All-inorganic up-conversion display
Through the over-crystal bonding technology, the complex process and low efficiency of all-inorganic upconversion components are solved due to the lattice mismatch, and the low driving voltage and high light response to light frequency are achieved. All-inorganic upconverter display.
Patent Information
- Application Number
- CN202310554707.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-17
- Publication Date
- 2024-11-22
AI Technical Summary
The existing all-inorganic upconversion components have complex processes, high driving voltage, and low light response to light to light frequency due to lattice mismatch.
The photodiode array is combined with the solder bumps of the light emitting diode array by using over-crystal bonding technology to form a nanometer-type inorganic semiconductor photodiode array and light emitting diode array, reducing the driving voltage and increasing the light response to light to light frequency.
The low driving voltage and high light response to light frequency of inorganic semiconductor materials are achieved, which solves the problems caused by lattice matching and improves the photoelectric conversion efficiency and the application potential of the display.
Smart Images

Figure CN119008608A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to an up-converter, and in particular to a fully inorganic up-converter display. Background Art
[0002] Well-known upconversion devices (also called upconversion devices) can generally be divided into the following four types: inorganic photodiode combined with inorganic light-emitting diode (PD-LED), inorganic photodiode combined with organic light-emitting diode (PD-OLED), organic photodiode combined with organic light-emitting diode (OPD-OLED), and colloidal quantum dot (CQD).
[0003] There are two ways to make up-conversion elements using III-V inorganic compound semiconductors. One is to directly epitaxially grow the film structure of LED and PD on the same substrate during the epitaxial stage, and the other is to melt-bond the LED epitaxial wafer and the PD epitaxial wafer to bond the two epitaxial wafers together before the subsequent element manufacturing process. The former directly epitaxially grows the LED film structure and the PD film structure on the same substrate, and special considerations need to be given to the selection of material lattice match, the relationship between the material composition ratio and the energy gap. The latter requires the selection of appropriate temperature, pressure, and gas for wafer melting and bonding to bond the LED epitaxial wafer and the PD epitaxial wafer together. Improper temperature and pressure will cause wafer cracking or interface defects. Therefore, the size of the wafer melt bonding that can currently be used to make up-conversion elements is only 1mm×1mm, and the yield of the produced up-conversion elements is low, the photoelectric conversion efficiency is also low, and it only stays in the laboratory stage and is difficult to reach the scale of mass production.
[0004] At present, the mainstream of up-conversion display is all-organic up-conversion element or all-organic up-conversion element containing colloidal quantum dots. Because organic up-conversion element or OLED has the tendency of vertical current flow, all-organic up-conversion element can be directly made into pixelless display with large area. However, the luminous band of such display is mostly limited to green light or a few red light, and the light source that can be irradiated is also limited to infrared laser light below 1000nm, and its photoelectric conversion efficiency is almost below 10%. In addition, the highest light-to-light frequency is only 20kHz. More importantly, the luminous imaging of such display is almost only the English letter aperture of infrared laser light passing through black film, which is difficult to be used as a practical field application. Although the requirements for lattice matching of all-organic up-conversion element or PD-OLED hybrid up-conversion element are far less stringent than those of inorganic semiconductors. However, due to the large lateral diffusion current, leakage current and unfavorable interface layer of the organic layer, there are still problems such as low up-conversion efficiency from infrared to visible light and the need to use high bias voltage.
[0005] Since up-conversion components are widely used in the back-end, such as nighttime displays, biomedical imaging, and pathological testing, the relevant industry players are all seeking to improve up-conversion components to expand their uses. Although compared with organic up-conversion components, all-inorganic PD-LEDs have excellent photoelectric properties, such as the light conversion components disclosed by the applicant in the invention patent case No. TWI684801 in Taiwan, China. However, as mentioned above, there are many bottlenecks in the manufacturing process of all-inorganic up-conversion components, and they are still gradually abandoned.
[0006] It can be seen from the above description that solving the problem of all-inorganic up-conversion elements caused by lattice mismatch, reducing the driving voltage and improving the frequency response of light to light are issues to be overcome by relevant technicians in the technical field to which this case belongs. Summary of the invention
[0007] The object of the present invention is to provide an all-inorganic up-conversion display which can solve the problem of all-inorganic up-conversion elements caused by lattice mismatch so as to reduce the driving voltage and improve the frequency response of light to light.
[0008] The all-inorganic up-conversion display of the present invention comprises a photodiode array and a light-emitting diode array.
[0009] The photodiode array includes a substrate containing carriers of a first conductivity type, a buffer layer formed on a first surface of the substrate, an absorption layer formed on the buffer layer, a cap layer formed on the absorption layer, a patterned passivation layer formed on the cap layer and exposing an array of contact regions of the cap layer, a common electrode connected to the substrate, an electrode array, and an array of solder bumps. The common electrode of the photodiode array exhibits the electrical properties of the first conductivity type. Each contact region of the cap layer contains carriers of a second conductivity type opposite to the first conductivity type. Each electrode of the photodiode array is connected to its corresponding contact region and exhibits the electrical properties of the second conductivity type. Each solder bump of the photodiode array is connected to its corresponding electrode.
[0010] The light-emitting diode array includes a substrate, a light-emitting crystal array, a common electrode, a patterned passivation layer, and a solder bump array. Each light-emitting crystal has a first layer formed on the substrate and containing a first conductive type of carrier, a second layer formed on the first layer corresponding to each and containing a second conductive type of carrier, a light-emitting layer sandwiched between the first layer and the second layer corresponding to each, and a pixel electrode exhibiting the second conductive type of electrical property and electrically connected to the second layer corresponding to each, and the first layers of the light-emitting crystals are connected to each other. The common electrode of the light-emitting diode array exhibits the first conductive type of electrical property and is arranged on the first layer of each light-emitting crystal to surround the light-emitting layer corresponding to each. The patterned passivation layer of the light-emitting diode array covers the light-emitting crystal array and the common electrode, and exposes the end edges of each pixel electrode and the common electrode. Each solder bump of the light-emitting diode array is connected to the corresponding pixel electrode. In the present invention, each solder bump of the photodiode array is flip-chip bonded to each solder bump of the light-emitting diode array.
[0011] In the all-inorganic up-conversion display of the present invention, the common electrode of the photodiode array is formed on the second surface of the substrate which is opposite to the first surface.
[0012] In the all-inorganic up-conversion display of the present invention, each light-emitting crystal grain also has a current diffusion layer, and the current diffusion layer of each light-emitting crystal grain is sandwiched between the corresponding pixel electrode and the second layer.
[0013] In the all-inorganic up-conversion display of the present invention, the first conductive type carriers contained in the substrate of the photodiode array are N-type carriers, the second conductive type carriers contained in each contact area of the covering layer of the photodiode array are P-type carriers, the common electrode of the photodiode array is a common cathode, and each electrode of the photodiode array is an anode.
