Insulating paint applied to high-rotating-speed new energy motor stator and preparation method of insulating paint
By using the combination of polyesterimine resin, hydroxyacrylic resin, modified aliphatic epoxy resin and polytetrafluoroethylene dispersion in the insulating paint of new energy motors, the polyimide insulating paint was solved in the high-speed motor. The problem of insufficient heat resistance and bonding stability has achieved efficient improvement in insulation performance and shortened curing time.
Patent Information
- Application Number
- CN202411193258.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-28
- Publication Date
- 2024-11-26
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing polyimide insulating paints are insufficient in high-speed new energy motors, and have low solid content and large proportion of organic solvents, which affects the insulation performance.
Modified aliphatic epoxy resin and polyhydroxy silicon oxygen by using a combination of polyesterimine resin, hydroxyacrylic resin, aliphatic epoxy resin, polytetrafluoroethylene dispersion, nanoinorganic filler, curing agent and leveling agent. The reaction of alkyl can optimize the resin structure and curing reaction, and improve the adhesive properties, high temperature resistance and mechanical properties of insulating paint.
It significantly improves the adhesion, high temperature resistance, thermal conductivity, aging resistance and insulation properties of the insulating paint, shortens the curing time, reduces the amount of diluent, and enhances the mechanical properties and service life of the insulating layer.
Smart Images

Figure BDA0005015664980000051 
Figure BDA0005015664980000061 
Figure BDA0005015664980000071
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of insulating varnishes, and more specifically, to an insulating varnish for use in stators of high-speed new energy motors and a preparation method thereof. Background Art
[0002] New energy motors refer to electric motors used in new energy vehicles. They are currently mainly used in new energy vehicle fields such as pure electric vehicles, plug-in hybrid vehicles, and fuel cell vehicles.
[0003] With the development of technology, motors are developing towards high power, high speed and miniaturization, which greatly increases the heat generated by motors. New energy vehicle motors have higher requirements for the heat resistance and bonding stability of insulating paint. In order to improve the heat resistance of insulating paint, materials with good high temperature resistance are usually used as the main materials of insulating paint, such as polyimide resin. The main chain of polyimide contains imide rings, which makes the polyimide more stable, and has better high temperature resistance and aging resistance.
[0004] Existing polyimide insulating varnishes are mainly compounded with polyimide resin and volatile organic solvents such as cresol, N,N-dimethylformamide, and xylene. The solid content in the finished product is low, generally 25% to 35%, the proportion of organic solvents is large, and the bonding performance is poor. Summary of the invention
[0005] In order to improve the problem of poor compatibility between polyimide resin and epoxy resin, the present application provides an insulating varnish for use in a high-speed new energy motor stator and a preparation method thereof.
[0006] In the first aspect, the present application provides an insulating varnish for a stator of a high-speed new energy motor, which adopts the following technical solution: An insulating varnish for a high-speed new energy motor stator is prepared from the following raw materials in parts by weight: 50-70 parts of polyester imide resin liquid 40-80 parts of hydroxy acrylic resin Aliphatic epoxy resin 20-30 parts 5-9 parts of polytetrafluoroethylene dispersion 30-50 parts of nano inorganic filler 3-5 parts of curing agent 2-3 parts of leveling agent 20-30 parts of diluent.
[0007] By adopting the above technical solution, the prepared insulating varnish has good adhesion, high temperature resistance, thermal conductivity, aging resistance and insulation, and can form a good insulating layer on the stator surface. In the present application, by mixing polyester imide resin liquid, hydroxy acrylic resin, aliphatic epoxy resin and polytetrafluoroethylene dispersion liquid, only a small amount of diluent can be added to adjust the viscosity and improve the bonding performance of the insulating varnish. It is not necessary to add a large amount of diluent to dilute, and the curing time is further shortened.
