Device and method for manufacturing high-vanadium cast iron lining of double-screw plastic extruding machine
By using high vanadium cast iron and special riser subsidy technology in the bushing manufacturing of twin-screw extruders, the wear resistance and casting looseness are solved, and efficient bushing manufacturing is achieved, which significantly improves wear resistance and toughness and extends the Its service life and improves production efficiency.
Patent Information
- Application Number
- CN202411445161.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-16
- Publication Date
- 2024-11-26
AI Technical Summary
The wear resistance and strength of the existing twin-screw extruder bushings are insufficient, resulting in frequent replacement, and the looseness of the castings during the casting process affects service life and cleanliness.
The high vanadium cast iron bushing manufacturing device is adopted for the twin-screw extruder. By adding special riser subsidies, the casting flow and flow direction of the iron is guided to achieve all-round compactness and microporelessness of the bushing castings, combining the components of high vanadium ferrochromium ferrochromium molten and Pouring process improves wear resistance and toughness.
It significantly improves the wear resistance and toughness of the bushing, extends the service life, reduces the replacement frequency, and improves production efficiency and product quality.
Smart Images

Figure CN119016686A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of bushing production, and more specifically to a manufacturing device and method for a high-vanadium cast iron bushing for a twin-screw extruder. Background Art
[0002] With the rapid development of the global rubber and plastic, chemical, wood plastic, building materials and other industries, these industries are equipped with a large number of twin-screw extruders, and the bushing is a wear-prone part of the twin-screw extruder, which requires excellent processability and extremely high wear resistance and toughness.
[0003] At present, the bushing materials of twin-screw extruders are usually W6Mo5Cr4V2 high-speed steel and KMTBCr26 high-chromium cast iron. High-speed steel materials have high material and manufacturing costs, long production cycles, and insufficient wear resistance, which leads to frequent component replacement and production delays. Although the bushings made of KMTBCr26 material have low production costs and high efficiency, their wear resistance and toughness strength cannot meet the production requirements of high-strength production conditions such as reinforced nylon. Reinforced nylon is added with glass fiber during production. The greater the amount of glass fiber added, the greater the wear on the plasticizing components of the extruder and injection molding machine. The severe wear and frequent replacement of the plasticizing components have affected the production of the company. The market needs an upgraded product with high strength and high wear resistance.
[0004] Bushings produced by casting process Figure 1 As shown, it includes a bushing body 10 and a bushing inner hole 11 that penetrates transversely. The middle part of the bushing inner hole 11 is a shrinkage compensation part 12. The shrinkage compensation part 12, as the name implies, usually needs to use a riser for shrinkage compensation. The current shrinkage compensation method cannot completely solve the looseness inside the casting; and the bushing inner hole 11 is a key use part. The looseness (small holes) of the inner hole will not only reduce its service life, but also affect the cleanliness of the raw material (if there are holes in the bushing inner hole 11, when producing material A, material A will remain in the hole, affecting the color and performance of material B produced next time). Summary of the invention
[0005] 1. Technical problems to be solved by the invention:
[0006] In view of the problems that the bushings produced by the existing casting process have poor strength and wear resistance, and the looseness inside the casting leads to a short service life and affects the cleanliness of the extruded raw materials, the present invention provides a manufacturing device and method for high-vanadium cast iron bushings for twin-screw extruders. By adding a special riser subsidy to the bushing manufacturing device, the side cavity formed by the riser subsidy guides the flow rate and direction of molten iron during pouring, thereby achieving the purpose of making the bushing casting all-round dense, uniform and free of micropores.
[0007] 2. Technical solution:
[0008] In order to achieve the above object, the technical solution provided by the present invention is:
[0009] A manufacturing device for a high-vanadium cast iron bushing of a twin-screw extruder comprises risers arranged side by side, a bushing cavity is longitudinally arranged between two adjacent risers; the middle riser is connected with a sprue and a runner, and other risers and sprues are in parallel relationship and are all connected with the runner; an ingate is arranged at the bottom of the riser facing the side of the bushing cavity, a mud core adapted to the size and shape of the bushing is arranged inside the bushing cavity, and the device also comprises a riser subsidy, two sides of the riser subsidy are respectively close to the ingate and the bushing cavity, a riser subsidy is arranged between the ingate and the bushing cavity, and the flow rate and direction of molten iron during pouring are guided by the riser subsidy side cavities on both sides of the bushing cavity after molding, thereby at least solving the technical problems of low service life caused by looseness inside the bushing casting and affecting the cleanliness of extruded raw materials.
