production process of aconitic acid obtained by chemical synthesis is currently demanding and cannot be mass-produced. Therefore, the fermentation method is currently the most widely used method. However, the aconitic acid produced by this fermentation method will produce many impurities during the preparation process. The proportion of impurities is between 2-40%, and the impurities are mainly polysaccharides, pigments, and trace amounts of mycelium and protein.

[0030] At present, for the decolorization and purification methods of acids, the dissolution-precipitation method is used for acids with low solubility. By preparing a concentrated solution of the acid and heating it, due to its low solubility, it precipitates as the temperature decreases. At this time, the pigment impurities have not reached the precipitation limit, so they can be effectively purified; while the salt precipitation method is used for acids with high solubility. The acid is prepared into a concentrated solution and salt (such as calcium salt) is added to form a precipitate with the acid. The higher solubility can precipitate as much as possible, while the pigment impurities are precipitated less and can be further washed away, so effective purification can also be achieved.

[0031] Aconitic acid has a high solubility. When its concentrated solution is reduced with temperature to separate out the product, pigment impurities will also separate out together. When using the salt precipitation method, due to the still high solubility of aconitate, it is difficult to effectively precipitate out, and it is more difficult to retain the precipitated product when further cleaning and purification. If aconitic acid is decoloured and purified, it needs to be extracted by a polar organic solvent, and then decoloured with an adsorbent, the above steps are cumbersome and if the organic extract is not removed cleanly, it will affect the synthesis reaction of subsequent aconitic acid mixed esters, so the aconitic acid raw material is difficult to separate from the pigment in the early stage, so the aconitic acid mixed esters prepared by the aconitic acid are provided with pigment impurities. When the aconitic acid mixed esters containing the above-mentioned pigment impurities are added to PVC, it will not only affect the coloring performance of PVC products, but also reduce its own plasticity and tolerance.

[0032] Optionally, in step S1, aconitic acid and alcohols are mixed in a molar ratio of 1:(3-9), a catalyst is added, and an esterification reaction is carried out at 75-145° C. for 2-8 hours to obtain a mixed solution containing aconitic acid ester.

[0033] Preferably, the stirring speed is 100-1200 rpm.

[0034] Since the aconitic acid raw material is obtained by fermentation, a part of the polysaccharide impurities contained therein will be hydrolyzed into monosaccharides with a small molecular weight, such as mannose, glucose and galactose. Their molecules contain a large number of hydroxyl groups, which compete with alcohol for esterification, greatly reducing the purity of the product; the remaining polysaccharides have a large molecular weight and a complex structure, contain a large number of hydroxyl groups and also have a large steric hindrance. Although the reaction rate with aconitic acid is slow, once esterified, its large steric hindrance makes it difficult for the other two carboxylic acids to esterify, thus affecting the yield and purity of the product. In addition, polysaccharides will undergo a caramelization reaction under high temperature conditions. The caramelization reaction will increase the color of aconitate esters and reduce the purity of aconitate esters, further affecting the use of aconitate esters.

[0035] At the above-mentioned esterification temperature and time of aconitic acid and alcohols, the rate of aconitic acid reacting with alcohols is much greater than the rate of reaction with impure sugars. The reaction amounts of catalysts and alcohols enable aconitic acid to be esterified with alcohols as much as possible, thereby improving the reaction conversion rate of aconitic acid and ensuring the smooth synthesis of aconitic acid mixed esters. The proportion of aconitic acid complex esters of a certain specific structure in the aconitic acid mixed esters can also be controlled by temperature and esterification time, thereby obtaining aconitic acid mixed esters with optimal plasticizing and tolerance properties.

[0036] When the temperature is lower than 75℃, the efficiency of the esterification reaction will be greatly reduced. If a higher utilization rate or yield is required, a longer reaction time must be required. Polysaccharides are difficult to undergo esterification due to their large volume steric hindrance. However, a longer reaction time will cause the acidic catalyst to promote the hydrolysis of polysaccharides into monosaccharides, resulting in monosaccharides with rich hydroxyl groups competing with alcohols and the esterification reaction of aconitic acid. When the temperature is higher than 145℃, polysaccharides will undergo caramelization, which will produce dark brown sugar dehydrated polymers, deepening the color of aconitic acid mixed esters. A small amount of sugar dehydrated polymers can be absorbed by activated carbon. When the content is too high, it is difficult to remove and will block the adsorption pores of activated carbon, reducing the adsorption efficiency of activated carbon. Therefore, only at this temperature and after effective treatment can low-color and high-purity aconitic acid mixed esters be obtained.

[0037] The esterification time of the present application is also determined by the fermentation-derived aconitic acid, which has many impurities and greatly affects the reaction rate. When the time is too short, the reaction is incomplete and it is difficult to obtain a higher yield; when the time is long, a large amount of polysaccharide hydrolysis will occur in the reaction, and the hydrolyzed monosaccharides will compete with alcohols for the esterification reaction, resulting in low reaction purity. Therefore, the esterification reaction can only be carried out within this time period to obtain a high-purity, low-chroma, high-yield aconitic acid mixed ester.

[0038] Optionally, in step S2, the solute of the alkali solution is at least one of NaOH, NaHCO3 and Na2CO3, and the mass fraction of the solute in the alkali solution is 5 to 25%.

[0039] Optionally, in step S3, the desolvation temperature is 40-100° C., and the vacuum degree is 0.01 mbar to 100 mbar.

[0040] Optionally, the weight ratio of the catalyst to aconitic acid is 1:(2-100), and the catalyst is selected from a homogeneous catalyst and a heterogeneous catalyst. When a heterogeneous catalyst is used, no water-carrying agent is required, and when a homogeneous catalyst is used, a water-carrying agent needs to be added, and the molar ratio of the water-carrying agent to aconitic acid is (1-5):1.

[0041] Preferably, the homogeneous catalyst is selected from at least one of p-toluenesulfonic acid, p-toluenesulfonic acid monohydrate, dinitrobenzoic acid, diethylaminetetraacetic acid, trichloroacetic acid, methanesulfonic acid, ethanesulfonic acid, propanesulfonic acid, butanesulfonic acid, alkylsulfuric acid, dodecylbenzenesulfonic acid, sulfamic acid, tetrabutyl titanate, isopropyl titanate, stannous octoate, stannous chloride, antimony acetate, cobalt acetate, and manganese acetate, preferably toluenesulfonic acid and p-toluenesulfonic acid monohydrate. The above-mentioned homogeneous catalyst can promote the esterification reaction to be completed efficiently, fully, and rapidly to the greatest extent, reduce the generation of by-products, and the esterification reaction efficiency is high, the product quality is good, and the energy consumption is low. In the presence of the homogeneous catalyst, toluene, benzene or cyclohexane is used as a water-carrying agent to take water away from the reaction and separate the water, and at the same time, aconitic acid can be effectively mixed with alcohols to promote catalytic efficiency and increase reaction speed.