[0008] During use, the motor will not always remain in the changed state, nor will it always remain in the normal temperature installation state, but will alternate between high and low temperatures irregularly, which will affect the bonding stability of the insulating paint. The aliphatic epoxy resin contains epoxy groups, which can greatly improve the adhesion performance of the insulating paint under high temperature conditions. However, after adding aliphatic epoxy resin, the stress of the insulating layer will increase, the toughness and impact resistance will decrease. During use, microcracks or potential breaking points may appear inside the insulating layer, affecting the use of the insulating paint. In this application, an appropriate amount of hydroxyl acrylic resin is added to improve the problem of increased stress and decreased impact resistance of the insulating layer after adding aliphatic epoxy resin. At the same time, an appropriate amount of nano-inorganic filler is added in this application to be used together with polyester imide resin liquid, hydroxyl acrylic resin, and aliphatic epoxy resin, which can further improve the mechanical properties and insulation properties of the insulating paint. The addition of polytetrafluoroethylene dispersion can improve the leveling and wettability of the insulating paint, make the insulating layer smoother and more uniform, reduce the generation of defects such as bubbles and pinholes, and at the same time improve the insulation performance, heat resistance and impact resistance of the insulating paint.
[0009] The curing agent can promote the curing reaction of polyesterimide resin, hydroxy acrylic resin and aliphatic epoxy resin to form an insulating layer with good adhesion, good insulation, good high temperature resistance and good aging resistance; the leveling agent can effectively reduce the surface tension of the insulating paint, making the insulating paint easier to level during the coating process, thereby forming a smoother and flatter insulating layer.
[0010] Preferably, the polyester imine resin is an unsaturated polyester resin containing an imine structure and a hydroxyl group, with a hydroxyl value of 50-100 mgKOH / g, an acid value of 5-8 mgKOH / g, and an imine content of 10-30%.
[0011] By adopting the above technical scheme, the structure, hydroxyl value, acid ester and imine content of the polyester imide resin are optimized, so that the structure of the polyester imide resin is made tighter and cured with the aliphatic epoxy resin to form a stable structure, thereby improving the electrical insulation performance, thermal stability and corrosion resistance of the insulating paint, while improving the interaction between the insulating paint and the substrate, thereby improving the adhesion of the insulating paint.
[0012] Preferably, the aliphatic epoxy resin is a modified aliphatic epoxy resin, which is prepared by the following method: under the protection of inert gas, adding an aliphatic epoxy resin and an organic solvent into a reactor and heating to 100-120°C; starting stirring when the aliphatic epoxy resin is fully dissolved, slowly adding hydroxysilane and triethylamine dropwise at a uniform speed within 1-3 hours; stirring and reacting at a constant temperature for 3-4 hours, adding a mixed solution of hydroxysilane and an initiator and continuing to stir for 3-8 hours; then cooling to 40-50°C, continuing to react with stirring for 2-3 hours, testing the content of hydroxysilane, and if the content exceeds 1%, continuing to add the initiator and continuing the reaction until the hydroxysilane content is less than 1%, thereby obtaining a modified aliphatic epoxy resin.
[0013] By adopting the above technical solution, the heat resistance and curing speed of aliphatic epoxy resin are further improved, so that the insulating paint has good bonding performance, curing speed and high temperature resistance. Aliphatic epoxy resin can improve the bonding performance of insulating paint, but the molecular structure of aliphatic epoxy resin contains a long fatty chain and the reaction activity is relatively low, which leads to a slow curing speed.
[0014] In the present application, aliphatic epoxy resin is modified by using polyhydroxysiloxane, wherein the hydroxyl groups in the hydroxysiloxane can undergo a ring-opening reaction with the epoxy groups of the epoxy resin to form stable chemical bonds, which can increase the crosslinking density and speed of the epoxy resin and shorten the curing time; at the same time, there are silicon-oxygen bonds in the hydroxysiloxane, which can improve the mechanical properties and heat resistance of the aliphatic epoxy resin, thereby improving the heat resistance, insulation and adhesion performance of the insulating paint.
