Composite diaphragm for hydrogen production by alkaline electrolyzed water and preparation method of composite diaphragm

By using organic polymers and hydrophilic inorganic nanoparticles to prepare the support layer and coating, and adding aluminate coupling agent, the composite separator formulation is optimized, and the existing composite separator powder loss, block loss and insufficient conductivity of the existing composite separator is solved. The problem has improved the efficiency and safety of hydrogen production by electrolyzing water.

CN118996526APending Publication Date: 2024-11-22SUZHOU TUOJI NEW MATERIAL TECH CO LTD
View PDF 0 Cites 3 Cited by

Patent Information

Application Number
CN202411096173.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-12
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The existing inorganic-organic composite membranes have problems of powder loss and block loss during long-term operation, which leads to a reduced electrolytic water efficiency and may lead to a mix of hydrogen and oxygen, causing explosion risk, and insufficient resistance and ionic conductivity.

Method used

The supporting layer and coating are prepared using organic polymers and hydrophilic inorganic nanoparticles. The aluminate coupling agent is used to improve the affinity and binding force between materials, and the supporting layer and coating formula is designed and optimized to form uniform pore size. Composite separators with low membrane resistance and high ionic conductivity.

Benefits of technology

It solves the problem of coating peeling, improves the stability and performance of the composite membrane, and is suitable for alkaline electrolysis of hydrogen production, ensuring mechanical strength and gas barrier properties, and reducing the risk of explosion.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004988449520000081
    Figure BDA0004988449520000081
  • Figure BDA0004988449520000082
    Figure BDA0004988449520000082
  • Figure BDA0004988449520000083
    Figure BDA0004988449520000083
Patent Text Reader

Abstract

The invention relates to a composite diaphragm for hydrogen production from alkaline electrolyzed water and a preparation method thereof, the composite diaphragm comprises a supporting layer and a coating, and raw materials for preparing the supporting layer comprise an organic high-molecular polymer and hydrophilic inorganic nanoparticles; the coating is formed by phase inversion after a membrane casting solution is in contact with the supporting layer, the membrane casting solution comprises an organic high-molecular polymer, hydrophilic inorganic nanoparticles, an aluminate coupling agent and an organic solvent, and the organic high-molecular polymer and the hydrophilic inorganic nanoparticles in the supporting layer are the same as those in the membrane casting solution respectively. The prepared composite diaphragm has a homogeneous enhancement effect, and the coating does not peel off after long-time operation. In addition, the composite coating also has the advantages of uniform pore diameter, low membrane surface resistance, high ionic conductivity, strong gas barrier property, good durability, high mechanical strength and the like, and is suitable for hydrogen production by alkaline electrolysis of water.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of hydrogen production by water electrolysis, and specifically relates to a composite diaphragm for hydrogen production by alkaline water electrolysis and a preparation method thereof. Background Art

[0002] As a new generation of clean energy carrier for sustainable utilization, hydrogen has the following advantages: hydrogen and electrical energy can be efficiently converted to each other through water electrolysis technology, with high mass energy density, and is expected to be applied in energy management on a grid scale. Currently, the most mature water electrolysis hydrogen production process is alkaline water electrolysis technology, which has been commercialized on a large scale. Alkaline water electrolysis hydrogen production is an energy conversion device composed of several single electrolytic cells, each of which is composed of a cathode, an anode, a diaphragm and an electrolyte, which directly converts electrical energy into chemical energy. After direct current is introduced, water is decomposed in the electrolytic cell, and hydrogen and oxygen are produced at the cathode and anode respectively. The hydrogen production technology has a simple process and is easy to operate. It is one of the most mature hydrogen production methods currently.

[0003] As a key material of alkaline electrolyzer, the diaphragm has the dual functions of separating the gases generated in the positive and negative electrode chambers and providing a pathway for the migration of ions across the membrane in the electrolyte. Commonly used diaphragms can be divided into asbestos diaphragms, inorganic diaphragms, organic diaphragms and inorganic-organic composite diaphragms. Asbestos diaphragms are the earliest commercial alkaline diaphragm materials, but they will undergo severe swelling behavior in alkaline solutions, which will reduce the mechanical strength of the diaphragm; in addition, asbestos materials are also a carcinogen, and the World Health Organization has banned the use of asbestos and related products. Simply using inorganic or organic diaphragms cannot adapt well to the harsh conditions of alkaline water electrolysis. Therefore, inorganic-organic composite diaphragms have become the research direction of alkaline water electrolysis diaphragms.

