Method for inhibiting pearlite from being generated on surface layer of ultra-low carbon steel hot rolled plate
By controlling the carbon content of tundra cover agent and spraying water slag removal technology, combined with the weak oxidation atmosphere in the heat-smooth furnace, the problem of ultra-low carbon steel surface structure transformation is solved, and the surface defects of cast billets and hot-rolled materials are avoided, ensuring that Product quality.
Patent Information
- Application Number
- CN202410969986.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-18
- Publication Date
- 2024-11-26
AI Technical Summary
When ultra-low carbon steel comes into contact with carbon-containing materials at high temperatures, the surface structure of the surface is transformed from ferrite to pearlite, causing defects in the surface of cast billets and hot-rolled materials. The prior art may lead to protection when the carbon content of the protective slag is reduced. The slag melts too fast, causing defects such as casting roll slag.
By controlling the carbon content of the tundra cover agent to be 1.5-3.0%, controlling the fluctuation of the crystallizer level to be 1-5mm, using a high-pressure nozzle to spray water to remove slag, the CO2+O2 content in the heat-attachment furnace is 15-20%, and Prevent ferrite from transforming into pearlite and ensure that the surface layer of the casting is consistent with the matrix structure.
Without affecting normal production, the transition from ferrite to pearlite is systematically suppressed, the surface defects of the casting and hot-rolled materials are avoided, and the sameness between the surface layer and the matrix structure of the casting is achieved. It is simple to operate and No need to add devices.
Smart Images

Figure CN119016696A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of metallurgical steelmaking process, and in particular relates to a method for inhibiting the formation of pearlite on the surface of an ultra-low carbon steel hot-rolled plate. Background Art
[0002] Steel is smelted from iron ore, also known as iron-carbon alloy, which is an alloy composed of iron (Fe) and carbon (C), silicon (Si), manganese (Mn), phosphorus (P), sulfur (S) and other small amounts of elements (Cr, V, etc.). By adjusting the content of various elements in steel and the heat treatment process, a variety of metallographic structures can be obtained, so that steel has different physical properties.
[0003] The interstitial solid solution formed by carbon dissolving in the interstitial space of the α-Fe lattice is called ferrite, which is distributed in equiaxed polygonal grains and is represented by the symbol F. Its structure and properties are similar to those of pure iron, with good plasticity and toughness, but lower strength and hardness (30-100HB).
[0004] Cementite is a metal compound composed of carbon and iron in a certain proportion, expressed by the molecular formula Fe3C, with a carbon content of 6.69%, forming (Fe,M)3C in the alloy. Cementite is hard and brittle, with almost zero plasticity and impact toughness, high brittleness, and a hardness of 800HB. It is often distributed in steel in the form of a network, semi-net, flake, needle, or granular.
[0005] The mechanical mixture of ferrite and cementite is called pearlite, and its mechanical properties are between ferrite and cementite, with high strength and moderate hardness, and its carbon content is between 0.7% and 0.8%. Pearlite is the eutectoid transformation product of steel, and its morphology is that ferrite and cementite are arranged in layers, like fingerprints.
[0006] The continuous casting process is the process of casting molten steel that has been smelted and meets the requirements of composition and cleanliness into billets. The molten steel is carried by the ladle and sent to the continuous casting platform. The molten steel first flows into the tundish under the action of natural gravity. During the process, the molten steel will contact the refractory material of the tundish working layer and the tundish covering agent. After that, the molten steel will be transported to the crystallizer through the immersed nozzle connected to the tundish. The molten steel forms a billet shell in the crystallizer. The upper layer is covered with protective slag and flows between the billet shell and the crystallizer wall to play a lubricating role. The billet leaves the crystallizer and enters the second cooling section, gradually solidifies and cools down, and then is cut into a single billet. The billet will be sent to the heating furnace before hot rolling, heated to about 1200℃, and after 150-180 minutes of soaking, it will be taken out of the furnace and hot rolled into material.
[0007] Ultra-low carbon steel usually refers to steel with a carbon content of less than 0.06%. Due to the low carbon content of the steel itself, when it comes into contact with materials with high carbon content at high temperatures, the carbon in the material will migrate to the steel, causing carbon increase. The matrix structure of ultra-low carbon steel is usually ferrite, such as Figure 1 , especially the carbon increase on the surface of the ingot, which causes the surface structure to change from ferrite to pearlite (ingot failure) Figure 2 .