[0015] Preferably, the weight parts of raw materials used to prepare the modified aliphatic epoxy resin are as follows: Aliphatic epoxy resin 20-30 parts 30-40 parts of organic solvent Hydroxysilane 6-10 parts 4-6 parts of triethylamine 2-3 parts of initiator.
[0016] By adopting the above technical scheme, the amount of raw materials used in preparing modified aliphatic epoxy resin is optimized, firstly to improve the reaction efficiency; secondly to improve the heat resistance and curing efficiency of the aliphatic epoxy resin and shorten the curing time of the insulating varnish.
[0017] Preferably, the hydroxysilane includes at least one of diphenyldihydroxysilane, dimethyldihydroxysilane, trimethylhydroxysilane, triphenylhydroxysilane, hydroxymethyldiphenylsilane and tetrahydroxysilane.
[0018] By adopting the above technical scheme, polyhydroxysiloxane can react with aliphatic epoxy resin quickly and efficiently under the action of specific temperature and initiator, the reaction efficiency is high, and the modified aliphatic epoxy resin obtained by the reaction has mechanical properties and heat resistance, and the curing time is short.
[0019] Preferably, the initiator is any one of dibutyltin dilaurate, stannous isooctanoate, zinc isooctanoate or bismuth isooctanoate.
[0020] By adopting the above technical solution, the reaction efficiency of hydroxysiloxane and aliphatic epoxy resin is further improved, the reaction time is shortened, and the production efficiency is improved.
[0021] Preferably, the solid content of the polytetrafluoroethylene dispersion is 50-60%.
[0022] By adopting the above technical solution, the solid content of the polytetrafluoroethylene dispersion is optimized, the mechanical strength of the insulating paint is further improved, a tougher and more durable insulating layer is formed, and at the same time the surface of the insulating layer is made smoother and more uniform.
[0023] Preferably, the viscosity of the hydroxy acrylic resin is 5000-12000 cps / 25° C., the hydroxy content is 10-25 mgKOH / g, and the acid value is 2-6.
[0024] By adopting the above technical solution, the viscosity and hydroxyl content of the hydroxy acrylic resin are optimized, which is beneficial to improving the problems of increased stress and decreased impact resistance of the insulating layer after adding aliphatic epoxy resin, and improving the service life of the insulating layer.
[0025] Preferably, the nano inorganic filler includes at least one of boron nitride, silicon carbide, silicon dioxide, mica powder and ceramic powder.
[0026] By adopting the above technical solution, the insulation, heat resistance and mechanical strength of the insulating layer are further improved.
[0027] In the second aspect, the present application provides a method for preparing an insulating varnish for a stator of a high-speed new energy motor, using the following technical solution: An insulating varnish for a stator of a high-speed new energy motor includes the following preparation steps: (1) heating the polyester imide resin liquid, hydroxy acrylic resin and diluent to 80-100° C., adding aliphatic epoxy resin, stirring evenly, and cooling to 45-50° C. to obtain a mixed solution A; (2) Stirring the polytetrafluoroethylene dispersion at a speed of 1000-2000 r / min, adding the inorganic nanofiller, stirring and dispersing; after the inorganic nanofiller is added, the stirring speed is adjusted to 6000-8000 r / min, and the dispersion is carried out for 0.5-1 h. During the dispersion process, the material temperature is controlled at 45-50° C. to obtain a mixed solution B; (3) Mixing the mixed liquid A and the mixed liquid B at a stirring speed of 1000-1500 r / min, adding a curing agent and a leveling agent, and stirring for 1-2 hours to obtain an insulating paint for a stator of a high-speed new energy motor.