[0004] The support of the existing inorganic-organic composite membrane is mostly a polyphenylene sulfide mesh, and the coating is made of a casting liquid containing organic polymer substances and hydrophilic inorganic nanoparticles, such as the composite membranes disclosed in patents CN115161702A, CN117265588A, etc. However, the interaction between the support mesh and the organic-inorganic composite coating on this type of composite membrane is not strong, resulting in powder and block falling during long-term operation, which seriously affects the efficiency of water electrolysis, and also causes hydrogen and oxygen to mix, resulting in the risk of explosion. In addition, the resistance and ion conductivity of the existing composite membrane still need to be improved. Summary of the invention

[0005] The purpose of the present invention is to provide a composite diaphragm for producing hydrogen by alkaline water electrolysis, which has good compatibility between a coating and a supporting layer, good durability, high ion conductivity and low surface resistance, and a preparation method thereof.

[0006] In order to achieve the above object, the technical solution adopted by the present invention is:

[0007] A composite diaphragm for producing hydrogen by alkaline water electrolysis, the composite diaphragm comprising a support layer and a coating formed on the support layer, and based on the total mass of the support layer being 100%, the raw materials for preparing the support layer include:

[0008] Organic polymer 75-95%,

[0009] Hydrophilic inorganic nanoparticles 5-25%;

[0010] The coating is formed by phase transformation after the casting liquid contacts the support layer. Taking the total mass of the casting liquid as 100%, the casting liquid comprises:

[0011] Organic polymer 10-30%,

[0012] Hydrophilic inorganic nanoparticles 30-50%,

[0013] Aluminate coupling agent 1~10%,

[0014] Organic solvent 30~59%,

[0015] The organic high molecular polymer and the hydrophilic inorganic nanoparticles in the raw materials for preparing the support layer are respectively the same as the organic high molecular polymer and the hydrophilic inorganic nanoparticles in the casting solution.

[0016] Preferably, based on the total mass of the support layer being 100%, the raw materials for preparing the support layer include:

[0017] Organic polymer 80-90%,

[0018] Hydrophilic inorganic nanoparticles 10-20%.

[0019] Further preferably, based on the total mass of the support layer being 100%, the raw materials for preparing the support layer include:

[0020] Organic polymer 83-88%,

[0021] Hydrophilic inorganic nanoparticles 12-17%.

[0022] In some embodiments, the raw materials for preparing the support layer further include an aluminate coupling agent. The addition of the aluminate coupling agent can improve the affinity and binding force between the organic polymer and the hydrophilic inorganic nanoparticles, thereby increasing the bonding strength; and can also promote the bonding between the coating and the support layer.

[0023] Furthermore, based on the total mass of the support layer being 100%, the raw materials for preparing the support layer include:

[0024] Organic polymer 83-88%,

[0025] Hydrophilic inorganic nanoparticles 10-12%,

[0026] Aluminate coupling agent 2-5%.

[0027] Preferably, based on the total mass of the casting solution being 100%, the casting solution comprises:

[0028] Organic polymer 10-20%,

[0029] Hydrophilic inorganic nanoparticles 30-40%,

[0030] Aluminate coupling agent 1~10%,

[0031] Organic solvent 30~59%.

[0032] Further preferably, based on the total mass of the casting solution as 100%, the casting solution comprises:

[0033] Organic polymer 13-18%,

[0034] Hydrophilic inorganic nanoparticles 33-38%,

[0035] Aluminate coupling agent 3-8%,

[0036] Organic solvent 36~51%.

[0037] Preferably, the organic high molecular polymer is polysulfone. When the organic high molecular polymer is selected from other types of organic high molecular polymers, such as polypropylene, polyethylene, polyphenylene sulfide, polyamide / nylon, polyethersulfone, polyphenylsulfone, polyethylene terephthalate, polyetheretherketone, sulfonated polyetheretherketone, chlorotrifluoroethylene, copolymer of ethylene and tetrafluoroethylene, copolymer of ethylene and chlorotrifluoroethylene, polyimide, polyetherimide or meta-aramid, it can also play a role in homogeneous enhancement.

