Preparation method of porous silicon and germanium dioxide composite film electrode material
By preparing porous silicon and germanium dioxide composite thin film electrode materials, the problem of insufficient capacity and stability of the positive electrode materials of lithium-ion batteries is solved, and high lithium storage capacity and conductivity are improved, meeting the performance requirements of new energy batteries.
Patent Information
- Application Number
- CN202411153878.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-21
- Publication Date
- 2024-11-22
AI Technical Summary
The existing lithium-ion battery positive electrode materials have problems such as low battery capacity, low voltage and unstable charging and discharge, which limits the development of new energy batteries.
Using the preparation method of porous silicon and germanium dioxide composite thin film electrode materials, by grinding white carbon black, lithium aluminum hydride, carbon powder, hydrofluoric acid and other materials, calcining and soaking, mixing it with germanium dioxide at a molar ratio, and adding acetylene black and PVDF, an active positive electrode material is formed and coated on stainless steel foil.
It achieves a large lithium storage capacity while improving conductivity and discharge stability, meeting higher electrochemical performance requirements.
Smart Images

Figure HDA0005004372030000011 
Figure HDA0005004372030000012 
Figure HDA0005004372030000013
Abstract
Description
Technical Field
[0001] The invention relates to a method for preparing a porous silicon and germanium dioxide composite film electrode material. Background Art
[0002] With the continuous development and progress of the economy, various energy and environmental pollution problems have gradually become prominent. The development of economic, green, environmentally friendly and sustainable new energy technologies has become an inevitable trend. Therefore, driven by the demand for economic and sustainable electrochemical energy storage devices, people's demand for LIBs with better specification capacity, cycle stability, high rate capability and safety is becoming increasingly urgent, which has further stimulated the development of electrode material research, see the prior patent CN109310355B. In the process of new energy development and research, energy and environmental pollution issues have become the focus of people's attention. Based on this background, the development of green, efficient and environmentally friendly new energy technologies has become the dominant direction of the global environmental energy revolution.
[0003] In the current context, new energy batteries are widely used in the field of electronic equipment. However, many problems have also emerged, such as safety, cost, environment, and resources. A series of problems have restricted the development of new energy batteries. In order to solve these fundamental problems, it is urgent to find an energy device that is technologically advanced, safe, reliable, and economically reasonable. Lithium-ion batteries are used in various industries. In order to develop better clean energy, the research and development of their positive electrode materials is very important. The positive electrode materials of LIBs are limited by low battery capacity, low voltage, and unstable charging and discharging. Summary of the invention
[0004] The technical problem to be solved by the present invention is to provide a method for preparing a porous silicon composite film electrode material. The electrode material prepared by the method not only has a large lithium storage capacity, but also has good conductivity and discharge stability.
[0005] In order to solve the above technical problems, the present invention provides a method for preparing a porous silicon and germanium dioxide composite thin film electrode material, comprising the following steps:
[0006] (1) Take 0.6 g of white carbon black and 0.456 g of lithium aluminum hydride and grind them in a mortar for 10 min;
[0007] (2) placing the ground mixture in a crucible and spreading a layer of carbon powder about 0.8 mm thick on the surface;
[0008] (3) placing the crucible in a muffle furnace and heating it to 600°C for calcining for 6 hours, and after cooling to room temperature, taking out the mixed powder in the crucible and placing it in a beaker;
[0009] (4) Add hydrofluoric acid to the beaker and soak for 30 min, then wash and centrifuge with distilled water, 1.2 mol / L dilute hydrochloric acid, and distilled water in sequence;
[0010] (5) finally washing with anhydrous ethanol, filtering, placing in a drying oven, and drying at 600° C. for 12 h to obtain porous silicon;
[0011] (6) mixing the prepared porous silicon and germanium dioxide in a molar ratio of 1:0.8 to 1.2 and grinding for 30 minutes to obtain a composite material;
[0012] (7) Take 0.15 g of the composite material, grind and mix the composite material, acetylene black and PVDF in a molar ratio of 16:3:1 for 30 min, then add 10-15 drops of NMP solution and continue grinding for 30 min until it becomes viscous to obtain an active positive electrode material;
[0013] (8) Take a stainless steel foil of appropriate size, evenly coat the above active positive electrode material on the stainless steel foil, and then put it into a vacuum drying oven at 60°C for 6 hours before taking it out.