[0028] By adopting the above technical solution, the polyester imide resin liquid, hydroxy acrylic resin, aliphatic epoxy resin, polytetrafluoroethylene dispersion and inorganic nanofiller can be fully mixed and uniform, so that the insulating paint is not stratified, and an insulating layer with a smooth surface and uniform thickness is formed during the coating process. Polytetrafluoroethylene dispersion and inorganic nanofiller are difficult to mix evenly with other resins. For this reason, the present application stirs the polytetrafluoroethylene dispersion and inorganic nanofiller at a high speed so that the two are fully mixed first, and then mixed with other resins, thereby achieving the purpose of fully mixing each raw material.
[0029] In summary, this application has the following beneficial effects: 1. The present application prepares an insulating varnish by combining polyesterimide resin liquid, hydroxyl acrylic resin, aliphatic epoxy resin, polytetrafluoroethylene dispersion, nano inorganic filler, curing agent, leveling agent and diluent, wherein the synergistic use of polyesterimide resin liquid and polytetrafluoroethylene dispersion can greatly improve the high temperature resistance of the insulating varnish; aliphatic epoxy resin and tetrafluoroethylene dispersion can greatly improve the bonding performance of the insulating varnish; hydroxyl acrylic resin is used to improve the problem of increased stress and decreased impact resistance of the insulating layer after adding aliphatic epoxy resin.
[0030] 2. The modified aliphatic epoxy resin is prepared by mixing epoxy resin, hydroxysilane, triethylamine and initiator, which can effectively improve the heat resistance and curing speed of the aliphatic epoxy resin, thereby making the insulating paint have good bonding properties. DETAILED DESCRIPTION Example
[0031] Example 1 An insulating varnish for stator of a high-speed new energy motor is prepared by the following method: (1) 500 g of polyester imide resin liquid, 400 g of hydroxy acrylic resin and a diluent were heated to 80° C., 200 g of aliphatic epoxy resin was added, the mixture was stirred evenly, and the temperature was lowered to 45° C. to obtain a mixed solution A; (2) 50 g of polytetrafluoroethylene dispersion was stirred at a speed of 1000 r / min, and 300 g of inorganic nanofiller was added and stirred and dispersed; after the inorganic nanofiller was added, the stirring speed was adjusted to 6000 r / min, and the dispersion was carried out for 0.5 h. During the dispersion process, the material temperature was controlled at 45° C. to obtain a mixed solution B; (3) Mixing the mixed solution A and the mixed solution B was stirred at a stirring speed of 1000 r / min, 30 g of a curing agent and 20 g of a leveling agent were added, and stirred for 1 h to obtain an insulating paint for a stator of a high-speed new energy motor.
[0032] The polyester imine resin is an unsaturated polyester resin containing an imine structure and a hydroxyl group, with a hydroxyl value of 50 mgKOH / g, an acid value of 5 mgKOH / g, and an imine content of 20%.
[0033] Aliphatic epoxy resin was purchased from Shandong New Kinetic Energy Chemical Co., Ltd. with model number XZ 92466 92465.
[0034] The polytetrafluoroethylene dispersion has a solid content of 50% and was purchased from Shanghai Chen Yihui Plastic Chemical Co., Ltd. The brand is American 3M.
[0035] The difference between Example 2-3 and Example 1 is that the types, amounts and parameters of the raw materials used to prepare the stator insulating paint for high-speed new energy motors are different. The specific differences are shown in Table 1: Table 1 Types, amounts and parameters of raw materials for preparing insulating varnish for stator of high-speed new energy motors in Examples 1-3 Example 4 An insulating paint for a stator of a high-speed new energy motor. The difference between this embodiment and embodiment 1 is that the aliphatic epoxy resin is a modified aliphatic epoxy resin, which is prepared by the following method: Under the protection of inert gas, add 200g of aliphatic epoxy resin and 300g of organic solvent into the reactor and heat to 100°C; When the aliphatic epoxy resin is fully dissolved, start stirring, and slowly add 50 g of hydroxysilane and 40 g of triethylamine at a uniform speed within 1 hour; after stirring and reacting at a constant temperature for 3 hours, add a mixture of 10 g of hydroxysilane and 20 g of initiator and continue stirring for 3 hours; then cool to 40°C, continue to react with stirring for 2 hours, test the content of hydroxysilane, and the hydroxysilane content is less than 1%, thereby obtaining a modified aliphatic epoxy resin.