[0038] More preferably, the number average molecular weight of the polysulfone is 50,000 to 100,000, and even more preferably 60,000 to 90,000.

[0039] Preferably, the hydrophilic inorganic nanoparticles are selected from one or more of zirconium dioxide, cerium dioxide, calcium carbonate and barium sulfate.

[0040] Preferably, the aluminate coupling agent is selected from one or more of distearoyloxyisopropyl aluminate and anti-settling aluminate.

[0041] Preferably, the organic solvent is selected from one or more of N-methylpyrrolidone, N,N-dimethylformamide, N,N-dimethylacetamide and dimethyl sulfoxide.

[0042] Preferably, the support layer is a non-woven fabric or a mesh fabric made by processing the raw materials for preparing the support layer.

[0043] In some embodiments, the nonwoven fabric has a fiber diameter of 100 to 150 μm and a thickness of 200 to 300 μm.

[0044] In some implementations, the fiber diameter of the mesh cloth is 100-150 μm, the thickness is 170-270 μm, and the spacing between fibers on the mesh cloth is 50-500 μm.

[0045] Preferably, the thickness of the support layer accounts for 1 / 3 to 2 / 3 of the total thickness of the composite diaphragm, more preferably 0.4 to 0.55, and even more preferably 0.4 to 0.5.

[0046] More preferably, the thickness of the support layer is 150 to 300 μm, and even more preferably 150 to 250 μm.

[0047] Preferably, the coating is formed on both sides of the support layer along the thickness direction thereof and in pores on the support layer.

[0048] Preferably, the surface resistance of the composite diaphragm is ≤0.3Ω / cm 2 , OH - Conductivity ≥150mS / cm.

[0049] Further preferably, the contact angle of the composite membrane is ≤75°, the water absorption is ≥80wt%, the bubble point is ≥3.7bar, and the gas flux is ≤1.05mL / min / cm 2 / bar, tensile strength ≥28MPa.

[0050] The present invention also provides a method for preparing the composite diaphragm for producing hydrogen by alkaline water electrolysis as described above, comprising the following steps:

[0051] S1, the raw materials for preparing the support layer are processed into non-woven fabric or mesh fabric to obtain the support layer;

[0052] S2, coating the casting liquid onto the support layer, placing it in a coagulation bath for phase conversion after evaporation, and forming the composite coating.

[0053] Preferably, the evaporation time is controlled to be 60 to 120 seconds, and the temperature is controlled to be 20 to 70°C, more preferably 30 to 60°C, and even more preferably 35 to 45°C.

[0054] In some embodiments, the method for preparing the non-woven fabric includes: mixing the raw materials for preparing the support layer and heating them to a molten state, performing melt spinning through a spinning machine to make composite fibers, and then performing opening treatment, carding with a carding machine, hydroentanglement mechanical reinforcement and heat setting enhancement treatment on the composite fibers to obtain the non-woven fabric.

[0055] Furthermore, the heat setting enhancement treatment temperature is 100-200°C.

[0056] In some embodiments, the preparation method of the mesh cloth includes: mixing the raw materials for preparing the support layer and heating them to a molten state, performing melt spinning through a spinning machine to make composite fibers, and then weaving the composite fibers through warp and weft to form a grid structure, followed by heat setting and strengthening treatment to obtain the mesh cloth.

[0057] In other embodiments, the method for preparing the mesh cloth includes: mixing the raw materials for preparing the support layer and heating them to a molten state, casting the melt into a mesh groove with interlaced longitude and latitude, and forming the mesh cloth after the melt is cooled.

[0058] Preferably, the coagulation bath is a single solvent or a mixed solvent, the single solvent is selected from any one of methanol, ethanol, isopropanol, n-propanol, n-butanol, and water; the mixed solvent is a mixed solvent of one or more of methanol, ethanol, dimethyl sulfoxide, N,N-dimethylacetamide, N-methylpyrrolidone, N,N-dimethylformamide, methanesulfonic acid and water.