[0010] A further technical solution is that the riser subsidy is an arc-shaped segment with a thickness gradually decreasing from the middle to the upper and lower sides, so as to guide the flow rate and direction of molten iron during pouring and achieve an all-round shrinkage compensation effect.
[0011] A further technical solution is that the riser subsidy includes an integrally connected subsidy middle section and subsidy transition sections on its upper and lower sides; the subsidy middle section is a rectangular section, and the subsidy transition section is a semi-arc section with a thickness gradually decreasing toward both sides, and the curvature is respectively adapted to the upper and lower parts of the bushing cavity.
[0012] According to a further technical solution, an air vent is vertically fixed at the end of the mud core to further guide the flow rate and direction of molten iron during pouring, facilitate the exhaust of the mud core, and prevent the air vent from entering the mold cavity.
[0013] In a further casting structure, the width L of the riser subsidy is 1 / 4 to 1 / 3 of the length of the bushing cavity; the thickness H of the middle section of the subsidy is 2 / 5 to 1 / 2 of the thickness of the thin-walled position of the bushing.
[0014] A method for manufacturing a high-vanadium cast iron bushing for a twin-screw extruder, comprising the following steps:
[0015] Smelting high vanadium cast iron alloy into molten iron;
[0016] After the mold box including the manufacturing device is subjected to sand mixing, sand molding and box assembly, a bushing cavity is formed inside the molding sand, and side cavities in the shape of riser supplements are formed on both sides of the bushing cavity;
[0017] During pouring, after the molten iron passes through the sprue and the cross runner and fills the bushing cavity and the side cavities on both sides, the side cavities widen the flow channel of the molten iron to the highest point of the bushing cavity and on both sides of its length direction, and can transport more molten iron to the highest point and on both sides of its length direction, making the flow of molten iron smoother, guiding the flow rate and direction of molten iron during pouring, and thereby achieving the technical effect of making the bushing body all-round dense, uniform, and free of micropores.
[0018] Further manufacturing method, the high vanadium chromium iron molten iron composition is 2.6-3.1% C, 0.4-1.2% Si, 0.4-1.0% Mn, ≤0.03% P, ≤0.03% S, 4-6% Cr, 0.8-1.5% Mo, 8-11% V; the balance is Fe and other trace elements. The addition of high V components can form carbides-VC with very high hardness, which are basically spherical in shape. High hardness can improve wear resistance, and the spherical shape can reduce the splitting effect on the matrix, thereby meeting the product's requirements for wear resistance and toughness; the corresponding component of molybdenum can form Mo2C, which mostly appears in the form of eutectic components, which is very beneficial to the wear resistance of high chromium cast iron.
[0019] In the further manufacturing method, the order of adding high vanadium chromium iron water is to first add low carbon steel and pig iron, then add ferromolybdenum and baked high carbon ferrochrome, and finally add ferrovanadium; ferrovanadium is easy to burn and oxidize, so it is added last. When using a medium frequency furnace to melt molten steel, adding the smelting materials in the order of easy first and difficult later is conducive to reducing the difficulty of smelting alloy materials in the material, saving smelting time and reducing energy loss, thereby reducing production costs.
[0020] A further manufacturing method is to tap the molten iron at 1550-1650°C, and add silicon, manganese and 0.1% aluminum wire for deoxidation before tapping the molten iron; because the V element is an active metal element and can easily react with oxygen at high temperatures, effective deoxidation is beneficial to the smooth pouring and filling of the molten iron and the solidification and molding of the casting.
[0021] A further manufacturing method is to pour at a speed of 2.5 to 3.0 kg / s to achieve a pouring temperature of 1500 to 1550° C. for the molten iron to the bushing cavity (1). Since high-vanadium cast iron is prone to form an oxide film, a pouring temperature of 1500 to 1550° C. can improve the fluidity of the molten iron and allow for rapid pouring to prevent defects such as cold shut wrinkles and insufficient pouring.
