Contact lens with thermal management function and preparation method thereof

By converting the nanoparticle layer and porous structure on the upper surface design of silicon hydrogel contact lenses, combining PID algorithm and wireless power supply technology, the poor thermal conductivity of silicon hydrogel substrate and the defects of traditional thermistor power supply methods are solved, and the defects of the silicon hydrogel substrate are realized Better thermal management effects and reduce thermal damage to the eyes.

CN119002092APending Publication Date: 2024-11-22钱塘科技创新中心
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411078614.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-07
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

Silicon hydrogel base contact lenses have poor thermal conductivity, resulting in poor thermal management. The traditional external thermistor power supply method has problems such as low regulation accuracy and poor robustness.

Method used

The nanoparticle layer is designed to convert the nanoparticle layer on the front surface of the silicon hydrogel, thermal regulation is carried out in combination with the PID algorithm, and a porous silicon hydrogel substrate is used to improve heat dissipation performance, and wireless power supply technology is used to reduce the heat generated by the battery.

Benefits of technology

It effectively reduces the thermal adhesion area and heat generation power of contact lenses, improves the accuracy and robustness of temperature control, improves the heat dissipation performance of silicon hydrogel substrate, and reduces thermal damage to the eyes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119002092A_ABST
    Figure CN119002092A_ABST
Patent Text Reader

Abstract

The invention provides a contact lens with a thermal management function and a preparation method thereof. The contact lens sequentially comprises a silicone hydrogel front surface, a middle flexible circuit layer and a silicone hydrogel rear surface, wherein an up-conversion nanoparticle film with a view field correction function is arranged on the front surface of the silicone hydrogel; a flexible circuit and a chip are arranged on the middle flexible circuit layer; the flexible circuit adopts a double-layer wiring structure and is used for supplying energy to various temperatures, humidity, oxygen concentration and a power supply of the main control chip and acquiring and transmitting monitoring signals; and a porous structure is arranged on the rear surface of the silica hydrogel. The multifunctional contact lens is prepared based on a wireless power supply technology, an active thermal regulation and control technology and the like, and thermal management can be effectively carried out when a human body wears the contact lens.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention provides a contact lens with a thermal management function and a preparation method thereof, belonging to the technical field of contact lenses. Background Art

[0002] With the continuous development of information technology and manufacturing technology, traditional manufacturing products have been transformed towards intelligence and diversified functions. Among them, contact lenses made of silicone hydrogel, as daily necessities widely used in recent decades, have gradually developed from a single vision correction function to a diversified intelligent product with vision correction, signal monitoring and comfort integration. On the other hand, with the continuous improvement of modern living standards, the internal environment of the human eye is often faced with the threat of imbalance between high and low temperatures. Especially when wearing intelligent contact lenses, due to the poor self-regulation ability of the human eye, it is easy to cause eye burns, damage, discomfort and other negative effects due to the heat generated by the functional chips inside the contact lenses. At present, the thermal management technology of contact lenses prepared with silicone hydrogel substrates mostly adopts master thermal control technology, such as wired-powered micro-heating wires connected to thermistors.

[0003] Compared with traditional hydrogel substrates, contact lenses with silicone hydrogel substrates have greatly improved oxygen permeability and comfort. However, due to the poor thermal conductivity of hydrogel and silicone molecules, the thermal conductivity of the silicone hydrogel substrate itself is still a challenging problem that needs to be solved urgently. At the same time, there are many defects in the use of wired powered micro-heating wires with external thermistors to achieve active thermal control, including low control accuracy, poor robustness, and high delay error. Contact lenses are mostly powered by embedded rechargeable batteries, which need to be frequently disassembled and replaced, and the operation process is relatively complicated. At the same time, the heat generated by the battery during operation and the chemical components it contains are easy to cause damage to the human eye structure. Summary of the invention

[0004] In view of the above problems, the present invention provides a contact lens with thermal management function and a preparation method thereof. Based on the optical transition energy theory, an upconversion nanoparticle layer is designed on the surface of the front silicone hydrogel film, which can correct the field of view angle, reduce the use of internal control chips, and thus reduce the overall heat generation power. At the same time, on the basis of feedback thermal control by thermistors, a PID algorithm is added to further improve the temperature control accuracy. In addition, a porous silicone hydrogel substrate is designed, which can effectively solve the problem of poor heat dissipation performance of traditional silicone hydrogel substrates.