[0036] The difference between Example 5-6 and Example 4 is that the types, amounts and parameters of some raw materials for preparing the modified aliphatic epoxy resin are different. The specific differences are shown in Table 2: Table 2 Types, amounts and parameters of raw materials for preparing modified aliphatic epoxy resins in Examples 4-6 Example 7 A stator insulating varnish for high-speed new energy motors. The difference between this embodiment and embodiment 4 is that phthalic anhydride is used instead of hydroxysilane of equal mass, and the types, amounts and experimental parameters of other raw materials are consistent with those of embodiment 4.
[0037] Example 8 A stator insulating varnish for high-speed new energy motors. The difference between this embodiment and Example 4 is that an organic solvent (tetrahydrofuran) is used instead of an equal mass of hydroxysilane, and the types, amounts and experimental parameters of the remaining raw materials are consistent with those of Example 4.
[0038] Example 9 An insulating varnish for stator of a high-speed new energy motor. The difference between this embodiment and embodiment 1 is that the content of polyester imide resin imide is 50%, and the types, amounts and experimental parameters of other raw materials are consistent with those in embodiment 1.
[0039] Example 10 A stator insulating varnish for high-speed new energy motors. The difference between this embodiment and embodiment 1 is that the hydroxyl content of the hydroxylated acrylic resin is 30 mgKOH / g, and the types, amounts and experimental parameters of the remaining raw materials are consistent with those of embodiment 1.
[0040] Comparative Example Comparative Example 1 A stator insulating varnish for high-speed new energy motors. The difference between this comparative example and Example 1 is that polyurethane resin is used instead of aliphatic epoxy resin, and the types, amounts and experimental parameters of other raw materials are consistent with those in Example 1.
[0041] The polyurethane resin was purchased from Jining Fangyu Chemical Co., Ltd. with a brand name of ty and an active ingredient content of 98%.
[0042] Comparative Example 2 A stator insulating varnish for high-speed new energy motors. The difference between this comparative example and Example 1 is that acrylic resin is used instead of hydroxy acrylic resin, and the types, amounts and experimental parameters of other raw materials are consistent with those of Example 1.
[0043] Acrylic resin was purchased from Shanghai Maitian Chemical Co., Ltd., model LR-7940, brand Mitsubishi Rayon.
[0044] Comparative Example 3 A stator insulating varnish for high-speed new energy motors. The difference between this comparative example and Example 1 is that a solvent is used instead of a polytetrafluoroethylene dispersion, and the types, amounts and experimental parameters of other raw materials are consistent with those of Example 1.
[0045] Comparative Example 4 A stator insulating paint for high-speed new energy motors. The difference between this comparative example and Example 1 is that a solvent is used instead of an aliphatic epoxy resin, and the types, amounts, and experimental parameters of the remaining raw materials are consistent with those of Example 1. Performance testing tests were conducted on the insulating varnishes for stators of high-speed new energy motors prepared in Examples 1-10 and Comparative Examples 1-4, and subjected to volume resistivity, bonding strength under high temperature performance, curing time tests, and hot and cold shock tests.