[0022] 3. Beneficial effects:
[0023] Compared with the prior art, the technical solution provided by the present invention has the following beneficial effects:
[0024] (1) The manufacturing device and manufacturing method of the high vanadium cast iron bushing of the twin screw extruder of the present invention solves the looseness problem of the high vanadium cast iron bushing of the twin screw extruder by adding external subsidies, and increases the riser subsidies to guide and relax the flow channel of molten iron to the highest point and the farthest end, so that more molten iron can be transported to the highest point and the farthest end, thereby achieving the technical effect of all-round shrinkage compensation of the bushing and dense internal density without micropores;
[0025] (2) The high vanadium cast iron bushing and manufacturing method of the twin-screw extruder of the present invention adopts high vanadium cast iron molten iron casting to improve the wear resistance of the bushing casting. The wear resistance is 2.5 to 3 times that of bushing products made of W6Mo5Cr4V2 high-speed steel and KMTBCr26 high chromium cast iron. At the same time, it has excellent toughness, improves the impact resistance of the bushing product, meets the use requirements of the bushing product in a high-intensity working environment, and has obvious use effect. The replacement frequency of the bushing is reduced by more than half, the work efficiency is significantly improved, the cost is saved and the production capacity is increased. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 It is a schematic diagram of the structure of a high vanadium cast iron bushing for a twin-screw extruder in the prior art;
[0027] Figure 2 It is a schematic diagram of the structure of a twin-screw extruder bushing manufacturing device in the prior art;
[0028] Figure 3 for Figure 2 Schematic diagram of the local structure;
[0029] Figure 4 It is a structural schematic diagram of a manufacturing device for a high vanadium cast iron bushing for a twin-screw extruder according to a specific embodiment;
[0030] Figure 5 It is a schematic diagram of the bushing cavity and riser subsidy structure of a specific embodiment.
[0031] Figure 6 for Figure 4 A side view schematic diagram of the structure;
[0032] Figure 7 It is a schematic diagram of the structure of a high vanadium cast iron bushing for a twin-screw extruder according to a specific embodiment.
[0033] In the figure: 1. Bushing cavity; 2. Riser subsidy; 3. Riser; 5. Mud core; 6. Straight runner; 7. Cross runner; 10. Bushing body; 11. Bushing inner hole; 12. Shrinkage compensation part; 20. Riser subsidy raised section; 21. Subsidy middle section; 22. Subsidy transition section; 31. Inner gate; 51. Vent hole. DETAILED DESCRIPTION
[0034] In order to further understand the content of the present invention, the invention is described in detail with reference to the accompanying drawings.
[0035] Example 1
[0036] The manufacturing device of the high vanadium cast iron bushing of the twin screw extruder of the present embodiment is as follows: Figure 4As shown, it includes risers 3 arranged side by side, usually three risers 3 arranged side by side form a group; a bushing cavity 1 is longitudinally arranged between two adjacent risers 3; the middle riser 3 is connected with a sprue 6 and a runner 7, and the other risers 3 and the sprue 6 are in parallel relationship and are all connected with the runner 7; an inner gate 31 is arranged at the bottom of the riser 3 facing the side of the bushing cavity 1, and the inside of the bushing cavity 1 is a mud core 5 adapted to the size and shape of the bushing, and also includes a riser subsidy 2, and the two sides of the riser subsidy 2 are respectively close to the inner gate 31 and the bushing cavity 1. The riser subsidy 2 is an arc segment with a thickness gradually decreasing from the middle to the upper and lower sides, so as to guide the flow rate and flow direction of molten iron during pouring, so as to achieve a full range of shrinkage compensation effect. The riser subsidy 2 includes an integrally connected subsidy middle section 21 and subsidy transition sections 22 on its upper and lower sides; the subsidy middle section 21 is a rectangular section, and the subsidy transition section 22 is a semi-arc section with a thickness gradually decreasing toward both sides, and the curvature is respectively adapted to the upper and lower parts of the bushing cavity 1. An air outlet 51 is vertically fixed at the end of the mud core 5 to further guide the flow and direction of molten iron during pouring, and is conducive to the exhaust of the mud core to prevent the air hole from entering the cavity. Figure 5 , 6 As shown, the width L of the riser subsidy is 1 / 4 to 1 / 3 of the length of the bushing cavity; the thickness H of the middle section of the subsidy is 2 / 5 to 1 / 2 of the thickness of the thin-walled position of the bushing, which can achieve the effect of guiding the flow rate and flow direction of molten iron pouring. Taking the production of the 95 model bushing of the twin-screw extruder as an example, the width L of the riser subsidy 2 is preferably 125mm, and the thickness H of the middle section 21 of the subsidy is preferably 8mm, so as to achieve the optimal flow rate and flow direction of molten iron pouring to the bushing cavity 1 without dead ends.