[0042] Preferably, the heterogeneous catalyst is selected from sodium bisulfate monohydrate, sodium bisulfate, potassium bisulfate, copper sulfate, ferric sulfate, titanium sulfate, aluminum sulfate, yttrium, cerium sulfate, lanthanum sulfate, magnesium sulfate, ferrous sulfate, ferrous ammonium sulfate, cerium methanesulfonate, ferric chloride, tin tetrachloride, titanium chloride, rare earth chloride, potassium hydroxide, sodium hydroxide, potassium bicarbonate, sodium bicarbonate, sodium carbonate, anion exchange resin, strong acid cation exchange resin, weak acid cation exchange resin, potassium sulfamate, sodium sulfamate, tetrabutylammonium chloride, tetrabutylammonium bromide, copper methanesulfonate at least one, preferably sodium bisulfate monohydrate, sodium bisulfate. The heterogeneous catalyst can achieve under relatively low temperature conditions, to the greatest extent promote the esterification reaction to be completed efficiently, fully and rapidly, reduce the generation of by-products, the esterification reaction efficiency is high, the product quality is good, the energy consumption is low, and it is easy to separate, convenient for post-processing, and the recovered catalyst can continue to be used, further reducing the industrialization cost.

[0043] Optionally, when a heterogeneous catalyst is used, the reaction between aconitic acid and alcohol is followed by filtration to obtain the mixed solution containing aconitic acid ester.

[0044] Optionally, the water-carrying agent is selected from at least one of toluene, benzene and cyclohexane, preferably toluene.

[0045] In the traditional esterification reaction, concentrated sulfuric acid is used as a catalyst. Concentrated sulfuric acid has strong oxidizing properties and strong acidity at the same time. Although it can catalyze the reaction, it will carbonize the mycelium and protein in the fermented aconitic acid, resulting in the complexity and difficulty of aconitic acid mixed esters. The above-mentioned homogeneous catalyst and heterogeneous catalyst replace the traditional concentrated sulfuric acid. The catalyst does not have strong oxidizing properties and acidity at the same time, and the side reactions in the esterification reaction can be effectively suppressed. For example, the acidity of p-toluenesulfonic acid is strong but non-oxidizing, and the acidity of sodium bisulfate itself is weaker than concentrated sulfuric acid, and the side reactions are less than concentrated sulfuric acid, and the product chromaticity purity is high. Therefore, the types of the above-mentioned homogeneous catalyst and heterogeneous catalyst are all arranged based on the aconitic acid obtained by fermentation, and the yield and purity of aconitic acid mixed esters can be further improved in the esterification reaction of aconitic acid and alcohols, and the chromaticity of aconitic acid mixed esters can be reduced.

[0046] In the preparation method of the present application, bleaching decolorization and adsorption decolorization are performed in step S2 and step S4 respectively, which can selectively remove the water-soluble pigments and fat-soluble pigments in aconitic acid and reduce the impurity content in aconitic acid mixed esters to obtain high-purity aconitic acid mixed esters, thereby further improving the plasticizing properties and self-tolerance properties of aconitic acid esters.

[0047] Because there are more pigments in the aconitic acid raw material and different types of pigments have obvious differences in solubility for organic solvents and water. In this preparation method, the main oxidation destruction of bleaching and decolorization is the structure of fat-soluble pigments, because its structure mostly contains double bonds, such pigments and aconitic acid mixed esters have good compatibility, are difficult to be adsorbed, therefore, the double bonds in such pigments are destroyed by hydrogen peroxide oxidation, while removing the fat-soluble pigment chromaticity, the absorbance of fat-soluble pigments by decolorizing agents is increased, thus the decolorization of the decolorizing agent in conjunction with step S4 can effectively reduce the content of fat-soluble pigments in aconitic acid mixed esters, but hydrogen peroxide and aconitic acid mixed esters are not miscible, and decolorization needs to be washed with clean water. Therefore, the bleaching and decolorization with hydrogen peroxide is placed before the washing and desolventizing steps, which can not only fully decolorize the fat-soluble pigments, but also ensure that the hydrogen peroxide is removed by the subsequent washing step. If the bleaching and decolorization is placed after the desolventizing step, the introduction of hydrogen peroxide will cause the aconitic acid mixed esters to form oil-water separation, and the hydrogen peroxide still needs to be further removed, resulting in cumbersome steps and reducing the removal rate of fat-soluble pigments.

[0048] After the desolventizing step, decolorizing with a decolorizing agent is performed, and water-soluble pigments are mainly removed. The decolorizing agent used can be evenly distributed in the aconitic acid mixed esters, and the aconitic acid mixed esters are evenly decolorized in only one phase, thereby effectively reducing the content of water-soluble pigments in the aconitic acid mixed esters. If the decolorizing agent is placed before the washing step or decolorized together with hydrogen peroxide, the decolorizing agent has different affinities with the aconitic acid mixed esters and the solvent liquid phase, resulting in the decolorizing agent being absorbed by different liquid phases to form lumps. The lumps are dispersed in the aconitic acid mixed esters and are difficult to be evenly mixed with the aconitic acid mixed esters, resulting in insufficient contact between the aconitic acid mixed esters and the aconitic acid mixed esters, a decrease in the decolorization effect, and a reduction in the removal rate of the water-soluble pigments.

[0049] Optionally, in step S2, hydrogen peroxide is used for bleaching and decolorization, the concentration of the hydrogen peroxide is 33-40%, and the weight of the hydrogen peroxide accounts for 1-5% of the weight of the organic phase A.

[0050] Optionally, in step S4, the decolorizing agent is selected from at least one of activated carbon, diatomaceous earth, kaolin, basic alumina, and neutral alumina.

[0051] Optionally, the weight ratio of the decolorizing agent to the purified product is 1:(2-100).

[0052] The double bond in the fat-soluble pigment is the double bond in the alkyl chain, and there is no large steric hindrance around itself, which is easily destroyed. The double bond of aconitic acid is between two large sterically hindered ester groups, which is difficult to be destroyed. Therefore, the concentration and weight of the above-mentioned hydrogen peroxide can destroy the double bond of the fat-soluble pigment quickly, thereby improving the removal rate of the fat-soluble pigment, and the hydrogen peroxide of this concentration and weight can not destroy the double bond in the aconitic acid mixed ester, improve the productive rate of aconitic acid ester. The strong oxidizing property of hydrogen peroxide will be oxidized into non-color functional group with chromogenic functional group in the fat-soluble pigment, so the fat-soluble pigment material structure that the double bond is destroyed changes, and light is non-absorbent. The consumption of the discoloring agent can ensure that the discoloring agent is evenly dispersed in the aconitic acid mixed ester, improves the adsorption effect of the fat-soluble pigment and the water-soluble pigment that the structure changes, and is beneficial to the later stage removal of discoloring agent.

[0053] Optionally, the temperature for bleaching and decolorizing with hydrogen peroxide is 20-70°C and the time is 15-30 minutes.

[0054] Optionally, the temperature for adsorption decolorization by the decolorizing agent is 20-70°C and the time is 10-120 min.

[0055] Optionally, the fat-soluble pigment includes anthraquinone compounds; and the water-soluble pigment includes terreusin.

[0056] Temperature is an important factor affecting the decolorization of pigment impurities in aconitic acid. The higher the temperature, the lower the viscosity of the product system, the better the fluidity, and the more evenly the decolorant is distributed in the system. However, the higher the temperature, the more violent the Brownian motion of the molecules, the more difficult it is for the decolorant to adsorb the pigment, which leads to a decrease in the removal rate of pigment impurities. In the decolorization of citrate esters, since citric acid contains hydroxyl groups in its structure, the hydroxyl groups easily form hydrogen bonds with hydroxyl groups and ester groups on other molecules, causing the product molecules to aggregate. The activated carbon used has poor adsorption effect, so high temperature is required to destroy the aggregation of molecules to achieve the purpose of decolorization.

