NiCuZn ferrite material as well as preparation method and application thereof

By adjusting the Fe3+ ion distribution and using Bi2O3-Al2O3 composite film coating technology, the magnetic performance of NiCuZn ferrite materials is improved, the problems of high sintering temperature and low magnetic performance are solved, and high magnetic permeability and high DC bias are achieved Take into account the superposition characteristics.

CN119008163APending Publication Date: 2024-11-22HUNAN UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411257143.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-09
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

When the sintering temperature of existing NiCuZn ferrite materials is higher than the 850-900°C required by the stacked sheet process, it is difficult to take into account the characteristics of high magnetic permeability, saturated magnetic induction strength and high DC bias overlay characteristics, and the beginning of most literature reports The low permeability limits the practical application of the material.

Method used

By preferring the type and doping amount of doped ions Re3+, the pore distribution of Fe3+ ions in the spinel structure is adjusted, combined with water quenching preparation technology, the Bi2O3-Al2O3 composite film is coated with the substrate phase powder material. , adjust the grain size and uniformity, and improve magnetic performance.

Benefits of technology

It achieves the improvement of high starting magnetic permeability, saturated magnetic induction strength and coercive force, reduces the sintering temperature, improves the DC bias superposition characteristics and density of the material, and is suitable for stacked chip inductors.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005034436130000201
    Figure BDA0005034436130000201
  • Figure BDA0005034436130000241
    Figure BDA0005034436130000241
  • Figure HDA0005034436150000011
    Figure HDA0005034436150000011
Patent Text Reader

Abstract

The invention relates to the technical field of magnetic materials, in particular to a NiCuZn ferrite material and a preparation method and application thereof. The NiCuZn ferrite material comprises a spinel phase and a sintering aid, the spinel phase is composed of Ni + 20.35 Cu + 20.2 Zn + 20.45 Fe + 31.98-xRe < 3 + > xO4, Re < 3 + > is one or two of two kinds of ions, the radius of one kind of ions A is close to that of Fe < 3 + >, the radius difference value is smaller than or equal to + / -0.01 nm, and the magnetic moment is zero; the radius of the other type of ions B is at least 0.8 nm longer than that of Fe < 3 + >, and the ion magnetic moment of the other type of ions B is at least 2.0 B.M higher than that of Fe < 3 + >. The method is completed through one step of calcination and water quenching, spinel phase base material powder which is small in particle size, high in anisotropy and rich in hydroxyl functional groups on the surface is obtained, the sintering temperature of the final material is reduced, and the direct current bias superposition characteristic of the final material is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of magnetic materials, and in particular to a NiCuZn ferrite material and a preparation method and application thereof. Background Art

[0002] Due to a series of problems in the overall structural design and optimization of the performance of the base material, the multilayer chip inductor has become a technical bottleneck for further improving the performance of electronic components. The composition of the base material and the optimization of the preparation process have an important impact on the performance improvement of the inductor. NiCuZn ferrite is mainly used as the base material of multilayer chip inductors because of its series of performance advantages, but it also has a high sintering temperature (generally above 1100℃), which cannot be combined with the 850-900℃ sintering required by the multilayer chip process; the DC bias superposition characteristics and the contradiction between the initial magnetic permeability and saturation magnetization intensity need to be solved urgently.

[0003] At present, research on NiCuZn ferrite materials for multilayer chip inductor substrates has been reported one after another:

[0004] The Chinese patent application number is CN201910307835.4, and the invention name is "Low-temperature co-fired soft ferrite powder for laminated chip power inductors and preparation method thereof". The invention discloses a low-temperature co-fired soft ferrite powder for laminated chip power inductors and a preparation method thereof. The formula includes a base material and an additive, wherein the base material, by mass ratio, is Fe2O350.0-70.0%, NiO 5.0-15.0%, ZnO 15-30.0%, and CuO 3.84-9.40%; the additive, by mass ratio, is Bi2O3 1.0-6.0%, frit powder 0.5-6.0%; wherein, the formula of the frit is, by mass ratio, 9-12% alumina, 62-65% silicon dioxide, 5-8% calcium oxide, 0.5-1.0% magnesium oxide, 2.0-4.0% potassium oxide, 1.0-2.0% sodium oxide, 8.0-10.0% boron oxide. The base material is mixed with deionized water, stirred, mixed, dried, and pre-burned, and then the additive is added, mixed with deionized water, dried, and crushed. The magnetic permeability of the powder decreases with the addition of additives, and the DC bias resistance is good. Its sintering temperature is 900℃, and the initial magnetic permeability is about 100; its initial magnetic permeability is low.

[0005] The Chinese patent with application number CN201410629749.2 and invention name "Nickel-zinc ferrite material with high saturation flux density, high DC superposition and high Curie temperature and preparation method thereof" discloses a nickel-zinc ferrite material with high saturation flux density, high DC superposition and high Curie temperature, which contains the following main components: Fe2O3 is 48-52 mol%, ZnO is 18-22 mol%, NiO is 25-29 mol%, and the balance is CuO; relative to the total weight of the main components, it also contains the following content of secondary components: Bi2O3 is 0.01-0.04wt%, Nb2O5 is 0.01-0.05wt%, SnO2 is 0.01-0.06wt%, V2O5 is 0.02-0.06wt%, and the sintering temperature is 1250℃3h. The nickel-zinc ferrite material of the invention is particularly suitable for working at higher wide frequency and lower voltage, and has a higher saturation flux density at both room temperature and high temperature, and can also achieve a more stable inductance function in complex applications with large DC superposition and high integration. The Curie temperature T of the nickel-zinc ferrite material is c >330℃,resistivity P>1×10 6 Ω·m; Under the test condition of 4000A / m, the saturation flux density B of the nickel-zinc ferrite material at 25°C s >470mT, its residual magnetic density B r <350mT, saturation flux density B of the nickel-zinc ferrite material at 100°C s >390mT, its residual magnetic density B r <250mT; the density of the nickel-zinc ferrite material ρ=(5.15±0.05)×10 3 kg / m 3 However, the sintering temperature of the patent is too high at 1250°C, which cannot meet the 850-900°C sintering conditions required by the laminated sheet process.

[0006] The Chinese patent application number is CN201410432796.8, and the invention name is "Anti-bias low temperature sintered NiCuZn ferrite material and its preparation method". It discloses an anti-bias low temperature sintered NiCuZn ferrite material and its preparation method. The main phase of the ferrite material is a spinel structure, and the molecular structure expression is Ni 0.30-x Zn 0.47+x Cu 0.18 Co 0.05 Fe 1.95O4, where x ranges from 0 to 0.05. Based on the above NiCuZn ferrite material, Bi2O3, SnO2, SiO2 and CaCO3 are used as dopants, wherein Bi2O3: 0.5-1wt%, SnO2: 0.8-1.2wt%, SiO2: 0.1-0.2wt%, CaCO3: 0.1-0.2wt%. The ferrite obtained by the invention takes into account the requirements of high initial magnetic permeability and resistance to DC bias magnetic field, and can be widely used in laminated chip inductors that resist large DC bias magnetic fields or high power. However, the sintering densification of the patent sample is 900℃4h, the initial magnetic permeability is about 65, and the H70% is 845A / m, and its initial magnetic permeability is relatively low.

[0007] The Chinese patent application number is CN201710968240.4, and the invention name is "A low-temperature sintered NiCuZn ferrite material and its preparation method". The molecular structure expression of the invented material is Ni 0.29-x-y Zn 0.53+x Cu 0.18+y Fe 1.95 O4 (x = 0-0.02; y = 0-0.02), and BBSZ glass, Co2O3, TiO2 and CaCO3 are used as dopants. Through the above material formula, process optimization design and combined modification of the four dopants, low-temperature sintering at 900°C is achieved, while taking into account the initial magnetic permeability μ i The initial permeability is low between 80-96; the DC bias magnetic field H70% is 950-800A / m, and the specific temperature coefficient is ≤2×10 6 / ℃(20℃-80℃).

[0008] The Chinese patent with application number CN201810578005.0 and invention name "A low-temperature sintered NiCuZn ferrite with DC bias resistance and preparation method" discloses a low-temperature sintered NiCuZn ferrite with DC bias resistance and preparation method. The ferrite includes a main component and a secondary component, and the content of the main component calculated by the respective standard is: Fe2O3 47-50mol%, NiO18-22mol%, ZnO 18-22mol%, CuO 9-13mol%, Co2O3 0.1-0.4mol%, and the content of the secondary component calculated by its standard is: BZB: 0.3-0.6wt%, Bi2O3: 0.03-0.08wt%, CuO: 0-0.03wt%. The NiCuZn ferrite obtained by the invention improves the material's DC bias resistance while ensuring that it has a high sintering density and saturation magnetic induction intensity. The sample was sintered at about 900℃ for 2h, and its initial magnetic permeability was about 90, which is relatively low; the sample density was about 4.83g / cm3; the saturation magnetic induction intensity was 352mT, and the H0.7(μi) value was about 540A / m.

[0009] A Chinese patent with application number CN201210056750.1 and invention name “A high-strength, high-Bs nickel-zinc ferrite and a preparation method thereof” discloses a high-strength, high-Bs nickel-zinc ferrite suitable for power inductors and a preparation method thereof. The nickel-zinc ferrite has iron oxide, nickel oxide, zinc oxide and copper oxide as main components, and the contents thereof calculated based on respective standards are: Fe2O3 49-52.5mol%, NiO2 0-29.5mol%, ZnO 18-28mol%, CuO 2.5-5mol%; and auxiliary components include calcium carbonate, cobalt oxide, zirconium oxide, lithium carbonate, vanadium pentoxide and silicon dioxide, and the contents of auxiliary components relative to the total amount of main components, calculated based on respective standards, are: CaCO3 0.03-0.15wt%, Co2O3 0.01-0.05wt%, ZrO2 0.03-0.13wt%, Li2CO3 0.03-0.10wt%, V2O5 0.03-0.15wt%, SiO2 0.01-0.10wt%. The product is prepared by the oxide method, with a sintering temperature of 1180-1250℃. The crystal grain size of the sintered product is 3-5μm, with distinct grain boundaries; its initial magnetic permeability is 400±25%, saturation magnetic induction intensity Bs: 480±5%mT; Curie temperature Tc≥220℃, and mechanical strength≥210MPa. The product has the characteristics of high strength and high DC bias, which meets the dual requirements of high strength and high DC bias of the material for miniaturization of power inductors. However, the sintering temperature of the patent is too high at 1180-1250℃, which cannot meet the 850-900℃ sintering conditions required by the laminated chip process.