[0046] Detection method / test method The tests of volume resistivity and bonding strength at high temperature are carried out in accordance with the provisions of GB / T 1981.2-2003 Electrical Insulation Paint Part 2: Test Methods; Volume resistivity: refer to GB / T1410, sample baking condition 25±2℃, test after 24h; Bond strength under high temperature performance: refer to GB / T11028, the test temperature is 150℃; Curing time test: prepare a container with a length*width*thickness of 12cm*6cm*1cm, inject the insulating paint used for high-speed new energy motor stators until it is 1cm away from the container mouth, immerse a 5cm*5cm*0.5cm metal iron sheet in the insulating paint used for high-speed new energy motor stators, place it in an environment with a temperature of 100℃, and record the curing time of the insulating paint; Thermal shock test: The samples of the curing time test were subjected to thermal shock test, which specifically included: placing the samples in an environment with a temperature of 200°C, keeping the temperature for 24 hours, then cooling to -5°C, cooling for 1.5 hours, then heating to 200°C, heating for 1.5 hours, and keeping the temperature for 24 hours. This was used as a cycle for thermal cycle experiment, observing whether cracks appeared on the samples, and recording the number of cycles. The experimental data is shown in Table 3: Table 3 Experimental data of Examples 1-10 and Comparative Examples 1-4 From Examples 1-10 and Comparative Examples 1-4 in combination with Table 3, it can be seen that the present application prepares polyesterimide resin liquid, hydroxyl acrylic resin, aliphatic epoxy resin, polytetrafluoroethylene dispersion, nano inorganic filler, curing agent, leveling agent and diluent together for application in high-speed new energy motor stator insulating paint, which can greatly improve the bonding performance, insulation performance, high temperature resistance and impact resistance of the insulating paint, while reducing the amount of solvent used and shortening the curing time of the insulating glue.
[0047] Comparing Example 1 with Comparative Example 1, the bonding performance and volume resistivity of Comparative Example 1 are not as good as those of Example 1, and the curing time is also greatly prolonged. Cracks appeared in 96 cycles in the hot and cold shock test, indicating that the addition of aliphatic epoxy resin in this application can greatly improve the adhesion and insulation of the insulating varnish, while shortening the curing time of the insulating varnish.
[0048] Comparing Example 1 with Comparative Example 2, the bonding performance and volume resistivity of Comparative Example 2 are slightly reduced, cracks appear in 96 cycles in the hot and cold shock test, and the curing time is increased, indicating that the addition of hydroxyl acrylic resin can improve the adhesion and insulation of the insulating varnish and shorten the curing time of the insulating varnish.
[0049] Comparing Example 1 with Comparative Example 3, the volume resistivity of Comparative Example 3 is slightly reduced, and cracking occurs after 103 cycles in the thermal shock test, indicating that the insulation and high temperature resistance of the insulating varnish can be greatly improved by adding polytetrafluoroethylene dispersion.
[0050] Comparing Example 1 with Examples 4-6, the bonding performance and volume resistivity of Examples 4-6 are significantly improved, the curing time is substantially shortened by half, and cracking occurs after 150 cycles in the thermal shock test; Comparing Example 4 with Examples 7-8, the bonding performance of Example 7 is slightly improved, but the volume resistivity is reduced, and cracking occurs at 112 cycles in the thermal shock test; the volume resistivity of Example 8 is reduced, and cracking occurs at 108 cycles in the thermal shock test; It can be seen from Example 1 and Examples 4-6, and Example 4 and Examples 7-8 that the present application can effectively improve the adhesion, insulation, high temperature resistance and curing efficiency of the insulating varnish by modifying the aliphatic epoxy resin using hydroxy silane according to a specific method.
[0051] By comparing Example 1 with Examples 9-10, the volume resistivity of Examples 9-10 is reduced, and the cycle of crack appearance in the hot and cold shock test is lower than that of Example 1, indicating that the insulation performance and high temperature resistance of the insulating varnish can be improved by optimizing the imine content in the polyester imine resin and the solid content in the polytetrafluoroethylene dispersion.
[0052] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.
Claims
1. An insulating varnish for stator of high-speed new energy motor, characterized in that: Prepared from the following raw materials in parts by weight: 50-70 parts of polyester imide resin liquid 40-80 parts of hydroxy acrylic resin Aliphatic epoxy resin 20-30 parts 5-9 parts of polytetrafluoroethylene dispersion 30-50 parts of nano inorganic filler 3-5 parts of curing agent 2-3 parts of leveling agent 20-30 parts of diluent.