[0014] In the all-inorganic up-conversion display of the present invention, the first conductive type carriers contained in the first layer of the light-emitting crystal array are N-type carriers, the second conductive type carriers contained in the second layer of the light-emitting crystal array are P-type carriers, the common electrode of the light-emitting diode array is a common cathode, and the pixel electrode of each light-emitting crystal is a pixel anode.
[0015] In the all-inorganic up-conversion display of the present invention, each solder bump is made of a metal material selected from the following group: indium, gold, tin, gold-indium alloy, gold-tin alloy, indium-tin alloy, gold-indium-tin alloy, tin-lead alloy, gold-germanium alloy, and gold-silicon alloy.
[0016] The all-inorganic up-conversion display of the present invention has the photodiode array being a nanometer photodiode array, a sub-nanometer photodiode array, or a micro photodiode array, and the light-emitting diode array being a nanometer light-emitting diode array, a sub-nanometer light-emitting diode array, or a micro light-emitting diode array.
[0017] The beneficial effects of the present invention are that the photodiode array and the light-emitting diode array are not affected by lattice matching because they are formed on their own substrates, and each solder bump of the photodiode array is combined with each solder bump of the light-emitting diode array via flip chip bonding technology, which can solve the problem caused by lattice matching. In addition, the photodiode array and the light-emitting diode array are both made of inorganic semiconductor materials, which can reduce the driving voltage and improve the frequency response of light to light. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Other features and effects of the present invention will be clearly presented in the embodiments with reference to the accompanying drawings, in which:
[0019] Figure 1 is a front view schematic diagram illustrating an embodiment of the all-inorganic up-conversion display of the present invention;
[0020] Figure 2 is a front view schematic diagram illustrating a film structure of a short-wave infrared (SWIR) inorganic micro photodiode array (hereinafter referred to as MicroPD array) of a specific example of the all-inorganic up-conversion display of the present invention;
[0021] Figure 3 is a front view schematic diagram illustrating the film structure of a micro light emitting diode array (hereinafter referred to as MicroLED array) based on AlGaInP in the specific example of the present invention;
[0022] Figure 4 is a front view schematic diagram illustrating the film structure of a GaInN-based MicroLED array of the specific example of the present invention;
[0023] Figure 5is a field emission scanning electron microscope (FE-SEM) cross-sectional image, illustrating a microscopic image of the In bumps of the SWIR inorganic MicroPD array of the specific example of the present invention being flip-chip bonded to the In bumps of the GaInN-based MicroLED array;
[0024] Figure 6 It is a color image. Figure 6 (a) to Figure 6 (g) illustrates the red, orange, yellow, green, blue, purple and yellow-green (hereinafter referred to as UV-A) images of a 512×512 all-inorganic up-conversion display excited by 1550 nm laser light;
[0025] Figure 7a is a graph of the relationship between photocurrent and photoresponsivity and input laser power, illustrating the 512×512 all-inorganic up-conversion display excited by 1550nm input laser power to red, orange and yellow, which are biased at 9V, 9V and 8V respectively;
[0026] Figure 7b is a graph of photocurrent and photoresponsivity versus input laser power, illustrating a 512×512 all-inorganic up-conversion display excited to green, blue, violet and UV-A by an input laser power of 1550 nm, which is biased at 4V, 6V, 5V and 5V respectively;
[0027] Figure 8a is a graph of the relationship between output power, external quantum efficiency and power-to-power efficiency versus input laser power, illustrating the use of 1550nm input laser power to excite red, orange and yellow 512×512 all-inorganic up-conversion displays, which are biased at 9V, 9V and 8V respectively;
[0028] Figure 8b is a graph of output power, external quantum efficiency and power efficiency versus input laser power, illustrating a 512×512 all-inorganic up-conversion display excited to green, blue, violet and UV-A with an input laser power of 1550 nm, which is biased at 4V, 6V, 5V and 5V respectively;
[0029] Fig. 9 is a measured frequency response;
[0030] Fig.10 is a schematic diagram of a visible light imaging system;
[0031] Fig.11is a pattern of a shaped aperture of a black mask;
[0032] Fig.12 It is Fig.10 The images of the red, orange, yellow, green, blue, purple and UV-A rings of 512×512 all-inorganic up-conversion display biased at 9V, 9V, 8V, 4V, 6V, 5V and 5V respectively obtained by the visible light imaging system;
[0033] Fig.13 It is Fig.10 The images of the panda in red, orange, yellow, green, blue, purple and UV-A obtained by the visible light imaging system of the 512×512 all-inorganic up-conversion display biased at 9V, 9V, 8V, 4V, 6V, 5V and 5V respectively;
[0034] Fig.14 It is Fig.10 The visible light imaging system obtained the images of the leopard in red, orange, yellow, green, blue, violet and UV-A with the 512×512 all-inorganic up-conversion display biased at 9V, 9V, 8V, 4V, 6V, 5V and 5V respectively;
[0035] Fig.15 It is Fig.10 The visible light imaging system obtained the images of red, orange, yellow, green, blue, violet and UV-A of the 512×512 all-inorganic up-conversion display biased at 9V, 9V, 8V, 4V, 6V, 5V and 5V respectively;
[0036] Fig.16 It is Fig.10 The visible light imaging system obtained the images of the 512×512 all-inorganic up-conversion display of red, orange, yellow, green, blue, purple and UV-A with ODEL biased at 9V, 9V, 8V, 4V, 6V, 5V and 5V respectively;
[0037] Fig.17 is a schematic diagram illustrating the application of the all-inorganic up-conversion display of the present invention to a night camera;
[0038] Fig.18 is a schematic diagram of another visible light imaging system; and
[0039] Fig.19 It is a color image. Fig.19 (a) to (h) respectively describe Fig.18Tungsten filament images of a 512×512 all-inorganic up-conversion display in raw, red, orange, yellow, green, blue, violet and UV-A obtained by a visible light imaging system, which are biased at 0V, 9V, 9V, 8V, 4V, 6V, 5V and 5V respectively. DETAILED DESCRIPTION
[0040] See also Figure 1 An embodiment of the all-inorganic up-conversion display D of the present invention includes a photodiode 2 array and a light-emitting diode 3 array.
[0041] The photodiode 2 array includes a substrate 21 containing carriers of the first conductivity type, a buffer layer 22 formed on a first surface 211 of the substrate 21, an absorption layer 23 formed on the buffer layer 22, a cover layer 24 formed on the absorption layer 23, a patterned passivation layer 25 formed on the cover layer 24 and exposing an array of contact areas 241 of the cover layer 24, a common electrode 26 connected to the substrate 21, an electrode 27 array, and a solder bump 28 array. The common electrode 26 of the photodiode 2 array exhibits the electrical properties of the first conductivity type. Each contact area 241 of the cover layer 24 contains carriers of the second conductivity type opposite to the first conductivity type. Each electrode 27 of the photodiode 2 array is connected to the corresponding contact area 241 and exhibits the electrical properties of the second conductivity type. Each solder bump 28 of the photodiode 2 array is connected to the corresponding electrode 27. In the embodiment of the present invention, the common electrode 26 of the photodiode array 2 is formed on a second surface 212 of the substrate 2 opposite to the first surface 211 .