[0010] The paper "Tang X, Zhang H, Su H, et al. Influence of Microstructure on the DCBias-Superposition Characteristics of NiZn Ferrites[J]. IEEE Transactions on Magnetics, 2011, 47(10):4332-4335" The main component of ferrite is Ni 0.3 Zn 0.55 Cu 0.15 Fe2O4, pre-synthesis temperature is 950℃, sintering temperature is 1100-1190℃; mainly by adjusting the sintering temperature to obtain a microstructure dominated by fine grains, the best DC bias resistance H 0.7 (μi): 50A / m, magnetic permeability: 500-730, saturation magnetic induction intensity Bs: 290-332mT. However, the sintering temperature of the paper is too high at 1100-1190℃, which cannot meet the 850-900℃ sintering conditions required by the laminated chip process.

[0011] "Su H, Tang X, Zhang H, et al. Effects of Nb2O5 on DC Bias-Superposition Characteristic of the Low-Temperature-Fired NiCuZn Ferrites[J]. IEEE Transactions on Magnetics, 2013, 49(7): 4222-4225" Changing the saturation magnetic induction intensity B of the sample by doping different contents of Nb2O5 in NiZnCu ferrite s And anti-DC bias performance, the material composition is: Ni 0.38 Cu 0.18 Zn 0.44 Fe 1.95 O4, sintering temperature is 900℃, initial magnetic permeability μi is between 51-125, its initial magnetic permeability is relatively low; saturation magnetic induction intensity Bs is between 240-445mT, H 0.7 (μ i ) is 190-680A / m.

[0012] The paper "Peng Wang, Xiaoli Tang, Huaiwu Zhang, et al. Effects of Al2O3 addition on the DC-bias-superposition characteristic of the low-temperature-fired NiCuZn ferrites[J]. Journal of Alloys and Compounds 803(2019)812-817" prepared low-temperature NiCuZn ferrites with added Al2O3 (0-2wt%) by conventional solid-phase reaction. The effects of different Al2O3 doping amounts on phase composition, microstructure and magnetic properties were studied, especially the DC bias superposition characteristics. The results show that adding an appropriate amount of Al2O3 to NiCuZn ferrite can increase the coercive force and thickness of the non-magnetic grain boundaries, thereby increasing the demagnetization field and reducing the magnetic permeability under the superposition magnetic field. At the same time, with the increase of Al2O3 doping amount, the magnetic permeability and saturation flux density decrease monotonically. When 1.5wt% Al2O3 is added, the sample obtains a relatively high initial permeability (μi=70.7) and an ideal DC bias superposition characteristic (H70%=840A / m). This ferrite material has good application prospects in chip inductors that can carry large currents. However, its initial permeability is low.

[0013] The paper "Yang Wang, Yulan Jing, Peng Wang, et al. Effects of MgO addition on the DC-bias-superposition characteristic of low temperature-fired NiCuZnferrites[J]. Journal of Magnetism and Magnetic Materials 514(2020)167-182" studied the microstructure and magnetic properties of MgO-doped low-temperature sintered NiCuZn ferrites, especially the DC bias superposition characteristics. X-ray diffraction (XRD) showed that all samples were single-phase spinel structures. The microstructure did not change much with the MgO content. The initial magnetic permeability, sintered density and saturation flux density showed a monotonically decreasing trend; with the increase of MgO content, the coercive force gradually increased. When the MgO addition amount was 1.5wt%-2.5wt%, the initial magnetic permeability μi of the ferrite was 70-85, and H0.7 was 846-700A / m, but its initial magnetic permeability was low. It has good application prospects in the field of chip power magnetic devices. However, based on the addition of MgO in the form of powder, in order to achieve uniform distribution of MgO in the ferrite matrix, a large amount of addition is required, which will lead to a decrease in the magnetic properties of the material after sintering because MgO is non-magnetic.

[0014] Analysis of the above literature reports on improving the DC bias superposition characteristics of NiCuZn ferrite materials found that the initial magnetic permeability reported in most literature is less than 100. If the magnetic permeability is higher than 100, its DC superposition resistance will significantly decrease; there are also literatures that increase the magnetic permeability by increasing the sintering temperature, but there are certain problems with co-firing with the silver layer of the chip inductor. In addition, the above research mainly focuses on optimizing the composition of the ferrite base phase, changing the sintering temperature, or doping with different types and contents of additives, all of which are aimed at obtaining a fine grain structure and thus improving the DC bias superposition characteristics of the sample; however, the above results all have certain shortcomings, which limit the practical application of the material. Summary of the invention

[0015] The object of the present invention is to provide a NiCuZn ferrite material having higher magnetic permeability, saturation magnetic induction intensity and high DC bias superposition characteristics and a preparation method thereof.

[0016] In order to achieve the above object, the technical solution of the present invention is as follows:

[0017] A NiCuZn ferrite material comprises a spinel phase and a sintering aid, wherein the spinel phase is composed of Ni +2 0.35 Cu + 20.2 Zn +2 0.45 Fe +3 1.98-x Re 3+ x O4, among which, Re 3+ One or both of the two types of ions, the radius of one type of ion A is similar to that of Fe 3+ The radius difference is less than or equal to ±0.01nm, and the magnetic moment is zero; the radius of another type of ion B is smaller than that of Fe 3+ The radius is at least 0.8nm longer, and the ionic magnetic moment is larger than that of Fe 3+ The ionic magnetic moment is at least 2.0BM; the sintering aids include aids that promote sintering and aids that limit grain growth during sintering.

[0018] In a preferred embodiment, the sintering aid is one or both of Bi2O3 and Nb2O5. The melting point of Bi2O3 is 817°C, and the melting point of Nb2O5 is 1485°C±5°C, so Bi2O3 is preferred as the sintering aid.

[0019] In a preferred embodiment, the additive for limiting grain growth during sintering is one or more of Al2O3, SiO2 and MgO.

[0020] In a preferred embodiment, ion A is Ga 3+ 、Al 3+ One or both of the following.

[0021] Fe 3+ The ionic radius of Ga is 0.055nm and the magnetic moment is 5.92BM. 3+ The ionic radius is 0.062nm and the ionic magnetic moment is 0.00BM; Al 3+ The ionic radius is 0.050nm and the ionic magnetic moment is 0B.M.

[0022] Ion A is Ga 3+ 、Al 3+ When there are two types, control the total addition amount not to exceed the set value.

[0023] These ions enter the spinel lattice ferrite and can adjust the Fe 3+ The distribution at the A and B positions of the spinel structure improves the magnetic properties of the powder and ultimately improves the DC bias superposition characteristics of the material.

[0024] In a preferred embodiment, ion B is Gd 3+ 、Dy 3+ One or both of the following.

[0025] Ion B is Gd 3+ 、Dy 3+ When there are two types, control the total addition amount not to exceed the set value.

[0026] G 3+ :0.938nm,ionic magnetic moment:7.94BM;Dy 3+ : 0.908nm, ion magnetic moment: 10.68BM. Ions enter the spinel structure ferrite, causing structural distortion, which can increase the coercivity of the ferrite base powder, and then improve the DC superposition resistance of the sintered magnetic ring or magnetic sheet.

[0027] In a preferred embodiment, Re 3+ There are two types of ions A and B; the molar ratio of ions A and B is 1-2:1-2.

[0028] Within this range, the magnetic permeability and magnetic induction intensity of the base phase can be effectively improved.

[0029] Based on the existing solid phase method, the present invention selects Re 3+ The type and amount of addition, adjust the Ni 2+ and Fe 3+ The distribution of plasma in tetrahedral pores (A site) and octahedral pores (B site) in the spinel structure increases the magnetic permeability and magnetic induction intensity of the base phase.

[0030] Based on the same inventive concept, the present invention also claims a method for preparing the NiCuZn ferrite material by low temperature sintering, comprising the following steps:

[0031] S1, drying, ball-milling, sintering nickel oxide, copper oxide, zinc oxide, iron oxide and dopant Re2O3, dispersing in water for water quenching, and then drying again to obtain a basic spinel phase;

[0032] S2, adding an alcohol solvent and water to an auxiliary agent precursor for promoting sintering and an auxiliary agent precursor for limiting grain growth during sintering, stirring, adding an acid, and reacting in a water bath to obtain a Bi-Al sol;

[0033] S3, mixing the basic spinel phase and the Bi-Al sol, and then ball milling, drying, and heat treating to obtain a composite powder with a core-shell structure;

[0034] S4, after ball-milling the composite powder, adding a binder and continuing ball-milling to obtain a slurry; spray-granulating the slurry and pressing it to obtain a green body; drying and sintering the green body to obtain the NiCuZn ferrite material.

[0035] The present invention prepares the NiCuZn ferrite material by water quenching, because water has high specific heat, high boiling point, simple structure and low price. Water quenching is actually pouring high-temperature ferrite powder into water. When a certain amount of high-temperature powder is poured into the liquid, the liquid temperature may rise and boil. At the same time, H + and OH - It can react with nickel, copper, zinc, iron and other elements on the surface of ferrite particles to introduce hydroxyl groups; this is beneficial to the coating of the composite sol in the next step; while other solvents will form other functional groups on the surface of ferrite particles, which is not conducive to the coating of the composite sol in the next step.

[0036] In a preferred embodiment, the nickel oxide, copper oxide, zinc oxide, iron oxide and dopant Re2O3 are all micrometer-sized.

[0037] In a preferred embodiment, the particle size D50 of the nickel oxide, copper oxide, zinc oxide, iron oxide and dopant Re2O3 is 0.3-2.5 μm, preferably 0.8-2.0 μm.

[0038] Generally speaking, the particle size of the original powder used in ferrite ceramics is preferably 0.8-2.0 mm.

[0039] If the particle size of the raw material is too large, the pre-synthesis process of the ferrite may result in incomplete reaction and the generation of impurity phases. It may also cause the particle size of the ferrite phase after pre-synthesis to be too large, which is not conducive to the sintering and densification of the ferrite material. Both of these factors will lead to a decrease in the performance of the ferrite after the final sintering. If the particle size of the raw material is too small, on the one hand, it will lead to a significant increase in cost, the smaller the particle size, the more expensive the powder. On the other hand, because the surface energy of nanoparticles is relatively high, the ball milling mixing process is easy to agglomerate, resulting in uneven mixing, which makes the pre-synthesis of ferrite also prone to the generation of impurity phases.

[0040] In a preferred embodiment, the molar ratio of nickel oxide, copper oxide, zinc oxide, iron oxide and dopant Re2O3 is 0.175:0.2:0.45:0.99:0.5x, 0.01≤x≤0.15.

[0041] In a preferred embodiment, the drying and secondary drying in step S1 are performed at a temperature of 60-90° C. and for a time of 20-30 hours.