[0059] Preferably, the preparation method further comprises, after step S2, a step of placing the composite diaphragm in deionized water to remove the organic solvent thereon.

[0060] Preferably, the coating comprises single-blade slot coating and / or double-blade casting coating.

[0061] In some embodiments, the single blade slit coating includes fixing the support layer in the middle of the batching box through a limit axis before the support layer is fixed to the blade, pre-infiltrating the support layer with the casting liquid for 1 to 5 minutes, and coating the composite diaphragm after passing through the blade slit with a spacing of 400 to 700 μm. Alternatively, the coating can be performed according to the existing coating method.

[0062] In some embodiments, the double-blade casting coating includes placing the upper and lower sides of the support layer in a sealed chamber filled with the casting liquid, the sealed chamber does not contact the support layer, the front end of the sealed chamber has an opening with a blade, the opening spacing is 50-300 μm, the casting liquid is controlled by a metering pump, and a certain amount of the casting liquid is cast through the opening onto the support layer to form a composite diaphragm. Alternatively, the coating can also be performed by referring to the existing coating method.

[0063] Preferably, the mass ratio of the support layer to the casting solution is 1:(0.5-1.5), and more preferably 1:(0.8-1.2).

[0064] The present invention also provides a water electrolyzer, comprising the composite diaphragm as described above.

[0065] Due to the application of the above technical solution, the present invention has the following advantages compared with the prior art:

[0066] The present invention uses organic high molecular polymer and hydrophilic inorganic nanoparticles of the same material as the support layer to prepare the coating, which has a homogeneous reinforcement effect and solves the problem of coating peeling after long-term operation.

[0067] Through further design of the support layer and coating formula, the prepared composite membrane has the advantages of uniform pore size, low membrane surface resistance, high ion conductivity, strong gas barrier properties, good durability, and high mechanical strength, and is suitable for hydrogen production by alkaline water electrolysis. BRIEF DESCRIPTION OF THE DRAWINGS

[0068] Figure 1 This is an electron microscope image of the cross section of the composite diaphragm of Example 1;

[0069] Figure 2 This is an electron microscope image of the cross section of the composite diaphragm of Comparative Example 1. DETAILED DESCRIPTION

[0070] The present invention is further described below in conjunction with the examples. However, the present invention is not limited to the following examples. The implementation conditions used in the examples can be further adjusted according to the different requirements of specific use, and the implementation conditions not specified are conventional conditions in the industry. The technical features involved in each embodiment of the present invention can be combined with each other as long as they do not conflict with each other.

[0071] Unless otherwise specified, the raw materials and instruments used in the specific examples and comparative examples herein can be purchased commercially or can be prepared according to existing technical methods. Among them, polysulfone was purchased from Solvay with the brand name P-1700; distearoyloxyisopropylaluminate was purchased from SG-Al821.

[0072] Example 1

[0073] 85g of polysulfone with a molecular weight of 80,000 and 15g of zirconium oxide are melted at 250°C and melt-spun through a spinning machine to obtain composite fibers; the prepared composite fibers are opened to disperse them into single fibers with a diameter of 100 to 150 μm; the dispersed composite fibers are formed into a uniform fiber web through a carding machine; then, the composite fiber web is reinforced by a hydroentanglement mechanical reinforcement method to form a grey cloth, and the grey cloth is heat-set and strengthened by a hot rolling process at 150°C to obtain a non-woven fabric with a thickness of 200 μm.

[0074] 15 g of polysulfone with a molecular weight of 80,000, 35 g of zirconium oxide and 5 g of distearoyloxyisopropylaluminate are dissolved in 45 g of N,N-dimethylacetamide, and the solution is fully stirred at a temperature of 80°C for 5 hours to obtain a completely dissolved solution, and the solution is allowed to stand for degassing to obtain a casting solution; the entire casting solution is coated on the prepared non-woven fabric by double-blade cast coating to form a composite diaphragm, and the composite diaphragm is further placed in water after evaporation at 40°C for 60 seconds to complete the phase inversion process, thereby obtaining the composite diaphragm; the prepared composite diaphragm is placed in deionized water at 25°C for 12 hours to wash away the residual N,N-dimethylacetamide solvent to obtain the composite diaphragm.

