UV curing ink and preparation method thereof

By using silica-coated metal oxide particles and silver-cubous oxide-laden carboxylated chitosan composite powder in UV ink, the problem of insufficient adhesion and antibacterial properties of UV ink is solved, and high adhesion is achieved , water resistance, salt resistance and long-lasting antibacterial properties are improved, while ensuring the environmental protection of the process.

CN118994965AActive Publication Date: 2024-11-22XIAMEN OUHUA IND
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411243347.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-05
Publication Date
2024-11-22
Estimated Expiration
2044-09-05

AI Technical Summary

Technical Problem

The low adhesion and insufficient antibacterial properties of UV inks limit their application in the printing field.

Method used

Silica-coated metal oxide particles were prepared by microemulsion method, and combined with silver-cubous oxide-laden carboxylated chitosan composite powder to improve the adhesion and antibacterial properties of the ink.

Benefits of technology

It significantly improves the curing speed, adhesion, water resistance and salt resistance of UV curing ink, while giving it a long-lasting antibacterial performance. The process is completely free of toxic volatile organic solvents, which has the advantages of green and environmental protection.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005029917270000071
    Figure BDA0005029917270000071
  • Figure BDA0005029917270000081
    Figure BDA0005029917270000081
Patent Text Reader

Abstract

The preparation method comprises the following steps: mixing an emulsifier with a polar organic solvent, then adding a non-polar organic solvent, heating and stirring uniformly, adding a metal oxide particle dispersion liquid into the obtained mixture, and stirring uniformly to obtain the UV-cured ink. Fully stirring and reacting to obtain microemulsion containing metal oxide particles; adding a silicon source precursor into the obtained microemulsion, and continuously heating and reacting to obtain metal oxide particles coated with silicon dioxide; adding the obtained silicon dioxide coated metal oxide particles into a monomer to prepare a dispersion system; and adding the prepolymer, the photoinitiator, the pigment, the auxiliary agent, the defoaming agent, the antibacterial agent and the filler into the dispersion system, stirring and pre-dispersing until no solid powder exists in the system, and then feeding into a sand mill for grinding and dispersing to obtain the UV curing ink. The UV curing ink provided by the invention not only has excellent mechanical properties, but also has the advantages of high curing speed, excellent antibacterial property, good water resistance and salt resistance and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of ink materials, and in particular relates to a UV curing ink and a preparation method thereof. Background Art

[0002] UV ink refers to an ink that uses ultraviolet light of different wavelengths and energies to polymerize the monomers in the ink binder into polymers to form a film and dry. Compared with traditional inks, UV inks are completely different in terms of both curing mechanism and curing method: specifically, UV inks must be exposed to ultraviolet light before they can be cured, so the curing speed is very fast; while traditional inks are generally cured by penetration drying, volatile drying or oxidative film drying, and usually require natural air drying or heating drying to cure, so the curing speed is very fast (Cao Zhengmin, Wang Xiaomin, Jiao Liyong. UV ink composition and curing influencing factors [J]. Mechanical and Electrical Information, 2005 (2): 19-20). In addition, traditional inks also contain 30%-70% toxic organic solvents, which have adverse effects on the health of operators and the surrounding environment during the printing process. UV inks replace the solvents in traditional inks with diluent monomers that participate in the photocuring reaction, so that there is basically no solvent volatilization and emission after the film layer is cured, which fully meets the requirements of low-carbon environmental protection; therefore, it can be said that UV curing ink is an energy-saving and environmentally friendly ink that came into being under the call of low-carbon environmental protection policies.