[0037] The manufacturing method of the high vanadium cast iron bushing of the twin screw extruder of this embodiment is to make the bushing of the twin screw extruder model 95, and the steps are as follows:
[0038] Step 1: After the mold box including the above manufacturing device is mixed with sand, molded and assembled, a hollow cavity structure of the bushing cavity 1 is formed inside the molding sand, and side cavities in the shape of riser patches 2 are generated on both sides of the bushing cavity 1;
[0039] Step 2: During pouring, the pouring temperature of molten iron is 1500-1550°C. After the molten iron enters the bushing cavity 1 and the side cavities on both sides thereof through the runner 6, the pouring structure widens the flow channel of the molten iron toward the highest point of the bushing cavity 1 and the far ends on both sides thereof in the length direction.
[0040] like Figure 2 , 3 As shown, the side casting mold of the prior art has Figure 3 Except for the riser direct feeding part 12 in the red circle, the other parts of the bushing cavity 1 are thin-walled. Although the riser feeding part 12 is relatively thick, it is difficult for the riser to feed the thin-walled part at the highest point and the farthest end of the product. Figure 4 ,5 As shown in Figure 6, the manufacturing device of the high vanadium cast iron bushing of the twin-screw extruder of this embodiment increases the thickness of the product at the riser 3 by adding the riser subsidy 2, so that the molten iron at this part gradually solidifies slowly from the middle to both sides, and then this part of the molten iron is pushed to the highest point and the farthest thin-wall position in stages. The molten iron pouring temperature is 1500-1550℃, which cooperates with the special pouring structure to transport more molten iron in stages along the semi-arc subsidy transition section 22 to the highest point and both sides of its length direction, so that the circulation of molten iron is smoother, and then the flow rate and flow direction of the molten iron during pouring are guided to the bushing cavity 1 without dead ends.
[0041] The twin-screw extruder high vanadium cast iron bushing manufacturing device of this embodiment, during the process of producing the bushing, sets a riser subsidy 2 between the inner gate 31 and the bushing cavity 1, and guides the flow rate and direction of molten iron pouring through the riser subsidy 2 side cavities on both sides of the bushing cavity 1 after molding, thereby at least solving the technical problems of low service life caused by loose internal part of the bushing casting and affecting the cleanliness of the extruded raw materials.
[0042] Example 2
[0043] The twin-screw extruder high vanadium cast iron bushing manufacturing device of this embodiment has the same basic structure and bushing manufacturing steps as Example 1, and the difference or improvement lies in that the air outlet 51 is in the shape of a cone closing upward, which plays a role in collecting and guiding the air, and further guides the flow rate and direction of the molten iron when pouring through the air pressure flow direction.
[0044] The molten iron is molten iron after smelting high vanadium cast iron alloy, and the composition of the molten iron after smelting is 2.6-3.1% C, 0.4-1.2% Si, 0.4-1.0% Mn, ≤0.03% P, ≤0.03% S, 4-6% Cr, 0.8-1.5% Mo, 8-11% V, and the balance is Fe and other trace elements. In the present embodiment, preferably 2.8% C, 0.8% Si, 0.7% Mn, ≤0.01% P, ≤0.01% S, 6% Cr, 1.3% Mo, 10% V, and the balance is Fe and other trace elements. Compared with the molten iron composition of the bushing in the prior art, a relatively high content of 8-11% V is added to the chromium-containing cast iron, which is a high wear-resistant cast iron. The vanadium V element is a strong carbide-forming element. When cast, 8-11% V can not only form primary carbides to refine the alloy structure of the high-chromium cast iron, stabilize the carbides of the high-chromium cast iron, but also form secondary carbides to make it easier to obtain martensite in the cast state. The extremely small vanadium carbide particles are evenly distributed in the organization, thereby greatly improving the wear resistance of the high-chromium cast iron. The addition of high V components can form carbides-VC with very high hardness. The carbide is basically spherical in shape. The high hardness can improve the wear resistance, and the spherical shape can reduce the splitting effect on the matrix, thereby meeting the product's requirements for wear resistance and toughness. The addition of an appropriate amount of Mo element can effectively ensure the hardenability of the casting, and molybdenum can also form Mo2C, which mostly appears in the form of eutectic components, which is very beneficial to the wear resistance of the high-chromium cast iron.
