Tunneling oxide passivation contact structure with laminated polycrystalline silicon and preparation method thereof

Through the stacked polysilicon structure, combined with nano-silicon oxide and doped polysilicon thin film, the metal burn-through problem caused by thinning of polysilicon layer in TOPCon batteries is solved, the passivation performance and open circuit voltage of the battery are improved, and the production process is simplified.

CN119008736APending Publication Date: 2024-11-22CHINA SCI & TECH (NINGBO) CO LTD
View PDF 0 Cites 4 Cited by

Patent Information

Application Number
CN202411171591.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-26
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The existing TOPCon batteries are difficult to prevent metal burning through during the process of thinning the polysilicon layer, resulting in an increase in saturation current density and require precise alkali etching parameter control, affecting passivation performance.

Method used

Using a laminated polysilicon structure, including nano-silicon oxide film, phosphorus-doped polysilicon film and multi-element doped polysilicon film, through high-temperature annealing, combined with passivation and anti-reverse layer, a multi-layer structure with functional elements is formed to prevent metal paste from burning. Pass and reduce electrode contact resistance.

Benefits of technology

Effectively prevent metal slurry from burning through, reduce the recombination current in the metallized area, increase the open circuit voltage, reduce the thickness of the polysilicon layer, reduce parasitic absorption, improve battery performance, and be compatible with existing processes and simplify production processes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119008736A_ABST
    Figure CN119008736A_ABST
Patent Text Reader

Abstract

The invention provides a tunneling oxide passivation contact structure with laminated polycrystalline silicon and a preparation method of the tunneling oxide passivation contact structure, and the tunneling oxide passivation contact structure comprises a nano silicon oxide thin film arranged on a crystalline silicon substrate, and a phosphorus-doped polycrystalline silicon thin film and a multi-element-doped polycrystalline silicon thin film which are alternately arranged on the nano silicon oxide thin film, phosphorus and functional elements are doped in the multi-element-doped polycrystalline silicon thin films, the functional elements are selected from one or more of carbon, nitrogen and oxygen, the number of the phosphorus-doped polycrystalline silicon thin films is n, the number of the multi-element-doped polycrystalline silicon thin films is m, n is larger than or equal to 2, m is larger than or equal to 1, and n-m is larger than or equal to 1 and larger than or equal to 1. The invention provides an innovative tunneling oxide passivation contact structure, and by adding the polycrystalline silicon insertion layer containing carbon / nitrogen / oxygen elements, the burning through of the metal slurry can be effectively prevented, the recombination current of a metallization region is reduced, and the open-circuit voltage of the battery is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of crystalline silicon solar cells, and in particular to a laminated polycrystalline silicon structure and a preparation method thereof, and a TOPCon cell. Background Art

[0002] Tunneling oxide passivation contact (TOPCon) cell technology uses extremely thin silicon oxide and heavily doped polysilicon layers as back-side passivation contact layers. With its excellent passivation performance, low contact resistance, high photoelectric conversion efficiency, and high compatibility with PERC technology, it has become the best candidate for the next generation of crystalline silicon cell technology upgrades.

[0003] Industrial solar cell manufacturers regard screen-printed metallization paste as a cost-effective metallization solution because of its low cost and high yield. For the back of the TOPCon cell, the industry is constantly thinning the thickness of the polysilicon layer to alleviate the parasitic absorption of carriers and improve the optical performance of the cell. However, the problem that comes with it is that the thinner polysilicon layer is difficult to resist the metal burn-through during the sintering process, which in turn causes a larger saturation current density. In response to this problem, the industry has provided an improvement method, namely, the use of poly-finger technology (see patent documents CN202110748415.7, CN202111219995.7). The principle of this technology is to keep the polycrystalline layer under the metallized area thicker, and the non-metallized area is thinned by alkaline etching to ensure low parasitic absorption. However, this method still has corresponding disadvantages, that is, extremely precise alkaline etching parameter control and process management are required to balance the relationship between low parasitic absorption and high passivation, and over-etching is prone to occur in the actual production process, which affects the passivation performance of the TOPCon structure. Summary of the invention

[0004] In view of the shortcomings of the prior art, the technical problem to be solved by the present invention is how to ensure the passivation performance and excellent contact performance of the battery while preventing the metal slurry from burning through.