[0005] The specific technical solution is:

[0006] A contact lens with a thermal management function, comprising, in sequence, a silicone hydrogel front surface, an intermediate flexible circuit layer, and a silicone hydrogel rear surface;

[0007] Wherein, an upconversion nanoparticle film having a field of view correction function is provided on the front surface of the silicone hydrogel;

[0008] The middle flexible circuit layer is equipped with flexible circuits and chips. The flexible circuit adopts a double-layer wiring structure for power supply and monitoring signal collection and transmission of various temperature, humidity, oxygen concentration and main control chips;

[0009] The rear surface of the silicone hydrogel is provided with a porous structure.

[0010] The preparation method of the silicone hydrogel front surface is:

[0011] (1) First, LuCl3.6H2O (0.5 mmol), GdCl3.6H2O (0.3 mmol), YbCl3.6H2O (0.2 mmol) and TmCl3.6H2O (0.005 mmol) were mixed with 15 ml of 1-octadecene and 6 ml of oleic acid in a 100 ml three-necked round-bottom flask.

[0012] (2) The mixture in the flask was degassed under vacuum and stirred at 380 rpm for 10 minutes at room temperature, then stirred at 120°C ± 5°C for 20 minutes and at 160°C ± 5°C for 10 minutes to obtain a transparent solution. The solution was cooled to 50°C, the vacuum was released, and 10 mL of a methanol solution containing 2.5 mmol NaOH and 4 mmol NH4F was injected at a rate of 1 mL / min, and the turbid mixture was stirred at 50°C ± 4°C for 30 minutes.

[0013] (3) Slowly heat the flask under Ar flow to remove the methanol and restore vacuum to 90-100°C. The solution is further degassed under vacuum at 120°C ± 5°C for 10 minutes. Then, resume Ar flow, remove vacuum, and increase the temperature to 300°C at a rate of 10-17°C / min. Maintain the reaction at 300°C ± 3°C for 120 minutes before cooling to room temperature.

[0014] (4) Oleate-terminated NaLuF4:Tm 3+ (0.5%) / Yb 3+ (20%) / Gd 3+ The (30%) upconversion nanoparticles were precipitated by centrifugation at 4000 rpm for 10 minutes. The nanoparticles were then redispersed in 5 mL of hexane, induced to precipitate with 20 mL of ethanol, centrifuged at 4000 rpm for 10 minutes to collect the precipitate, and the supernatant was discarded for washing the nanoparticles. After the washing process was repeated twice, the prepared upconversion nanoparticles were embedded in the front surface of the contact lens silicone hydrogel to form an upconversion nanoparticle film layer.

[0015] The intermediate flexible circuit layer includes a sensor, a main control chip, a signal filtering module, a power protection chip, and a flexible wireless power supply antenna; the sensor is used for signal monitoring and collection of the internal environment of the eye, and is transmitted to the main control chip through the signal filtering module to remove noise measurement interference, and then through the flexible wireless power supply antenna, information transmission and interaction are carried out with external matching devices in an interactive real-time communication manner.

[0016] The method for preparing the intermediate flexible circuit layer is as follows:

[0017] First, draw the structural schematic diagram of the double-layer circuit in the CAD software, and then import the design schematic diagram into the supporting design software of the ultraviolet laser processing system. Use laser cutting of PI copper-clad film to produce the upper and lower circuit structures respectively, and connect the two layers of circuit structure through the lead perforations to form a flexible double-layer circuit structure.

[0018] Corresponding devices are attached according to the pad positions of the flexible circuit and chip layer chips to form a flexible circuit layer structure with complete signal detection and transmission functions.

[0019] The preparation method of the silicone hydrogel rear surface is:

[0020] (1) First, the NaCl particles are crushed by a high-speed multifunctional crusher;

[0021] (2) Alginate polymer and acrylamide in a mass ratio of 1:8 were mixed into 30 ml of deionized water solution (2.2 mol), and 4 ml of N, N-methylenebisacrylamide (0.06 wt%) and 4 ml of ammonium persulfate (0.06 wt%) were added thereto, mixed and degassed. After adding 2 ml of n, n, n', n'-tetramethylethylenediamine (0.25 wt%) and 1 mol of NaCl particles prepared in step (1), the mixture was poured into a custom-made silicone hydrogel substrate mold.