[0045] The specific steps of manufacturing are:
[0046] Step 1: Melt the high-vanadium cast iron alloy into molten iron: The order of adding high-vanadium chromium iron molten iron is to add low-carbon steel and pig iron first, then add ferromolybdenum and roasted high-carbon ferrochrome, and finally add ferrovanadium; ferrovanadium is easy to burn and oxidize, so it is added last. When using a medium-frequency furnace to melt molten steel, adding the smelting materials in the order of easy first and difficult later is beneficial to reduce the difficulty of smelting alloy materials in the material, save smelting time and reduce energy loss, thereby reducing production costs; molten iron is discharged at 1550-1650℃, and silicon, manganese and 0.1% aluminum wire are added before the molten iron is discharged for deoxidation; because the V element is an active metal element, it is easy to react with oxygen at high temperature, and effective deoxidation is beneficial to the smooth pouring and filling of molten iron and the solidification and forming of castings;
[0047] Step 2: Sand mixing, the sand properties are controlled at 5.5-6.5% moisture, 110-140 air permeability, 120-150 kPa wet compression strength, and 38-42% compaction rate;
[0048] Step 3: manufacturing the device mold, including sand mixing, sand molding and box assembly, forming a hollow cavity structure of the bushing cavity 1 inside the molding sand, and generating side cavities in the shape of riser patches 2 on both sides of the bushing cavity 1;
[0049] Step 4: pouring, including pouring with high vanadium chromium iron molten iron, the molten iron enters the bushing cavity 1 of the barrel bushing of the twin-screw extruder through the sprue 6, the cross runner 7, the riser runner and the inner gate 31, until the molten iron completely fills the bushing cavity 1; the pouring speed is 2.5-3.0 kg / s, and the pouring temperature of the molten iron reaches 1500-1550°C to the bushing cavity 1. Since high vanadium cast iron is easy to form an oxide film, the pouring temperature of 1500-1550°C can improve the fluidity of the high vanadium chromium iron molten iron and quickly pour it to prevent defects such as cold shut wrinkles and insufficient pouring.
[0050] Step 5: Unpack after 4 hours of heat preservation. Keep the heat preservation site dry to prevent the casting from cracking.
[0051] Step 6: Beat the box to remove the sand, including knocking the box to vibrate it, so that the sand and the casting fall together, and the mud core 5 also collapses and falls off at the same time, and then the casting is taken out with a hook;
[0052] Step 7: Remove the side riser 3;
[0053] Step 8: Shot blasting and polishing: using a hook-type shot blasting machine to perform shot blasting and polishing to obtain a high-vanadium cast iron bushing for a twin-screw extruder;
[0054] like Figure 7 As shown, the obtained high-vanadium cast iron bushing for the twin-screw extruder includes a bushing body 10 and a bushing inner hole 11 that runs through the bushing body 10 transversely, and also includes a riser subsidy convex section 20 that is symmetrically side-casted on both sides of the middle of the bushing body 10. The riser subsidy convex section 20 is generated after the side cavity in the shape of the riser subsidy 2 is filled with molten iron. The shape and size of the riser subsidy convex section 20 are adapted to the shape of the riser subsidy 2. It is an arc-shaped section whose thickness gradually decreases from the middle to the upper and lower sides, and the curvature is adapted to the upper and lower parts of the bushing body 10 respectively. By using the riser subsidy 2 to compensate for the shrinkage of the casting and using high-vanadium cast iron for casting, not only can the quality of the bushing be improved and surface cracking be reduced, but also the generation of shrinkage cavities and shrinkage can be effectively prevented, and the strength, impact toughness and wear resistance of the bushing casting can be improved.