2. The insulating varnish for stator of high-speed new energy motor according to claim 1, characterized in that: The polyester imine resin is an unsaturated polyester resin containing an imine structure and a hydroxyl group, with a hydroxyl value of 50-100 mgKOH / g, an acid value of 5-8 mgKOH / g, and an imine content of 10-30%.
3. The insulating varnish for high-speed new energy motor stator according to claim 1 is characterized in that: The aliphatic epoxy resin is a modified aliphatic epoxy resin, which is prepared by the following method: Under the protection of inert gas, add aliphatic epoxy resin and organic solvent into the reactor and heat to 100-120°C; When the aliphatic epoxy resin is fully dissolved, start stirring, and slowly drop hydroxysilane and triethylamine at a uniform speed within 1-3 hours; after stirring and reacting at a constant temperature for 3-4 hours, add a mixture of hydroxysilane and initiator and continue stirring for 3-8 hours; then cool to 40-50°C, continue to react with stirring for 2-3 hours, test the content of hydroxysilane, if the content exceeds 1%, continue to add initiator, and continue the reaction until the hydroxysilane content is less than 1%, thereby obtaining a modified aliphatic epoxy resin.
4. The insulating varnish for stator of high-speed new energy motor according to claim 3 is characterized in that: The weight parts of raw materials used to prepare the modified aliphatic epoxy resin are as follows: Aliphatic epoxy resin 20-30 parts 30-40 parts of organic solvent Hydroxysilane 6-10 parts 4-6 parts of triethylamine 2-3 parts of initiator.
5. The insulating varnish for stator of high-speed new energy motor according to claim 4 is characterized in that: The hydroxysilane includes at least one of diphenyldihydroxysilane, dimethyldihydroxysilane, trimethylhydroxysilane, triphenylhydroxysilane, hydroxymethyldiphenylsilane and tetrahydroxysilane.
6. The insulating varnish for stator of high-speed new energy motor according to claim 4 is characterized in that: The initiator is any one of dibutyltin dilaurate, stannous isooctanoate, zinc isooctanoate or bismuth isooctanoate.
7. The insulating varnish for stator of high-speed new energy motor according to claim 1, characterized in that: The solid content of the polytetrafluoroethylene dispersion is 50-60%.
8. The insulating varnish for stator of high-speed new energy motor according to claim 1, characterized in that: The hydroxy acrylic resin has a viscosity of 5000-12000 cps / 25° C., a hydroxy content of 10-25 mgKOH / g, and an acid value of 2-6.
9. The insulating varnish for stator of high-speed new energy motor according to claim 1, characterized in that: The nano inorganic filler includes at least one of boron nitride, silicon carbide, silicon dioxide, mica powder and ceramic powder.
10. A method for preparing an insulating varnish for a stator of a high-speed new energy motor as claimed in any one of claims 1 to 9, characterized in that: The method comprises the following preparation steps: (1) Heat polyesterimide resin liquid, polyimide resin liquid, hydroxy acrylic resin and diluent to 80-100°C, add aliphatic epoxy resin, stir evenly, and cool to 45-50°C to obtain mixed solution A; (2) Stirring the polytetrafluoroethylene dispersion at a speed of 1000-2000 r / min, adding the inorganic nanofiller, stirring and dispersing; after the inorganic nanofiller is added, the stirring speed is adjusted to 6000-8000 r / min, dispersing for 0.5-1 h, and the material temperature is controlled at 45-50° C. during the dispersing process to obtain a mixed solution B; (3) Mix the mixed liquid A and the mixed liquid B at a stirring speed of 1000-1500 r / min, add a curing agent and a leveling agent, and stir for 1-2 hours to obtain an insulating paint for stator of a high-speed new energy motor.
Citation Information
Patent Citations
Insulating material with high temperature resistance and strong acid corrosion resistance for electric control solid propellant electrode
CN106380954A