[0014] Advantages of the present invention: Si or Ge electrodes alone cannot meet the requirements of actual commercialization. The composite material of Si and Ge can synergistically exert the advantages of both. The Si component provides a higher lithium storage capacity, and the Ge component ensures high capacity while improving the defect of poor Si conductivity. The electrode material prepared by the present invention not only has a large lithium storage capacity, but also has good conductivity and discharge stability.
[0015] Porous silicon (porous Si) is a new type of one-dimensional nanophotonic crystal material with a "quantum sponge" microstructure with nano-silicon atom clusters as the skeleton. It can be formed by electrochemical anodic corrosion or chemical corrosion of single-crystalline silicon. Porous silicon has good electroluminescent properties. It can generate electrons and holes under the excitation of light or electricity. These carriers can recombine and emit light, move in a directional manner under the action of the electric field, generate electrical signals, and store energy. The optical and electrical properties of porous silicon have opened up a new path for the integration and development of all-silicon-based optoelectronics, and quickly triggered a wave of research on porous silicon at home and abroad. Because porous silicon has a large specific surface area and is easy to oxidize, it is used as a structural isolation layer in integrated circuits. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] Figure 1 It is the XRD pattern of porous silicon.
[0017] Figure 2 It is a SEM picture of porous silicon.
[0018] Figure 3 It is a schematic diagram of the structure of a button battery.
[0019] Figure 4 This is the voltammetric curve of the P-Si / GeO2 composite film with zinc sheet as the negative electrode.
[0020] Figure 5 This is the voltammetric curve of the P-Si / GeO2 composite film with lithium sheet as the negative electrode.
[0021] Figure 6 This is the XRD pattern of P-Si / GeO2.
[0022] Figure 7 This is the SEM image of P-Si / GeO2. DETAILED DESCRIPTION
[0023] A method for preparing a porous silicon composite thin film electrode material comprises the following steps:
[0024] (1) Take 0.6 g of white carbon black and 0.456 g of lithium aluminum hydride and grind them in a mortar for 10 min;
[0025] (2) placing the ground mixture in a crucible and spreading a layer of carbon powder about 0.8 mm thick on the surface;
[0026] (3) placing the crucible in a muffle furnace and heating it to 600°C for calcining for 6 hours, and after cooling to room temperature, taking out the mixed powder in the crucible and placing it in a beaker;
[0027] (4) Add hydrofluoric acid to the beaker and soak for 30 min, then wash and centrifuge with distilled water, 1.2 mol / L dilute hydrochloric acid, and distilled water in sequence;
[0028] (5) finally washing with anhydrous ethanol, filtering, placing in a drying oven, and drying at 600° C. for 12 h to obtain porous silicon;
[0029] (6) mixing the prepared porous silicon and germanium dioxide in a molar ratio of 1:0.8 to 1.2 and grinding for 30 minutes to obtain a composite material;
[0030] (7) Take 0.15 g of the composite material, grind and mix the composite material, acetylene black and PVDF in a molar ratio of 16:3:1 for 30 min, then add 10-15 drops of NMP solution and continue grinding for 30 min until it becomes viscous to obtain an active positive electrode material;
[0031] (8) Take a stainless steel foil of appropriate size, evenly coat the above active positive electrode material on the stainless steel foil, and then put it into a vacuum drying oven at 60°C for 6 hours before taking it out.
[0032] The experimental reagents and equipment used in the above examples are:
[0033] Chemical name Chemical formula Molar mass Production Company White Carbon Black <![CDATA[SiO2]]> 60.08 Maclean Lithium aluminum hydride <![CDATA[LiAlH4]]> 37.95 Braun Welk Ethanol <![CDATA[CH3CH2OH]]> 46.07 Sinopharm Group hydrochloric acid HCl 36.5 Xilong Scientific Reagent Company Hydrofluoric acid HF 20.1 Yongda Chemical Reagent Company Germanium Dioxide <![CDATA[GeO2]]> 104.64 Maclean
[0034] Instrument Name Specifications Production Company Muffle furnace OTF-1200X Hefei Kejing Materials Technology Co., Ltd. Magnetic stirrer DF-101S Yuhua Instrument Co., Ltd. Desktop low speed centrifuge L3-5K Catcher Instruments Co., Ltd. Circulation vacuum pump SHI-D(Ⅲ) Yuhua Instrument Co., Ltd. Programmable oven BXH-65S Shanghai Boxun Instrument Co., Ltd. X-ray diffractometer XRD-7000 Shimadzu Co., Ltd. Electrochemical workstation CHI660E Shanghai Chenhua Instrument Co., Ltd.