[0003] At present, the application of UV ink has covered all printing fields, especially in food, tobacco, wine, cosmetics and electronic products and other medium and high-end printing materials. This is because UV ink containing luminescent agent can usually produce a unique visual effect after light curing, which looks elegant, solemn and luxurious. However, in the application of UV ink, low adhesion has always been one of the important factors restricting its development (Jia, Xiaoxue; Huang, Beiqing; Wei, Xianfu; et al. Influence of monomer on the performance of UV waterless offset ink [J]. Advanced Materials Research, 2011, 174: 425-428). In addition, UV ink with antibacterial properties is also relatively rare on the market. Therefore, it is very promising to develop a UV ink with strong adhesion and antibacterial properties. Summary of the invention

[0004] The object of the present invention is to provide a UV curing ink and a preparation method thereof.

[0005] In order to achieve the above object, the solution of the present invention is:

[0006] A method for preparing UV curable ink comprises the following steps:

[0007] (1) mixing an emulsifier with a polar organic solvent, then adding a non-polar organic solvent and heating and stirring the mixture, adding a metal oxide particle dispersion to the mixture, stirring and reacting the mixture sufficiently to obtain a microemulsion containing metal oxide particles; adding a silicon source precursor to the microemulsion, continuing to heat and react, and obtaining silicon dioxide-coated metal oxide particles;

[0008] (2) adding the silicon dioxide-coated metal oxide particles obtained in step (1) to the monomer and stirring the mixture to obtain a dispersion containing the silicon dioxide-coated metal oxide particles;

[0009] (3) Add prepolymer, photoinitiator, pigment, additive, defoamer, antibacterial agent and filler to the dispersion containing silica-coated metal oxide particles obtained in step (2), stir and pre-disperse until there is no solid powder in the system, and then feed into a sand mill for grinding and dispersion to obtain the UV curing ink.

[0010] Preferably, the emulsifier described in step (1) is one of fatty alcohol polyoxyethylene ether, polyoxyethylene stearate or hexadecylphenol polyoxyethylene ether.

[0011] Preferably, the metal oxide in step (1) is composed of one or a combination of two or more of zinc oxide, cerium dioxide, titanium dioxide, magnesium oxide or aluminum oxide.

[0012] Preferably, the silicon source precursor in step (1) is one of methyl orthosilicate, ethyl orthosilicate or isopropyl orthosilicate.

[0013] Preferably, the monomer described in step (2) is one of lauryl acrylate, tripropylene glycol diacrylate, neopentyl glycol diacrylate or trimethylolpropane triacrylate.

[0014] Preferably, the prepolymer in step (3) is composed of one or a combination of two or more of epoxy acrylate, polyurethane acrylate or polyester acrylate.

[0015] Preferably, the photoinitiator described in step (3) is one of 2-hydroxy-2-methyl-1-phenylpropanone, 1-hydroxycyclohexyl phenyl ketone, 2-methyl-2-(4-morpholinyl)-1-[4-(methylthio)phenyl]-1-propanone, 2,4,6-trimethylbenzoyl-diphenylphosphine oxide, 2,4,6-trimethylbenzoylphenylphosphonic acid ethyl ester, 2-dimethylamino-2-benzyl-1-[4-(4-morpholinyl)phenyl]-1-butanone, 2-hydroxy-2-methyl-1-[4-(2-hydroxyethoxy)phenyl]-1-propanone or methyl benzoylformate.

[0016] Preferably, the grinding and dispersing speed in step (3) is 1000-2000 r / min, and the grinding and dispersing time is 0.5-2 h.

[0017] In the UV curing ink prepared by the above-mentioned method for preparing UV curing ink, the mass ratio of the metal oxide particles coated with silicon dioxide is 1.0-2.5%; and the mass ratio of the antibacterial agent is 0.1%-1.0%.