[0057] The bleaching decolorization temperature and adsorption decolorization temperature of the present application are relatively low. Firstly, they can reduce energy consumption in the decolorization step. Secondly, it has been found through research that the lower the decolorization temperature, the lower the Brownian motion of the molecules, and the better the decolorization effect. Therefore, the above-mentioned decolorization temperature and time can effectively improve the removal efficiency and removal rate of pigment impurities, thereby improving the purity of aconitic acid mixed esters.

[0058] Optionally, the iodine value of the activated carbon is greater than 800, and the Aran value is greater than 10; the particle size of the diatomaceous earth is 200-300 mesh; the particle size of the kaolin is 200-300 mesh; the particle size of the basic alumina and the neutral alumina are both 100-200 mesh, and the specific surface area is 60-90m 2 / g, average pore size 10-20nm. Under the setting of the above decolorizing agent, the decolorizing agent is evenly dispersed in the aconitate phase, avoiding agglomeration or aggregation of the decolorizing agent, and the decolorizing agent can increase the contact area with the water-soluble pigment and the fat-soluble pigment with the double bond destroyed, so that the above two pigments and other impurities are adsorbed and stored in the pores of the decolorizing agent itself, thereby improving the adsorption force on the pigment, preventing the pigment from escaping again after being adsorbed, and thus improving the removal effect of the water-soluble pigment, the fat-soluble pigment and the impurities.

[0059] Alumina itself has a large adsorption area and pores for adsorbing pigments. In the above system, since sugar and pigment impurities are generally acidic, when alkaline alumina and neutral alumina are selected in the decolorizer, the adsorption capacity for sugar and pigment impurities can be increased, and the removal rate of pigment impurities and sugars can be improved.

[0060] Optionally, the decolorizing agent is selected from activated carbon.

[0061] Optionally, the purity of the aconitic acid mixed esters is not less than 99%.

[0062] Optionally, the chromaticity of the mixed esters of aconitic acid is not higher than 50Pt-Co.

[0063] The purity of aconitic acid esters prepared by the traditional method can reach up to 95%, and the chromaticity is above 500Pt-Co, which is obtained by testing with a platinum-cobalt colorimetry. In the preparation method of the present application, during the synthesis of aconitic acid mixed esters, the conversion rate of aconitic acid is improved by controlling the temperature and time, thereby improving the purity of aconitic acid mixed esters, and combining bleaching and adsorption decolorization to improve the decolorization effect by an order of magnitude, not only reducing the chromaticity, but also reducing the impurity content, and increasing the purity of the product to greater than or equal to 99%, with a significant purification effect.

[0064] Optionally, the content of fat-soluble pigments in the aconitic acid mixed esters is less than 1000 ppm, and the content of water-soluble pigments is less than 1000 ppm.

[0065] Preferably, the content of fat-soluble pigments in the mixed esters of aconitic acid is less than 500 ppm, and the content of water-soluble pigments is less than 500 ppm.

[0066] According to another aspect of the present application, a composite material containing any of the above-mentioned aconitic acid mixed esters is provided, comprising: 100-120 parts of PVC resin, 5-90 parts of aconitic acid mixed esters, 0.5-10 parts of lubricant, and 2-10 parts of stabilizer.

[0067] Optionally, the K value of the PVC resin is 55-77 and the polydispersity index is 3-5;

[0068] Preferably, the polydispersity index of the PVC resin is 3.5-4.5.

[0069] When the PVC resin with the above K value is used, the obtained PVC material has better toughness because the macromolecular chains are entangled with each other and react with the aconitic acid mixed ester, lubricant and stabilizer components to cross-link to form a stable cross-linked network structure, thereby having better toughness, plasticity and tensile resistance.

[0070] The inventors found that when the polydispersity index of the PVC resin used is 3-5, the composite material has the best toughness and plasticity. This may be because when the polydispersity index of the PVC resin is 3-5, the material contains a variety of PVC resins with different molecular weights, and the resin materials with different molecular weights are mixed, which can better react with the mixed esters of aconitic acid containing different alkyl groups, effectively increase the dissolution amount of the mixed esters of aconitic acid, and can effectively combine to increase the interaction between molecular chains, so that the prepared PVC material has high toughness, high stability and plasticity, and good stability, and is not prone to problems such as phase separation.

[0071] Optionally, the lubricant is selected from at least one of oxidized polyethylene wax, glyceryl stearate, ethylene bisstearamide synthetic wax, paraffin and polyethylene wax, preferably oxidized polyethylene wax.

[0072] The above lubricants are generally compatible with PVC materials, so they will migrate to the surface of the product after mixing, forming a certain protective layer, and have a synergistic effect when used with aconitic acid mixed esters, a plasticizer that is resistant to extraction by various solvents. The surface lubricant can make the product easier to demould during processing and to a certain extent isolate the additives from migrating to the outside world.

[0073] Optionally, the stabilizer is selected from at least one of an organic tin heat stabilizer, dibutyltin laurate, dibutyl / octyltin sulfate, octyltin maleate, and methyltin mercaptan, preferably octyltin maleate.

[0074] The above-mentioned heat stabilizer is non-toxic, transparent and odorless, and is widely used in industries with high safety requirements such as food and medical care. When used with aconitic acid mixed ester, a plasticizer that has all-round safety, it has a synergistic effect and jointly improves the material's tolerance in complex environments.

[0075] Optionally, the preparation method of the composite material is:

[0076] The aconitic acid mixed ester, PVC resin, stabilizer and lubricant are mixed, mixed at 30-80° C. for 10-60 min using a high-speed mixer, then mixed at 130-190° C. for 5-20 min in a two-roll open mill, and finally placed in a flat vulcanizer for vulcanization at 140-190° C. and 10-15 MPa for 5-15 min.

[0077] The above composite materials can be used for hoses, cables and packaging materials, among which the materials are mainly used to produce mineral water bottles, beverage bottles, cosmetic bottles, PTP packaging for medicines, and packaging for refined oils. The use environment of hoses and cables is relatively complex, and the temperature difference in the use scenarios is large. They need to have good tolerance to both high and low temperatures. The production, transportation, storage and use environments of packaging materials are different, and they need to have good tolerance to complex contact environments. The hoses, cables and packaging materials prepared by the composite materials have high comprehensive performance and can be used in various complex environments. They have high universality and tolerance in complex environments, and have good stability in complex environments, which prolongs the use time of the products.

[0078] The beneficial effects of this application include but are not limited to:

[0079] 1. The mixed esters of aconitic acid of the present application have ester groups of different carbon chain lengths in their molecular structure, which can not only balance the plasticizing effect, heat resistance and tolerance of the product, but also balance the product's resistance to extraction of water solvents and organic solvents.

[0080] 2. The present application contains both ester groups with 1-5 carbon atoms and mixed esters of aconitic acid with 6 or more carbon atoms. The ester groups with 6 or more carbon atoms can effectively increase the relative molecular mass of aconitic acid ester, making it more difficult to separate from a high temperature environment. The ester groups with 1-5 carbon atoms have good compatibility with the PVC molecular chain, and the two ester groups are combined together at the molecular level to achieve both good plasticizing performance and good safety performance. Therefore, this type of mixed ester of aconitic acid can effectively improve the upper temperature limit and service life of the composite material while maintaining a high plasticizing efficiency.