[0042] In a preferred embodiment, the ball milling medium in step S1 is ethanol or water, preferably ethanol; corundum balls, zirconia balls or agate balls are used as grinding balls, the ball milling time is 4-24 hours, and the ball mill speed is 100-600 rpm. -1 .

[0043] Considering the price, corundum balls are the best.

[0044] Experiments show that if the ball milling time is too short, several oxides are not easy to mix evenly; if the time is too long, the production efficiency is reduced.

[0045] Influence of rotation speed: If the speed of the ball mill is too slow, several oxides are not easy to mix evenly; if the speed is too fast, the energy consumption is high, the equipment is worn out, and the grinding chips generated by the ball mill and grinding balls increase, resulting in an increase in the impurity content in the raw materials, which ultimately leads to a decrease in the performance of the ferrite.

[0046] When ethanol is used as the ball milling medium, the powder obtained after drying the slurry is relatively loose, which may be because ethanol has a relatively small chemical polarity; while when deionized water is used as the ball milling medium, the powder obtained is easy to agglomerate, which is not conducive to the subsequent process, so ethanol is preferred.

[0047] In a preferred embodiment, the ball milling time in step S1 is 8-16 hours, and the ball mill speed is 200-500 rpm. -1 .

[0048] In a preferred embodiment, during the ball milling process in step S1, the mass ratio of material: ball: medium is 1:1-2:1-2.

[0049] The volume of the ball mill is fixed, therefore:

[0050] 1. Influence of materials: If there are too many materials, the several oxides in the raw materials cannot be mixed evenly; if there are too few materials, the slurry obtained in each batch is too small, and the production efficiency is reduced;

[0051] 2. The influence of the medium is just the opposite of that of the material: too much medium, that is, too much water or ethanol, the output of each batch decreases, and the solid content of the slurry is low, which affects the effect of spray granulation;

[0052] Too little medium is equivalent to too much material, and the several oxides in the raw materials cannot be mixed evenly.

[0053] 3. The influence of grinding balls: Too many magic balls will lead to more grinding chips on the one hand, and on the other hand, the output of each batch is too small, and the production efficiency is reduced; too few grinding balls will make it difficult to mix the several oxides in the raw materials.

[0054] In a preferred embodiment, the sintering in step S1 is: 0.2-10°C·mim -1 The heating rate is increased to 400-1200℃ and then kept at this temperature for 0.5-8h; then heated at 0.5-5℃·min -1 The cooling rate is reduced to 200-600℃ and then kept warm for 0.2-4h.

[0055] Influence of heating rate: If the heating rate is too low, production efficiency will be affected and energy consumption will be increased; if the heating rate is too high, there will be a significant temperature difference between the surface and the inside of the mixed powder pile in the furnace. Because the thermal conductivity of the oxide raw materials and the pre-synthesized ferrite powder is relatively low, it is easy for the pre-synthesized ferrite on the surface to be slightly sintered, while the oxide raw materials inside have not yet completely reacted;

[0056] Influence of insulation temperature: If the insulation temperature is too low, the mixed oxides cannot react completely to form ferrite; if the insulation temperature is too high, the formed ferrite powder will produce a certain degree of sintering, which is not good for the water quenching / ball milling mixing in the next process.

[0057] The effect of holding time is similar to that of temperature; a shorter holding time is similar to a lower temperature; a longer holding time is similar to a higher temperature.

[0058] In a preferred embodiment, the heating rate of sintering in step S1 is 2-8°C·min -1 The sintering temperature is 600-1000℃, and the holding time is 0.2-2h; the temperature after cooling is 300-500℃.

[0059] In a preferred embodiment, during the water quenching process in step S1, the molar ratio of the material to water is 1:540-60.

[0060] The molar ratio of material to water is the ratio of material to water. If the molar ratio is too high, it means that there is more material and less water. Because water quenching is actually pouring high-temperature ferrite powder into water, the water temperature will rise due to heat exchange. If the amount of water is too little, it may cause the water to boil or vaporize and splash out, which will cause certain safety hazards in the operation. At the same time, the goal of water quenching - using the temperature difference to break the powder;

[0061] A molar ratio that is too low means that there is less material and more water. This is no problem in principle, but after water quenching, the powder needs to be centrifuged from the water for the next step. Too much water will result in too much workload for the separation operation.

[0062] After water quenching, a base phase powder with fine particle size and rich hydroxyl functional groups on the surface is obtained.

[0063] In a preferred embodiment, the molar ratio of the sintering-promoting auxiliary agent precursor to the basic spinel phase in step S2 is 0.001-0.01:1, preferably 0.002-0.01:1.

[0064] If the ratio is too small, it means that the amount of sintering aid added is too small, which cannot play the role of promoting sintering. The final sintered ferrite has a low density and poor performance.

[0065] If the ratio is too large, it means that too much sintering aid is added, which will cause excessive grain growth during the sintering process. The porosity of the ferrite after sintering is high and the grain size is large, which will lead to poor performance of the final sintered ferrite. After all, water quenching or composite sol coating is to avoid excessive grain growth and ultimately obtain a fine and uniform grain distribution, thereby improving the magnetic properties of the ferrite.

[0066] In a preferred embodiment, the molar ratio of the auxiliary agent precursor for limiting grain growth during sintering to the basic spinel phase in step S2 is 0.001-0.20:1, preferably 0.02-0.15:1.

[0067] If the ratio is too small, it means that the amount of limiting agent added is too little, which will not play the role of limiting the grain growth during the sintering process, and the effect is similar to that of adding too much sintering aid;

[0068] If the ratio is too large, it means that too much limiting agent is added, which will cause the grains to fail to grow or grow with difficulty during the sintering process, and the porosity of the ferrite after sintering is high, resulting in poor performance of the final sintered ferrite.

[0069] In a preferred embodiment, the alcohol solvent is isopropanol or butanol, preferably isopropanol.

[0070] In a preferred embodiment, the acid is a mixed solution of nitric acid and acetic acid.

[0071] In a preferred embodiment, the acid is a mixed solution of hydrochloric acid and acetic acid.

[0072] In a preferred embodiment, the molar ratio of the sintering-promoting auxiliary agent precursor, the auxiliary agent precursor for limiting grain growth during sintering, the alcohol solvent, deionized water, nitric acid and acetic acid is 0.001-1:0.001-1:0.15:25:0.1:0.1.

[0073] In a preferred embodiment, Al in Bi-Al sol 3+ and Bi 3+ The total concentration is 0.004-4mol / L.

[0074] Al in Bi-Al sol 3+ and Bi 3+ If the total concentration of is too high, the stability and fluidity are poor: poor stability means that the sol is easy to gel, and it cannot be used after gelation; poor fluidity will cause the shell layer or thickness formed after the sol coats the powder to be uneven, or the shell layer will not coat the powder completely, resulting in a decrease in the performance of the ferrite;

[0075] Al in Bi-Al sol3+ and Bi 3+ If the total concentration is too low, the shell layer formed by the sol coating on the surface of the powder will be too thin and cannot play the insulating role of the non-magnetic layer.

[0076] In a preferred embodiment, the temperature of the water bath reaction in step S2 is 70-90° C., and the reaction time is 2-3 h.

[0077] If the temperature is too high, water evaporates too quickly, which can easily affect the expected sol concentration; if the temperature is too low, the precursor dissolves too slowly, affecting the progress of the experiment.

[0078] If the time is too long, it will easily affect the expected sol concentration; if the time is too short, the precursor will not be fully dissolved.

[0079] In a preferred embodiment, the water bath reaction in step S2 is allowed to stand to obtain the Bi-Al sol, and the standing time is 200-280 hours.

[0080] In a preferred embodiment, the molar ratio of the basic spinel phase to the Bi-Al sol in step S3 is 1:0.001-0.20.

[0081] The molar ratio of the basic spinel phase to the Bi-Al sol is too large, which means that the addition amount of the sintering aid and the inhibitor is too much at the same time. First of all, the sintering aid and the inhibitor are both non-magnetic materials. If they are added too much, the overall magnetic properties of the ferrite material will decrease after sintering. As for the effect of adding too much at the same time on the composition and microstructure of the ferrite, this has not been studied, and no one has tried to do this.

[0082] The molar ratio of the basic spinel phase to the Bi-Al sol is too small, which means that the amount of sintering aid and inhibitor added is too small at the same time. The limit is that no addition is made, resulting in a significant decrease in the density of the ferrite after sintering, and thus a decrease in magnetic properties.

[0083] In a preferred embodiment, the ball milling medium in step S3 is Bi-Al sol, corundum balls are used as grinding balls, the ball milling time is 1-12 hours, and the ball mill speed is 100-600 rpm. -1 .

[0084] In a preferred embodiment, the ball milling time in step S3 is 2-10 hours, and the rotation speed is 100-500 rpm. -1 .

[0085] In a preferred embodiment, the drying temperature in step S3 is 60-100° C. and the drying time is 20-30 hours.

[0086] In a preferred embodiment, the heating rate of the heat treatment in step S3 is 0.5-4°C·min -1 , the sintering temperature is 200-600℃, and the sintering time is 0.2-4h.

[0087] The essence of heat treatment is the process of shrinking the dried gel to form an oxide network. A certain amount of Al-OH, Al-OR (organic functional group), Bi-OH and other functional groups still exist in the dried dry gel; after heat treatment, a network structure such as Al-O-Al-O- or Al-O-Bi-O- or Bi-O-Bi- is formed. The dry gel coated on the surface of the particles has a certain thickness. When the heating rate is too fast, the surface layer of the gel first dehydrates or dealcoholizes and shrinks to form a dense network, while the inside of the gel has not completed these reactions and will continue to dehydrate or dealcoholize. Because the surface layer is dense, the water or alcohol inside cannot escape quickly and remain inside the film layer. After the temperature rises, the volume of the vapor formed by water and alcohol will increase rapidly, and finally the gel film layer will rupture; if the heating rate is too slow, there is no problem in principle, but the production efficiency is low and the energy consumption is high.

[0088] If the holding time is too short, the dehydration and dealcoholization reactions of the gel cannot be completed completely. These reactions will be completed in the next step of ferrite sintering (because the sintering process temperature is higher), and the water or alcohol produced by the reaction will escape from the inside of the block material in the form of vapor, causing the ferrite to crack and the magnetic properties to decrease. If the holding time is too long, there is no problem in principle, but the production efficiency is low and the energy consumption is high.

[0089] If the sintering temperature is too low, the dehydration and dealcoholization reaction of the gel after drying cannot be carried out thoroughly, and the consequences are similar to those of a short insulation time; if the sintering temperature is too high, the ferrite powder may stick together due to the initial sintering, which is not conducive to the uniform mixing of the binder in the next ball milling process.