[0018] The specific principle of the preparation method of UV curable ink provided by the present invention is as follows:

[0019] The preparation method of UV curable ink provided by the present invention first prepares a microemulsion containing metal oxide particles by using a microemulsion method, and then adds a silicon source precursor to prepare silicon dioxide-coated metal oxide particles by multiphase reaction; a series of different silicon dioxide-coated metal oxide particles are obtained by coating with different metal oxide particles, and then a series of UV curable inks with different properties are prepared; this application specifically examines in detail the effects of different silicon dioxide-coated metal oxide particles on the performance of UV curable inks, especially on the curing speed and adhesion. Specifically, silicon dioxide-coated metal oxide particles have strong ultraviolet light absorption ability, and adding them to UV curable ink can effectively promote the ink's absorption of ultraviolet light, thereby increasing the drying speed of the ink; and different silicon dioxide-coated metal oxide particles have different ultraviolet light absorption abilities. In addition, we also added silver-cuprous oxide-loaded carboxylated chitosan composite powder, a substance with antibacterial properties, into the UV-curable ink, so that the antibacterial agent can continue to exert its antibacterial properties in the prepared ink, which not only makes the ink have excellent antibacterial properties but also further improves the mechanical properties of the prepared ink.

[0020] Compared with the existing UV curable ink and its preparation method, the gain effect of the present invention is as follows:

[0021] 1. The preparation method of UV curable ink provided by the present invention can effectively improve the curing speed and adhesion of the prepared ink by using silica-coated metal oxide particles. However, the adhesion, water resistance and salt resistance of the obtained ink can be further improved by compounding the prepolymer polyester acrylate and polyurethane acrylate.

[0022] 2. The preparation method of the UV curable ink provided by the present invention uses silver-cuprous oxide loaded carboxylated chitosan composite powder to make the prepared ink have long-lasting and excellent antibacterial properties.

[0023] 3. The preparation method of the UV curable ink provided by the present invention does not use any toxic volatile organic solvents throughout the process, and has the advantage of being green and environmentally friendly. DETAILED DESCRIPTION

[0024] The present invention is further described in detail below in conjunction with the embodiments. It should also be understood that the following embodiments are only used to further illustrate the present invention and cannot be construed as limiting the scope of protection of the present invention. The specific quality, reaction time and temperature, process parameters, etc. in the examples are only examples within the appropriate ranges. Some non-essential improvements and adjustments made by those skilled in the art according to the above content of the present invention all belong to the scope of protection of the present invention.

[0025] All reagents used were commercial reagents unless otherwise specified and were not further purified before use.

[0026] The pigments used in the embodiments of the present invention are all commercial reagents, and the added pigments and fillers can be adjusted according to the specific color requirements. For example, phthalocyanine blue pigment can be used for blue, carbon black pigment can be used for black, and carbon dioxide powder can be used for white.

[0027] The preparation method of the antibacterial agent silver-cuprous oxide loaded carboxylated chitosan composite powder used in the embodiment of the present invention is as follows: 15g of chitosan is dissolved in 1.25L of 9% acetic acid solution, and stirred for reaction for 2.5h, and then a mixture powder consisting of 15g of coconut shell charcoal and 15g of diatomaceous earth is added, and stirring is continued for 2h. After filtering, the obtained solid is washed with deionized water until the pH value of the collected eluate is close to 7, and the washed solid is dried at 110°C to prepare a carboxylated chitosan composite carrier; the carboxylated chitosan composite carrier prepared in the step is added to 200ml of acetic acid solution with a mass concentration of 5%, and then 80ml of copper nitrate solution with a molar concentration of 50mmol / L is slowly dripped and stirred evenly, and stirring is continued, 20ml of ascorbic acid solution with a mass concentration of 10% is added, and the pH value is adjusted to 40% with dilute ammonia water. 6.5, the obtained mixture is hydrothermally reacted at 200° C. for 2 h, and after cooling, the solution is centrifuged, washed with 250 ml of deionized water for 3 times, washed with 250 ml of anhydrous ethanol for 3 times, and the obtained solid is collected after freeze-drying to obtain a cuprous oxide-loaded carboxylated chitosan composite material; the obtained cuprous oxide-loaded carboxylated chitosan composite material, 15 ml of an ascorbic acid solution with a mass concentration of 10%, 0.6 g of sodium citrate and 1.1 g of polyvinyl pyrrolidone (average relative molecular mass of 40000) are added to 500 ml of deionized water and stirred evenly, and then 40 ml of a silver nitrate solution with a molar concentration of 50 mmol / L is slowly dripped into it, and the obtained mixture is placed in a microwave reactor for microwave reaction at 100° C. for 45 min, and filtered to obtain a silver-cuprous oxide-loaded carboxylated chitosan composite powder.