[0042] The photodiode 2 applicable to the embodiment of the present invention may be an avalanche photodiode (APD) or a pin photodiode (positive-intrinsic-negative photodiode, pin PD) mainly made of group IV semiconductor materials or group III-V semiconductor materials.
[0043] The light emitting diode 3 array includes a substrate 31, an array of light emitting crystal grains 32, a common electrode 33, a patterned passivation layer 34, and an array of solder bumps 35. Each light emitting crystal grain 32 has a buffer layer 320 formed on the substrate 31, a first layer 321 formed on the buffer layer 320 and containing first conductive type carriers, a second layer 322 formed on the first layer 321 corresponding to each other and containing second conductive type carriers, a light emitting layer 323 sandwiched between the first layer 321 and the second layer 322 corresponding to each other, and a pixel electrode 324 exhibiting the second conductive type electrical property and electrically connected to the second layer 322 corresponding to each other, and the first layers 321 of the light emitting crystal grains 32 are connected to each other. The common electrode 33 of the light emitting diode 3 array exhibits the first conductive type electrical property and is disposed on the first layer 321 of each light emitting crystal grain 32 to surround the light emitting layer 323 corresponding to each other. The patterned passivation layer 34 of the light emitting diode 3 array covers the light emitting crystal grains 32 array and the common electrode 33, and exposes one end edge of each pixel electrode 324 and the common electrode 33. Each solder bump 35 of the light emitting diode 3 array is connected to the corresponding pixel electrode 324. In this embodiment of the present invention, each solder bump 28 of the photodiode 2 array is flip-chip bonded to each solder bump 35 of the light emitting diode 3 array.
[0044] Preferably, each light-emitting crystal grain 32 further has a current diffusion layer 325. The current diffusion layer 325 of each light-emitting crystal grain 32 is sandwiched between the corresponding pixel electrode 324 and the second layer 322. Each solder bump 28, 35 suitable for this embodiment of the present invention is made of a metal material selected from the group consisting of: indium (In), gold (Au), tin (Sn), gold-indium alloy, gold-tin alloy, indium-tin alloy, gold-indium-tin alloy, tin-lead alloy, gold-germanium alloy, and gold-silicon (Si) alloy.
[0045] In this embodiment of the present invention, the first conductive type carriers contained in the substrate 21 of the photodiode 2 array are N-type carriers, the second conductive type carriers contained in each contact area 241 of the covering layer 24 of the photodiode 2 array are P-type carriers, the common electrode 26 of the photodiode 2 array is a common cathode, and each electrode 27 of the photodiode 2 array is an anode; the first conductive type carriers contained in the first layer 321 of the light-emitting crystal grain 32 array are N-type carriers, the second conductive type carriers contained in the second layer 322 of the light-emitting crystal grain 32 array are P-type carriers, the common electrode 33 of the light-emitting diode 3 array is a common cathode, and the pixel electrode 324 of each light-emitting crystal grain 32 is a pixel anode.
[0046] The photodiode 2 array of the present invention is a nanometer photodiode array, a sub-nanometer photodiode array, or a micro photodiode array; the light emitting diode 3 array of the present invention is a nanometer light emitting diode array, a sub-nanometer light emitting diode array, or a micro light emitting diode array. In the embodiment of the present invention, the photodiode 2 array and the light emitting diode 3 array are respectively described by taking the micro photodiode array and the micro light emitting diode array as examples, but are not limited thereto.
[0047] The present invention provides a specific example according to this embodiment. In the all-inorganic up-conversion display D of this specific example of the present invention, 512×512 pixels are used as an example for explanation; that is, this specific example of the present invention is used as an example of flip-chip bonding of the solder bumps on each anode of a 512×512 MicroPD (pin planar MicroPD) array to the solder bumps on each pixel anode of a 512×512 mesa-type MicroLED array, which has a pixel size of 15μm and a pitch of 21μm, and a resolution of up to 1210 PPI. Specifically, this specific example of the present invention is to produce a plurality of 512×512 all-inorganic up-conversion displays and then conduct electrical analysis and back-end applications on each of them. Therefore, the produced 512×512 all-inorganic up-conversion display includes a plurality of short-wave infrared (hereinafter referred to as SWIR) inorganic (InGaAs / InP) MicroPD arrays 4 (see Figure 2 , only showing a single SWIR inorganic MicroPD array 4), multiple AlGaInP-based MicroLED arrays 5 (see Figure 3 , only a single AlGaInP-based MicroLED array 5) and multiple GaInN-based MicroLED arrays 6 (see Figure 4 , only a single GaInN-based MicroLED array 6 is shown); wherein, the solder bumps on an anode array of a portion of each SWIR inorganic MicroPD array 4 are flip-chip bonded to the solder bumps on an anode array of the corresponding AlGaInP-based MicroLED array 5, and the solder bumps on an anode array of the remaining portion of each SWIR inorganic MicroPD array 4 are flip-chip bonded to the solder bumps on an anode array of the corresponding GaInN-based MicroLED array 6. The specific method of making each 512×512 all-inorganic up-conversion display of this specific example of the present invention is described in detail as follows.
[0048] <Process of manufacturing each SWIR inorganic MicroPD array 4>
[0049] First, a film structure 42 of each SWIR inorganic MicroPD array 4 is deposited on a S-doped n-type substrate by metal organic chemical vapor deposition (MOCVD). + On an upper surface 411 of the InP (100) substrate 41, a 0.5 μm undoped InP buffer layer 421, a 3 μm undoped In 0.53 Ga 0.47 As absorption layer 422, and a 1 μm undoped InP cap layer 423. The designed thickness is 3 μm undoped InP 0.53 Ga 0.47 The As absorption layer 422 is expected to have a higher photocurrent and thus a higher photoresponsivity.
[0050] Next, a 300nm SiNx dielectric layer is deposited on each corresponding undoped InP cap layer 423 by plasma-assisted chemical vapor deposition (PECVD) at 300°C and 20W plasma power to serve as a mask for subsequent rapid thermal diffusion (hereinafter referred to as RTD), and finally as a SiNx passivation layer 43 of each SWIR inorganic MicroPD array 4. For the fabrication of a p-type contact region of each SWIR inorganic MicroPD (pin planar MicroPD) array 4, it sequentially includes (i) implementing a window array process, (ii) implementing a Zn drive-in process, and (iii) implementing a wet etching process, which are described in detail as follows. It should be noted here that each 300nm SiNx passivation layer 43 is formed in two stages, and the film thickness of each stage is 150nm.