[0005] To solve the above problems, the first aspect of the present invention provides a tunneling oxide passivation contact structure with stacked polysilicon, including a nano-silicon oxide film arranged on a crystalline silicon substrate, and a phosphorus-doped polysilicon film and a multi-element doped polysilicon film alternately arranged on the nano-silicon oxide film, the multi-element doped polysilicon film being doped with phosphorus and functional elements, the functional elements being selected from one or more of carbon, nitrogen, and oxygen, the number of the phosphorus-doped polysilicon film being n layers, the number of the multi-element doped polysilicon film being m layers, n≥2, m≥1, and 1≥nm≥-1.

[0006] The present invention proposes an innovative tunneling oxide passivation contact structure, which can effectively prevent metal slurry from burning through, reduce the composite current in the metallization area, and improve the open circuit voltage of the battery by adding a polysilicon insertion layer containing carbon / nitrogen / oxygen elements.

[0007] Furthermore, the number m of the multi-element doped polysilicon thin film is 2 to 3. The multi-element doped polysilicon thin film is repeatedly provided with multiple layers to ensure the effect of preventing the metal slurry from penetrating.

[0008] Furthermore, the functional element doping concentration in the multi-element doped polysilicon film is 1×10 18 ~5×10 21 cm -3 , the phosphorus doping concentration is 5×10 19 ~1×10 21 cm -3 The doping of carbon / nitrogen / oxygen elements will greatly reduce the activation concentration of phosphorus dopants, that is, reduce the electron concentration in polysilicon. Therefore, multi-element doped polysilicon film can inhibit the growth and puncture of silver crystals, prevent the silver electrode from penetrating the nano-silicon oxide film, and maintain the passivation quality.

[0009] Furthermore, the thickness of the multi-element doped polysilicon film is 5-200 nm. The multi-element doped polysilicon film can inhibit the growth and penetration of metal crystals, use a polysilicon film with a smaller thickness overall, and reduce the optical parasitic absorption of the back polysilicon.

[0010] Furthermore, the phosphorus doping concentration in the phosphorus-doped polysilicon film is 6×10 19 ~2×10 21 cm -3 The phosphorus-doped polysilicon film ensures that the double-layer polysilicon structure maintains good lateral and longitudinal conductivity, and does not cause significant negative impact on battery carrier transport.

[0011] Furthermore, the thickness of the phosphorus-doped polysilicon film is 5-200 nm. The structural design prevents the metal paste from burning through, so that a polysilicon film with a smaller thickness can be used, thereby reducing the optical parasitic absorption of the back polysilicon.

[0012] Furthermore, the thickness of the nano silicon oxide film is 1-3 nm, and the absorption coefficient k of the nano silicon oxide film at a wavelength above 500 nm is less than 0.1 cm -1 .

[0013] Furthermore, the nano silicon oxide film contains carbon and / or nitrogen elements, thereby improving the interface stability, increasing the hydrogen content in the nano silicon oxide film, and improving the passivation effect.

[0014] Furthermore, the tunnel oxide passivation contact structure with stacked polysilicon further includes a passivation anti-reflection layer arranged at the outermost layer. The passivation anti-reflection layer is used for hydrogen injection and reflection reduction.

[0015] A second aspect of the present invention provides a method for preparing a tunnel oxide passivation contact structure having stacked polysilicon, comprising the following steps: S1, prepare silicon wafer and perform RCA cleaning; S2, preparing a nano silicon oxide film on the surface of the substrate; S3, alternately depositing phosphorus-doped amorphous silicon films and multi-element doped amorphous silicon films on the surface of the nano silicon oxide film, the number of phosphorus-doped amorphous silicon films is n layers, the number of doped amorphous silicon films is m layers, n≥2, m≥1, and 1≥nm≥-1; S4. High temperature annealing in the temperature range of 600°C to 1200°C, so that the phosphorus-doped amorphous silicon film is converted into a phosphorus-doped polycrystalline silicon film, and the multi-element doped amorphous silicon film is converted into a multi-element doped polycrystalline silicon film.

[0016] The preparation method of the present invention is simple to operate and is fully compatible with existing battery production line technology. A tunneling oxide passivation contact structure with stacked polycrystalline silicon can be formed by alternately depositing phosphorus-doped amorphous silicon films and multi-element doped amorphous silicon films.

[0017] Furthermore, the preparation method further comprises the following steps: S6, depositing a passivation anti-reflection layer on the surface of the substrate; S7, hydrogenation post-treatment, including annealing and light injection treatment, the temperature range is 300 ° C ~ 900 ° C, the protective atmosphere is an inert atmosphere or an inert atmosphere containing hydrogen.

[0018] Hydrogenation post-treatment can improve the passivation performance of tunnel oxide passivation contact structures.