[0028] Embodiment 1:

[0029] The preparation steps of UV curing ink are as follows:

[0030] (1) 18 g of emulsifier polyoxyethylene stearate and 16 g of n-hexanol were mixed, and then 13 g of cyclohexane was added, heated to 32° C. and stirred evenly. 10 mL of ZnO dispersion was added to the obtained mixture (1.0 g of ZnO was added to 10 mL of deionized water and ultrasonically dispersed for 5 min to obtain a ZnO dispersion). The reaction temperature was continued to be precisely controlled at 32° C. and the reaction was stirred at constant temperature for 2 h to obtain a ZnO microemulsion. Then 0.3 g of tetraethyl orthosilicate was added and the stirring was continued. After stirring evenly, the obtained mixture was transferred to an ultrasonic reactor and ultrasonically oscillated at 30° C. for 35 min. After centrifugation, the obtained solid was washed three times with 50 ml of 60% by volume ethanol aqueous solution. The obtained solid was placed in a vacuum drying oven and dried at 65° C. for 5 h. After that, it was placed in a muffle furnace and calcined at 400° C. for 3 h to obtain silicon dioxide-coated zinc oxide particles.

[0031] (2) adding 1 g of the silicon dioxide-coated zinc oxide particles prepared in step (1) to 45 g of neopentyl glycol diacrylate and stirring the mixture to obtain a dispersion containing silicon dioxide-coated zinc oxide particles;

[0032] (3) Add 40 g of epoxy acrylate, 2 g of 2-hydroxy-2-methyl-1-phenylacetone, 10 g of carbon black, 0.5 g of silicone oil, 0.5 g of CI-2212 defoamer, 0.1 g of silver-cuprous oxide-loaded carboxylated chitosan composite powder and 0.9 g of calcium carbonate to the dispersion containing the silicon dioxide-coated zinc oxide particles obtained in step (2), stir and pre-disperse until there is no solid powder in the system, and then send it into a sand mill for grinding and dispersion, set the speed of the sand mill to 1400 r / min, the time to 30 min, and finally filter with a 300-mesh gauze to obtain the UV-curable ink; the obtained UV-curable ink is recorded as NPGDA-EA-ZnO@SiO2-1.

[0033] The curing time test method of the prepared UV curing ink is as follows:

[0034] Treatment of printing substrate: Cut the tinplate sheet into a test plate with a size of 50mm×120mm×0.3mm, wipe the surface clean with alcohol and dry it under an infrared lamp, and print the prepared UV curing ink on the freshly treated tinplate sheet using an IGT printability tester, with 0.1ml of ink used each time.

[0035] Ink curing: Place the tinplate printed with ink in a UV curing box, turn on the 2KW strong light button to expose, and press the stopwatch to start timing. This application uses the time required for complete curing as the curing time; the finger scratching method is used to indicate whether it is completely cured, that is, use the fingernail to lightly scratch the cured film layer, and no ink falling off or scratching indicates complete curing. The test results are shown in Table 1.