[0051] The window array process of each SWIR inorganic MicroPD array 4 is to complete the first stage SiNx passivation layer 43 after the n +The -InP (100) substrate 41 is sequentially immersed in an acetone / isopropyl alcohol (hereinafter referred to as ACE / IPA) solution for 5 minutes, cleaned with deionized water for 3 minutes, and dried with a nitrogen gun. Then, a first SiO2 layer (not shown) is sequentially deposited on each SiNx passivation layer 43 completed in the first stage, a first patterned negative photoresist layer (not shown) is formed on each first SiO2 layer by a lithography process to partially expose each first SiO2 layer, the first SiO2 layer exposed outside each first patterned negative photoresist layer is removed by reactive ion etching (RIE) and the SiNx passivation layer 43 thereunder is removed, and each first patterned negative photoresist layer is peeled off, thereby defining a window array exposing each corresponding undoped InP capping layer 423 in each corresponding first SiO2 layer and the 150nm SiNx passivation layer 43, each window having a diameter of 15μm and a spacing of 21μm between adjacent windows.
[0052] In the Zn driving process of each SWIR inorganic MicroPD array 4, each n-type window array is first formed. + -InP (100) substrate 41 is sequentially immersed in ACE / IPA solution for 5 minutes, cleaned with deionized water for 3 minutes, and blown dry with a nitrogen gun. In addition, a zinc phosphorus dopant coating (Zinc phosphorus dopant coating, hereinafter referred to as ZPDC) is coated on each of the multiple sapphire wafers (not shown) as a Zn dopant source, so that each sapphire wafer coated with each ZPDC becomes a source wafer, and then each source wafer is placed on a heating plate (200°C) and heated for 3 minutes; wherein the ZPDC is an organic solvent mixture containing Zn and P dopants. Then, each source wafer is facing its corresponding n + The first SiO2 layer of the -InP (100) substrate 41 is placed face to face with each ZPDC and the first SiO2 layer corresponding to each ZPDC and placed in a nearly sealed graphite fixture (not shown). The RTD is performed by heating in a rapid annealing (RTA) furnace containing nitrogen (heating rate 20°C / sec, 540°C for 30 seconds) to volatilize the zinc vapor in each ZPDC and diffuse toward each window of the first SiO2 layer corresponding to each ZPDC into the undoped InP capping layer 423 corresponding to each ZPDC, so as to become a p of each SWIR inorganic MicroPD array 4. + -InP contact area 4231 array, thereby completing the corresponding Zn drive-in process; wherein each p + The hole concentration of the InP contact region 4231 is about 5×10 18 cm -3 .
[0053] The wet etching process of each SWIR inorganic MicroPD array 4 is to form each p + - Each n of the InP contact region 4231 + The -InP (100) substrates 41 were sequentially immersed in a buffered oxide etchant (BOE) for 20 seconds to etch away the first SiO2 layers corresponding to each other, cleaned with deionized water for 3 minutes, and dried with a nitrogen gun.
[0054] After the p-type contact region of each SWIR inorganic MicroPD array 4 is fabricated, a P-metal deposition is performed. Specifically, each P-metal deposition is first performed by PECVD on the SiNx passivation layer 43 of each SWIR inorganic MicroPD array 4 and the p-type contact region of each SWIR inorganic MicroPD array 4. + A 1 μm second SiO2 layer (not shown) is deposited on the -InP contact region 4231 as an insulating layer; then, a second patterned negative photoresist layer (not shown) is formed on each second SiO2 layer by a lithography process so that a portion of the second SiO2 layer is exposed outside the corresponding second patterned negative photoresist layer, and then the second SiO2 layer exposed outside the corresponding second patterned negative photoresist layer and the SiNx passivation layer 43 under the second SiO2 layer are removed by a dry etching method, thereby defining a 3.5 μm diameter and exposing each p-type contact region between each second SiO2 layer and the SiNx passivation layer 43. + -InP contact area 4231 and an array of through holes 430 for setting indium solder bumps; subsequently, thermal evaporation is used on each second negative photoresist layer and each p + A 15nm / 120nm Cr / AuZn multilayer film is deposited on the InP contact region 4231 to serve as a P-metal (i.e., anode) 44 of each SWIR inorganic MicroPD array 4; finally, each n-type 15nm / 120nm Cr / AuZn multilayer film is formed. + The -InP(100) substrate 41 is immersed in acetone until the 15nm / 120nm Cr / AuZn multilayer film coated on each second negative photoresist layer is peeled off, and the corresponding second SiO2 layer is removed with BOE and immersed in ACE / IPA solution for 5 minutes, cleaned with deionized water for 3 minutes, blown dry with a nitrogen gun, and dried with UV-ozone at 120°C for 30 minutes, thereby completing the deposition of P-metal of each SWIR inorganic MicroPD array 4.
[0055] After the P-metal deposition of each SWIR inorganic MicroPD array 4 is completed, the N-metal deposition is performed. Specifically, each N-metal deposition is firstly performed by PECVD on the n-metal of each SWIR inorganic MicroPD array 4. +A 1 μm third SiO2 layer (not shown) is deposited on a lower surface 412 of the -InP (100) substrate 41; then, a third patterned negative photoresist layer (not shown) is formed on each third SiO2 layer by a lithography process so that a portion of the third SiO2 layer is exposed outside the corresponding third patterned negative photoresist layer, and then the third SiO2 layer exposed outside the corresponding third patterned negative photoresist layer is removed by dry etching, thereby defining a partially exposed portion of each n-type layer in each third SiO2 layer. + - A through hole on the lower surface 412 of the InP (100) substrate 41; Subsequently, a thermal evaporation method is used to form a through hole on each third patterned negative photoresist layer and each n + A 20nm / 100nm / 160nm Au / AuGe / Au multilayer film is deposited on the lower surface 412 of the n+-InP(100) substrate 41 to serve as an N-metal 45 (i.e., a common cathode) of the SWIR inorganic MicroPD array 4; finally, each n+-InP(100) substrate 41 formed with each 20nm / 100nm / 160nm Au / AuGe / Au multilayer film is immersed in acetone until the 20nm / 100nm / 160nm Au / AuGe / Au multilayer film on each third patterned negative layer is peeled off, and then the corresponding third SiO2 layer is removed by BOE etchant, and then immersed in ACE / IPA solution for 5 minutes, cleaned with deionized water for 3 minutes, blown dry with a nitrogen gun, and dried with UV-ozone at 120°C for 30 minutes, thereby completing the deposition of N-metal of each SWIR inorganic MicroPD array 4.