[0090] In a preferred embodiment, the heating rate of the heat treatment in step S3 is 0.5-2°C·min -1 , the sintering temperature is 300-500℃, and the sintering time is 0.5-1.5h.

[0091] After sintering, a composite powder with a core-shell structure of Bi2O3-Al2O3 film encapsulating the base phase powder is obtained.

[0092] In a preferred embodiment, the ball milling medium in step S4 is water, and corundum balls are used as grinding balls; during the ball milling process, the mass ratio of material, balls and water is 1:2:1-2.

[0093] In a preferred embodiment, the binder in step S4 is a polyvinyl alcohol aqueous solution, a carboxymethyl cellulose aqueous solution or a dextrin aqueous solution.

[0094] In a preferred embodiment, the concentration of the binder in step S4 is 8-12 wt %.

[0095] If the concentration of the binder is too low, in order to obtain a green body with a certain strength (after the granulated powder is molded, the unsintered sample is called a green body), a large amount of binder aqueous solution needs to be added to ensure that the amount of PVA added reaches a certain value. Because after the green body is formed, it needs to be dried before sintering, and drying will cause water to volatilize, resulting in a higher porosity of the green body. In this way, under the same sintering process, the bulk density of the ferrite obtained after sintering is low, and the magnetic properties are not ideal.

[0096] If the concentration of the binder is too high, its viscosity will be high, and it will not be easy to mix with the ferrite powder during the ball milling process. The distribution of the binder in the granulated powder will be uneven, and the green body after molding will have obvious defects. For example, the powder without binder cannot be molded or has low strength. It will also cause the density of the ferrite after sintering to be uneven, the performance will be reduced, and the batch stability will be very poor.

[0097] In a preferred embodiment, the amount of the binder added in step S4 is 5-15 wt % of the mass of the material to be ground.

[0098] If the amount of binder added is too little, the green body strength and density of the formed body are low, which is not only easy to break, but also the density of the ferrite after sintering is poor and the magnetic properties are low;

[0099] If too much binder is added, the moisture content in the green body will be high and the content of organic PVA will also be high. Therefore, the density of the green body after drying will be low. At the same time, PVA will decompose or be oxidized during the debinding process. These two factors will lead to low density and poor magnetic properties of ferrite after sintering.

[0100] In a preferred embodiment, the ball milling time in step S4 is 0.5-6.0 hours, and the ball mill speed is 50-300 rpm. -1 .

[0101] In a preferred embodiment, the ball milling time in step S4 is 0.5-4 hours, and the ball mill speed is 100-200 rpm. -1 .

[0102] In a preferred embodiment, the spray granulation and compression molding in step S4 are common techniques in the art.

[0103] In a preferred embodiment, the spray granulation process in step S4 is as follows: the slurry solid content is 40-55wt%, and the binder content is 0.5-1.0wt%; during the spray granulation process, the hot air temperature at the dryer inlet is 350-400°C, and the outlet temperature is controlled at 90-110°C.

[0104] In a preferred embodiment, the compression molding process in step S4 is as follows: placing the granulated powder into a mold of a desired diameter, using a 70 MPa pressure to mold, and maintaining the pressure for 1 minute, i.e., compression molding.

[0105] In a preferred embodiment, the green body is dried at a temperature of 60-90° C. for 20-30 hours in step S4.

[0106] In a preferred embodiment, the heating rate of sintering in step S4 is 1-6°C·min -1 , sintering temperature is: 400-1200℃, and sintering time is 1-8h.

[0107] Influence of sintering temperature: If the temperature is too low, sintering cannot be performed and the density of ferrite is poor; if the temperature is too high, the ferrite will have abnormal grain growth and decomposition on the surface; these factors will lead to lower magnetic properties of ferrite after sintering;

[0108] Influence of heating rate: If the heating rate is too fast, the trace moisture in the green body and the gas phase products produced by the decomposition or oxidation of PVA in the debinding section cannot be discharged in time, which will cause cracks or even cracks in the block, making it waste and unusable. If the heating rate is too fast, it is not a problem in principle, but it will lead to a decrease in production efficiency and an increase in energy consumption.

[0109] Influence of holding time: If the holding time is too short, the sintering densification process will not be thorough, the density of the ferrite after sintering will be low, and the magnetic properties will not be ideal; if the holding time is too long, the ferrite grains will grow abnormally and the surface ferrite will decompose a small amount, which will lead to the decline of ferrite performance. At the same time, it will also lead to increased energy consumption and reduced production efficiency.

[0110] In a preferred embodiment, the heating rate of sintering in step S4 is 1-4°C·min -1 , sintering temperature is: 600-1000℃, and sintering time is 2-6h.

[0111] Based on the same inventive concept, the present invention also claims to protect the use of the NiCuZn ferrite material in the preparation of a laminated chip inductor.

[0112] The beneficial effects of the present invention are:

[0113] 1. By preferentially doping ions Re 3+ The type and doping amount of some ions can adjust the Fe content of NiCuZn ferrite. 3 + The distribution number of ions in tetrahedral pores (A position) and octahedral pores (B position) in the base phase spinel structure can improve the initial magnetic permeability and magnetic induction intensity of the base phase powder; some ions can cause the spinel structure of ferrite to distort and increase the coercive force of the base powder. Both methods are beneficial to improve the magnetic properties such as the initial magnetic permeability and DC bias superposition characteristics of ferrite after sintering;

[0114] 2. Through calcination-water quenching in one step, a spinel phase base material powder with fine particle size, strong anisotropy and rich surface hydroxyl functional groups is obtained. The fine particle size of the powder is conducive to reducing the sintering temperature of the final material, and the strong anisotropy is conducive to improving the DC bias superposition characteristics of the final material; the functional groups on the surface of the powder are conducive to improving the uniformity and density of the Bi2O3-Al2O3 composite film wrapping it;

[0115] 3. The base phase powder after water quenching is uniformly coated with a Bi2O3-Al2O3 composite film. On the one hand, it can reduce the amount of sintering aids (Bi2O3) and inhibitors (Al2O3) added, and at the same time, it can effectively control the size and uniformity of the grains of the sintered material, thereby obtaining a dense microstructure with uniform grain size, which improves the DC bias superposition characteristics of the material while ensuring a high sintering density.

[0116] The initial magnetic permeability of the NiCuZn ferrite material prepared by the present invention is 386.1 (Example 1), the maximum magnetic permeability is 1076 (Example 1), the saturation magnetic induction intensity is 372.2mT (Example 1), and the coercive force is 73.3A / m (Example 1). The higher saturation magnetic induction intensity and coercive force result in the NiCuZn ferrite material having a higher magnetic product energy. In the industrial sense, the larger the magnetic energy product of the magnetic material, the less magnetic material is required to produce the same effect, which is conducive to the miniaturization of the device. BRIEF DESCRIPTION OF THE DRAWINGS

[0117] Figure 1 The particle size distribution curves of the base phase powder after water quenching in Example 1 and the base phase powder without water quenching in Comparative Example 2;

[0118] Figure 2 SEM images of the water-quenched base phase powder of Example 1 and the un-water-quenched base phase powder of Comparative Example 2; (a) base phase powder after water quenching; (b) base phase powder without water quenching;

[0119] Figure 3 SEM photos of the ferrite-based powder before and after the powder is coated with the Al-Bi shell layer in Example 1; (a) without shell layer; (b) with shell layer;

[0120] Figure 4 The XRD patterns of the ferrite materials obtained after sintering of Examples 1, 2 and Comparative Example 1;

[0121] Figure 5 The SEM images of the ferrite materials obtained after sintering Example 1 and Comparative Examples 3 and 4; (a) Example 1; (b) Comparative Example 3; (c) Comparative Example 4;

[0122] Figure 6 The XPS spectra of the ferrite materials obtained after sintering of Examples 1, 2 and Comparative Example 1; (a) full spectrum peaks of the three materials; (b) fine peaks of Ni2p and corresponding analytical peaks; (c) fine peaks of Cu2p and corresponding analytical peaks; (d) fine peaks of Zn2p and corresponding analytical peaks; (e) fine peaks of Fe2p and corresponding analytical peaks; (f) fine peaks of Ga2p and corresponding analytical peaks;

[0123] Figure 7 The incremental permeability curves of the sintered ferrites obtained in Examples 1, 2 and Comparative Example 1; DETAILED DESCRIPTION

[0124] The technical scheme of the present invention is further illustrated by specific examples below. Those skilled in the art should understand that the examples are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0125] Example 1Ga 3+ =0.05

[0126] (1) D 50 The five powders of μm-Ni2O3, μm-CuO, μm-ZnO, μm-Fe2O3 and μm-Ga2O3 with a purity of 1.2 μm and a purity of ≥99% are dried at 80°C for 24 hours for use. Bi(NO3)3·5H2O and Al(O-(CH(CH3)2)3 with a purity of ≥99% are used directly. The five powders are weighed respectively according to the molar ratio of Ni2O3:CuO:ZnO:Fe2O3:Ga2O3 equal to 0.175:0.2:0.45:0.965:0.025;

[0127] (2) Weighed μm-Ni2O3, μm-CuO, μm-ZnO, μm-Fe2O3 and μm-Ga2O3 powders were added into a ball mill, with ethanol as the medium and corundum balls as the grinding balls. The ratio of material: ball: ethanol was 1:2:1.5 (mass ratio). The ball mill was first milled for 12 h at a speed of 400 rpm. -1 The slurry was dried at 80 °C for 24 h and then heated at 5 °C·min -1 The temperature was raised to 850℃ and then kept at this temperature for 2h to obtain the spinel Ni 0.35 Cu0.2 Zn 0.45 Fe 1.93 Ga 0.05 O4 base phase powder; then at 2℃·mim -1 The temperature was lowered to 500℃ at a rate of 1:50 and kept at this temperature for 0.5h. The powder was taken out and poured into a certain mole number of deionized water at 25℃ (the ratio of base phase powder to deionized water was 1:50 (molar ratio)). -1 The suspension was stirred for 2 hours, and then dried at 80° C. to obtain a base phase powder with fine particle size and rich surface hydroxyl functional groups after water quenching;

[0128] (3) According to the ratio of water-quenched powder: Bi-N: Al-iso-p of 1:0.004:0.07 (molar ratio), Bi(NO3)3·5H2O and Al(O-(CH(CH3)2)3 were weighed respectively, and then the corresponding solvents were measured according to the ratio of Bi-N: Al-iso-p: isopropanol: deionized water: nitric acid: acetic acid of 0.004 mol: 0.07 mol: 0.15 mol: 25 mol: 0.1 mol: 0.1 mol. The weighed Al-iso-p and Bi-N were first added to the mixed solvent of isopropanol and deionized water, and stirred in a water bath at 80°C until the solution was clear. Then, the nitric acid and acetic acid solutions were added to the solution in sequence, and the solution was stirred in a water bath at 80°C for 2 h. After sealing, the solution was allowed to stand for 24 h to obtain a Bi-Al sol with a stability time of more than 240 h at room temperature.