[0036] The prepared UV curable ink 1NPGDA-EA-ZnO@SiO2-1 was made into a coating and then the performance was tested; wherein, the NPGDA-EA-ZnO@SiO2-1 coating was prepared according to the method provided in GB / T1727-1992, and the specific steps are as follows: the tinplate sheet conforming to the GB / T2520-2017 specification was cut into a test plate with a size of 50mm×120mm×0.3mm, and the test plate was cleaned according to the provisions of GB9271-1988 for the test plate. The NPGDA-EA-ZnO@SiO2-1 material was evenly applied on the tinplate test plate with a scraper, and then cured completely with ultraviolet light, and its various properties were tested. The hardness, adhesion, water resistance and salt spray corrosion resistance of the coating film were measured according to the corresponding national standards, as follows: the hardness was measured according to the national standard GB / T1730-93, the adhesion was measured according to the national standard GB / T1720-79, the resistance to distilled water (40°C immersion) / h was measured according to the national standard GB / T5209-85, and the resistance to 3% NaCl (40°C) / h was measured according to the national standard GB / T1763-79. The results are shown in Table 1.

[0037] The antibacterial properties of the prepared UV curable ink coating were tested by the film sticking method according to the implementation standard QB / T 2591-2003 (QB / T2591-2003, Test methods and antibacterial effects of antibacterial plastics [S]. Beijing: National Development and Reform Commission of the People's Republic of China, 2003.), and the antibacterial rate of the antibacterial plastic after contact with the test bacteria for 24 hours was investigated. The total number of colonies was determined according to GB / T 4789.2-2016 (GB / T 4789.2-2016, Determination of the total number of colonies in food microbiology [S]. Beijing: National Health and Family Planning Commission of the People's Republic of China, State Food and Drug Administration, 2016.), and the antibacterial rate was calculated according to the following formula:

[0038] R%=(BA) / B×100%

[0039] Wherein: R: antibacterial rate, %; A: average number of recovered colonies of Ag / NH2-MgO / SiO2-EP coating samples after culturing for 24 hours; B: average number of recovered colonies of blank control samples after culturing for 24 hours, the blank control sample is a coating made of pure EP and curing agent polyamide resin (mass ratio is 1:1) according to the same method; the results are shown in Table 1.

[0040] Embodiment 2:

[0041] The preparation of UV curable ink refers to Example 1, except that the metal oxide ZnO used in step (1) is replaced by CeO2, and the amount of CeO2 used is 1 g; the remaining steps are the same as Example 1, and the obtained UV curable ink is recorded as NPGDA-EA-CeO2@SiO2-2.

[0042] The preparation and performance characterization of NPGDA-EA-CeO2@SiO2-2 coating are the same as those in Example 1; the results are shown in Table 1.

[0043] Embodiment 3:

[0044] The preparation of UV curable ink refers to Example 1, except that the metal oxide ZnO used in step (1) is replaced by TiO2, and the amount of TiO2 used is 1 g; the remaining steps are the same as Example 1, and the obtained UV curable ink is recorded as NPGDA-EA-TiO2@SiO2-3.

[0045] The preparation and performance characterization of NPGDA-EA-TiO2@SiO2-3 coating are the same as those in Example 1; the results are shown in Table 1.

[0046] Embodiment 4:

[0047] The preparation of UV curable ink is referred to Example 1, except that the metal oxide ZnO used in step (1) is replaced by MgO, and the amount of MgO used is 1 g; the remaining steps are the same as Example 1, and the obtained UV curable ink is recorded as NPGDA-EA-MgO@SiO2-4.

[0048] The preparation and performance characterization of NPGDA-EA-MgO@SiO2-4 coating are the same as those in Example 1; the results are shown in Table 1.

[0049] Embodiment 5:

[0050] The preparation of UV curable ink refers to Example 1, except that the metal oxide ZnO used in step (1) is replaced by Al2O3, and the amount of Al2O3 used is 1 g; the remaining steps are the same as Example 1, and the obtained UV curable ink is recorded as NPGDA-EA-Al2O3@SiO2-5.

[0051] The preparation and performance characterization of NPGDA-EA-Al2O3@SiO2-5 coating are the same as those in Example 1; the results are shown in Table 1.