[0081] 3. The mixed ester of aconitic acid of the present application has aconitic acid as the main structure. On the one hand, aconitic acid is of biological origin, environmentally friendly, safe and non-toxic. On the other hand, aconitic acid, as a tricarboxylic acid structure, has excellent product designability and can be esterified to form a triester structure. The triester structure has a larger steric volume than the diester structure (phthalic acid), and can more effectively weaken the interaction between the main molecular chains of the material to achieve the purpose of plasticization. At the same time, compared with other tricarboxylic acids, especially citric acid, the lack of hydroxyl groups in aconitic acid can avoid useless chemical reactions or the formation of hydrogen bonds, thereby improving the modification effect, and the extra double bonds can increase the interaction between the plasticizer and the material, giving the material special properties and stability.

[0082] 4. According to the preparation method of aconitic acid mixed esters of the present application, aconitic acid and alcohol compounds are catalytically synthesized into aconitic acid mixed esters. This synthesis route has good atom economy, does not produce impurities that are difficult to remove, and has a high yield.

[0083] 5. According to the preparation method of aconitic acid mixed esters of the present application, by neutralizing, bleaching and decolorizing, desolventizing and adsorption decolorizing the synthesized mixed solution containing aconitic acid esters, high-purity, low-chroma, low-acid value and transparent aconitic acid mixed esters are obtained without affecting the yield of the aconitic acid mixed ester plasticizer, and the processing process is simple, efficient and low-cost, which is conducive to large-scale industrial production and application. DETAILED DESCRIPTION

[0084] The present application is described in detail below with reference to embodiments, but the present application is not limited to these embodiments.

[0085] Unless otherwise specified, the raw materials in the examples of this application were purchased through commercial channels.

[0086] Example 1

[0087] Aconitic acid mixed ester 1#

[0088] The preparation method of aconitic acid mixed ester 1# comprises the following steps:

[0089] S1: Mix aconitic acid, n-butanol and isooctyl alcohol in a molar ratio of 1:6:3, add sodium bisulfate catalyst, and perform esterification reaction at 125°C and 300 rpm for 6 hours to obtain a mixed solution containing aconitic acid ester, wherein the weight ratio of sodium bisulfate to aconitic acid is 1:10;

[0090] S2: At 40°C, an equal volume of Na2CO3 alkali solution is used to neutralize the mixed solution containing aconitate for 20 minutes, the mass fraction of the solute in the alkali solution is 5%, and the mixture is separated to obtain an organic phase A after three times of repeated treatment. Then, the organic phase A is bleached and decolorized at 30°C for 15 minutes with 35% hydrogen peroxide, the weight of which accounts for 3% of the weight of the organic phase A. Then, the organic phase B is obtained after washing with water and separation.

[0091] S3: desolventizing the organic phase B at 70° C. and a vacuum degree of 50 mbar until no fraction is distilled out to obtain a purified product;

[0092] S4: Add activated carbon decolorizer with an iodine value of 810 and a cyanide value of 12 to the purified product for adsorption decolorization at 30°C for 30 minutes. The weight ratio of activated carbon to purified product is 1:7. After filtration, aconitic acid mixed ester 1# is obtained.

[0093] Aconitic acid mixed ester 2#

[0094] The preparation method of the present aconitic acid mixed ester 2# is different from that of the aconitic acid mixed ester 1# in that, in step S1, a mixture of aconitic acid, n-butanol and isooctyl alcohol in a molar ratio of 1:3:6 is used for esterification reaction, and the remaining steps and material amounts are the same as those of the aconitic acid mixed ester 1#, so as to obtain aconitic acid mixed ester 2#.

[0095] Aconitic acid mixed ester 3#

[0096] The preparation method of aconitic acid mixed ester 3# comprises the following steps:

[0097] S1: Mix aconitic acid, ethanol and benzyl alcohol in a molar ratio of 1:4:2, add iron sulfate catalyst, and perform esterification reaction at 145°C and 100 rpm for 8 hours to obtain a mixed solution containing aconitic acid ester, wherein the weight ratio of iron sulfate to aconitic acid is 1:2;

[0098] S2: At 20°C, the mixed solution containing aconitate is neutralized with an equal volume of NaOH alkali solution for 30 minutes, the mass fraction of the solute in the alkali solution is 15%, and the process is repeated three times, followed by separation to obtain an organic phase A, followed by bleaching and decolorizing the organic phase A with 33% hydrogen peroxide at 20°C for 30 minutes, the weight of the hydrogen peroxide accounting for 5% of the weight of the organic phase A, followed by washing with water and separation to obtain an organic phase B;

[0099] S3: desolventizing the organic phase B at 40° C. and a vacuum degree of 100 mbar until no fraction is distilled out to obtain a purified product;

[0100] S4: Add activated carbon decolorizer with an iodine value of 810 and a cyanide value of 12 to the purified product for adsorption decolorization at 70°C for 10 minutes. The weight ratio of activated carbon to purified product is 1:2. After filtration, aconitic acid mixed ester 3# is obtained.

[0101] Aconitic acid mixed ester 4#

[0102] The preparation method of aconitic acid mixed ester 4# is different from that of aconitic acid mixed ester 3# in that a mixture of aconitic acid, ethanol and benzyl alcohol in a molar ratio of 1:2:4 is used in step S1 for esterification reaction, and the remaining steps and material amounts are the same as those of aconitic acid mixed ester 3#, so as to obtain aconitic acid mixed ester 4#.

[0103] Aconitic acid mixed ester 5#

[0104] The preparation method of aconitic acid mixed ester 5# comprises the following steps:

[0105] S1: Mix aconitic acid, isooctyl alcohol and chloroethanol in a molar ratio of 1:2:1, add p-toluenesulfonic acid monohydrate catalyst and toluene water agent, and perform esterification reaction at 75°C and 1200 rpm for 2 hours to obtain a mixed solution containing aconitic acid ester, wherein the weight ratio of p-toluenesulfonic acid monohydrate to aconitic acid is 1:100, and the molar ratio of toluene water agent to aconitic acid is 5:1;

[0106] S2: At 70°C, the mixed solution containing aconitate is neutralized with an equal volume of NaHCO3 alkali solution for 15 minutes, the mass fraction of the solute in the alkali solution is 25%, and the mixture is separated to obtain an organic phase A after three times of repeated treatment. The organic phase A is then bleached and decolorized with 40% hydrogen peroxide at 70°C for 15 minutes, the weight of the hydrogen peroxide accounting for 1% of the weight of the organic phase A, and then washed with water and separated to obtain an organic phase B;

[0107] S3: desolventizing the organic phase B at 100° C. and a vacuum degree of 0.01 mbar until no fraction is distilled out to obtain a purified product;

[0108] S4: Add activated carbon decolorizer with an iodine value of 810 and a cyanide value of 12 to the purified product for adsorption decolorization at 20°C for 120 minutes. The weight ratio of activated carbon to purified product is 1:100. After filtration, aconitic acid mixed ester 5# is obtained.

[0109] Aconitic acid mixed ester 6#

[0110] The preparation method of aconitic acid mixed ester 6# is different from that of aconitic acid mixed ester 5# in that a mixture of aconitic acid, isooctyl alcohol and chloroethanol in a molar ratio of 1:1:2 is used in step S1 for esterification reaction, and the remaining steps and material amounts are the same as those of aconitic acid mixed ester 5#, so as to obtain aconitic acid mixed ester 6#.