[0056] After the deposition of each P-metal and each N-metal is completed, each n-metal having a Cr / AuZn multilayer film (P-metal 44) of 15nm / 120nm and an Au / AuGe / Au multilayer film (N-metal 45) of 20nm / 100nm / 160nm is formed. +The -InP (100) substrate 41 is placed in a N2 environment and annealed at 400°C for 60 seconds. After annealing of the P-metal and N-metal of each SWIR inorganic MicroPD array 4 is completed, the corresponding second-stage SiNx passivation layer 43 is deposited on each first-stage SiNx passivation layer 43 by PECVD; subsequently, a fourth patterned negative photoresist layer (not shown) is formed on each second-stage SiNx passivation layer 43 by lithography to expose part of the second-stage SiNx passivation layer 43 outside the fourth patterned negative photoresist layer, and the second-stage SiNx passivation layer 43 partially exposed outside the fourth patterned negative photoresist layer is removed by RIE, thereby defining the through hole 430 array on the side of each SWIR inorganic MicroPD array 4 in the corresponding second-stage SiNx passivation layer 43, so that the corresponding P-metal 44 is exposed outside, and the corresponding fourth patterned negative photoresist layer is removed. Each through hole 430 on the side of each SWIR inorganic MicroPD array 4 is used to set a corresponding In bump 46 in the subsequent process.
[0057] <Production process of each MicroLED array>
[0058] The manufacturing process of each 512×512 platform-type MicroLED array is divided into two parts, one part is the MicroLED array 5 based on AlGaInP, and the other part is the MicroLED array 6 based on GaInN.
[0059] See also Figure 3 For each AlGaInP-based MicroLED array 5, a 4-inch first film layer structure 52 is first grown on a surface of a p-GaAs substrate (not shown) by MOCVD epitaxial growth. Specifically, each first film layer structure 52 with the n-side facing upward is, from bottom to top, a 0.4μm InGaP barrier layer (not shown), a 0.2μm p-GaAs ohmic contact layer 521, a 2μm p-AlGaInP electron cladding layer 522, a 0.5μm p-AlInP electron cladding layer 523, a 0.41μm and five pairs of AlInP / AlGaInP multiple quantum wells (MQW) 524, a 0.55μm n-AlInP hole cladding layer 525, and a 1.5μm n-GaP ohmic contact layer 526. In each AlInP / AlGaInP multiple quantum well (MQW) 524 (Al x Ga 1-x ) 0.52 In 0.48The component x in the P well is 0.2, 0.3 and 0.4 when emitting red light, orange light and yellow light, respectively. Then, a SiOx film 510 is deposited on an upper surface of each n-GaP ohmic contact layer 526 and a surface 511 of a plurality of c-plane sapphire transfer substrates 51, respectively, so that the SiOx film 510 on each n-GaP ohmic contact layer 526 faces the SiOx film 510 of the corresponding c-plane sapphire transfer substrate 51, and wafer bonding is performed at 370° C. and 13500 kg for 90 minutes, so that the corresponding first film layer structure 52 is transferred to the surface 511 of the corresponding c-plane sapphire transfer substrate 51 (such as Figure 3 As shown). Next, a wet etchant (NH4OH:H2O2) is used to remove the corresponding p-GaAs substrate to expose the corresponding InGaP barrier layer. Then, a mixed acid etchant (HCl:H3PO4) is used to remove the corresponding InGaP barrier layer. Subsequently, annealing is performed in a nitrogen environment at 200°C for 15 minutes to eliminate the stress generated during the wafer bonding process. Subsequently, a chemical mechanical planarization (CMP) process is used to improve the flatness of each first film layer structure 52 after transfer to achieve a first film layer structure 52 with the p-side facing up.
[0060] See also Figure 4 For each GaInN-based MicroLED array 6, a 4-inch second film structure 62 is epitaxially grown on a c-plane patterned sapphire substrate 61 by MOCVD. Each second film structure 62 includes a 0.5 μm undoped GaN buffer layer 621, a 2.5 μm n + -GaN(~1×10 19 cm -3 ) contact layer 622, a 0.315 μm and five pairs of In 1-x Ga x N / AlGaN multi-quantum well (MQW) 623, a 30nm p-AlGaN confinement layer (p~8×10 16 cm -3 )624, with a 0.1μm p-GaN cap layer (p~3×10 17 cm -3 )625. In each second film structure 62 1-x Ga x In N / AlGaN Multi-Quantum Well (MQW) 623 1-x Ga x The component x in the N well is 0.25, 0.15, 0.11 and 0.08 under green, blue, violet and UV-A light emission, respectively.
[0061] Next, each c-plane sapphire transfer substrate 51 with each first film layer structure 52 transferred thereon and each c-plane patterned sapphire substrate 61 with each second film layer structure 62 formed thereon were sequentially immersed in ACE / IPA solution for 5 minutes, cleaned with deionized water for 3 minutes, and dried with a nitrogen gun.
[0062] The pixel manufacturing process of each 512×512 platform-type MicroLED array is described in detail as follows, which sequentially includes a step (1), a step (2), a step (3), a step (4), and a step (5).
[0063] In step (1), the pixels of each MicroLED array 5 based on AlGaInP and each MicroLED array 6 based on GaInN are defined by a photolithography aligner (SUSS-MJB4). First, a 70nm patterned indium tin oxide (ITO) layer 53, 63 is deposited on the top of the p-GaAs ohmic contact layer 521 of each first film structure (based on AlGaInP) 52 and the top of the p-GaN cap layer 625 of each second film structure (based on GaInN) 62 by radio frequency sputtering to form a corresponding ohmic contact layer. Next, an 80nm patterned Ni layer 54, 64 is deposited on the corresponding patterned ITO layer 53, 63 by electron beam evaporation to partially expose the corresponding p-GaAs ohmic contact layer 521 and the corresponding p-GaN cap layer 625 to serve as a hard mask in the subsequent inductively coupled plasma reactive ion etching (ICP-RIE).
[0064] In step (2), each patterned Ni layer 54, 64 is used as a hard mask for each first film structure (mainly AlGaInP) 52 and each second film structure (mainly GaInN) 62, and ICP-RIE is used to etch from each corresponding p-GaAs ohmic contact layer 521 and each corresponding p-GaN cap layer 625 toward each corresponding c-plane sapphire transfer substrate 51 and each corresponding c-plane patterned sapphire substrate 61 to each corresponding n-GaP ohmic contact layer 526 and each corresponding n-GaP ohmic contact layer 527. +-GaN contact layer 622, thereby forming a corresponding platform. More specifically, the ICP-RIE conditions of each MicroLED array 5 based on AlGaInP are 50W bias power, 5sccm Cl2 flow, 4sccm BCl3 flow, 200W ICP power, 0.8Pa working pressure, 20°C ambient temperature, and 260 seconds etching time. In addition, the ICP-RIE conditions of each MicroLED array 6 based on GaInN are 10W bias power, 50sccm Cl2 flow, 200W ICP power, 0.5Pa working pressure, 20°C ambient temperature, and 8 minutes etching time. The etching rate estimated by the above-mentioned ICP-RIE conditions is about 7.5nm / second.
[0065] In step (3), a 1 μm thick patterned SiO2 layer 55, 65 is deposited on the top of each platform (i.e., on each patterned Ni layer 54, 64) by PECVD to define an array of through holes 550, 650 on the side of the MicroLED array for the indium solder bump to be set and having a diameter of 3.5 μm, and to expose the bottom of each platform (i.e., to expose each n-GaP ohmic contact layer 526 and each n + -GaN contact layer 622).