[0019] In summary, the present invention has the following beneficial effects compared with the prior art: (1) The tunneling oxide passivation contact structure of the present invention has a stacked polysilicon composed of a phosphorus-doped polysilicon film and a multi-element doped polysilicon film, which effectively prevents metal slurry from burning through, reduces the composite current in the metallization area, and improves the open circuit voltage of the battery.

[0020] (2) The tunneling oxide passivation contact structure of the present invention promotes the lateral growth of metal crystals, reduces the contact resistivity of the electrode, and improves the battery fill factor.

[0021] (3) The tunnel oxide passivation contact structure of the present invention can use a polysilicon film with a smaller thickness to reduce parasitic absorption; at the same time, doping functional elements in the multi-element doped polysilicon film is also beneficial to reducing its parasitic absorption, thereby increasing the short-circuit current of the battery.

[0022] (4) The preparation method of the tunnel oxide passivation contact structure of the present invention is simple, has high production efficiency, and is fully compatible with existing processes. Production does not require additional equipment and investment costs, and has good prospects for mass production applications. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 It is a schematic structural diagram of a tunnel oxide passivation contact structure in a specific implementation manner of the present invention.

[0024] Figure 2 It is a schematic structural diagram of a tunnel oxide passivation contact structure in another specific embodiment of the invention.

[0025] Figure 3 This is a schematic diagram of the structure of the TOPCon battery prepared in Example 3 of the present invention.

[0026] Figure 4 This is a schematic diagram of the structure of the TOPCon battery prepared in Example 4 of the present invention.

[0027] Figure 5 This is a schematic diagram of the structure of the TOPCon battery prepared in Comparative Example 3 of the present invention.

[0028] Description of reference numerals: 1-crystalline silicon substrate, 2-nano silicon oxide film, 3-phosphorus-doped polysilicon film, 4-multi-element doped polysilicon film, 5-emitter, 6-diffusion layer, 7-back passivation anti-reflection layer, 8-front passivation anti-reflection layer, 9-back metal electrode, 10-front metal electrode. DETAILED DESCRIPTION

[0029] In order to make the above-mentioned purposes, features and advantages of the present invention more obvious and easy to understand, the specific embodiments of the present invention are described in detail below in conjunction with the accompanying drawings. It should be noted that the following embodiments are only used to illustrate the implementation method and typical parameters of the present invention, and are not used to limit the parameter range described in the present invention. Reasonable changes derived therefrom are still within the scope of protection of the claims of the present invention.

[0030] It should be noted that the endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, and these numerical ranges should be regarded as specifically disclosed in this article.

[0031] The specific embodiment of the present invention provides a tunnel oxide passivation contact structure that can inhibit metal paste burn-through, which has a special laminated polysilicon structure, can improve the back passivation effect of the battery and improve the battery performance. Figure 1 As shown, the stacked passivation structure includes a nano silicon oxide film 2 disposed on a crystalline silicon substrate, and a phosphorus-doped polysilicon film 3 and a multi-element doped polysilicon film 4 alternately disposed on the nano silicon oxide film 2. Figure 1 As shown in , the number of phosphorus-doped polysilicon films 3 and multi-element doped polysilicon films are both 2, the polysilicon in contact with the nano silicon oxide film 2 is the phosphorus-doped polysilicon film 3, and the polysilicon located in the outermost layer is the multi-element doped polysilicon film 4.

[0032] In other embodiments, the order of the phosphorus-doped polysilicon film 3 and the multi-element doped polysilicon film 4 can be exchanged, such as Figure 2 As shown, the polysilicon in contact with the nano silicon oxide film 2 is a multi-element doped polysilicon film 4 , and the polysilicon located on the outermost layer is a phosphorus doped polysilicon film 3 .

[0033] In some specific embodiments, the number of phosphorus-doped polysilicon films 3 and multi-element doped polysilicon films 4 can be adjusted, and the number of phosphorus-doped polysilicon films 3 is defined as n layers, and the number of multi-element doped polysilicon films 4 is defined as m layers, satisfying n≥2, m≥1, and 1≥nm≥-1. Preferably, the number m of multi-element doped polysilicon films 4 is 2 to 3 layers.

[0034] In the tunneling oxide passivation contact structure, the main components of the nano silicon oxide film 2 are silicon (Si), oxygen (O), and hydrogen (H), with a typical thickness range of 1-3 nm, preferably 1.5-1.8 nm; its absorption coefficient k at wavelengths above 500 nm is less than 0.1 cm -1 In some embodiments, the nano silicon oxide film 2 also contains carbon and nitrogen elements to improve interface stability and help increase hydrogen content.