[0111] Aconitic acid mixed esters 7#

[0112] The preparation method of aconitic acid mixed ester 7# is different from that of aconitic acid mixed ester 1# in that aconitic acid, n-butanol, isooctyl alcohol and 1-chloro-2-propanol in a molar ratio of 1:3:3:3 are mixed for esterification in step S1, and the remaining steps and material amounts are the same as those of aconitic acid mixed ester 1#, so as to obtain aconitic acid mixed ester 7#.

[0113] Aconitic acid mixed ester 8#

[0114] The preparation method of aconitic acid mixed ester 8# is different from that of aconitic acid mixed ester 1# in that aconitic acid, n-butanol, isooctyl alcohol and phenylethanol in a molar ratio of 1:3:3:3 are mixed for esterification in step S1, and the remaining steps and material amounts are the same as those of aconitic acid mixed ester 1#, so as to obtain aconitic acid mixed ester 8#.

[0115] Aconitic acid mixed esters 9#

[0116] The preparation method of the present aconitic acid mixed ester 2# is different from that of the aconitic acid mixed ester 1# in that, in step S1, aconitic acid, benzyl alcohol and 3-chloro-1-propanol are mixed in a molar ratio of 1:3:6 for esterification reaction, and the remaining steps and the amount of substances used are the same as those of the aconitic acid mixed ester 1#, so as to obtain aconitic acid mixed ester 9#.

[0117] Aconitic acid mixed esters 10#

[0118] The preparation method of the present aconitic acid mixed ester 10# is different from that of the aconitic acid mixed ester 3# in that, in step S1, a mixture of aconitic acid, ethanol and chloroethanol in a molar ratio of 1:2:4 is used for esterification reaction, and the remaining steps and material amounts are the same as those of the aconitic acid mixed ester 3#, so as to obtain aconitic acid mixed ester 10#.

[0119] Aconitic acid mixed ester 11#

[0120] The preparation method of aconitic acid mixed ester 11# is different from that of aconitic acid mixed ester 5# in that a mixture of aconitic acid, isooctyl alcohol and phenylethanol in a molar ratio of 1:1:2 is used in step S1 for esterification reaction, and the remaining steps and material amounts are the same as those of aconitic acid mixed ester 5#, so as to obtain aconitic acid mixed ester 11#.

[0121] Aconitic acid mixed ester 12#

[0122] The preparation method of the aconitic acid mixed ester 12# is different from that of the aconitic acid mixed ester 1# in that the concentration of the hydrogen peroxide in step S2 is 30%, and the remaining steps and the amount of substances used are the same as those of the aconitic acid mixed ester 1#, so as to obtain the aconitic acid mixed ester 12#.

[0123] Aconitic acid mixed ester 13#

[0124] The preparation method of aconitic acid mixed ester 13# is different from that of aconitic acid mixed ester 1# in that the concentration of hydrogen peroxide in step S2 is 45%, and the remaining steps and material amounts are the same as those of aconitic acid mixed ester 1#, so as to obtain aconitic acid mixed ester 13#.

[0125] Aconitic acid mixed ester 14#

[0126] The preparation method of the present aconitic acid mixed ester 14# is different from that of the aconitic acid mixed ester 1# in that the weight of the hydrogen peroxide in step S2 accounts for 8% of the weight of the organic phase A, and the remaining steps and material amounts are the same as those of the aconitic acid mixed ester 1#, so as to obtain the aconitic acid mixed ester 14#.

[0127] Aconitic acid mixed esters 15#

[0128] The preparation method of the present aconitic acid mixed ester 14# is different from that of the aconitic acid mixed ester 1# in that the weight of the hydrogen peroxide in step S2 accounts for 0.5% of the weight of the organic phase A, and the remaining steps and material amounts are the same as those of the aconitic acid mixed ester 1#, so as to obtain aconitic acid mixed ester 15#.

[0129] Aconitic acid mixed esters 16#

[0130] The preparation method of the present aconitic acid mixed ester 16# is different from that of the aconitic acid mixed ester 1# in that the decolorization temperature of the hydrogen peroxide in step S2 is 80°C, and the remaining steps and the amount of substances used are the same as those of the aconitic acid mixed ester 1#, so as to obtain the aconitic acid mixed ester 16#.

[0131] Aconitic acid mixed esters 17#

[0132] The preparation method of the aconitic acid mixed ester 17# is different from that of the aconitic acid mixed ester 1# in that the decolorization time of the hydrogen peroxide in step S2 is 10 minutes, and the remaining steps and the amount of substances used are the same as those of the aconitic acid mixed ester 1#, so as to obtain the aconitic acid mixed ester 17#.

[0133] Aconitic acid mixed esters 18#

[0134] The preparation method of the present aconitic acid mixed ester 18# is different from that of the aconitic acid mixed ester 1# in that the weight ratio of activated carbon to the purified product in step S4 is 1:120, and the remaining steps and material amounts are the same as those of the aconitic acid mixed ester 1#, so as to obtain aconitic acid mixed ester 18#.

[0135] Aconitic acid mixed esters 19#

[0136] The preparation method of the present aconitic acid mixed ester 19# is different from that of the aconitic acid mixed ester 1# in that the decolorization temperature of the activated carbon in step S4 is 80°C, and the remaining steps and material amounts are the same as those of the aconitic acid mixed ester 1#, so as to obtain aconitic acid mixed ester 19#.

[0137] Aconitic acid mixed esters 20#

[0138] The preparation method of the present aconitic acid mixed ester 20# is different from that of the aconitic acid mixed ester 1# in that the decolorization temperature of the activated carbon in step S4 is 10°C, and the remaining steps and the amount of materials used are the same as those of the aconitic acid mixed ester 1#, so as to obtain aconitic acid mixed ester 20#.

[0139] Aconitic acid mixed ester 21#

[0140] The preparation method of the present aconitic acid mixed ester 21# is different from that of the aconitic acid mixed ester 1# in that the decolorization time of the activated carbon in step S4 is 5 minutes, and the remaining steps and the amount of materials used are the same as those of the aconitic acid mixed ester 1#, so as to obtain the aconitic acid mixed ester 21#.

[0141] Aconitic acid mixed ester 22#

[0142] The preparation method of the present aconitic acid mixed ester 22# is different from that of the aconitic acid mixed ester 1# in that the iodine value of the activated carbon in step S4 is 700 and the alanine value is 10, and the remaining steps and material amounts are the same as those of the aconitic acid mixed ester 1#, so as to obtain aconitic acid mixed ester 22#.

[0143] Aconitic acid mixed esters 23#

[0144] The preparation method of aconitic acid mixed ester 23# is different from that of aconitic acid mixed ester 1# in that the particle size of the aconitic acid mixed ester 23# is 200 mesh and the specific surface area of ​​the aconitic acid mixed ester 1# is 90 m 2 / g, basic alumina with an average pore size of 15 nm replaced the activated carbon, and the remaining steps and material amounts were the same as those of aconitic acid mixed ester 1#, to obtain aconitic acid mixed ester 23#.

[0145] Aconitic acid mixed ester 24#

[0146] The preparation method of the present aconitic acid mixed ester 24# is different from that of the aconitic acid mixed ester 1# in that, in step S1, the esterification reaction is carried out at 200°C and 300 rpm for 6 hours to obtain a mixed solution containing aconitic acid ester, and the remaining steps and material amounts are the same as those of the aconitic acid mixed ester 1#, so as to obtain aconitic acid mixed ester 24#.