[0066] The purpose of step (4) is to make the current flow evenly and reduce the series resistance of each pixel of each MicroLED array 5 mainly composed of AlGaInP and each MicroLED array 6 mainly composed of GaInN. The n-electrodes of each MicroLED array 5 and 6 are designed to be respectively disposed on each n-GaP ohmic contact layer 526 and connected to each n- +-A grid pattern on the GaN contact layer 622 (i.e., a common cathode). For each AlGaInP-based MicroLED array 5, a p-electrode (120nm AuBe) and an n-electrode (20nm / 130nm / 150nm Au / AuGeNi / Au) are deposited on the top of each corresponding platform (i.e., on the patterned Ni layer 54 on each p-GaAs ohmic contact layer 521) in the through hole 550 and on the corresponding n-GaP ohmic contact layer 526 by thermal evaporation to serve as a pixel anode 56 array and a common cathode 57. Then, annealing is performed in a nitrogen environment at 400°C for 30 seconds. For each GaInN-based MicroLED array 6, a corresponding pixel anode 66 array (30 / 120 / 40 / 60nm Ti / Al / Ti / Au) and a common cathode 67 (30 / 120 / 40 / 60nm Ti / Al / Ti / Au) are directly deposited on the top of the corresponding platform (that is, on the patterned Ni layer 64 on each p-GaN cap layer 625) in the through hole 650 array and the corresponding n + - On the GaN contact layer 622. Then, annealing is performed in a nitrogen environment at 550°C for 300 seconds.
[0067] This step (5) is to reduce the leakage current caused by ICP-RIE damage. A 300nm patterned Al2O3 passivation layer 58, 68 is deposited on each MicroLED array 5 based on AlGaInP and each MicroLED array 6 based on GaInN by plasma assisted atomic layer deposition (PE-ALD). Each patterned Al2O3 passivation layer 58, 68 defines an array of through holes 580, 680 that exposes the corresponding pixel anode 55, 65 array, and exposes one end edge of the corresponding common cathode 57, 67, thereby completing the process of each MicroLED array.
[0068] <Process of flip-chip bonding each MicroPD array to its corresponding MicroLED array>
[0069] Each 512×512 all-inorganic up-conversion display is a display in which each P-metal 44 of each SWIR inorganic MicroPD array 4 faces each corresponding pixel anode 55 of each AlGaInP-based MicroLED array 5 and each pixel anode 65 of each GaInN-based MicroLED array 6. It should be added that, in order to facilitate external contact connection, each AlGaInP-based MicroLED array 5 and each GaInN-based MicroLED array 6 are laser cut into a plurality of small units with a size of 18mm×18mm, and each SWIR inorganic MicroPD array 4 is laser cut into a plurality of small units with a size of 10mm×10mm. After laser cutting of each SWIR inorganic MicroPD array 4, each AlGaInP-based MicroPD array 5, and each GaInN-based MicroLED array 6, a 4 μm In layer is deposited into each through hole 430 on the side of each MicroPD array, each through hole 580 of each AlGaInP-based MicroLED array 5, and each through hole 680 of each GaInN-based MicroLED array 6 by electron beam evaporation to contact each corresponding P-metal 44 and each corresponding pixel anode 56, 66, thereby forming an In bump 46 array of each SWIR inorganic MicroPD array 4 and an In bump 59, 69 array of each AlGaInP-based MicroLED array 5 and each GaInN-based MicroLED array 6. Then, a reflow process is performed on each In bump 46, 59, 69. According to a test of a daisy chain design, each In bump 46 , 59 , 69 has an average resistance of about 67 mΩ.
[0070] As can be seen from the above description, when the flip-chip bonding process is implemented, the SWIR inorganic MicroPD array 4 of the small unit is flip-chip bonded to each small unit's MicroLED array 5 based on AlGaInP and each small unit's MicroLED array 6 based on GaInN, which are described together here.
[0071] Each 512×512 all-inorganic up-conversion display of this embodiment of the present invention is completed by performing a flip chip bonding process using a SET FC150 bonding machine, and its placement accuracy is ±0.5μm, and the post-bond accuracy is ±1μm. In detail, when performing each flip chip bonding process in this embodiment of the present invention, the force increase rate and temperature increase rate used are 0.25kg / s and 8.3℃ / s respectively. The force and temperature used in a soak segment of each flip chip bonding process are 245N and 80℃ respectively, and the process duration of force and temperature is 200 seconds.
[0072] Depend on Figure 5 From the FE-SEM cross-sectional image shown, it can be seen that after one of the SWIR inorganic MicroPD arrays 4 is flip-chip bonded to one of the GaInN-based MicroLED arrays 6, the In bumps at the bottom of one of the SWIR inorganic MicroPD arrays are precisely bonded to the In bumps at the top of one of the GaInN-based MicroLED arrays.
[0073] After flip chip bonding, the pixel yield of each 512×512 all-inorganic up-conversion display can be analyzed by an imageJ image processing software, which is usually used to analyze the full-brightness image and calculate how many pixels or areas need to be illuminated. Figure 6 (a) to Figure 6 (g) shows the red, orange, yellow, green, blue, purple and UV-A images of the 512×512 all-inorganic up-conversion display excited by 1550nm laser light. The operability of the color image of the 512×512 all-inorganic up-conversion display analyzed by the image J image processing software is 99.8%, 93.5%, 90.4%, 95.0%, 95.0%, 95.5% and 92.7% respectively; that is, the surviving pixels corresponding to the total 262144 (or 512×512) pixels after flip chip bonding are 261620, 245105, 236978, 249037, 249037, 250348, 243007 respectively.
[0074] Figure 7aA graph of photocurrent and photoresponsivity versus input laser power is shown, which illustrates the excitation of a 1550nm input laser power to a 512×512 all-inorganic up-conversion display in red, orange, and yellow, biased at 9 V, 9 V, and 8 V, respectively. At input laser power up to 35 mW, the photocurrent of the 512×512 all-inorganic up-conversion display in red, orange, and yellow remains almost constant and increases linearly to 29.3 mA, and the corresponding photoresponsivity can reach 0.83 A / W.
[0075] Figure 7b A graph showing the relationship between photocurrent and photoresponsivity versus input laser power is shown, illustrating a 512×512 all-inorganic up-conversion display excited by 1550nm input laser power to green, blue, violet and UV-A, biased at 4V, 6V, 5V and 5V respectively. Figure 7b It can be seen that the photocurrent of the 512×512 all-inorganic up-conversion display of green, blue, purple and UV-A increases linearly to 29.0mA, 25.4mA, 30.0mA and 31.5mA respectively at an input laser light power of up to 35mW, and the corresponding photoresponses are 0.83A / W, 0.73A / W, 0.86A / W and 0.90A / W respectively.