[0075] The cross-sectional electron microscope image of the composite diaphragm prepared in this embodiment is shown in Figure 1 The pore size distribution of the composite membrane is relatively uniform, the coating formed by the non-woven fabric and the casting solution can be well combined together, and has good interface compatibility.

[0076] Example 2

[0077] 85g of polysulfone with a molecular weight of 80,000 and 15g of zirconium oxide were melted at 250°C and melt-spun through a spinning machine to obtain composite fibers with a single fiber diameter of 100μm. A grid structure was formed by weaving warp and weft. The grid was then heat-set and strengthened by a hot rolling process at 150°C. The prepared grid cloth had a thickness of 200μm and a spacing of 300μm between fibers.

[0078] 15 g of polysulfone with a molecular weight of 80,000, 35 g of zirconium oxide and 5 g of distearoyloxyisopropylaluminate are dissolved in 45 g of N,N-dimethylacetamide, and the solution is fully stirred at a temperature of 80°C for 5 hours to obtain a completely dissolved solution, and the solution is allowed to stand for degassing to obtain a casting solution; the entire casting solution is coated on the prepared mesh cloth by double-blade cast coating to form a composite diaphragm, and the composite diaphragm is further placed in water after evaporation at 40°C for 60 seconds to complete the phase inversion process, thereby obtaining the composite diaphragm; the prepared composite diaphragm is placed in deionized water at 25°C for 12 hours to wash away the residual N,N-dimethylacetamide solvent to obtain the composite diaphragm.

[0079] Example 3

[0080] 85g of polysulfone with a molecular weight of 80,000 and 15g of zirconium oxide were melted at 250°C and cast into a grid groove with alternating longitude and latitude. The groove diameter was 200μm, the thickness was 200μm, and the spacing between the grooves was 300μm. After the melt temperature dropped and cooled, a grid was formed.

[0081] 15 g of polysulfone with a molecular weight of 80,000, 35 g of zirconium oxide and 5 g of distearoyloxyisopropylaluminate are dissolved in 45 g of N,N-dimethylacetamide, and the solution is fully stirred at a temperature of 80°C for 5 hours to obtain a completely dissolved solution, and the solution is allowed to stand for degassing to obtain a casting solution; the entire casting solution is coated on the prepared mesh cloth by double-blade cast coating to form a composite diaphragm, and the composite diaphragm is further placed in water after evaporation at 40°C for 60 seconds to complete the phase inversion process, thereby obtaining the composite diaphragm; the prepared composite diaphragm is placed in deionized water at 25°C for 12 hours to wash away the residual N,N-dimethylacetamide solvent to obtain the composite diaphragm.

[0082] Comparative Example 1

[0083] 15 g of polysulfone with a molecular weight of 80,000, 35 g of zirconium oxide and 5 g of distearoyloxyisopropylaluminate were dissolved in 45 g of N, N-dimethylacetamide, and the solution was fully stirred at 80°C for 5 hours to obtain a completely dissolved solution, and the solution was allowed to stand for degassing to obtain a casting solution; all of the casting solution was coated on a polyphenylene sulfide mesh cloth (purchased from Haining Protech New Materials Co., Ltd., with a thickness of 200 μm and a fiber spacing of 400 μm) by double-blade cast coating to form a composite diaphragm, and the composite diaphragm was further placed in water after evaporation at 40°C for 60 seconds to complete the phase inversion process, thereby obtaining the composite diaphragm; the prepared composite diaphragm was placed in deionized water at 25°C for 12 hours to wash away the residual N, N-dimethylacetamide solvent to obtain the composite diaphragm.

[0084] The cross-sectional electron microscope image of the composite diaphragm prepared in this comparative example is shown in Figure 2 The coating formed by the composite diaphragm polyphenylene sulfide mesh cloth and the casting liquid has poor bonding properties.

[0085] Comparative Example 2

[0086] The method is substantially the same as Example 1, except that the aluminate coupling agent DL-411 is used to replace the distearoyloxyisopropylaluminate in the casting solution.