[0129] (4) Add the water-quenched base phase powder and the Bi-Al sol prepared in the previous step into a ball mill, use the Bi-Al sol as the medium and corundum balls as the grinding balls, and ball mill for 8 hours at a speed of 400 rpm. -1 The milled slurry was dried at 90°C and then heated to 1°C·min -1 The heating rate is increased to 500°C and kept for 1 hour to obtain a spinel-based composite powder wrapped with a Bi2O3-Al2O3 composite film;

[0130] (5) Add the composite powder into a ball mill, using water as the medium and corundum balls as the grinding balls. The material: ball: water ratio is 1:2:1.5 (mass ratio), and a binder polyvinyl alcohol aqueous solution (the concentration of the binder aqueous solution is 5wt%) is added at 10wt% of the total mass of the powder. The ball milling time is 2h and the ball mill speed is 200 rpm. -1 The ball milled slurry is sprayed and granulated, and then pressed to obtain a green body; the green body is dried at 80°C for 24 hours, and then buried with powder at 2°C·mim -1 The temperature is raised to 950°C and kept for 3 hours to obtain the target material.

[0131] Take SEM photos of the ferrite-based powder before and after the powder is coated with the Al-Bi shell layer in Example 1. Figure 3 As shown in the figure, (a) without shell layer; (b) with shell layer. It can be seen from the figure that the Al-Bi shell layer is evenly coated on the surface of the ferrite matrix powder particles.

[0132] Example 2Ga 3+ =0.025;

[0133] (1) D 50 The five powders of μm-Ni2O3, μm-CuO, μm-ZnO, μm-Fe2O3 and μm-Ga2O3 with a purity of 1.2 μm and a purity of ≥99% are dried at 80°C for 24 hours for use. Bi(NO3)3·5H2O and Al(O-(CH(CH3)2)3 with a purity of ≥99% are used directly. The five powders are weighed respectively according to the molar ratio of Ni2O3:CuO:ZnO:Fe2O3:Ga2O3 equal to 0.175:0.2:0.45:0.9775:0.0125;

[0134] (2) Weighed μm-Ni2O3, μm-CuO, μm-ZnO, μm-Fe2O3 and μm-Ga2O3 were added to a ball mill, with ethanol as the medium and corundum balls as the grinding balls. The ratio of material: ball: ethanol was 1:2:1.5 (mass ratio). The ball mill was first milled for 12 h at a speed of 400 rpm. -1 The slurry was dried at 80 °C for 24 h and then heated at 5 °C·min -1 The temperature was raised to 850℃ and then kept at this temperature for 2h to obtain the spinel Ni 0.35 Cu 0.2 Zn 0.45 Fe 1.955 Ga 0.025 O4 base phase powder; then at 2℃·mim -1 The temperature was lowered to 500℃ at a rate of 1:50 and kept at this temperature for 0.5h. The powder was taken out and poured into a certain mole number of deionized water at 25℃ (the ratio of base phase powder to deionized water was 1:50 (molar ratio)). -1 The suspension was stirred for 2 hours, and then dried at 80° C. to obtain a base phase powder with fine particle size and rich surface hydroxyl functional groups after water quenching;

[0135] (3) According to the ratio of water-quenched powder: Bi-N: Al-iso-p of 1:0.004:0.07 (molar ratio), Bi(NO3)3·5H2O and Al(O-(CH(CH3)2)3 were weighed respectively, and then the corresponding solvents were measured according to the ratio of Bi-N: Al-iso-p: isopropanol: deionized water: nitric acid: acetic acid of 0.004 mol: 0.07 mol: 0.15 mol: 25 mol: 0.1 mol: 0.1 mol. The weighed Al-iso-p and Bi-N were first added to the mixed solvent of isopropanol and deionized water, and stirred in a water bath at 80°C until the solution was clear. Then, the nitric acid and acetic acid solutions were added to the solution in sequence, and the solution was stirred in a water bath at 80°C for 2 h. After sealing, the solution was allowed to stand for 24 h to obtain a Bi-Al sol with a stability time of more than 240 h at room temperature.

[0136] (4) Add the water-quenched base phase powder and the Bi-Al sol prepared in the previous step into a ball mill, use the Bi-Al sol as the ball milling medium, and corundum balls as the grinding balls. Ball milling for 8 hours at a speed of 400 rpm -1 The milled slurry was dried at 90°C and then heated to 1°C·min -1 The heating rate is increased to 500°C and kept for 1 hour to obtain a spinel-based composite powder wrapped with a Bi2O3-Al2O3 composite film;

[0137] (5) Add the composite powder into a ball mill, using water as the medium and corundum balls as the grinding balls. The material: ball: water ratio is 1:2:1.5 (mass ratio), and a binder polyvinyl alcohol aqueous solution (the concentration of the binder aqueous solution is 5wt%) is added at 10wt% of the total mass of the powder. The ball milling time is 2h and the ball mill speed is 200 rpm. -1 The ball milled slurry is sprayed and granulated, and then pressed to obtain a green body; the green body is dried at 80°C for 24 hours, and then buried with powder at 2°C·mim -1 Raise the temperature to 950℃ and keep it for 3h to obtain the target material.

[0138] Example 3A1 3+ =0.05

[0139] (1) D 50 The five powders of μm-Ni2O3, μm-CuO, μm-ZnO, μm-Fe2O3 and μm-Al2O3 with a purity of 1.2 μm and a purity of ≥99% are dried at 80°C for 24 hours for use. Bi(NO3)3·5H2O and Al(O-(CH(CH3)2)3 with a purity of ≥99% are used directly. The five powders are weighed respectively according to the molar ratio of Ni2O3:CuO:ZnO:Fe2O3:Al2O3 equal to 0.175:0.2:0.45:0.965:0.025;

[0140] (2) Weighed μm-Ni2O3, μm-CuO, μm-ZnO, μm-Fe2O3 and μm-Al2O3 were added to a ball mill, with ethanol as the medium and corundum balls as the grinding balls. The ratio of material: ball: ethanol was 1:2:1.5 (mass ratio). The ball mill was first milled for 12 h at a speed of 400 rpm. -1 The slurry was dried at 80 °C for 24 h and then heated at 5 °C·min -1 The temperature was raised to 850℃ and then kept at this temperature for 2h to obtain the spinel Ni 0.35 Cu 0.2 Zn 0.45 Fe 1.93 Al 0.05 O4 base phase powder; then at 2℃·mim -1 The temperature was lowered to 500℃ at a rate of 1:50 and kept at this temperature for 0.5h. The powder was taken out and poured into a certain mole number of deionized water at 25℃ (the ratio of base phase powder to deionized water was 1:50 (molar ratio)). -1 The suspension was stirred for 2 hours, and then dried at 80° C. to obtain a base phase powder with fine particle size and rich surface hydroxyl functional groups after water quenching;

[0141] (3) According to the ratio of water-quenched powder: Bi-N: Al-iso-p of 1:0.004:0.07 (molar ratio), Bi(NO3)3·5H2O and Al(O-(CH(CH3)2)3 were weighed respectively, and then the corresponding solvents were measured according to the ratio of Bi-N: Al-iso-p: isopropanol: deionized water: nitric acid: acetic acid of 0.004 mol: 0.07 mol: 0.15 mol: 25 mol: 0.1 mol: 0.1 mol. The weighed Al-iso-p and Bi-N were first added to the mixed solvent of isopropanol and deionized water, and stirred in a water bath at 80°C until the solution was clear. Then, the nitric acid and acetic acid solutions were added to the solution in sequence, and the solution was stirred in a water bath at 80°C for 2 h. After sealing, the solution was allowed to stand for 24 h to obtain a Bi-Al sol with a stability time of more than 240 h at room temperature.

[0142] (4) Add the water-quenched base phase powder and the Bi-Al sol prepared in the previous step into a ball mill, use the Bi-Al sol as the medium and corundum balls as the grinding balls, and ball mill for 8 hours at a speed of 400 rpm. -1 The milled slurry was dried at 90°C and then heated to 1°C·min -1 The heating rate was increased to 500°C and kept for 1 hour to obtain a spinel-based composite powder wrapped with a Bi2O3-Al2O3 composite film having a core-shell structure;

[0143] (5) Add the composite powder into a ball mill, using water as the medium and corundum balls as the grinding balls. The material: ball: water ratio is 1:2:1.5 (mass ratio), and a binder polyvinyl alcohol aqueous solution (the concentration of the binder aqueous solution is 5wt%) is added at 10wt% of the total mass of the powder. The ball milling time is 2h and the ball mill speed is 200 rpm. -1 The ball milled slurry is sprayed and granulated, and then pressed to obtain a green body; the green body is dried at 80°C for 24 hours, and then buried with powder at 2°C·mim -1 The temperature is raised to 950°C and kept for 3 hours to obtain the target material.

[0144] Example 4Gd 3+ =0.05

[0145] (1) D 50 The five powders of μm-Ni2O3, μm-CuO, μm-ZnO, μm-Fe2O3 and μm-Gd2O3 with a purity of 1.2 μm and a purity of ≥99% are dried at 80°C for 24 hours for use. Bi(NO3)3·5H2O and Al(O-(CH(CH3)2)3 with a purity of ≥99% are used directly. The five powders are weighed respectively according to the molar ratio of Ni2O3:CuO:ZnO:Fe2O3:Gd2O3 equal to 0.175:0.2:0.45:0.965:0.025;

[0146] (2) Weighed μm-Ni2O3, μm-CuO, μm-ZnO, μm-Fe2O3 and μm-Gd2O3 were added to a ball mill, with ethanol as the medium and corundum balls as the grinding balls. The ratio of material: ball: ethanol was 1:2:1.5 (mass ratio). The ball mill was first milled for 12 h at a speed of 400 rpm. -1 The slurry was dried at 80 °C for 24 h and then heated at 5 °C·min -1 The temperature was raised to 850℃ and then kept at this temperature for 2h to obtain the spinel Ni 0.35 Cu 0.2 Zn 0.45 Fe 1.93 G 0.05 O4 base phase powder; then at 2℃·mim -1 The temperature was lowered to 500℃ at a rate of 1:50 and kept at this temperature for 0.5h. The powder was taken out and poured into a certain mole number of deionized water at 25℃ (the ratio of base phase powder to deionized water was 1:50 (molar ratio)). -1 The suspension was stirred for 2 hours, and then dried at 80° C. to obtain a base phase powder with fine particle size and rich surface hydroxyl functional groups after water quenching;

[0147] (3) According to the ratio of water-quenched powder: Bi-N: Al-iso-p of 1:0.004:0.07 (molar ratio), Bi(NO3)3·5H2O and Al(O-(CH(CH3)2)3 were weighed respectively, and then the corresponding solvents were measured according to the ratio of Bi-N: Al-iso-p: isopropanol: deionized water: nitric acid: acetic acid of 0.004 mol: 0.07 mol: 0.15 mol: 25 mol: 0.1 mol: 0.1 mol. The weighed Al-iso-p and Bi-N were first added to the mixed solvent of isopropanol and deionized water, and stirred in a water bath at 80°C until the solution was clear. Then, the nitric acid and acetic acid solutions were added to the solution in sequence, and the solution was stirred in a water bath at 80°C for 2 h. After sealing, the solution was allowed to stand for 24 h to obtain a Bi-Al sol with a stability time of more than 240 h at room temperature.