[0052] Embodiment 6:

[0053] The preparation of UV curable ink refers to Example 1, except that the metal oxide ZnO used in step (1) is replaced by a mixed powder composed of TiO2 and MgO, the amount of TiO2 used is 0.5g, and the amount of MgO used is 0.5g; the remaining steps are the same as Example 1, and the obtained UV curable ink is recorded as NPGDA-EA-MgO-TiO2@SiO2-6.

[0054] The preparation and performance characterization of NPGDA-EA-MgO-TiO2@SiO2-6 coating are the same as those in Example 1; the results are shown in Table 1.

[0055] Table 1 Effect of different oxides on the performance of UV curing inks

[0056] Example Curing time hardness Adhesion Water resistance Salt tolerance Antibacterial rate A Antibacterial rate B 1 9s 0.85 Level 2 144h 144h 89.2% 93.0% 2 6s 0.84 Level 2 144h 144h 82.3% 87.1% 3 4s 0.88 Level 1 144h 144h 87.9% 90.2% 4 6s 0.92 Level 1 144h 144h 88.5% 90.8% 5 13s 0.93 Level 2 144h 144h 83.7% 88.4% 6 4s 0.91 Level 1 144h 144h 89.1% 91.0%

[0057] Embodiment 7-9:

[0058] The preparation of UV curable ink is based on Example 1, except that the metal oxide ZnO used in step (1) is replaced by a mixed powder composed of TiO2 and MgO, the amount of TiO2 used is 0.5 g, and the amount of MgO used is 0.5 g; the neopentyl glycol diacrylate in step (2) is replaced by lauryl acrylate, tripropylene glycol diacrylate and trimethylolpropane triacrylate in sequence; the remaining steps are the same as in Example 1, and the preparation and performance characterization of the obtained ink coating are the same as in Example 1; the results are shown in Table 2.

[0059] Table 2 Effect of different monomers or prepolymers on the performance of UV curing inks

[0060]

[0061]

[0062] Note: Water resistance and salt resistance both refer to the time without change; antibacterial rate A refers to the antibacterial rate against Escherichia coli, and antibacterial rate B refers to the antibacterial rate against Staphylococcus aureus.

[0063] Embodiment 10-12:

[0064] The preparation of UV curable ink is based on Example 1, except that the metal oxide ZnO used in step (1) is replaced by a mixed powder composed of TiO2 and MgO, the amount of TiO2 used is 0.5 g, and the amount of MgO used is 0.5 g; the neopentyl glycol diacrylate in step (2) is replaced by trimethylolpropane triacrylate; the epoxy acrylate in step (3) is replaced by polyurethane acrylate and polyester acrylate in sequence; the remaining steps are the same as in Example 1, and the preparation and performance characterization of the obtained ink coating are the same as in Example 1; the results are shown in Table 2.

[0065] Embodiment 13:

[0066] The preparation of UV curable ink is based on Example 1, except that the metal oxide ZnO used in step (1) is replaced by a mixed powder composed of TiO2 and MgO, the amount of TiO2 is 0.5 g, and the amount of MgO is 0.5 g; the neopentyl glycol diacrylate in step (2) is replaced by trimethylolpropane triacrylate; the epoxy acrylate in step (3) is replaced by a composite prepolymer composed of epoxy acrylate, polyurethane acrylate and polyester acrylate in a mass ratio of 1:1:2; the remaining steps are the same as in Example 1, and the preparation and performance characterization of the obtained ink coating are the same as in Example 1; the results are shown in Table 2.

[0067] Embodiment 14:

[0068] The preparation of UV curable ink is based on Example 1, except that the metal oxide ZnO used in step (1) is replaced by a mixed powder composed of TiO2 and MgO, the amount of TiO2 is 0.5 g, and the amount of MgO is 0.5 g; the neopentyl glycol diacrylate in step (2) is replaced by trimethylolpropane triacrylate; the epoxy acrylate in step (3) is replaced by a composite prepolymer composed of epoxy acrylate, polyurethane acrylate and polyester acrylate in a mass ratio of 1:1:2; the amount of the silver-cuprous oxide loaded carboxylated chitosan composite powder in step (3) is changed to 0 g; the remaining steps are the same as in Example 1, and the preparation and performance characterization of the obtained ink coating are the same as in Example 1; the results are shown in Table 2.