[0022] (3) The mixture was polymerized by curing with ultraviolet light for 2 hours to produce a porous PAAm hydrogel film. The PAAm hydrogel film prepared by curing was subjected to demolding treatment in a water bath at 80°C to obtain a porous silicon hydrogel substrate.

[0023] The multifunctional contact lenses prepared by the present invention based on wireless power supply technology and active thermal regulation technology can effectively perform thermal management when the human body wears contact lenses. The up-conversion nanoparticle film on the front surface of the contact lens can effectively perform the field of view correction function, thereby reducing the design envelope size of the contact lens and the number of adjustment chips in the circuit structure, and reducing the thermal attachment area and heat generation power under normal working conditions. The wireless power supply technology used can not only facilitate the charging and discharging of the contact lenses, but also reduce the excess heat generated by the battery operation, which is of great help in realizing the thermal management of the contact lenses. In addition, the main control thermal control PID technology used can change the insufficient control accuracy brought by the traditional thermal resistance feedback method, and improve the real-time accuracy and robustness of temperature control. The porous silicone hydrogel substrate also improves the problem of poor heat dissipation performance of the traditional silicone hydrogel substrate, and better realizes the thermal management function of the contact lenses. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 It is a schematic diagram of the structure of the present invention;

[0025] Figure 2 is a schematic diagram of the rear surface structure of the silicone hydrogel of the present invention;

[0026] Figure 3 is a schematic diagram of the structure of the intermediate flexible circuit layer of the present invention;

[0027] Figure 4 is a power supply diagram of the wireless antenna of the present invention;

[0028] Figure 5 It is a schematic diagram of the porous silicon hydrogel structure of the present invention. DETAILED DESCRIPTION

[0029] The specific technical solution of the present invention is described in conjunction with the accompanying drawings.

[0030] The contact lens with thermal management function in the present invention is mainly divided into three parts: Figure 1 The three-layer structure of the contact lens mainly includes the front surface 1 of the silicone hydrogel of the contact lens, the middle flexible circuit layer 2 and various chips, and the back surface 3 of the silicone hydrogel of the contact lens. Figure 1 As shown, the up-conversion nanoparticle film 11 with field correction function is located on the upper surface 1 of the contact lens, and the flexible circuit of the middle flexible circuit layer 2 adopts a double-layer wiring structure for power supply and monitoring signal collection and transmission of various temperature, humidity, oxygen concentration and main control chip, such as Figure 2 As shown, the rear surface 3 of the silicone hydrogel is designed as a porous structure 31, which is more conducive to guiding the dissipation of heat accumulated by the contact lens during operation.

[0031] The up-conversion nanoparticle film 11 on the front surface of the contact lens has the advantages of large anti-Stoke shift, little damage to biological tissue, low toxicity and high signal-to-noise ratio, and has wavefront aberration correction and vision correction functions. The preparation process is as follows:

[0032] (1) First, LuCl3.6H2O (0.5 mmol), GdCl3.6H2O (0.3 mmol), YbCl3.6H2O (0.2 mmol) and TmCl3.6H2O (0.005 mmol) were mixed with 15 ml of 1-octadecene and 6 ml of oleic acid in a 100 ml three-necked round-bottom flask.

[0033] (2) After that, the mixture in the flask was degassed under vacuum and stirred at 380 rpm for 10 minutes at room temperature, then stirred at 120°C ± 5°C for 20 minutes and at 160°C ± 5°C for 10 minutes to obtain a transparent solution. The solution was cooled to 50°C, the vacuum was released, and 10 mL of a methanol solution containing 2.5 mmol NaOH and 4 mmol NH4F was injected at a rate of 1 mL / min, and the turbid mixture was stirred at 50°C ± 4°C for 30 minutes.

[0034] (3) To remove the methanol, slowly heat the flask under an Ar flow, and once most of the methanol is removed, restore the vacuum to 90-100°C. The solution is further degassed under vacuum at 120°C ± 5°C for 10 minutes. Then, resume the Ar flow, remove the vacuum, and increase the temperature to 300°C at a rate of 10-17°C / min. Maintain the reaction at 300°C ± 3°C for 120 minutes before cooling to room temperature.