[0087] Comparative Example 3

[0088] The method is substantially the same as Example 1, except that after the composite diaphragm is formed, the mixture is evaporated for 30 seconds and then placed in water to further complete the phase conversion process.

[0089] Comparative Example 4

[0090] The method is substantially the same as Example 1, except that after the composite diaphragm is formed, the mixture is evaporated for 150 seconds and then placed in water to further complete the phase conversion process.

[0091] Comparative Example 5

[0092] It is substantially the same as Example 1, except that the ratio of the casting liquid is different. In this example, the casting liquid is composed of 35 g of polysulfone with a molecular weight of 80,000, 15 g of zirconium oxide, 5 g of distearoyloxyisopropylaluminate, and 45 g of N,N-dimethylacetamide.

[0093] Comparative Example 6

[0094] It is substantially the same as Example 1, except that the ratio of the composite fiber is different. The composite fiber in this example is made by melt spinning 65 g of polysulfone with a molecular weight of 80,000, 30 g of zirconium oxide and 5 g of distearoyloxyisopropylaluminate.

[0095] Performance Testing

[0096] 1. Performance testing method

[0097] 1.1 Thickness: Measure the thickness of the diaphragm in accordance with the national electronic industry standard SJ-T10171.1-1991 "Alkaline Battery Diaphragm Performance Test Method Determination of Diaphragm Thickness", and take the average value of the measurements of 3 samples as the measurement result.

[0098] 1.2 Surface contact angle test: Use a contact angle tester to measure the pure water contact angle on the diaphragm surface, and take the average value of the measurements of 3 samples as the measured value.

[0099] 1.3 Water absorption: The water content of the diaphragm is determined by weight analysis, and the calculation formula is as follows:

[0100]

[0101] Where W represents the water absorption (wt%), m 湿 Represents the weight of the wet film (g), m 干 Represents the weight of dry film (g).

[0102] 1.4 Bubble point pressure refers to the pressure at which the gas in the diaphragm begins to permeate at a certain temperature. The test method refers to GB / T32361-2015 "Bubble point and average flow method for separation membrane pore size test method", and the average value of the measurements of 3 samples is taken as the measurement result.

[0103] 1.5 Gas flux: refers to the permeability of gas to polymer materials such as films, coatings, and fabrics. The volume of gas permeating through the membrane per square centimeter per unit time is measured using an isobaric method and a chemical sensor, and the average value of the measurements of three samples is taken as the measurement result.

[0104] 1.6 Diaphragm surface resistance: Diaphragm resistance reflects the conductivity of the diaphragm immersed in the electrolyte. The electrochemical impedance of the diaphragm in alkaline electrolyte is measured using an electrochemical workstation, and the average value of measurements of three samples is taken as the measured value.

[0105] 1.7OH - The conductivity represents the OH transport capacity of the membrane. - The capacity is calculated by the following formula:

[0106]

[0107] Where σ represents ionic conductivity (mS / cm), l represents the thickness of the sample to be tested (cm), R represents the resistance to be tested (Ω), and A represents the area of ​​the sample (cm 2 ).

[0108] 1.8 Average pore size: 30 holes are randomly measured on the electron microscope image of the diaphragm, and the average value is taken as the average pore size of the diaphragm.

[0109] 1.9 Porosity: The porosity of the membrane is the percentage of the pore volume of the membrane to the volume of the membrane. It is measured by weighing, that is, the pore volume V of the membrane is determined based on the weight change before and after the membrane is soaked in pure water. 孔 The skeleton volume of the material can be obtained by the raw material density and dry weight V 骨 , then the porosity of the porous material can be calculated using the following formula:

[0110]

[0111] The average value of the measurements of 3 samples was taken as the measurement result.

[0112] 1.10 Tensile strength: tested by a tensile testing machine, refer to standard GBT3923.1-2013 Tensile properties of textile fabrics Part 1: Determination of breaking strength and elongation at break (strip method), and take the average value of the measurements of 3 specimens as the measurement result.