Claims

1. A method for preparing a UV curable ink, characterized in that: The steps include: (1) mixing an emulsifier with a polar organic solvent, then adding a non-polar organic solvent and heating and stirring the mixture, adding a metal oxide particle dispersion to the mixture, stirring and reacting the mixture sufficiently to obtain a microemulsion containing metal oxide particles; adding a silicon source precursor to the microemulsion, continuing to heat and react, and obtaining silicon dioxide-coated metal oxide particles; (2) adding the silicon dioxide-coated metal oxide particles obtained in step (1) to the monomer and stirring the mixture to obtain a dispersion containing the silicon dioxide-coated metal oxide particles; (3) Add prepolymer, photoinitiator, pigment, additive, defoamer, antibacterial agent and filler to the dispersion containing silica-coated metal oxide particles obtained in step (2), stir and pre-disperse until there is no solid powder in the system, and then feed into a sand mill for grinding and dispersion to obtain the UV curing ink.

2. The method for preparing UV curable ink according to claim 1, characterized in that: The emulsifier described in step (1) is one of fatty alcohol polyoxyethylene ether, polyoxyethylene stearate or hexadecylphenol polyoxyethylene ether.

3. The method for preparing UV curable ink according to claim 1, characterized in that: The metal oxide described in step (1) is composed of one or a combination of two or more of zinc oxide, cerium dioxide, titanium dioxide, magnesium oxide or aluminum oxide.

4. The method for preparing UV curable ink according to claim 1, characterized in that: The silicon source precursor described in step (1) is one of methyl orthosilicate, ethyl orthosilicate or isopropyl orthosilicate.

5. The method for preparing UV curable ink according to claim 1, characterized in that: The monomer described in step (2) is one of lauryl acrylate, tripropylene glycol diacrylate, neopentyl glycol diacrylate or trimethylolpropane triacrylate.

6. The method for preparing UV curable ink according to claim 1, characterized in that: The prepolymer described in step (3) is composed of one or a combination of two or more of epoxy acrylate, polyurethane acrylate or polyester acrylate.

7. The method for preparing UV curable ink according to claim 1, characterized in that: The photoinitiator described in step (3) is one of 2-hydroxy-2-methyl-1-phenylpropanone, 1-hydroxycyclohexyl phenyl ketone, 2-methyl-2-(4-morpholinyl)-1-[4-(methylthio)phenyl]-1-propanone, 2,4,6-trimethylbenzoyl-diphenylphosphine oxide, 2,4,6-trimethylbenzoylphenylphosphonic acid ethyl ester, 2-dimethylamino-2-benzyl-1-[4-(4-morpholinyl)phenyl]-1-butanone, 2-hydroxy-2-methyl-1-[4-(2-hydroxyethoxy)phenyl]-1-propanone or methyl benzoylformate.

8. The method for preparing UV curable ink according to claim 1, characterized in that: The grinding and dispersing speed in step (3) is 1000-2000 r / min, and the grinding and dispersing time is 0.5-2 h.

9. A UV curable ink obtained by the method for preparing a UV curable ink according to any one of claims 1 to 9, characterized in that: The mass ratio of the metal oxide particles coated with silicon dioxide is 1.0-2.5%; the mass ratio of the antibacterial agent is 0.1-1.0%.

Citation Information

Patent Citations

  • UV (ultraviolet)-LED curing ink and preparation method and application thereof

    CN105885524A

  • Odor-removing formaldehyde-removing paint as well as preparation method and application thereof

    CN114591672A

  • Anti-aging fluorescent carbon quantum dot antibacterial functional film

    CN117487226A