[0035] In the tunnel oxide passivation contact structure, the main components of the phosphorus-doped polysilicon film 3 are silicon (Si), phosphorus (P), and hydrogen (H). The typical thickness range is 5 to 200 nm, preferably 10 to 20 nm. The thickness of each layer of the phosphorus-doped polysilicon film 3 can be the same or different. The typical concentration of phosphorus doping is 6×10 19 ~2×10 21 cm -3 In some embodiments, the phosphorus-doped polysilicon film 31 also contains carbon, nitrogen, and oxygen elements to improve the passivation performance.

[0036] In the tunnel oxide passivation contact structure, the main components of the multi-element doped polysilicon film 4 are one or more functional elements of silicon (Si), phosphorus (P), hydrogen (H), carbon (C), nitrogen (N), and oxygen (O). The doping concentration of the functional elements is generally 1×10 18 ~5×10 21 cm -3 , the phosphorus doping concentration is generally 5×10 19 ~1×10 21 cm -3 The typical thickness range of the multi-element doped polysilicon thin film 4 is 5-200 nm, preferably 10-20 nm, and the thickness of each layer of the multi-element doped polysilicon thin film 4 may be the same or different.

[0037] The above-mentioned tunneling oxide passivation contact structure can effectively inhibit the burn-through of metal slurry. The principle is as follows: during the battery metallization process, the glass component in the sintered metal slurry will cause the metal to oxidize to form metal oxide, and dissolve in the glass component in the form of metal ions. During the cooling process, the reduction of metal ions in polysilicon requires the participation of electrons. The multi-element doped polysilicon film 4 with functional element doping will greatly reduce the activation concentration of the phosphorus dopant, that is, reduce the electron concentration in the polysilicon. Therefore, the polysilicon containing functional elements can inhibit the growth and puncture of metal crystals, and prevent the metal electrode from penetrating the underlying nano-silicon oxide film, thereby maintaining the passivation quality; at the same time, the bond energy of carbon silicon, nitrogen silicon, and oxygen silicon is larger, which helps to reduce the penetration ability of the metal and maintain the passivation quality.

[0038] In addition, the above-mentioned tunneling oxide passivation contact structure with stacked polysilicon also has the following advantages: the alternately arranged phosphorus-doped polysilicon film 3 and the multi-element doped polysilicon film 4 can maintain good lateral and longitudinal conductivity, and does not cause significant negative impact on the battery carrier transport; the alternately arranged phosphorus-doped polysilicon film 3 and the multi-element doped polysilicon film 4, on the one hand, inhibit the longitudinal penetration of metal crystals, and on the other hand, promote their lateral growth in polysilicon, thereby reducing the contact resistivity of the electrode; the effect of blocking metal slurry is achieved through structural improvement, so that a polysilicon film with a smaller thickness can be used, reducing the optical parasitic absorption of the back polysilicon; the parasitic absorption of polysilicon containing functional elements is low, which can reduce the parasitic absorption of the passivation structure and improve the battery efficiency.

[0039] In some embodiments, the tunnel oxide passivation contact structure further includes a passivation anti-reflection layer disposed at the outermost layer, the passivation anti-reflection layer is composed of an aluminum oxide film and / or a silicon nitride film, and is used for hydrogen injection and reflection reduction.

[0040] The typical preparation method of the above tunnel oxide passivation contact structure is as follows: (1) Prepare silicon wafers for RCA cleaning.

[0041] (2) Preparation of nano-silicon oxide thin films on the substrate surface. Common preparation methods include: wet chemical method, plasma-assisted oxidation method, thermal oxidation method, ozone oxidation method, etc.

[0042] (3) Prepare phosphorus-doped amorphous silicon thin film on the substrate surface. The preparation methods include APCVD, LPCVD, PECVD, etc. The commonly used preparation method is PECVD, and the deposition temperature range is 100℃ ~600℃.

[0043] (4) Prepare multi-element doped amorphous silicon thin films on the substrate surface. The preparation methods include APCVD, LPCVD, PECVD, etc. The commonly used preparation method is PECVD, and the deposition temperature range is 100℃ ~600℃.

[0044] In some embodiments, the order of step (3) and step (4) can be interchanged.

[0045] (5) Steps (3) and (4) are repeated at least once.