[0035] (4) Oleate-terminated NaLuF4:Tm 3+ (0.5%) / Yb 3+ (20%) / Gd 3+ The (30%) upconversion nanoparticles were precipitated by centrifugation at 4000 rpm for 10 minutes. The nanoparticles were then washed by redispersing the nanoparticles in 5 mL of hexane, inducing precipitation with 20 mL of ethanol, collecting the precipitate by centrifugation at 4000 rpm for 10 minutes, and discarding the supernatant. After this process was repeated twice, the prepared upconversion nanoparticles were embedded in the front surface of the contact lens silicone hydrogel to form an upconversion nanoparticle film layer.

[0036] The internal structure of the middle flexible circuit layer 2 is as follows Figure 3As shown, it mainly includes temperature sensor 21, humidity sensor 22, oxygen sensor 23, main control chip 24, signal filtering module 25, power protection chip 26, flexible wireless power supply antenna 27 and other structures. Among them, temperature sensor 21, humidity sensor 22, oxygen sensor 23 are mainly used for signal monitoring and collection of the internal environment of the eye, and are transmitted to the main control chip 24 through the signal filtering module 25 to remove noise measurement interference, and then the flexible wireless power supply antenna 27 interactively communicates with the external matching equipment in real time to transmit information.

[0037] For the design and preparation of the double-layer circuit structure, first draw the structural schematic diagram of the double-layer circuit in CAD software, as shown in the following figure. Figure 4 As shown. Then import the design schematic into the supporting design software of the UV laser processing system, and generate the upper and lower circuit structures respectively by laser cutting the PI copper-clad film, and connect the two layers of circuit structure through the lead perforation to form a flexible double-layer circuit structure. After that, the corresponding devices are attached according to the pad positions of the flexible circuit and the chip layer chip to form a flexible circuit layer structure with complete signal detection and transmission functions. The flexible wireless power supply antenna can realize the energy supply of the circuit structure in a non-contact manner, and can effectively integrate the functions with the curved surface structure of the eye. The main control chip has a built-in PID control algorithm, and the output power in the circuit structure can be adjusted in time according to the value fed back by the temperature sensor, reducing the accumulation of a large amount of adverse heat generated by the functional chip, preventing damage to the fragile microstructure of the human eye, and realizing the thermal management function of the contact lens working in the internal environment of the eye.

[0038] The silicone hydrogel rear surface 3 as a porous silicone hydrogel substrate can effectively guide the heat loss in the contact lens and prevent the thermal damage effect of the human eye structure caused by adverse heat. The specific preparation method is as follows:

[0039] (1) First, the NaCl particles are processed by a high-speed multifunctional pulverizer to obtain NaCl particles with a diameter of less than 0.075 mm, which are then used in the subsequent preparation of the silicone hydrogel film.

[0040] (2) 2.2 mol of alginate polymer and acrylamide particles (mass ratio of 1:8) were mixed into 30 ml of deionized water solution, and 4 ml of N, N-methylenebisacrylamide (0.06 wt%) and 4 ml of ammonium persulfate (0.06 wt%) were added thereto, mixed and degassed. After adding 2 ml of n, n, n', n'-tetramethylethylenediamine (0.25 wt%) and 1 mol of NaCl particles prepared in step (1), the mixture was poured into a custom-made silicone hydrogel substrate mold.

[0041] (3) Next, the mixture was polymerized by curing with ultraviolet light for 2 hours to produce a porous PAAm hydrogel film. The PAAm hydrogel film prepared by curing was subjected to demolding treatment in an 80°C water bath to obtain a porous silica hydrogel substrate, such as Figure 5 shown.

Claims

1. A contact lens with thermal management function, characterized in that: It comprises, in sequence, a silicone hydrogel front surface (1), an intermediate flexible circuit layer (2), and a silicone hydrogel rear surface (3); An upconversion nanoparticle film (11) having a field of view correction function is provided on the front surface (1) of the silicone hydrogel; The middle flexible circuit layer (2) is provided with a flexible circuit and a chip. The flexible circuit adopts a double-layer wiring structure for power supply and monitoring signal collection and transmission of various temperature, humidity, oxygen concentration and main control chip; The rear surface (3) of the silicone hydrogel is provided with a porous structure (31).

2. A contact lens with thermal management function according to claim 1, characterized in that: The intermediate flexible circuit layer (2) includes a sensor, a main control chip, a signal filtering module, a power protection chip, and a flexible wireless power supply antenna; the sensor is used for monitoring and collecting signals in the intraocular environment, and is transmitted to the main control chip through the signal filtering module to remove noise and measurement interference, and then the flexible wireless power supply antenna uses an interactive real-time communication method to perform information transmission and interaction with external matching devices.