[0148] (4) Add the water-quenched base phase powder and the Bi-Al sol prepared in the previous step into a ball mill, use the Bi-Al sol as the medium and corundum balls as the grinding balls, and ball mill for 8 hours at a speed of 400 rpm. -1 The milled slurry was dried at 90°C and then heated to 1°C·min -1 The heating rate is increased to 500°C and kept for 1 hour to obtain a spinel-based composite powder wrapped with a Bi2O3-Al2O3 composite film;

[0149] (5) Add the composite powder into a ball mill, using water as the medium and corundum balls as the grinding balls. The material: ball: water ratio is 1:2:1.5 (mass ratio), and a binder polyvinyl alcohol aqueous solution (the concentration of the binder aqueous solution is 5wt%) is added at 10wt% of the total mass of the powder. The ball milling time is 2h and the ball mill speed is 200 rpm. -1 The ball milled slurry is sprayed and granulated, and then pressed to obtain a green body; the green body is dried at 80°C for 24 hours, and then buried with powder at 2°C·mim -1 Raise the temperature to 950℃ and keep it for 3h to obtain the target material.

[0150] Example 5Dy 3+ =0.05

[0151] (1) D 50 The five powders of μm-Ni2O3, μm-CuO, μm-ZnO, μm-Fe2O3 and μm-Dy2O3 with a purity of 1.2 μm and a purity of ≥99% are dried at 80°C for 24 hours for use. Bi(NO3)3·5H2O and Al(O-(CH(CH3)2)3 with a purity of ≥99% are used directly. The five powders are weighed respectively according to the molar ratio of Ni2O3:CuO:ZnO:Fe2O3:Dy2O3 equal to 0.175:0.2:0.45:0.965:0.025;

[0152] (2) Weighed μm-Ni2O3, μm-CuO, μm-ZnO, μm-Fe2O3 and μm-Dy2O3 were added to a ball mill, with ethanol as the medium and corundum balls as the grinding balls. The ratio of material: ball: ethanol was 1:2:1.5 (mass ratio). The ball mill was first milled for 12 h at a speed of 400 rpm. -1 The slurry was dried at 80 °C for 24 h and then heated at 5 °C·min -1 The temperature was raised to 850℃ and then kept at this temperature for 2h to obtain the spinel Ni 0.35 Cu 0.2 Zn 0.45 Fe 1.93 Dy 0.05 O4 base phase powder; then at 2℃·mim -1 The temperature was lowered to 500℃ at a rate of 1:50 and kept at this temperature for 0.5h. The powder was taken out and poured into a certain mole number of deionized water at 25℃ (the ratio of base phase powder to deionized water was 1:50 (molar ratio)). -1 The suspension was stirred for 2 hours, and then dried at 80° C. to obtain a base phase powder with fine particle size and rich surface hydroxyl functional groups after water quenching;

[0153] (3) According to the ratio of water-quenched powder: Bi-N: Al-iso-p of 1:0.004:0.07 (molar ratio), Bi(NO3)3·5H2O and Al(O-(CH(CH3)2)3 were weighed respectively, and then the corresponding solvents were measured according to the ratio of Bi-N: Al-iso-p: isopropanol: deionized water: nitric acid: acetic acid of 0.004 mol: 0.07 mol: 0.15 mol: 25 mol: 0.1 mol: 0.1 mol. The weighed Al-iso-p and Bi-N were first added to the mixed solvent of isopropanol and deionized water, and stirred in a water bath at 80°C until the solution was clear. Then, the nitric acid and acetic acid solutions were added to the solution in sequence, and the solution was stirred in a water bath at 80°C for 2 h. After sealing, the solution was allowed to stand for 24 h to obtain a Bi-Al sol with a stability time of more than 240 h at room temperature.

[0154] (4) Add the water-quenched base phase powder and the Bi-Al sol prepared in the previous step into a ball mill, use the Bi-Al sol as the medium and corundum balls as the grinding balls, and ball mill for 8 hours at a speed of 400 rpm. -1 The milled slurry was dried at 90°C and then heated to 1°C·min -1 The heating rate is increased to 500°C and kept for 1 hour to obtain a spinel-based composite powder wrapped with a Bi2O3-Al2O3 composite film;

[0155] (5) Add the composite powder into a ball mill, using water as the medium and corundum balls as the grinding balls. The material: ball: water ratio is 1:2:1.5 (mass ratio), and a binder polyvinyl alcohol aqueous solution (the concentration of the binder aqueous solution is 5wt%) is added at 10wt% of the total mass of the powder. The ball milling time is 2h and the ball mill speed is 200 rpm. -1 The ball milled slurry is sprayed and granulated, and then pressed to obtain a green body; the green body is dried at 80°C for 24 hours, and then buried with powder at 2°C·mim -1 Raise the temperature to 950℃ and keep it for 3h to obtain the target material.

[0156] Example 6Ga 3+ =0.025, Gd 3+ =0.025;

[0157] (1) D 50 The six powders of μm-Ni2O3, μm-CuO, μm-ZnO, μm-Fe2O3, μm-Ga2O3 and μm-Gd2O3 with a purity of 1.2 μm and a purity of ≥99% are dried at 80°C for 24 hours for use. Bi(NO3)3·5H2O and Al(O-(CH(CH3)2)3 with a purity of ≥99% are used directly. The six powders are weighed respectively according to the molar ratio of Ni2O3:CuO:ZnO:Fe2O3:Ga2O3:Gd2O3 equal to 0.175:0.2:0.45:0.965:0.0125:0.0125;

[0158] (2) Weighed μm-Ni2O3, μm-CuO, μm-ZnO, μm-Fe2O3, μm-Ga2O3 and μm-Gd2O3 were added to a ball mill, with ethanol as the medium and corundum balls as the grinding balls. The ratio of material: ball: ethanol was 1:2:1.5 (mass ratio). The ball mill was first milled for 12 h at a speed of 400 rpm. -1 The slurry was dried at 80 °C for 24 h and then heated at 5 °C·min -1 The temperature was raised to 850℃ and then kept at this temperature for 2h to obtain the spinel Ni 0.35 Cu 0.2 Zn 0.45 Fe 1.93 Ga 0.025 G 0.025 O4 base phase powder; then at 2℃·mim -1 The temperature was lowered to 500℃ at a rate of 1:50 and kept at this temperature for 0.5h. The powder was taken out and poured into a certain mole number of deionized water at 25℃ (the ratio of base phase powder to deionized water was 1:50 (molar ratio)). -1 The suspension was stirred for 2 hours, and then dried at 80° C. to obtain a base phase powder with fine particle size and rich surface hydroxyl functional groups after water quenching;

[0159] (3) According to the ratio of water-quenched powder: Bi-N: Al-iso-p of 1:0.004:0.07 (molar ratio), Bi(NO3)3·5H2O and Al(O-(CH(CH3)2)3 were weighed respectively, and then the corresponding solvents were measured according to the ratio of Bi-N: Al-iso-p: isopropanol: deionized water: nitric acid: acetic acid of 0.004 mol: 0.07 mol: 0.15 mol: 25 mol: 0.1 mol: 0.1 mol. The weighed Al-iso-p and Bi-N were first added to the mixed solvent of isopropanol and deionized water, and stirred in a water bath at 80°C until the solution was clear. Then, the nitric acid and acetic acid solutions were added to the solution in sequence, and the solution was stirred in a water bath at 80°C for 2 h. After sealing, the solution was allowed to stand for 24 h to obtain a Bi-Al sol with a stability time of more than 240 h at room temperature.

[0160] (4) Add the water-quenched base phase powder and the Bi-Al sol prepared in the previous step into a ball mill, use the Bi-Al sol as the ball milling medium, and corundum balls as the grinding balls. Ball milling for 8 hours at a speed of 400 rpm -1 The milled slurry was dried at 90°C and then heated to 1°C·min -1 The heating rate is increased to 500°C and kept for 1 hour to obtain a spinel-based composite powder wrapped with a Bi2O3-Al2O3 composite film;

[0161] (5) Add the composite powder into a ball mill, using water as the medium and corundum balls as the grinding balls. The material: ball: water ratio is 1:2:1.5 (mass ratio), and a binder polyvinyl alcohol aqueous solution (the concentration of the binder aqueous solution is 5wt%) is added at 10wt% of the total mass of the powder. The ball milling time is 2h and the ball mill speed is 200 rpm. -1 The ball milled slurry is sprayed and granulated, and then pressed to obtain a green body; the green body is dried at 80°C for 24 hours, and then buried with powder at 2°C·mim -1 Raise the temperature to 950℃ and keep it for 3h to obtain the target material.