[0046] (6) High temperature annealing, the temperature range is 600℃~1100℃, the protective atmosphere is nitrogen, and the annealing time is 5~500 min, so that the phosphorus-doped amorphous silicon film is converted into phosphorus-doped polycrystalline silicon film, and the multi-element doped amorphous silicon film is converted into multi-element doped polycrystalline silicon film.

[0047] (7) Depositing an aluminum oxide film and a silicon nitride film on the surface of the substrate to obtain a passivation anti-reflection layer.

[0048] (8) Entering hydrogenation post-treatment, including annealing and light injection treatment, the temperature range is 300℃ ~900℃, and the protective atmosphere is an inert atmosphere such as nitrogen or an inert atmosphere containing hydrogen.

[0049] The above preparation method is simple to operate, is fully compatible with existing battery production line technology, does not require additional equipment and investment costs, and has good prospects for mass production applications.

[0050] The technical solutions and effects of the present invention are described below through specific embodiments.

[0051] Example 1

[0052] (1) Prepare n-type silicon wafers and perform double-sided alkaline polishing. The wafer parameters are as follows: thickness 140 μm, resistivity 1 Ω·cm.

[0053] (2) After standard RCA cleaning, the silicon wafer was placed in a PECVD chamber and a 1.5 nm nano-silicon oxide film was prepared on the surface of the crystalline silicon substrate using N2O plasma.

[0054] (3) Subsequently, a 25 nm phosphorus-doped amorphous silicon film, a 25 nm multi-element doped amorphous silicon film containing carbon and phosphorus, and a 40 nm phosphorus-doped amorphous silicon film are sequentially deposited, with a total thickness of 90 nm.

[0055] (4) The sample was placed in a tube furnace and annealed at 880°C for 30 min. The phosphorus-doped amorphous silicon film was converted into a phosphorus-doped polycrystalline silicon film, and the multi-element doped amorphous silicon film was converted into an element-doped polycrystalline silicon film.

[0056] (5) Aluminum oxide film was deposited on the sample surface by ALD, and then silicon nitride film was deposited by PECVD.

[0057] (6) The sample was transferred to a tube furnace and post-treated by hydrogenation under a nitrogen atmosphere and annealed at 450 °C for 30 min to obtain a passivated sheet.

[0058] The surface saturation current density was measured J 0,s 1.3 fA / cm 2 .

[0059] Example 2

[0060] (1) Prepare n-type silicon wafers and perform double-sided alkaline polishing. The wafer parameters are as follows: thickness 140 μm, resistivity 1 Ω·cm.

[0061] (2) After standard RCA cleaning, the silicon wafer was placed in a PECVD chamber and a 1.5 nm nano-silicon oxide film was prepared on the surface of the crystalline silicon substrate using N2O plasma.

[0062] (3) Subsequently, a 10 nm phosphorus-doped amorphous silicon film, a 20 nm multi-element doped amorphous silicon film containing carbon and phosphorus, a 15 nm phosphorus-doped amorphous silicon film, a 15 nm multi-element doped amorphous silicon film containing carbon and phosphorus, and a 20 nm phosphorus-doped amorphous silicon film are sequentially deposited, with a total thickness of 80 nm.

[0063] (4) The sample was placed in a tube furnace and annealed at 880°C for 30 min. The phosphorus-doped amorphous silicon film was converted into a phosphorus-doped polycrystalline silicon film, and the multi-element doped amorphous silicon film was converted into an element-doped polycrystalline silicon film.

[0064] (5) Aluminum oxide film was deposited on the sample surface by ALD, and then silicon nitride film was deposited by PECVD.

[0065] (6) The sample was transferred to a tube furnace and post-treated by hydrogenation under a nitrogen atmosphere and annealed at 450 °C for 30 min to obtain a passivated sheet.

[0066] The surface saturation current density was measured J 0,s 1.1 fA / cm 2 .

[0067] Comparative Example 1 (1) Prepare n-type silicon wafers and perform double-sided alkaline polishing. The wafer parameters are as follows: thickness 140 μm, resistivity 1 Ω·cm.

[0068] (2) After standard RCA cleaning, the silicon wafer was placed in a PECVD chamber and a 1.5 nm nano-silicon oxide film was prepared on the surface of the crystalline silicon substrate using N2O plasma.

[0069] (3) Then, a 110 nm phosphorus-doped amorphous silicon film is deposited.

[0070] (4) The sample was placed in a tube furnace and annealed at 880°C for 30 min to transform the phosphorus-doped amorphous silicon film into phosphorus-doped polycrystalline silicon film.