[0076] Figure 8a The relationship between output power, external quantum efficiency and power efficiency versus input laser power is shown, which illustrates the excitation of red, orange and yellow 512×512 all-inorganic up-conversion displays with input laser power of 1550nm, which are biased at 9V, 9V and 8V respectively. Figure 8a It can be seen that the output power increases almost linearly with the input laser light power. The output power of the red, orange and yellow 512×512 all-inorganic up-conversion displays reaches 1.50mW, 1.46mW and 0.76mW respectively, and the corresponding power efficiency is 4.3%, 4.2% and 2.22% (W / W), and the corresponding maximum quantum efficiency is 1.8%, 1.68% and 0.85% respectively.
[0077] Figure 8b A graph showing the relationship between output power, external quantum efficiency and power efficiency versus input laser power is shown, which illustrates a 512×512 all-inorganic up-conversion display excited by 1550nm input laser power to green, blue, violet and UV-A, biased at 4V, 6V, 5V and 5V respectively. Figure 8bIt can be seen that the output power increases almost linearly with the input laser light power. The output power of the 512×512 all-inorganic up-conversion display of green, blue, purple and UV-A reaches 6.25, 8.01, 6.31 and 1.93mW respectively. The corresponding power efficiency is 18%, 23.5%, 18% and 6.22% (W / W), and the corresponding maximum quantum efficiency is 6.7%, 8.7%, 6.9% and 1.5% respectively.
[0078] As shown in detail in FIGS. 7 and 8 , the all-inorganic up-conversion displays based on GaInN (green, blue, purple) always have higher photocurrent, photoresponsivity, output power and power efficiency than the all-inorganic up-conversion displays based on AlGaInP (red, orange, yellow).
[0079] The light-to-light frequency response of each 512×512 all-inorganic up-conversion display of the embodiment of the present invention is measured by a network analyzer (Agilent E5062A, 300kHz to 3GHz). The network analyzer provides a sine sweep frequency signal, which is then connected to an EA-DFB module (purchased from Shenzhen Realphoton Co., LTD) with a DC bias. Then, the EA-DFB module generates a 1550nm laser light with a signal thereon. When each SWIR inorganic MicroPD array 4 of each 512×512 all-inorganic up-conversion display receives the laser light, the photocurrent with the signal will flow to the corresponding MicroLED array 5 based on AlGaInP and each MicroLED array 6 based on GaInN, thereby driving the corresponding MicroLED arrays 5 and 6. The light emitted from each MicroLED array 5, 6 is collected by an O / E photodiode (Graviton 850nm SPA-3 2GHz). Finally, the signal detected by the O / E photodiode is transmitted to the network analyzer and the overall response of each 512×512 all-inorganic up-conversion display is calculated.
[0080] Fig. 9 Shown are the measured light-to-light frequency responses for 7-dBm (5.01-mW) 1550nm input laser power excited into a 512×512 all-inorganic up-conversion display with red, orange, yellow, green, blue, and violet colors biased at 9V, 9V, 8V, 4V, 6V, 5V, and 5V, respectively. Fig.10As shown, the 512×512 all-inorganic up-conversion display of red, orange, yellow, green, blue and purple shows a 3dB frequency response at 13.2MHz, 12.6MHz, 11.4MHz, 1.0MHz, 3.8MHz and 4.8MHz respectively. The frequency response of each SWIR inorganic MicroPD array 4 at an input laser power of 1550nm (1mW) and a reverse bias of 10V and the frequency response of each MicroLED array 5 and 6 at an input laser power of 1550nm and a forward current of 3mA (not shown), Fig. 9 The frequency response analysis results shown illustrate that the 3dB frequency response of each 512×512 all-inorganic up-conversion display is dominated by the MicroLED array with a lower 3dB frequency response, rather than by the MicroPD array.
[0081] Compared with the 10V, 240kHz and 10kHz obtained by conventional all-organic up-conversion devices irradiated with 980nm and 940nm laser light, respectively (i.e., Organic up-conversion imager with dual electronic and optical readouts for shortwave infrared light detection published by N. Li et al. in Adv. Funct. Mater. 31, 2100565 (2021), and A high-performance solution-processed organic photodetector for near-infrared sensing published by JF Huang et al. in Adv. Mater. 32, 1906027 (2020), the MHz-level 3dB frequency response of each 512×512 all-inorganic up-conversion display of this specific example of the present invention has always been the highest record for up-conversion devices. It should be noted here that many back-end applications of up-conversion devices require a fast response speed, that is, the ability to accurately detect rapidly changing infrared signals in visible light.
[0082] This specific example of the present invention also provides the following applications and results for the backend application (display).
[0083] See also Fig.10, showing a visible light imaging system 7. The visible light imaging system 7 includes an IR laser device 71, a black mask 72, an IR lens 73, each 512×512 all-inorganic up-conversion display, a power supply 74 electrically connected to each 512×512 all-inorganic up-conversion display, and a camera 75, which are arranged in sequence along an optical axis direction X; wherein the power supply 74 provides a bias voltage to the SWIR inorganic MicroPD array 4, the AlGaInP-based MicroLED array 5, and the GaInN-based MicroLED array 6 of the 512×512 all-inorganic up-conversion display. In detail, an IR laser light (1550nm) emitted from the IR laser device 71 passes through a shaped aperture (i.e., as shown in FIG. 1 ) of the black mask 72 in sequence along the optical axis direction X. Fig.11 The IR scene (IR scene) after passing through the forming aperture (the aforementioned pattern) of the black mask 72 and the IR lens 73 is collimated into a uniform light beam through the IR lens 73 to illuminate each SWIR inorganic MicroPD array 4 of each 512×512 all-inorganic up-conversion display, so that each SWIR inorganic MicroPD array 4 generates a photocurrent and then flows through its In bump 46 to the In bump 59, 69 of the corresponding MicroLED array 5, 6, so that the corresponding MicroLED array 5, 6 displays a clear visible light (red, orange, yellow green, blue, purple and UV-A) image that is the same as the imaging aperture (the aforementioned pattern) of the black mask 72, and finally an image is formed by a lens of the camera 75.
[0084] See also Fig.12 , Fig.13 , Fig.14 , Fig.15 , Fig.16 , respectively showing clear color images formed by the 512×512 all-inorganic up-conversion display (red, orange, yellow green, blue, purple and UV-A). It can be seen that the resolution of the 512×512 all-inorganic up-conversion display of this embodiment of the present invention is clear, and its superiority is sufficient to meet most back-end applications, such as night cameras or video cameras, night vision goggles, or wavelength converters. The all-inorganic up-conversion display D of this embodiment of the present invention is applied to a Fig.17For example, the night camera 9 shown in the figure has a lens 91 which includes an IR focusing lens 911, the all-inorganic up-conversion display D of the embodiment of the present invention, a visible light focusing lens 912, and a complementary metal oxide semiconductor (hereinafter referred to as CMOS) field effect transistor image sensor 913 in sequence along a camera optical axis a. When an infrared image 90 located outside the lens 91 is irradiated toward the lens 91 along the camera optical axis a, the infrared image 90 can be focused by the IR focusing lens 911 and then input into the photodiode 2 array toward the all-inorganic up-conversion display D to generate a photocurrent which then flows to the light emitting diode 3 array, so that the light emitting diode 3 array displays a clear visible light image (not shown) identical to the infrared image 90, and the visible light image is focused by the visible light focusing lens 912 and finally imaged by the CMOS field effect transistor image sensor 913.