[0055] Through cross-section metallographic inspection, the bushing of the twin-screw extruder model 95, which is made by the corresponding casting process through the above casting structure, has a dense and uniform overall internal structure without obvious micropores; its wear resistance is 2.5 to 3 times that of bushing products made of W6Mo5Cr4V2 high-speed steel and KMTBCr26 high-chromium cast iron. At the same time, it has excellent toughness, which improves the impact resistance of the bushing product and meets the use requirements of the bushing product in high-intensity working environment. The use effect is obvious, and the replacement frequency of the bushing is reduced by more than half.
[0056] The above schematically describes the present invention and its implementation methods, which are not restrictive. The drawings show only one implementation method of the present invention, and the actual structure and manufacturing steps are not limited thereto. Therefore, if a person skilled in the art is inspired by it and, without departing from the purpose of the invention, designs a structure and an implementation method similar to the technical solution without creativity, they shall all fall within the protection scope of the present invention.
Claims
1. A manufacturing device for a high-vanadium cast iron bushing of a twin-screw extruder, comprising risers (3) arranged side by side, a bushing cavity (1) being longitudinally arranged between two adjacent risers (3); the middle riser (3) being connected with a sprue (6) and a runner (7), and the other risers (3) and the sprue (6) being in parallel relationship and all being connected with the runner (7); an inner gate (31) being arranged at the bottom of the riser (3) facing the side of the bushing cavity (1), and a mud core (5) matching the size and shape of the bushing being arranged inside the bushing cavity (1), characterized in that: It also includes a riser patch (2), the two side surfaces of which are respectively in close contact with the inner gate (31) and the bushing cavity (1).
2. The manufacturing device for high vanadium cast iron bushing of twin-screw extruder according to claim 1 is characterized in that: The riser subsidy (2) is an arc-shaped segment whose thickness gradually decreases from the middle to the upper and lower sides.
3. The manufacturing device according to claim 2, characterized in that: The riser patch (2) comprises an integrally connected patch middle section (21) and patch transition sections (22) on its upper and lower sides; the patch middle section (21) is a rectangular section, and the patch transition section (22) is a semi-arc section with a thickness gradually decreasing toward both sides, and the curvature is respectively adapted to the upper and lower parts of the bushing cavity (1).
4. The manufacturing device according to claim 2, characterized in that: An air outlet hole (51) is vertically fixed at the end of the mud core (5).
5. A method for manufacturing a high vanadium cast iron bushing for a twin-screw extruder, characterized in that: The steps are: Smelting high vanadium cast iron alloy into molten iron; After the mold box comprising the manufacturing device according to any one of claims 1 to 4 is subjected to sand mixing, sand casting and box assembly, a bushing cavity (1) is formed inside the molding sand, and side cavities in the shape of riser patches (2) are formed on both sides of the bushing cavity (1); During pouring, molten iron is introduced into and fills the bushing cavity (1) and the side cavities on both sides thereof through the sprue (6) and the cross runner (7).
6. The manufacturing method according to claim 5, characterized in that: The composition of high vanadium chromium iron molten iron is 2.6-3.1% C, 0.4-1.2% Si, 0.4-1.0% Mn, ≤0.03% P, ≤0.03% S, 4-6% Cr, 0.8-1.5% Mo, 8-11% V; the remainder is Fe and other trace elements.
7. The manufacturing method according to claim 6, characterized in that: The order of adding materials to high-vanadium ferrochrome molten iron is to add low-carbon steel and pig iron first, then add ferromolybdenum and baked red high-carbon ferrochrome, and finally add ferrovanadium.
8. The manufacturing method according to claim 7, characterized in that: The molten iron is tapped at 1550-1650℃, and silicon, manganese and 0.1% aluminum wire are added for deoxidation before tapping.
9. The manufacturing method according to claim 8, characterized in that: The pouring speed is 2.5~3.0kg / s.
Citation Information
Patent Citations
Pipe-like thin-wall steel part casting die and design method thereof
CN107931543A
Casting process for producing barrel liner of double-screw plastic extruding machine by using high-vanadium-chromium iron
CN107962151A
Mold for batch casting of double-screw plastic extruder barrel liner and casting method thereof
CN109317620A
High vanadium high-wear-resistant alloy and its preparation method
CN1380436A
High-vanadium cast iron lining manufacturing device of double-screw plastic extruding machine
CN223338304U
Cited By