[0071] (5) Aluminum oxide film was deposited on the sample surface by ALD, and then silicon nitride film was deposited by PECVD.

[0072] (6) The sample was transferred to a tube furnace and post-treated by hydrogenation under a nitrogen atmosphere and annealed at 450 °C for 30 min to obtain a passivated sheet.

[0073] The surface saturation current density was measured J 0,s 2.9 fA / cm 2 .

[0074] Comparative Example 2 (1) Prepare n-type silicon wafers and perform double-sided alkaline polishing. The wafer parameters are as follows: thickness 140 μm, resistivity 1 Ω·cm.

[0075] (2) After standard RCA cleaning, the silicon wafer was placed in a PECVD chamber and a 1.5 nm nano-silicon oxide film was prepared on the surface of the crystalline silicon substrate using N2O plasma.

[0076] (3) Then, a 60 nm phosphorus-doped amorphous silicon film is deposited.

[0077] (4) Deposit 1.5 nm nano-silicon oxide film again.

[0078] (5) Then, a 60 nm phosphorus-doped amorphous silicon film is deposited.

[0079] (6) The sample was placed in a tube furnace and annealed at 880°C for 30 min to transform the phosphorus-doped amorphous silicon film into phosphorus-doped polycrystalline silicon film.

[0080] (7) Aluminum oxide film was deposited on the sample surface by ALD, and then silicon nitride film was deposited by PECVD.

[0081] (8) The sample was transferred to a tube furnace and post-treated by hydrogenation under a nitrogen atmosphere and annealed at 450 °C for 30 min to obtain a passivated sheet.

[0082] The surface saturation current density was measured J 0,s 2.6 fA / cm 2 .

[0083] The performance of the samples prepared in Examples 1 and 2 and Comparative Examples 1 and 2 are shown in Table 1 below. The results show that the tunneling oxide passivation contact structure of the present invention can improve the passivation quality and reduce the surface saturation current density.

[0084] Table 1 Comparison of passivation performance of samples of embodiments and comparative examples sample Example 1 Example 2 Comparative Example 1 Comparative Example 2 <![CDATA[ J 0,s (fA / cm 2 )]]> 1.3 1.1 2.9 2.6

[0085] Example 3

[0086] (1) Prepare n-type silicon wafers and perform double-sided alkaline polishing. The wafer parameters are as follows: thickness 140 μm, resistivity 1 Ω·cm.

[0087] (2) The front side of the silicon wafer is textured and BCl3 boron is diffused to form an emitter 5.

[0088] (3) After standard RCA cleaning, the silicon wafer is placed in a PECVD chamber, and a 1.5 nm nano-silicon oxide film 2 is prepared on the surface of the crystalline silicon substrate 1 using N2O plasma.

[0089] (3) Subsequently, a 25 nm phosphorus-doped amorphous silicon film, a 25 nm multi-element doped amorphous silicon film containing carbon and phosphorus, and a 40 nm phosphorus-doped amorphous silicon film are sequentially deposited, with a total thickness of 90 nm.

[0090] (4) The sample is placed in a tube furnace and annealed at 880°C for 30 min. The phosphorus-doped amorphous silicon film is transformed into a phosphorus-doped polycrystalline silicon film 3, the multi-element doped amorphous silicon film is transformed into an element-doped polycrystalline silicon film 4, and a diffusion layer 6 is formed on the shallow surface of the back side of the crystalline silicon substrate 1.

[0091] (5) Aluminum oxide film and silicon nitride film are deposited on both sides of the sample to form a back passivation anti-reflection layer 7 and a front passivation anti-reflection layer 8.

[0092] (6) The sample was transferred to a tube furnace and post-treated by hydrogenation under a nitrogen atmosphere and annealed at 450 °C for 30 min to obtain a passivated sheet.

[0093] (7) Screen printing metal grid lines, high temperature sintering, and laser enhanced contact optimization (LECO) processing to form a back metal electrode 9 and a front metal electrode 10 to obtain a TOPCon battery.

[0094] The TOPCon battery structure prepared in this embodiment is as follows Figure 3 As shown, the silver crystal penetration position of the back metal electrode 9 is near the multi-element doped polysilicon film 4. Test battery performance, metallization area surface saturation current density J 0, metal 85fA / cm 2 , open circuit voltage V oc is 737.6 mV, short-circuit current J sc is 41.91 mA, fill factor FF It is 84.91% and the battery efficiency is 26.25%.

[0095] Example 4

[0096] (1) Prepare n-type silicon wafers and perform double-sided alkaline polishing. The wafer parameters are as follows: thickness 140 μm, resistivity 1 Ω·cm.