[0113] 2. Test results

[0114] Table 1

[0115]

[0116]

[0117] Comparative Example 1: Polyphenylene sulfide mesh cloth is used as a support layer, polysulfone, inorganic nanoparticles, aluminate coupling agent and solvent are mixed to prepare a casting solution, and the obtained composite diaphragm has good mechanical properties and hydrophilicity, but Figure 2It can be seen that the compatibility of the coating formed by the support layer and the casting liquid is poor. Powder and block fall occurs during long-term operation, which seriously affects the efficiency of water electrolysis and even causes hydrogen and oxygen to mix, posing an explosion risk. More importantly, the composite diaphragm has a large surface resistance and OH - Low conductivity.

[0118] The inventors used the same organic polymer and inorganic nanoparticles as the casting solution to make the support layer, which not only improved the interface compatibility between the support layer and the coating, solved the problem of coating peeling off during long-term operation, improved the stability of the composite diaphragm, but also greatly improved the surface resistance and OH of the composite diaphragm. - Conductivity.

[0119] The inventors further discovered that when a support layer made of the same organic high molecular polymer and inorganic nanoparticles as the casting liquid is used, there is a solvation effect between the support layer and the casting liquid. When the contact time between the two is too long, the prepared composite membrane will have macroporous defects (such as Comparative Example 4); when the contact time between the two is too short, it will make it difficult for the casting liquid to be tightly combined with the support membrane, and the performance of the composite membrane will also be poor (such as Comparative Example 3). By controlling the contact time between the two (i.e., the above-mentioned evaporation time) to 60 to 120 seconds, the performance of the prepared composite membrane is better. In addition to controlling the contact time, in the process of preparing the support layer, a layer of oblique fibers is woven on the warp and weft woven grid to increase the number of nodes in the grid; or a three-dimensional woven grid is used, and the two layers of grids are woven together by interlacing fibers up and down to form a three-dimensional grid structure, which can also enhance the strength of the support layer and reduce the influence of the solvation effect on the support layer.

[0120] When an aluminate coupling agent is added to the casting solution and distearyloxyisopropylaluminate is selected as the aluminate coupling agent, it can increase the compatibility between the inorganic nanoparticles and the organic high molecular polymer, and can also form a chemical bond with the organic high molecular polymer to increase the crosslinking density, while also connecting the support layer and the coating to enhance the mechanical strength and impact toughness of the material. When other types of aluminate coupling agents are selected (such as Comparative Example 2), the tensile strength and bubble point pressure of the composite diaphragm are significantly reduced.

[0121] In addition, the component ratio of the support layer and the coating is also very important. When the component ratio is inappropriate, the performance of the prepared composite membrane is poor (such as Comparative Examples 5 and 6).

[0122] When a support layer made of the same organic high molecular polymer and inorganic nanoparticles as the casting liquid is used, whether it is a non-woven fabric made by melt spinning, opening, carding and other processes as the support layer, or a warp and weft woven grid made by melt spinning, warp and weft weaving and other processes as the support layer, or a grid made of warp and weft staggered grid grooves as the support layer, they all have better compatibility with the casting liquid, and the performance of the composite diaphragm obtained is excellent, among which the composite diaphragm made with non-woven fabric as the support layer has the best performance.

[0123] The above detailed description of the present invention is intended to enable persons familiar with the art to understand the contents of the present invention and implement them. It does not limit the protection scope of the present invention. Any equivalent changes or modifications made according to the spirit of the present invention should be included in the protection scope of the present invention.

Claims

1. A composite diaphragm for producing hydrogen by alkaline water electrolysis, the composite diaphragm comprising a support layer and a coating formed on the support layer, characterized in that: Taking the total mass of the support layer as 100%, the raw materials for preparing the support layer include: Organic polymer 75-95%, Hydrophilic inorganic nanoparticles 5-25%; The coating is formed by phase transformation after the casting liquid contacts the support layer. Taking the total mass of the casting liquid as 100%, the casting liquid comprises: Organic polymer 10-30%, Hydrophilic inorganic nanoparticles 30-50%, Aluminate coupling agent 1~10%, Organic solvent 30~59%, The organic high molecular polymer and the hydrophilic inorganic nanoparticles in the raw materials for preparing the support layer are respectively the same as the organic high molecular polymer and the hydrophilic inorganic nanoparticles in the casting solution.