[0162] Comparative Example 1: No Ga2O3

[0163] (1) D 50 Four kinds of powders, namely, μm-Ni2O3, μm-CuO, μm-ZnO and μm-Fe2O3, with a purity of 1.2 μm and ≥99%, were dried at 80°C for 24 hours for later use. Bi(NO3)3·5H2O and Al(O-(CH(CH3)2)3 with a purity of ≥99% were used directly. The four kinds of powders were weighed respectively according to the molar ratio of Ni2O3:CuO:ZnO:Fe2O3 being 0.175:0.2:0.45:0.99;

[0164] (2) Weighed μm-Ni2O3, μm-CuO, μm-ZnO and μm-Fe2O3 were added to a ball mill, with ethanol as the medium and corundum balls as the grinding balls. The ratio of material: ball: ethanol was 1:2:1.5 (mass ratio). The ball mill was first milled for 12 h at a speed of 400 rpm. -1 The slurry was dried at 80 °C for 24 h and then heated at 5 °C·min -1 The temperature was raised to 850℃ and then kept at this temperature for 2h to obtain the spinel Ni 0.35 Cu 0.2 Zn 0.45 Fe 1.98 O4 base phase powder; then at 2℃·mim -1 The temperature was lowered to 500℃ at a rate of 1:50 and kept at this temperature for 0.5h. The powder was taken out and poured into a certain molar number of deionized water at 25℃ (the ratio of base phase powder to deionized water was 1:50 (molar ratio)). -1 The suspension was stirred for 2 hours, and then dried at 80° C. to obtain a base phase powder with fine particle size and rich surface hydroxyl functional groups after water quenching;

[0165] (3) According to the ratio of water-quenched powder: Bi-N: Al-iso-p of 1:0.004:0.07 (molar ratio), Bi(NO3)3·5H2O and Al(O-(CH(CH3)2)3 were weighed respectively, and then the corresponding solvents were measured according to the ratio of Bi-N: Al-iso-p: isopropanol: deionized water: nitric acid: acetic acid of 0.004 mol: 0.07 mol: 0.15 mol: 25 mol: 0.1 mol: 0.1 mol. The weighed Al-iso-p and Bi-N were first added to the mixed solvent of isopropanol and deionized water, and stirred in a water bath at 80°C until the solution was clear. Then, the nitric acid and acetic acid solutions were added to the solution in sequence, and the solution was stirred in a water bath at 80°C for 2 h. After sealing, the solution was allowed to stand for 24 h to obtain a Bi-Al sol with a stability time of more than 240 h at room temperature.

[0166] (4) Add the water-quenched base phase powder and the Bi-Al sol prepared in the previous step into a ball mill, use the Bi-Al sol as the medium and corundum balls as the grinding balls, and ball mill for 8 hours at a speed of 400 rpm. -1 The milled slurry was dried at 90°C and then heated to 1°C·min -1 The heating rate is increased to 500°C and kept for 1 hour to obtain a spinel-based composite powder wrapped with a Bi2O3-Al2O3 composite film;

[0167] (5) Add the composite powder into a ball mill, using water as the medium and corundum balls as the grinding balls. The material: ball: water ratio is 1:2:1.5 (mass ratio), and a binder polyvinyl alcohol aqueous solution (the concentration of the binder aqueous solution is 5wt%) is added at 10wt% of the total mass of the powder. The ball milling time is 2h and the ball mill speed is 200 rpm. -1 The ball milled slurry is sprayed and granulated, and then pressed to obtain a green body; the green body is dried at 80°C for 24 hours, and then buried with powder at 2°C·mim -1 Raise the temperature to 950℃ and keep it for 3h to obtain the target material.

[0168] The ferrite materials obtained after sintering of Examples 1, 2 and Comparative Example 1 were subjected to XRD patterns. Figure 4 As shown in the figure, it can be seen that the compositions of the three materials are all spinel structure ferrites, and no impurity phase is generated, which indicates that Ga 3+ Doping does not change the crystal structure of ferrite. At the same time, no characteristic peaks of crystal growth limiter (Al2O3) and sintering aid (Bi2O3) were detected, which may be due to the small amount of these two additives added.

[0169] The ferrite materials obtained after sintering of Examples 1, 2 and Comparative Example 1 were subjected to XPS spectra. Figure 6 As shown, (a) full spectrum peaks of the three materials; (b) fine peaks of Ni2p and corresponding analytical peaks; (c) fine peaks of Cu2p and corresponding analytical peaks;

[0170] (d) Fine peak of Zn2p and its corresponding analytical peak; (e) Fine peak of Fe2p and its corresponding analytical peak; (f) Fine peak of Ga2p and its corresponding analytical peak.

[0171] The summary results are listed in Table 1.

[0172] Table 1 Ni content in ferrite materials obtained after sintering of Examples 1, 2 and Comparative Example 1 2+ 2p , Cu 2+ 2p 、Zn 2+ 2p , Fe 3+ 2p and Ga 3 + 2p Binding energy data and relative area of ​​ions

[0173]

[0174] It can be seen from the table that Zn 2+ and Ga 3+ Mainly occupy tetrahedral positions, while Cu 2+ , Ni2+ and Fe 3+ It can occupy both tetrahedral and octahedral pore positions at the same time. 3+ As the amount of Ni added increases, 2+ and Fe 3+ The content of octahedral pores in the spinel structure increases, while Cu 2+ The content of tetrahedral pores increases. 2+ The ionic magnetic moment (1.73BM) is significantly smaller than that of Ni 2 + and Fe 3+ The corresponding values ​​of Ga 3+ As the amount of addition increases, the molecular magnetic moment of the material increases and its magnetic properties are improved, which is consistent with the results in Table 2.

[0175] The sintered ferrites obtained in Examples 1, 2 and Comparative Example 1 were plotted as incremental permeability curves. Figure 7 As shown in the figure, when the magnetic permeabilities of Examples 1, 2 and Comparative Example 1 are 70% of the initial values, the corresponding strengths of the external bias magnetic field are 346 A / m, 323 A / m and 282 A / m respectively.

[0176] Comparative Example 2 is not water quenched, compared with Example 1

[0177] (1) D 50 The five powders of μm-Ni2O3, μm-CuO, μm-ZnO, μm-Fe2O3 and μm-Ga2O3 with a purity of 1.2 μm and a purity of ≥99% are dried at 80°C for 24 hours for use. Bi(NO3)3·5H2O and Al(O-(CH(CH3)2)3 with a purity of ≥99% are used directly. The five powders are weighed respectively according to the molar ratio of Ni2O3:CuO:ZnO:Fe2O3:Ga2O3 equal to 0.175:0.2:0.45:0.965:0.025;

[0178] (2) Weighed μm-Ni2O3, μm-CuO, μm-ZnO, μm-Fe2O3 and μm-Ga2O3 were added to a ball mill, with ethanol as the medium and corundum balls as the grinding balls. The ratio of material: ball: ethanol was 1:2:1.5 (mass ratio). The ball mill was first milled for 12 h at a speed of 400 rpm. -1 The slurry was dried at 80 °C for 24 h and then heated at 5 °C·min -1 The temperature was raised to 850℃ and then kept at this temperature for 2h to obtain the spinel Ni 0.35 Cu 0.2 Zn 0.45 Fe 1.93 Ga 0.05O4 base phase powder;

[0179] (3) According to the ratio of powder: Bi-N: Al-iso-p of 1:0.004:0.07 (molar ratio), Bi(NO3)3·5H2O and Al(O-(CH(CH3)2)3 were weighed respectively, and then the corresponding solvents were measured according to the ratio of Bi-N: Al-iso-p: isopropanol: deionized water: nitric acid: acetic acid of 0.004mol:0.07mol:0.15mol:25mol:0.1mol:0.1mol. The weighed Al-iso-p and Bi-N were first added to the mixed solvent of isopropanol and deionized water, and stirred in a water bath at 80°C until the solution was clear. Then, the nitric acid and acetic acid solutions were added to the solution in sequence, and the solution was stirred in a water bath at 80°C for 2h. After sealing, the solution was allowed to stand for 24h to obtain a Bi-Al sol with a stability time of more than 240h at room temperature.

[0180] (4) Add the base phase powder and the Bi-Al sol prepared in the previous step into a ball mill, use the Bi-Al sol as the medium and corundum balls as the grinding balls, and ball mill for 8 hours at a speed of 400 rpm. -1 The milled slurry was dried at 90°C and then heated to 1°C·min -1 The heating rate is increased to 500°C and kept for 1 hour to obtain a spinel-based composite powder wrapped with a Bi2O3-Al2O3 composite film;

[0181] (5) The composite powder is added to a ball mill, with water as the ball milling medium and corundum balls as the grinding balls. The material: ball: water ratio is 1:2:1.5 (mass ratio), and a binder polyvinyl alcohol aqueous solution (the concentration of the binder aqueous solution is 5wt%) is added at 10wt% of the total mass of the powder. The ball milling time is 2h and the ball mill speed is 200 rpm. -1 The ball milled slurry is sprayed and granulated, and then pressed to obtain a green body; the green body is dried at 80°C for 24 hours, and then buried with powder at 2°C·mim -1 The temperature is raised to 950°C and kept for 3 hours to obtain the target material.

[0182] The particle size distribution curves of the water-quenched base phase powder of Example 1 and the unquenched base phase powder of Comparative Example 2 are plotted as follows: Figure 1 As shown in the figure, it can be seen that after water quenching, the secondary particle size D50 of the base phase powder decreases from 11.16 μm to 7.28 μm, and the distribution is more concentrated, which is conducive to the improvement of the magnetic properties of the ferrite material after sintering.

[0183] The water-quenched base phase powder of Example 1 and the un-water-quenched base phase powder of Comparative Example 2 were taken as SEM images. Figure 2As shown in the figure, before and after water quenching, the particle shape and primary particle size of the base phase powder did not change significantly, roughly between 200-700nm, but after water quenching, the particles had multiple fractures (as shown in the red circles in the figure), which led to a significant decrease in its secondary particle size, which is consistent with the particle size analysis results.