[0097] (2) The front side of the silicon wafer is textured and BCl3 boron is diffused to form an emitter 5.

[0098] (3) After standard RCA cleaning, the silicon wafer is placed in a PECVD chamber, and a 1.5 nm nano-silicon oxide film 2 is prepared on the surface of the crystalline silicon substrate 1 using N2O plasma.

[0099] (3) Subsequently, a 10 nm phosphorus-doped amorphous silicon film, a 20 nm multi-element doped amorphous silicon film containing carbon and phosphorus, a 15 nm phosphorus-doped amorphous silicon film, a 15 nm multi-element doped amorphous silicon film containing carbon and phosphorus, and a 20 nm phosphorus-doped amorphous silicon film are sequentially deposited, with a total thickness of 80 nm.

[0100] (4) The sample is placed in a tube furnace and annealed at 880°C for 30 min. The phosphorus-doped amorphous silicon film is transformed into a phosphorus-doped polycrystalline silicon film 3, the multi-element doped amorphous silicon film is transformed into an element-doped polycrystalline silicon film 4, and a diffusion layer 6 is formed on the shallow surface of the back side of the crystalline silicon substrate 1.

[0101] (5) Aluminum oxide film and silicon nitride film are deposited on both sides of the sample to form a back passivation anti-reflection layer 7 and a front passivation anti-reflection layer 8.

[0102] (6) The sample was transferred to a tube furnace and post-treated by hydrogenation under a nitrogen atmosphere and annealed at 450 °C for 30 min to obtain a passivated sheet.

[0103] (7) Screen printing metal grid lines, high temperature sintering, and laser enhanced contact optimization (LECO) processing to form a back metal electrode 9 and a front metal electrode 10 to obtain a TOPCon battery.

[0104] The TOPCon battery structure prepared in this embodiment is as follows Figure 4 As shown, the silver crystal density of the back metal electrode 9 is greater than that of Example 3, the penetration depth is smaller, and the penetration position is near the first and second layers of multi-element doped polysilicon thin films 4. Test battery performance, metallization area surface saturation current density J 0, metal 72 fA / cm 2 , open circuit voltage V oc is 738.1 mV, short-circuit current J sc is 41.93 mA, fill factor FF It is 84.98% and the battery efficiency is 26.30%.

[0105] Comparative Example 3 (1) Prepare n-type silicon wafers and perform double-sided alkaline polishing. The wafer parameters are as follows: thickness 140 μm, resistivity 1 Ω·cm.

[0106] (2) The front side of the silicon wafer is textured and BCl3 boron is diffused to form an emitter 5.

[0107] (3) After standard RCA cleaning, the silicon wafer is placed in a PECVD chamber, and a 1.5 nm nano-silicon oxide film 2 is prepared on the surface of the crystalline silicon substrate 1 using N2O plasma.

[0108] (3) Then, a 110 nm phosphorus-doped amorphous silicon film is deposited.

[0109] (4) The sample was placed in a tube furnace and annealed at 880°C for 30 min to transform the phosphorus-doped amorphous silicon film into phosphorus-doped polycrystalline silicon film 3.

[0110] (5) Aluminum oxide film and silicon nitride film are deposited on both sides of the sample to form a back passivation anti-reflection layer 7 and a front passivation anti-reflection layer 8.

[0111] (6) The sample was transferred to a tube furnace and post-treated by hydrogenation under a nitrogen atmosphere and annealed at 450 °C for 30 min to obtain a passivated sheet.

[0112] (7) Screen printing metal grid lines, high temperature sintering, and laser enhanced contact optimization (LECO) processing to form a back metal electrode 9 and a front metal electrode 10 to obtain a TOPCon battery.

[0113] The TOPCon battery structure prepared in this comparative example is as follows Figure 5 As shown, the silver crystal density of the back metal electrode 9 is smaller than that of Example 3, and the penetration depth is greater, and the penetration position is near the nano silicon oxide film 2. Test battery performance, metallization area surface saturation current density J 0, metal 126 fA / cm 2, open circuit voltage V oc is 734.2 mV, short-circuit current J sc is 41.85 mA, fill factor FF It is 84.21% and the battery efficiency is 25.87%.

[0114] The performance of the TOPCon cells prepared in Examples 3 and 4 and Comparative Example 3 is shown in Table 2 below. The results show that the use of the tunneling oxide passivation contact structure of the present invention can improve the cell performance.