3. The method for preparing a contact lens with thermal management function according to claim 1 or 2, characterized in that: The preparation method of the silicone hydrogel front surface (1) is as follows: (1) First, LuCl3·6H2O, GdCl3·6H2O, YbCl3·6H2O and TmCl3·6H2O were mixed with 1-octadecene and 6 ml of oleic acid in a 100 ml three-necked round-bottom flask; (2) The mixture in the flask was degassed under vacuum and stirred at 380 rpm for 10 minutes at room temperature, then stirred at 120°C ± 5°C for 20 minutes and at 160°C ± 5°C for 10 minutes to obtain a transparent solution; the solution was cooled to 50°C, the vacuum was released, and a methanol solution containing NaOH and NH4F was injected at a rate of 1 mL / min, and the turbid mixture was stirred at 50°C ± 4°C for 30 minutes; (3) Slowly heat the flask under Ar flow to remove methanol and restore vacuum to 90-100°C; the solution is further degassed under vacuum at 120°C ± 5°C for 10 minutes; then, resume Ar flow, remove vacuum, and increase the temperature to 300°C at a rate of 10-17°C / min; maintain the reaction at 300°C ± 3°C for 120 minutes before cooling to room temperature; (4) Oleate-terminated NaLuF4:Tm 3+ / Yb 3+ / Gd 3 The upconversion nanoparticles were precipitated by centrifugation at 4000 rpm for 10 minutes; the nanoparticles were then redispersed in hexane, induced to precipitate with ethanol, and the precipitate was collected by centrifugation at 4000 rpm for 10 minutes, and the supernatant was discarded for washing the nanoparticles; after the washing process was repeated twice, the prepared upconversion nanoparticles were embedded in the front surface of the contact lens silicone hydrogel to form an upconversion nanoparticle film layer; The preparation method of the intermediate flexible circuit layer (2) is as follows: First, draw the structural schematic diagram of the double-layer circuit in the CAD software, then import the design schematic diagram into the supporting design software of the UV laser processing system, and use laser cutting to cut the PI copper film to produce the upper and lower circuit structures respectively, and connect the two layers of circuit structure through the lead perforation to form a flexible double-layer circuit structure; Attach corresponding components according to the pad positions of the flexible circuit and chip layer chips to form a flexible circuit layer structure with complete signal detection and transmission functions; The preparation method of the silicone hydrogel rear surface (3) is as follows: (1) First, the NaCl particles are crushed by a high-speed multifunctional crusher; (2) alginate polymer and acrylamide particles in a mass ratio of 1:8 were dissolved in a deionized water solution, N,N-methylenebisacrylamide and ammonium persulfate were added thereto, mixed and degassed; n,n,n′,n′-tetramethylethylenediamine and NaCl particles were then added, and the mixture was poured into a customized silicone hydrogel substrate mold; (3) The mixture was polymerized by curing with ultraviolet light for 2 hours to produce a porous PAAm hydrogel film; the PAAm hydrogel film prepared by curing was subjected to demolding treatment in an 80°C water bath to obtain a porous silicon hydrogel substrate.

4. The preparation method according to claim 3, characterized in that: The amount of raw materials used in each step of the preparation method of the silicone hydrogel front surface (1) is: In step (1), LuCl3·6H2O, 0.5mmol; GdCl3·6H2O, 0.3mmol; YbCl3·6H2O, 0.2mmol; TmCl3·6H2O, 0.005mmol; 1-octadecene, 15ml; oleic acid 6ml; In step (2), 10 mL of a methanol solution containing 2.5 mmol NaOH and 4 mmol NH4F was injected at a rate of 1 mL / min; In step (4), the nanoparticles were redispersed in 5 mL of hexane and 20 mL of ethanol was used to induce precipitation.

5. The preparation method according to claim 3, characterized in that: The raw material concentrations of each step in the preparation method of the silicone hydrogel rear surface (3) are: In step (2), the aqueous solution of alginate polymer and acrylamide, 2.2 mol; 0.06 wt% N,N-methylenebisacrylamide, 4 ml; 0.06 wt% ammonium persulfate, 4 ml; 0.25 wt% n,n,n',n'-tetramethylethylenediamine, 2 ml; 1 mol NaCl particles.