[0147] Aconitic acid mixed ester 25#

[0148] The preparation method of the present aconitic acid mixed ester 25# is different from that of the aconitic acid mixed ester 1# in that an alkali solution is used for neutralization at 80°C in step S2, and the remaining steps and the amount of substances used are the same as those of the aconitic acid mixed ester 1#, so as to obtain aconitic acid mixed ester 25#.

[0149] Comparison with aconitic acid mixed ester D1#

[0150] The preparation method of the comparative aconitic acid mixed ester D1# comprises the following steps:

[0151] S1: Mix aconitic acid, n-butanol and isooctyl alcohol in a molar ratio of 1:6:3, add sodium bisulfate catalyst, and perform esterification reaction at 125°C and 300 rpm for 6 hours to obtain a mixed solution containing aconitic acid ester, wherein the weight ratio of sodium bisulfate to aconitic acid is 1:10;

[0152] S2: At 40°C, an equal volume of Na2CO3 alkali solution is used to neutralize the mixed solution containing aconitate for 20 minutes. The mass fraction of the solute in the alkali solution is 5%. Repeat three times and separate the liquids to obtain an organic phase.

[0153] S3: The organic phase was desolventized at 70° C. and a vacuum degree of 50 mbar until no fraction was distilled out, thereby obtaining aconitic acid mixed ester D1#.

[0154] Comparison with aconitic acid mixed ester D2#

[0155] The preparation method of the comparative aconitic acid mixed ester D2# comprises the following steps:

[0156] S1: Same as Example 1;

[0157] S2: At 40°C, an equal volume of Na2CO3 alkali solution was used to neutralize the mixed solution containing aconitate for 20 minutes. The mass fraction of the solute in the alkali solution was 5%. After three times of separation, an organic phase A was obtained. Then, an activated carbon decolorizer with an iodine value of 810 and a ylan value of 12 was added to the organic phase A for adsorption and decolorization at 30°C for 30 minutes. The weight ratio of activated carbon to organic phase A was 1:7. After filtering and washing with water, the organic phase B was obtained after separation.

[0158] S3: desolventizing the organic phase B at 70° C. and a vacuum degree of 50 mbar until no fraction is distilled out to obtain a purified product;

[0159] S4: Add 35% hydrogen peroxide to the purified product at 30°C to bleach and decolorize the organic phase A for 15 minutes, wherein the weight of the hydrogen peroxide accounts for 3% of the weight of the organic phase A. Then, the hydrogen peroxide is removed by washing with clean water, and the mixture is desolventized at 70°C and a vacuum degree of 50 mbar until no fraction is distilled out, thereby obtaining aconitic acid mixed ester D2#.

[0160] Comparison with Aconitic Acid Mixed Esters D3#

[0161] The preparation method of the comparative aconitic acid mixed ester D3# comprises the following steps:

[0162] (1) Same as Example 1;

[0163] (2) At 40° C., an equal volume of Na2CO3 alkali solution was used to neutralize the mixed solution containing aconitate for 20 minutes, the mass fraction of the solute in the alkali solution was 5%, and the mixture was separated after three times to obtain an organic phase A. To the organic phase A, 3% by weight of the organic phase A and 35% by weight of hydrogen peroxide and activated carbon with an iodine value of 810 and a yran value of 12 were added, and the weight ratio of the activated carbon to the organic phase A was 1:7. The mixture was decolorized at 30° C. for 30 minutes, and then filtered, washed with water, and separated to obtain an organic phase B;

[0164] S3: The organic phase B was desolventized at 70° C. and a vacuum degree of 50 mbar until no fraction was distilled out, thereby obtaining aconitic acid mixed ester D3#.

[0165] Test Example 1

[0166] The acid value, purity, chromaticity, yield, triester conversion rate and water content of the mixed esters of aconitic acid prepared in Example 1 were tested. The specific test results are shown in Table 1 below. The test method is as follows:

[0167] 1. Acid value: Take 50mL of ethanol and add 0.25mL of phenolphthalein indicator solution to make two portions for later use. -1 Neutralize with potassium hydroxide aqueous solution until it turns slightly pink, and record the consumed volume V0. Weigh 1g of the sample (accurate to 0.01g) in a ground-mouth conical flask, then add a portion of the neutralized solution above. After the sample is completely dissolved, add 0.02mol·L -1 Titrate the sample with potassium hydroxide ethanol standard titration solution (titration must be completed within 30 seconds) until a slightly pink color appears and remains unchanged for 5 seconds, which is the end point. Record the consumed volume V.

[0168] Acid value: X = (V-V0) cM) / m;

[0169] Where: X is the acid value of the sample (in KOH), in milligrams per gram (mg·g -1 ), V is the volume of potassium hydroxide-ethanol standard titration solution consumed by the sample, in milliliters (mL), V0 is the volume of potassium hydroxide-ethanol standard titration solution consumed by the blank test, in milliliters (mL), and c is the exact concentration of potassium hydroxide-ethanol standard titration solution, in moles per liter (mol·L -1 ), m is the mass of the sample in grams (g), M is the molar mass of potassium hydroxide in grams per mole (g·mol-1 )[M=56.11].

[0170] 2. Purity: Use high performance liquid chromatography, and the instrument sensitivity and stability of the detector should comply with the provisions of GB / T16631-2008. Chromatographic column: C18 column; Injector: 10μL micro syringe; Solvent: acetonitrile (HPLC grade); Collection time: 15min; Mobile phase: 80% acetonitrile (HPLC grade), 20% deionized water; Injection volume / : 1μL; Wavelength: 230nm.

[0171] Test: Adjust the instrument as specified above. After the baseline is stable, inject 0.2 μL of sample with a microsyringe. Simultaneously start the integrator or chromatography workstation. The instrument will automatically give the area percentage of each component.

[0172] Purity calculation formula: Purity = (integrated area of ​​aconitate / total integrated area) × 100%.

[0173] 3. Chroma: Preparation of No. 500 platinum-cobalt colorimetric standard stock solution: Weigh 1.2450g potassium chloroplatinate and 1.0000g cobalt chloride to an accuracy of 0.0002g, dissolve in 100mL hydrochloric acid, and then dilute to 1000mL with distilled water. This solution is the No. 500 colorimetric standard colorimetric solution.

[0174] Preparation of colorimetric standards less than No. 500 Take different amounts of No. 500 stock solution and dilute it with distilled water to the volume of the colorimetric tube to prepare colorimetric standards of any number. The calculation formula is as follows:

[0175] V=(N×V1) / 500

[0176] Where: V is the volume of No. 500 standard stock solution used to prepare No. N colorimetric standard solution, mL; V1 is the volume of the colorimetric tube used, mL; N is the number of the colorimetric standard solution to be prepared.

[0177] After the sample is evenly mixed, it is injected into a colorimetric tube and observed with the naked eye. It should be a transparent oily liquid with no turbidity and no obvious mechanical impurities. The colorimetric determination is carried out at 25°C.

[0178] 4. Yield: The efficiency of the reaction synthesis route is characterized by the yield, and the yield calculation formula is: Yield = (mass of the final product obtained / mass of the theoretically obtained aconitate) × 100%.

[0179] 5. Trisester conversion rate: The characteristic peak of aconitate (about 6.8) was analyzed by NMR spectrum, and the triester conversion rate was calculated as follows: Trisester conversion rate = (integral area of ​​aconitate triester / total area of ​​aconitate and aconitate (monoester, diester, triester) in this area) × 100%.

[0180] 6. Water content: Use Karl Fischer titrator to test the water content (retain to two decimal places).