[0115] Table 2 Comparison of battery performance between examples and comparative examples sample Example 3 Example 4 Comparative Example 3 <![CDATA[ J 0,metal (fA / cm 2 )]]> 85 72 126 <![CDATA[ V oc (mV)]]> 737.6 738.1 734.2 <![CDATA[ J sc (mA / cm 2 )]]> 41.91 41.93 41.85 (%) 84.91 84.98 84.21 (%) 26.25 26.30 25.87 Although the present invention is disclosed as above, the present invention is not limited thereto. Any person skilled in the art can make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, the protection scope of the present invention shall be subject to the scope defined by the claims.

Claims

1. A tunnel oxide passivation contact structure with stacked polysilicon, characterized in that: It includes a nano silicon oxide film arranged on a crystalline silicon substrate, and a phosphorus-doped polysilicon film and a multi-element doped polysilicon film alternately arranged on the nano silicon oxide film, the multi-element doped polysilicon film is doped with phosphorus and functional elements, the functional elements are selected from one or more of carbon, nitrogen and oxygen, the number of the phosphorus-doped polysilicon film is n layers, the number of the multi-element doped polysilicon film is m layers, n≥2, m≥1, and 1≥nm≥-1.

2. The tunnel oxide passivation contact structure with stacked polysilicon according to claim 1, characterized in that: The number m of the multi-element doped polysilicon thin films is 2 to 3 layers.

3. The tunnel oxide passivation contact structure with stacked polysilicon according to claim 1, characterized in that: The functional element doping concentration in the multi-element doped polysilicon film is 1×10 18 ~5×10 21 cm -3 , the phosphorus doping concentration is 5×10 19 ~1×10 21 cm -3 .

4. The tunnel oxide passivation contact structure with stacked polysilicon according to any one of claims 1 to 3, characterized in that: The thickness of the multi-element doped polysilicon film is 5-200 nm.

5. The tunnel oxide passivation contact structure with stacked polysilicon according to claim 1, characterized in that: The phosphorus doping concentration in the phosphorus-doped polysilicon film is 6×10 19 ~2×10 21 cm -3 .

6. The tunnel oxide passivation contact structure with stacked polysilicon according to claim 1 or 5, characterized in that: The thickness of the phosphorus-doped polysilicon film is 5-200 nm.

7. The tunnel oxide passivation contact structure with stacked polysilicon according to claim 1, characterized in that: The thickness of the nano silicon oxide film is 1-3 nm, and the absorption coefficient k of the nano silicon oxide film at a wavelength above 500 nm is less than 0.1 cm -1 .

8. The tunnel oxide passivation contact structure with stacked polysilicon according to claim 7, characterized in that: The nano silicon oxide film contains carbon and / or nitrogen elements.

9. The tunnel oxide passivation contact structure with stacked polysilicon according to claim 1, characterized in that: The invention also comprises a passivation anti-reflection layer arranged on the outermost layer.

10. A method for preparing a tunnel oxide passivation contact structure with stacked polysilicon according to any one of claims 1 to 9, characterized in that: The following steps are involved: S1, prepare silicon wafer and perform RCA cleaning; S2, preparing a nano silicon oxide film on the surface of the substrate; S3. Preparing a phosphorus-doped amorphous silicon film and a multi-element doped amorphous silicon film on the surface of the nano silicon oxide film in sequence, wherein the number of phosphorus-doped amorphous silicon films is n layers, and the number of doped amorphous silicon films is m layers, where n≥2, m≥1, and 1≥nm≥-1; S4. High temperature annealing in the temperature range of 600°C to 1200°C, so that the phosphorus-doped amorphous silicon film is converted into a phosphorus-doped polycrystalline silicon film, and the multi-element doped amorphous silicon film is converted into a multi-element doped polycrystalline silicon film.

11. The method for preparing a tunnel oxide passivation contact structure with stacked polysilicon according to claim 10, characterized in that: The following steps are also included: S5, depositing a passivation anti-reflection layer on the surface of the substrate; S6. Post-hydrogenation treatment, including annealing and light injection treatment, with a temperature range of 300°C to 900°C and a protective atmosphere of an inert atmosphere or an inert atmosphere containing hydrogen.

Citation Information

Cited By

  • Front surface structure and back surface structure of TOPCon solar cell, TOPCon solar cell and preparation of TOPCon solar cell

    CN119342908A

  • TOPCon solar cell front structure, back structure, TOPCon solar cell and its preparation

    CN119342908B

  • Photovoltaic cell, manufacturing method thereof and photovoltaic module