[0184] Comparative Example 3 does not add growth limiting agent, compared with Example 1

[0185] (1) D 50 The five powders of μm-Ni2O3, μm-CuO, μm-ZnO, μm-Fe2O3 and μm-Ga2O3 with a purity of 1.2 μm and ≥99% were dried at 80°C for 24 hours for use, and Bi(NO3)3·5H2O with a purity of ≥99% was used directly. The five powders were weighed according to the molar ratio of Ni2O3:CuO:ZnO:Fe2O3:Ga2O3 equal to 0.175:0.2:0.45:0.965:0.025;

[0186] (2) Weighed μm-Ni2O3, μm-CuO, μm-ZnO, μm-Fe2O3 and μm-Ga2O3 were added to a ball mill, with ethanol as the medium and corundum balls as the grinding balls. The ratio of material: ball: ethanol was 1:2:1.5 (mass ratio). The ball mill was first milled for 12 h at a speed of 400 rpm. -1 The slurry was dried at 80 °C for 24 h and then heated at 5 °C·min -1 The temperature was raised to 850℃ and then kept at this temperature for 2h to obtain the spinel Ni 0.35 Cu 0.2 Zn 0.45 Fe 1.93 Ga 0.05 O4 base phase powder; then at 2℃·mim -1 The temperature was lowered to 500℃ at a rate of 1:50 and kept at this temperature for 0.5h. The powder was taken out and poured into a certain mole number of deionized water at 25℃ (the ratio of base phase powder to deionized water was 1:50 (molar ratio)). -1 The suspension was stirred for 2 hours, and then dried at 80° C. to obtain a base phase powder with fine particle size and rich surface hydroxyl functional groups after water quenching;

[0187] (3) Weigh Bi(NO3)3·5H2O in a ratio of 1:0.004 (molar ratio) of water-quenched powder:Bi-N, and then weigh the corresponding solvents in a ratio of 0.004mol:0.15mol:25mol:0.1mol:0.1mol of Bi-N:isopropanol:deionized water:nitric acid:acetic acid. First, add the weighed Bi-N to the mixed solvent of isopropanol and deionized water, stir in a water bath at 80°C until the solution is clear, then add the measured nitric acid and acetic acid solutions to the solution in turn, continue stirring in a water bath at 80°C for 2h, seal and let stand for 24h to obtain a Bi sol with a stability time of more than 240h at room temperature;

[0188] (4) Add the water-quenched base phase powder and the Bi sol prepared in the previous step into a ball mill, use the sol as the medium and corundum balls as the grinding balls, and ball mill for 8 hours at a speed of 400 rpm. -1 The milled slurry was dried at 90°C and then heated to 1°C·min -1 The heating rate was increased to 500°C and kept for 1 hour to obtain a spinel-based composite powder with a core-shell structure and a Bi2O3 film wrapped therein;

[0189] (5) Add the composite powder into a ball mill, using water as the medium and corundum balls as the grinding balls. The ratio of raw material: ball: water is 1:2:1.5 (mass ratio), and a binder polyvinyl alcohol aqueous solution (the concentration of the binder aqueous solution is 5wt%) is added to the total weight of the powder. The ball milling time is 2h, and the ball mill speed is 200 rpm. -1 The ball milled slurry is sprayed and granulated, and then pressed to obtain a green body; the green body is dried at 80°C for 24 hours, and then buried with powder at 2°C·mim -1 The temperature is raised to 950°C and kept for 3 hours to obtain the target material.

[0190] Comparative Example 4 does not add sintering aids, compared with Example 1

[0191] (1) D 50 The five powders of μm-Ni2O3, μm-CuO, μm-ZnO, μm-Fe2O3 and μm-Ga2O3 with a purity of 1.2 μm and ≥99% were dried at 80°C for 24 hours for use, and Al(O-(CH(CH3)2)3 with a purity of ≥99% was used directly. The five powders were weighed according to the molar ratio of Ni2O3:CuO:ZnO:Fe2O3:Ga2O3 equal to 0.175:0.2:0.45:0.965:0.025;

[0192] (2) Weighed μm-Ni2O3, μm-CuO, μm-ZnO, μm-Fe2O3 and μm-Ga2O3 were added to a ball mill, with ethanol as the medium and corundum balls as the grinding balls. The ratio of material: ball: ethanol was 1:2:1.5 (mass ratio). The ball mill was first milled for 12 h at a speed of 400 rpm. -1 The slurry was dried at 80 °C for 24 h and then heated at 5 °C·min -1 The temperature was raised to 850℃ and then kept at this temperature for 2h to obtain the spinel Ni 0.35 Cu 0.2 Zn 0.45 Fe 1.93 Ga 0.05 O4 base phase powder; then at 2℃·mim -1 The temperature was lowered to 500℃ at a rate of 1:50 and kept at this temperature for 0.5h. The powder was taken out and poured into a certain mole number of deionized water at 25℃ (the ratio of base phase powder to deionized water was 1:50 (molar ratio)). -1 The suspension was stirred for 2 hours, and then dried at 80° C. to obtain a base phase powder with fine particle size and rich surface hydroxyl functional groups after water quenching;

[0193] (3) Al(O-(CH(CH3)2)3 is weighed in a ratio of 1:0.07 (molar ratio) of water-quenched powder to Al-iso-p, and then the corresponding solvents are respectively measured in a ratio of 0.07 mol:0.15 mol:25 mol:0.1 mol:0.1 mol of Al-iso-p:isopropanol:deionized water:nitric acid:acetic acid. The weighed Al-iso-p is first added to the mixed solvent of isopropanol and deionized water, and stirred in a water bath at 80°C until the solution is clear. Then, the nitric acid and acetic acid solutions are added to the solution in sequence, and stirring is continued in a water bath at 80°C for 2 hours. After sealing, the solution is allowed to stand for 24 hours to obtain an Al sol with a stability time of more than 240 hours at room temperature.

[0194] (4) Add the water-quenched base phase powder and the Al sol prepared in the previous step into a ball mill, use the Al sol as the medium and corundum balls as the grinding balls, and ball mill for 8 hours at a speed of 400 rpm. -1 The milled slurry was dried at 90°C and then heated to 1°C·min -1 The heating rate was increased to 500°C and kept for 1 hour to obtain a spinel-based composite powder with a core-shell structure and Al2O3 film wrapped therein;

[0195] (5) Add the composite powder into a ball mill, using water as the medium and corundum balls as the grinding balls. The material: ball: water ratio is 1:2:1.5 (mass ratio), and a binder polyvinyl alcohol aqueous solution (the concentration of the binder aqueous solution is 5wt%) is added at 10wt% of the total mass of the powder. The ball milling time is 2h and the ball mill speed is 200 rpm. -1 The ball milled slurry is sprayed and granulated, and then pressed to obtain a green body; the green body is dried at 80°C for 24 hours, and then buried with powder at 2°C·mim -1 Raise the temperature to 950℃ and keep it for 3h to obtain the target material.

[0196] The ferrite materials obtained after sintering Example 1 and Comparative Examples 3 and 4 were taken as SEM images. Figure 5 As shown in the figure, it can be seen that at the same sintering temperature, the microscopic morphology of the obtained ferrite materials is very different: in the comparative example 3 without adding the crystal growth restrictor, the ferrite grains grow abnormally, and the grain size is about 25μm ( Figure 5 -b), significantly higher than that of adding crystal growth limiting agent Figure 5 -a and 5-c are about 1 μm; while the morphology of the ferrite material obtained without adding sintering aids is shown in Figure 5 -c (Comparative Example 4), compared Figure 5 -a (Example 1), the density of the obtained material is significantly reduced, and the pores are significantly increased.

[0197] The volume density and main magnetic properties of the ferrite materials of the embodiment and the comparative example were measured, and the results were as follows:

[0198] Table 2 Volume density and magnetic properties of sintered ferrite obtained in Examples and Comparative Examples

[0199]

[0200] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A NiCuZn ferrite material, characterized in that: It includes spinel phase and sintering aid, and the spinel phase composition is Ni +2 0.35 Cu +2 0.2 Zn +2 0.45 Fe +3 1.98-x Re 3+ x O4, among which, Re 3+ One or both of the two types of ions, the radius of one type of ion A is similar to that of Fe 3+ The radius difference is less than or equal to ±0.01nm, and the magnetic moment is zero; the radius of another type of ion B is smaller than that of Fe 3+ The radius is at least 0.8nm longer, and the ionic magnetic moment is larger than that of Fe 3+ The ionic magnetic moment is at least 2.0BM; the sintering aids include aids that promote sintering and aids that limit grain growth during sintering.

2. The NiCuZn ferrite material according to claim 1, characterized in that: The auxiliary agent for promoting sintering is one or two of Bi2O3 and Nb2O5; the auxiliary agent for limiting grain growth during sintering is one or more of Al2O3, SiO2 and MgO.

3. The NiCuZn ferrite material according to claim 1 or 2, characterized in that: Ion A is Ga 3+ 、Al 3+ One or two of the following; ion B is Gd 3+ 、Dy 3+ One or both of the following.

4. A method for preparing the NiCuZn ferrite material according to any one of claims 1 to 3, characterized in that: The following steps are involved: S1, drying, ball-milling, sintering nickel oxide, copper oxide, zinc oxide, iron oxide and dopant Re2O3, dispersing in water for water quenching, and then drying again to obtain a basic spinel phase; S2, adding an alcohol solvent and water to an auxiliary agent precursor for promoting sintering and an auxiliary agent precursor for limiting grain growth during sintering, stirring, adding an acid, and reacting in a water bath to obtain a Bi-Al sol; S3, mixing the basic spinel phase and the Bi-Al sol, and then ball milling, drying, and heat treating to obtain a composite powder with a core-shell structure; S4, after ball-milling the composite powder, adding a binder and continuing ball-milling to obtain a slurry; spray-granulating the slurry and pressing it to obtain a green body; drying and sintering the green body to obtain the NiCuZn ferrite material.

5. The preparation method according to claim 4, characterized in that: The particle size D50 of the nickel oxide, copper oxide, zinc oxide, iron oxide and dopant Re2O3 is 0.3-2.5 μm, preferably 0.8-2.0 μm; the molar ratio of the nickel oxide, copper oxide, zinc oxide, iron oxide and dopant Re2O3 is 0.175:0.2:0.45:0.99:0.5x, 0.01≤x≤0.

15.

6. The preparation method according to claim 4, characterized in that: The drying and secondary drying in step S1 are performed at a temperature of 60-90°C for 20-30 hours; the ball milling medium is ethanol or water, preferably ethanol; corundum balls, zirconia balls or agate balls are used as grinding balls, the ball milling time is 4-24 hours, and the ball mill speed is 100-600 rpm. -1 ; During the ball milling process, the mass ratio of material: ball: medium is 1:1-2:1-2.

7. The preparation method according to claim 4, characterized in that: The sintering in step S1 is: 0.2-10°C·mim -1 The heating rate is increased to 400-1200℃ and then kept at this temperature for 0.5-8h; then heated at 0.5-5℃·min -1 The cooling rate is reduced to 200-600°C and then kept warm for 0.2-4h; during the water quenching process in step S1, the molar ratio of the material to water is 1:540-60.

8. The preparation method according to claim 4, characterized in that: The molar ratio of the auxiliary agent precursor for promoting sintering to the basic spinel phase in step S2 is 0.001-0.01:1; preferably 0.002-0.01:1; the molar ratio of the auxiliary agent precursor for limiting grain growth during sintering to the basic spinel phase in step S2 is 0.001-0.20:1; preferably 0.02-0.15:1; Al in Bi-Al sol 3+ and Bi 3+ The total concentration is 0.004-4 mol / L; the temperature of the water bath reaction in step S2 is 70-90°C, and the reaction time is 2-3h.

9. The preparation method according to claim 4, characterized in that: The heating rate of the heat treatment in step S3 is 0.5-4°C·min -1 The sintering temperature is 200-600°C, and the sintering time is 0.2-4h; the sintering heating rate in step S4 is 1-6°C·mim -1 , sintering temperature is: 400-1200℃, and sintering time is 1-8h.

10. Use of the NiCuZn ferrite material according to any one of claims 1 to 3 in preparing a laminated chip inductor.