[0181] 7. Residual amount of fat-soluble pigment and residual amount of water-soluble pigment: Use high performance liquid chromatography, and the instrument sensitivity and stability of the detector shall comply with the provisions of GB / T 16631-2008. Chromatographic column: C18 column; Injector: 10μL micro-syringe; Solvent: acetonitrile (HPLC grade); Collection time: 15min; Mobile phase: 80% acetonitrile (HPLC grade), 20% deionized water; Injection volume / : 1μL; Wavelength: 230nm.

[0182] Test: Adjust the instrument as specified above. After the baseline is stable, inject 0.2 μL with a micro syringe and start the integrator or chromatographic workstation at the same time. By testing the integrated area of ​​pigments of different concentrations, a standard curve of pigment concentration-integrated area is established. When measuring the pigment content, the instrument automatically gives the corresponding pigment integrated area, and the pigment concentration is obtained by comparing it with the standard curve. The ratio of the pigment concentration to the sample concentration is the pigment content.

[0183] Table 1

[0184]

[0185]

[0186]

[0187] According to the contents of Table 1, the mixed aconitic acid esters prepared by the preparation method of the present application can remove pigment impurities carried by aconitic acid itself during the preparation process, reduce the content of fat-soluble pigments and water-soluble pigments, and improve the purity and yield of aconitic acid esters.

[0188] According to the comparison between aconitic acid mixed esters 12#-15# and aconitic acid mixed ester 1#, it can be seen that the concentration and dosage of hydrogen peroxide can affect the removal effect of fat-soluble pigments. If the concentration of hydrogen peroxide is too low or the dosage is too little, the product pigment will be incompletely bleached and the pigment will not meet the requirements; if the concentration of hydrogen peroxide is too high or the dosage is too much, the chromaticity of the product will increase, and more hydrogen peroxide will participate in the hydrolysis of aconitic acid esters, which will reduce the yield although the reaction rate is very slow.

[0189] According to the comparison between aconitic acid mixed esters 16#-17# and aconitic acid mixed ester 1#, it can be seen that the higher the decolorization temperature of hydrogen peroxide, the more hydrogen peroxide will decompose, and the oxidation effect on fat-soluble pigments will be poor, so that the residual amount of fat-soluble pigments will increase, and then the chroma of aconitate will increase and the purity will decrease. At the same time, it will promote the hydrolysis of aconitate by hydrogen peroxide, so that the yield of aconitate will decrease; the decolorization time of hydrogen peroxide is shortened, which affects the destructive effect of hydrogen peroxide on the main structure of fat-soluble pigments, and then the chroma of aconitate will increase and the purity will decrease.

[0190] According to the comparison between aconitic acid mixed ester 18# and aconitic acid mixed ester 1#, it can be seen that when the amount of activated carbon is reduced, the adsorption amount of water-soluble pigments decreases, so the residual amount of water-soluble pigments increases, causing the chromaticity of aconitic acid ester to increase and the purity to decrease.

[0191] According to the comparison between aconitic acid mixed esters 19#-20# and aconitic acid mixed ester 1#, it can be seen that the decolorization temperature of the decolorizing agent affects the decolorization effect on water-soluble pigments. The higher the temperature, the more violent the Brownian motion of the molecules, and the more difficult it is for the decolorizing agent to adsorb the pigment, which leads to a decrease in the removal rate of water-soluble pigment impurities. The lower the temperature, the lower the adsorption capacity of the decolorizing agent for water-soluble pigments. In addition, the high viscosity of aconitic acid ester is not conducive to the uniform dispersion of the decolorizing agent, which will also lead to a decrease in the removal rate of water-soluble pigments, and then the purity of aconitic acid ester decreases and the chromaticity increases.

[0192] According to the comparison between aconitic acid mixed ester 21# and aconitic acid mixed ester 1#, it can be seen that the shorter the decolorization time of the decolorizing agent, the worse the decolorization effect on the water-soluble pigment, so that the chromaticity of aconitic acid ester increases and the purity decreases.

[0193] According to the comparison between aconitic acid mixed esters 22#-23# and aconitic acid mixed ester 1#, it can be seen that the type of decolorizing agent and the parameters of activated carbon will affect the removal effect of water-soluble pigments, thereby affecting the purity and chromaticity of aconitic acid ester products.

[0194] According to the comparison between aconitic acid mixed ester 24# and aconitic acid mixed ester 1#, it can be seen that the increase in esterification temperature causes the polysaccharide to undergo caramelization reaction. Under the same decolorization conditions, the contents of both types of pigments in the final aconitic acid ester increase, the product pigment increases and the purity decreases; and the monosaccharides produced by the decomposition of polysaccharides will compete with alcohols and aconitic acid for the esterification reaction, resulting in a decrease in the yield of aconitic acid ester and the triester conversion rate.

[0195] According to the comparison between aconitic acid mixed ester 25# and aconitic acid mixed ester 1#, it can be seen that the increase in neutralization temperature causes the product to be hydrolyzed in an alkaline environment, resulting in insufficient purity of the obtained product. The reduction in purity increases the relative content of pigments in the product, which in turn affects the one-step decolorization and two-step decolorization processes, resulting in an increase in the residual amount of fat-soluble pigments and water-soluble pigments, an increase in the chromaticity of aconitic acid esters and a decrease in purity, and the loss due to high-temperature hydrolysis causes a decrease in the yield of aconitic acid esters.

[0196] According to the comparison of aconitic acid mixed esters D1-D3# and aconitic acid mixed esters 1#, it can be seen that the aconitic acid mixed esters obtained without decolorization treatment have high contents of water-soluble pigments and fat-soluble pigments, the chromaticity of the product is greater than 500, and the purity is reduced. When the water-soluble pigments are removed first and then the fat-soluble pigments are removed, or when the two types of pigments are removed simultaneously, not only will the preparation processing process be increased, but also the removal effect of the two types of pigments will be affected, thereby resulting in an increase in the chromaticity of the aconitic acid ester and a decrease in purity. When the fat-soluble pigments and water-soluble pigments are removed at the same time, the activated carbon will agglomerate in the aqueous phase and be distributed in the organic phase. The decolorization effect of the two pigments of the product is poor, and the yield will decrease due to the agglomeration of the activated carbon.

[0197] Example 2

[0198] The present embodiment relates to a composite material containing aconitic acid mixed ester and a preparation method thereof. The composite material comprises: 100 parts of PVC resin (K value is 60, polydispersity index is 4), 30 parts of plasticizer, 2 parts of oxidized polyethylene wax, and 5 parts of octyltin maleate. The above raw materials are mixed at 60° C. for 40 minutes using a high-speed mixer, then mixed at 155° C. for 15 minutes in a two-roll open mill, and finally placed in a flat vulcanizer and vulcanized at 165° C. for 15 minutes.

[0199] The above-mentioned plasticizer is selected from the mixed ester of aconitic acid prepared in Example 1 to prepare composite materials according to the above-mentioned weight ratio and preparation method. At the same time, dioctyl phthalate, tributyl citrate, tributyl aconitate and triisooctyl aconitate are selected as plasticizers to prepare composite materials according to the above-mentioned weight ratio and preparation method. The performance of the above-mentioned composite materials is tested. The results are shown in Tables 2 and 3. The test method is as follows:

[0200] 1. Hardness: According to GB / T531-2008 "Indentation hardness test method, Shore hardness tester method" standard, make specimens and test them. Select 3 points for each group of specimens, measure each point once, and take the median value.