2. The composite diaphragm for producing hydrogen by alkaline water electrolysis according to claim 1, characterized in that: The organic macromolecular polymer is polysulfone; and / or, The hydrophilic inorganic nanoparticles are selected from one or more of zirconium dioxide, cerium dioxide, calcium carbonate, and barium sulfate; and / or, The aluminate coupling agent is selected from one or more of distearoyloxyisopropyl aluminate and anti-settling aluminate; and / or, The organic solvent is selected from one or more of N-methylpyrrolidone, N,N-dimethylformamide, N,N-dimethylacetamide and dimethyl sulfoxide.

3. The composite diaphragm for producing hydrogen by alkaline water electrolysis according to claim 1, characterized in that: The support layer is a non-woven fabric or a mesh fabric made by processing the raw materials for preparing the support layer.

4. The composite diaphragm for producing hydrogen by alkaline water electrolysis according to claim 3, characterized in that: The nonwoven fabric has a fiber diameter of 100 to 150 μm and a thickness of 200 to 300 μm; and / or, The fiber diameter of the mesh cloth is 100-150 μm, the thickness is 170-270 μm, and the spacing between fibers on the mesh cloth is 50-500 μm.

5. The composite diaphragm for producing hydrogen by alkaline water electrolysis according to claim 1, characterized in that: The thickness of the support layer accounts for 1 / 3 to 2 / 3 of the total thickness of the composite diaphragm.

6. The composite diaphragm for producing hydrogen by alkaline water electrolysis according to claim 1, characterized in that: The coating layer is formed on both sides of the support layer along the thickness direction thereof and in the pores on the support layer.

7. The method for preparing a composite diaphragm for producing hydrogen by alkaline water electrolysis according to any one of claims 1 to 6, characterized in that: The preparation method comprises the following steps: S1, the raw materials for preparing the support layer are processed into non-woven fabric or mesh fabric to obtain the support layer; S2, coating the casting liquid onto the support layer, placing it in a coagulation bath for phase conversion after evaporation, and forming the composite coating.

8. The preparation method according to claim 7, characterized in that: The evaporation time is controlled to be 60 to 120 seconds and the temperature is controlled to be 20 to 70°C.

9. The preparation method according to claim 7, characterized in that: The preparation method of the non-woven fabric comprises: mixing the raw materials for preparing the support layer and heating them to a molten state, performing melt spinning through a spinning machine to prepare composite fibers, and then performing opening treatment, carding with a carding machine, mechanically reinforcing with water spunlace and heat setting and strengthening treatment on the composite fibers to obtain the non-woven fabric.

10. The preparation method according to claim 7, characterized in that: The preparation method of the mesh cloth comprises: mixing the raw materials for preparing the support layer and heating them to a molten state, performing melt spinning through a spinning machine to prepare composite fibers, and then weaving the composite fibers into a mesh structure through warp and weft weaving, and then performing heat setting and strengthening treatment to obtain the mesh cloth; or, The preparation method of the mesh cloth comprises: mixing the raw materials for preparing the support layer and heating them to a molten state, casting the melt into a mesh groove with interlaced longitude and latitude, and forming the mesh cloth after the melt is cooled.

11. The preparation method according to claim 7, characterized in that: The coagulation bath is a single solvent or a mixed solvent, and the single solvent is selected from any one of methanol, ethanol, isopropanol, n-propanol, n-butanol, and water; The mixed solvent is a mixed solvent of one or more of methanol, ethanol, dimethyl sulfoxide, N,N-dimethylacetamide, N-methylpyrrolidone, N,N-dimethylformamide, methanesulfonic acid and water.

12. The preparation method according to claim 7, characterized in that: The preparation method further comprises, after step S2, placing the composite diaphragm in deionized water to remove the organic solvent thereon.

Citation Information

Cited By

  • Composite fiber diaphragm for alkaline electrolytic cell and preparation method of composite fiber diaphragm

    CN119663370A

  • High-selectivity composite diaphragm for seawater electrolysis hydrogen production and preparation method of high-selectivity composite diaphragm

    CN120400927A

  • Diaphragm and preparation method thereof, water electrolysis device and application

    CN121653684A