[0035] Characterization and testing: In order to verify the inventive effect of this application, the results of this embodiment are characterized.
[0036] 1. XRD characterization of P-Si:
[0037] See also Figure 1 The P-Si material characterization was studied and analyzed through X-ray powder diffraction patterns. In the spectrum of the sample, the 2Theta value and the crystal plane index of the sample diffraction peak are: P-Si [22.947° corresponding to (120), 39.412° for (302), 39.412° corresponding to (412), 58.348° for (333), 60.515° for (423)] crystal plane. According to the overlapping peaks, it can be seen that P-Si was successfully produced.
[0038] 2. Morphology characterization of P-Si:
[0039] See also Figure 2 , it can be seen that P-Si is composed of a large number of micron-sized spherical particles and flakes.
[0040] 3. Electrochemical performance test of P-Si\GeO2 as battery material (button battery):
[0041] See also Figure 3 , assemble the battery parts from top to bottom, including the positive electrode shell, active positive electrode material, diaphragm, lithium sheet, gasket, shrapnel, and negative electrode shell, and add secondary electrolyte.
[0042] Cyclic voltammetry (CV) analysis was performed at a scan rate of 0.001 V / s.
[0043] Figure 4 The results of the previous test using zinc sheets as negative electrode materials show that in the first cycle, the reduction peak is not obvious due to the irreversible side reaction. Therefore, the composite method in the experiment was improved, and lithium sheets were used as negative electrodes. The de- / insertion lithium behavior of P-Si / GeO2 composite films was characterized by testing and analysis. Figure 5 It can be seen that compared with the zinc sheet as the negative electrode, the overlap degree is higher when the lithium sheet is used as the negative electrode, indicating that a stable SEI film is formed between the material and the electrolyte, which greatly reduces the consumption of lithium ions in the battery and has better stability.
[0044] 4. XRD characterization of P-Si\GeO2 materials:
[0045] See also Figure 6The phase characterization of P-Si / GeO2 composite materials was studied and analyzed by X-ray powder diffraction patterns. In the spectrum of the sample, the 2Theta value and the crystal plane index of the sample diffraction peak are: GeO2 [20.605° corresponding to (100), 25.916° corresponding to (101), 35.923° corresponding to (110), 37.954° corresponding to (102), 39.418° corresponding to (111), 41.743° corresponding to (200), 48.544 ° corresponds to (112), 53.280° corresponds to (202), 58.790° corresponds to (211), 65.980° corresponds to (122), 66.970° corresponds to (031), 69.983° corresponds to (014)]; P-Si [35.903° corresponds to (003), 39.412° corresponds to (302), 58.218° corresponds to (333)] crystal plane, and a very obvious diffraction peak appears when the 2Theta value is 25.916°. According to the overlapping peaks, it can be seen that P-Si and GeO2 are well composited.
[0046] 5. Morphological characterization of P-Si\GeO2 materials:
[0047] See also Figure 7 It can be seen that other tiny particles are attached to the surface of micron-sized spherical particles, which can prove the effective compounding of P-Si and GeO2.
Claims
1. A method for preparing a porous silicon and germanium dioxide composite thin film electrode material, characterized in that: The following steps are involved: (1) Take 0.6 g of white carbon black and 0.456 g of lithium aluminum hydride and grind them in a mortar for 10 min; (2) placing the ground mixture in a crucible and spreading a layer of carbon powder about 0.8 mm thick on the surface; (3) placing the crucible in a muffle furnace and heating it to 600°C for calcining for 6 hours, and after cooling to room temperature, taking out the mixed powder in the crucible and placing it in a beaker; (4) Add hydrofluoric acid to the beaker and soak for 30 min, then wash and centrifuge with distilled water, 1.2 mol / L dilute hydrochloric acid, and distilled water in sequence; (5) finally washing with anhydrous ethanol, filtering, placing in a drying oven, and drying at 600° C. for 12 h to obtain porous silicon; (6) mixing the prepared porous silicon and germanium dioxide in a molar ratio of 1:0.8 to 1.2 and grinding for 30 minutes to obtain a composite material; (7) Take 0.15 g of the composite material, grind and mix the composite material, acetylene black and PVDF in a molar ratio of 16:3:1 for 30 min, then add 10-15 drops of NMP solution and continue grinding for 30 min until it becomes viscous to obtain an active positive electrode material; (8) Take a stainless steel foil of appropriate size, evenly coat the above active positive electrode material on the stainless steel foil, and then put it into a vacuum drying oven at 60°C for 6 hours before taking it out.