[0201] 2.100% tensile stress, elongation at break, elastic modulus: in accordance with GB / T1040-2006 "Plastic Tensile Properties Test", the stretching speed is 50mm / min, the temperature is 25℃.

[0202] 3. Compatibility: The water price method is used for testing. Since water molecules are polar, the compatibility of plasticizers with water can characterize the compatibility of plasticizers with polar materials (PVC, PLA and nitrile rubber). When a certain plasticizer has good compatibility with water, it has good compatibility with PVC, and vice versa. In the experiment, 2.5g of plasticizer and 25g of acetone were added to a beaker, and titrated with a burette filled with deionized water, stirring while titrating until turbidity appeared, and the volume of deionized water consumed was recorded.

[0203] 4. Glass transition temperature (T g ): The glass transition temperature was tested by a dynamic mechanical analyzer. The test conditions were: nitrogen as the carrier gas, the test temperature range was -40 to 80°C, the heating rate was 3°C / min, and the frequency was 1 Hz.

[0204] 5. Volatilization loss rate: The test is carried out in accordance with HG / T 4458-2012 "Determination of plasticizer loss in plastics - Activated carbon method", the test temperature is 70°C, and the test time is 24h.

[0205] 6. Water extraction rate: The test is carried out in accordance with the standard "ISO 175-2011 Plastics - Experimental method for determination of the effects of immersion of liquid chemicals". The test temperature is room temperature, the test time is 72h, and the extraction solvent is deionized water.

[0206] 7. Ethanol extraction rate: The test is carried out in accordance with the standard "ISO 175-2011 Plastics - Experimental method for determination of the effects of immersion of liquid chemicals". The test temperature is room temperature, the test time is 72h, and the extraction solvent is ethanol.

[0207] 8.Petroleum ether extraction rate: The test is carried out in accordance with the standard "ISO 175-2011 Plastics - Experimental method for determination of the effects of immersion of liquid chemicals". The test temperature is room temperature, the test time is 72h, and the extraction solvent is petroleum ether.

[0208] 9. Migration rate: The test is conducted in accordance with HG / T 4458-2012 “Determination of Migration of Plasticizers in Plastics”. The test temperature is 50°C and the test time is 48 hours. The absorbent sheet is made of polyethylene (PE) without additives and standard natural rubber (NR).

[0209] Table 2

[0210]

[0211]

[0212] Table 3

[0213]

[0214]

[0215]

[0216] According to the contents of Table 2 and Table 3, aconitic acid mixed esters can better balance plasticizing performance and stability performance, although not as efficient as short-chain esters (such as tributyl aconitate), and not as long-term stable as long-chain aconitate (such as tri-isooctyl aconitate), the products plasticized by aconitic acid mixed esters can adapt to more complex external environments, and can play both effective plasticizing and comprehensive stability under different environments. The structure of the above-mentioned aconitic acid mixed esters can affect its plasticizing performance to composite materials and the stability of the aconitic acid mixed esters themselves in the composite materials, and the content of water-soluble pigments, the content of fat-soluble pigments, purity and chromaticity in the above-mentioned aconitic acid mixed esters will affect the mechanical properties of the composite materials, and will also affect the volatility resistance, extraction resistance and migration resistance of the aconitic acid mixed esters.

[0217] The above is only the embodiment of the present application, and the protection scope of the present application is not limited by these specific embodiments, but is determined by the claims of the present application. For those skilled in the art, the present application can have various changes and variations. Any modification, equivalent replacement, improvement, etc. made within the technical ideas and principles of the present application should be included in the protection scope of the present application.

Claims

1. A mixed ester of aconitic acid, characterized in that: The structural formula of the aconitic acid mixed ester is as follows: Wherein, R1, R2, and R3 are independently selected from an alkyl group containing 1 to 5 carbon atoms, an alkyl group containing 6 or more carbon atoms, an alkyl group containing 1 to 5 carbon atoms and substituted by chlorine atoms, or an alkyl group containing an aromatic group, and at least two of R1, R2, and R3 are different.

2. The method for preparing the mixed esters of aconitic acid according to claim 1, characterized in that: The steps include: S1: mixing the aconitic acid obtained by fermentation with alcohols, and performing an esterification reaction under a catalyst to obtain a mixed solution containing aconitic acid ester; S2: neutralizing the mixed solution containing aconitate with an alkali solution, separating the liquids to obtain an organic phase A, then bleaching and decolorizing the organic phase A, washing, and separating the liquids to obtain an organic phase B; S3: performing a desolventizing treatment on the organic phase B to obtain a purified product; S4: adding a decolorizing agent to the purified product for adsorption decolorization, and filtering to obtain the aconitic acid mixed ester; The alcohol is selected from at least two of an alkyl alcohol having 1 to 5 carbon atoms, an alkyl alcohol having 6 or more carbon atoms, an alkyl alcohol having 2 to 5 carbon atoms and substituted by chlorine atoms, and an alkyl alcohol containing an aromatic group.

3. The preparation method according to claim 2, characterized in that: In step S1, aconitic acid and alcohols are mixed in a molar ratio of 1:(3-9), a catalyst is added, and an esterification reaction is carried out at 75-145° C. for 2-8 hours to obtain a mixed solution containing aconitic acid ester.

4. The preparation method according to claim 2, characterized in that: In step S2, the solute of the alkali solution is at least one of NaOH, NaHCO3 and Na2CO3, and the mass fraction of the solute in the alkali solution is 5-25%.

5. The preparation method according to claim 2, characterized in that: In step S2, hydrogen peroxide is used for bleaching and decolorization. The concentration of the hydrogen peroxide is 33-40%, and the weight of the hydrogen peroxide accounts for 1-5% of the weight of the organic phase A.

6. The preparation method according to claim 2, characterized in that: In step S3, the desolventizing temperature is 40-100°C, and the vacuum degree is 0.01 mbar to 100 mbar.

7. The preparation method according to claim 8, characterized in that: In step S4, the decolorizing agent is selected from at least one of activated carbon, diatomaceous earth, kaolin, basic alumina, and neutral alumina.

8. A composite material containing the mixed ester of aconitic acid according to claim 1, characterized in that: include: 100-120 parts of PVC resin, 5-90 parts of aconitic acid mixed esters, 0.5-10 parts of lubricant, 2-10 parts of stabilizer.

9. The composite material according to claim 8, characterized in that The K value of the PVC resin is 55-77, and the polydispersity index is 3-5.

10. The composite material according to claim 8, characterized in that The lubricant is selected from at least one of oxidized polyethylene wax, glyceryl stearate, ethylene bisstearamide synthetic wax, paraffin wax and polyethylene wax, preferably oxidized polyethylene wax; The stabilizer is selected from at least one of an organic tin heat stabilizer, dibutyltin laurate, dibutyl / octyltin sulfate, octyltin maleate, and methyltin mercaptan, preferably octyltin maleate.

Citation Information

Patent Citations

  • Aconitate polyvinyl chloride plasticizer, and preparation method and application thereof

    CN113817223A

  • Aconitate-based plasticizer composition and resin composition comprising same

    WO2023075475A1

Cited By

  • Electric car cable sheath material and preparation method thereof

    CN120025640A

  • A trolley cable jacket material and method of making the same

    CN120025640B

  • Bio-based trans-aconitate, preparation method therefor and use thereof

    EP4715056A1

  • Bio-based trans-aconitate, preparation method therefor and use thereof

    WO2024235233A1