[0085] In view of the undoped In of each SWIR inorganic MicroPD array 4 of this specific example of the present invention 0.53 Ga 0.47 The energy gap of the As absorption layer 422 at room temperature is 0.74 eV (or a cutoff wavelength of 1670 nm). This means that each undoped In 0.53 Ga 0.47 The As absorption layer 422 can absorb light wavelengths below 1670 nm (eg, 1550 nm). The inventors speculate that each undoped In 0.53 Ga 0.47 As absorption layer 422 should also be able to absorb shorter wavelength visible light. Therefore, the present invention also provides another visible light imaging system 8 (see Fig.18 ), which is substantially the same as the visible light imaging system 7, except that the other visible light imaging system 8 omits the black mask 72 and replaces the IR laser light device 71 with a tungsten filament bulb 76.
[0086] Fig.19 The color image formed by the camera 75 of the other visible light imaging system 8 is displayed. Fig.19 (a) to Fig.19 The images in (h) are tungsten images emitted by a 512×512 all-inorganic up-conversion display of original, red, orange, yellow, green, blue, violet and UV-A, which are biased at 0V, 9V, 9V, 8V, 4V, 6V, 5V and 5V, respectively.
[0087] According to the above detailed description of the present invention, each SWIR inorganic MicroPD array 4 is bonded to each corresponding AlGaInP-based MicroLED array 5 and each corresponding GaInN-based MicroLED array 6 through flip chip bonding technology to form each 512×512 all-inorganic up-conversion display, whose lowest driving voltage is only 4V and has a MHz-level 3dB light-to-light frequency response. In addition, the photocurrent, photoresponsivity, light output power and power efficiency of the 512×512 all-inorganic up-conversion display can reach up to 31.5mA, 0.9A / W, 8.01mW and 23.5% (W / W) respectively.
[0088] In summary, the photodiode 2 array and the light-emitting diode 3 array of the all-inorganic up-conversion display of the present invention are not affected by lattice matching because they are formed on their respective substrates 21 and 31, and the solder bumps 28 of the photodiode 2 array are combined with the solder bumps 35 of the light-emitting diode 3 array via flip chip bonding technology, which can solve the problems caused by lattice matching. Moreover, the photodiode 2 array and the light-emitting diode 3 array are both made of inorganic semiconductor materials, have low driving voltage, MHz-level 3dB light-to-light frequency response and excellent photocurrent, light responsiveness, light output power and power efficiency, so they can indeed achieve the purpose of the present invention.
[0089] However, the above is only an embodiment of the present invention and should not be used to limit the scope of the present invention. All simple equivalent changes and modifications made according to the claims and description of the present invention are still within the scope of the present invention.
Claims
1. An all-inorganic up-conversion display, characterized in that: Include: A photodiode array, comprising a substrate containing carriers of a first conductive type, a buffer layer formed on a first surface of the substrate, an absorption layer formed on the buffer layer, a covering layer formed on the absorption layer, a patterned passivation layer formed on the covering layer and exposing an array of contact regions of the covering layer, a common electrode connected to the substrate, an electrode array, and a solder bump array, wherein the common electrode exhibits electrical properties of the first conductive type, each contact region of the covering layer contains carriers of a second conductive type opposite to the first conductive type, each electrode is connected to a corresponding contact region and exhibits electrical properties of the second conductive type, and each solder bump is connected to a corresponding electrode; and A light-emitting diode array, comprising a substrate, a light-emitting crystal grain array, a common electrode, a patterned passivation layer, and a solder bump array, wherein each light-emitting crystal grain has a first layer formed on the substrate and containing a first conductive type of carrier, a second layer formed on the first layer corresponding to each light-emitting crystal grain and containing a second conductive type of carrier, a light-emitting layer sandwiched between the first layer and the second layer corresponding to each light-emitting crystal grain, and a pixel electrode exhibiting the second conductive type of electrical property and electrically connected to the second layer corresponding to each light-emitting crystal grain, wherein the first layers of the light-emitting crystal grains are connected to each other, the common electrode exhibits the first conductive type of electrical property and is disposed on the first layer of each light-emitting crystal grain to surround the light-emitting layer corresponding to each light-emitting crystal grain, the patterned passivation layer covers the light-emitting crystal grain array and the common electrode and exposes the end edges of each pixel electrode and the common electrode, and each solder bump is connected to the pixel electrode corresponding to each light-emitting crystal grain; Wherein, each solder bump of the photodiode array is flip-chip bonded to each solder bump of the light-emitting diode array.
2. The all-inorganic up-conversion display according to claim 1, characterized in that: The common electrode of the photodiode array is formed on a second surface of the substrate opposite to the first surface.
3. The all-inorganic up-conversion display according to claim 1, characterized in that: Each light-emitting crystal grain further has a current diffusion layer, and the current diffusion layer of each light-emitting crystal grain is sandwiched between the corresponding pixel electrode and the second layer.
4. The all-inorganic up-conversion display according to claim 1, characterized in that: The first conductive type carriers contained in the substrate of the photodiode array are N-type carriers, the second conductive type carriers contained in each contact area of the covering layer of the photodiode array are P-type carriers, the common electrode of the photodiode array is a common cathode, and each electrode of the photodiode array is an anode.
5. The all-inorganic up-conversion display according to claim 1, characterized in that: The first conductive type carriers contained in the first layer of the light-emitting crystal array are N-type carriers, the second conductive type carriers contained in the second layer of the light-emitting crystal array are P-type carriers, the common electrode of the light-emitting diode array is a common cathode, and the pixel electrode of each light-emitting crystal is a pixel anode.
6. The all-inorganic up-conversion display according to claim 1, characterized in that: Each solder bump is made of a metal material selected from the group consisting of: indium, gold, tin, gold-indium alloy, gold-tin alloy, indium-tin alloy, gold-indium-tin alloy, tin-lead alloy, gold-germanium alloy, and gold-silicon alloy.
7. The all-inorganic up-conversion display according to claim 1, characterized in that: The photodiode array is a nanometer photodiode array, a sub-nanometer photodiode array, or a micro photodiode array, and the light emitting diode array is a nanometer light emitting diode array, a sub-nanometer light emitting diode array, or a micro light emitting diode array.
Citation Information
Cited By
Photoelectric detection imaging integrated chip and use method thereof