[0008] At present, the production of pearlite structure on the surface of low-carbon steel is usually solved by reducing the carbon content of the mold slag, or even using carbon-free mold slag. The main problem is that carbon is an important component of the mold slag. Reducing the carbon content may cause the mold slag to melt too quickly, resulting in defects such as slag curling in the casting. Summary of the invention
[0009] The purpose of the present invention is to solve the above technical problems and provide a method for inhibiting the formation of pearlite on the surface of ultra-low carbon steel hot-rolled plates. Without affecting normal and stable production, the surface structure of the ingot is made the same as that of the matrix, thereby avoiding the generation of surface defects in the continuous casting ingot and subsequent hot-rolled materials.
[0010] To achieve the above object, the present invention provides a method for inhibiting the formation of pearlite on the surface of an ultra-low carbon steel hot-rolled plate, wherein the carbon content of the ultra-low carbon steel is less than 0.06%;
[0011] Control the carbon content of the tundish covering agent to 1.5-3.0%;
[0012] Control the crystallizer liquid level fluctuation to 1-5mm;
[0013] In the secondary cooling section, high-pressure nozzles are used to spray water to remove slag from the ingot;
[0014] During the heating process of the ingot casting, the CO2+O2 content in the soaking furnace is 15% to 20% of the total content of the furnace atmosphere.
[0015] Furthermore, the adding speed of the tundish covering agent is 8 to 12 kg / min.
[0016] Furthermore, the tundish covering agent includes CaO, SiO2 and Al2O3.
[0017] Furthermore, the pressure of water sprayed by a high-pressure nozzle for deslagging in the second cooling section of the cast billet is 10-20 MPa.
[0018] Furthermore, the amount of water used for deslagging by spraying water with a high-pressure nozzle in the secondary cooling section of the cast billet is 2.5 to 4 L / kg.
[0019] Furthermore, the content of O2 in the soaking furnace accounts for 1-5% of the total content of CO2 and O2.
[0020] Furthermore, the protective slag of the crystallizer includes CaO, SiO2, Al2O3, MgO and alkaline oxides.
[0021] Furthermore, the carbon content of the tundish covering agent is 1.5-2.0%.
[0022] Furthermore, the crystallizer liquid level fluctuation is 1 to 3 mm.
[0023] Furthermore, the CO2+O2 content in the soaking furnace is 15% to 17% of the total content of the atmosphere in the furnace.
[0024] Compared with the prior art, the beneficial effects of the present invention are as follows: the present invention realizes the same structure between the surface layer of the ingot and the matrix without affecting normal and stable production, thereby avoiding the generation of surface defects of the continuous casting ingot and subsequent hot-rolled materials; from molten steel casting to ingot hot rolling, the transformation from ferrite to pearlite is systematically suppressed, and the control effect is stable; and there is no need to add any equipment, the operation is simple, and the on-site production feasibility is strong. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 This is the surface organization diagram of low carbon steel;
[0026] Figure 2 This is the pearlite structure diagram of the surface of low carbon steel. DETAILED DESCRIPTION
[0027] The present invention will be further described below in conjunction with the accompanying drawings and specific embodiments.
[0028] For ultra-low carbon steel with [C] < 0.06%, the carbon content on the surface of the steel increases when it comes into contact with high-carbon materials during smelting and continuous casting, which causes the surface structure of the hot-rolled plate to change from ferrite to pearlite. A "three preventions and one promotion" control method is proposed, which includes preventing carbon increase in the liquid steel in the continuous casting tundish, preventing fluctuations in the stable casting of the crystallizer, preventing slag accumulation by rapid cooling and descaling at the end of the secondary cooling stage, and promoting decarburization by high-temperature weak oxidation in the heating furnace. A set of systematic control methods for the entire process from the continuous casting molten steel tundish - crystallizer - secondary cooling of the ingot - hot rolling soaking furnace is formed. This method achieves the same structure of the ingot surface and the matrix without affecting normal and stable production, and avoids the generation of surface defects of the continuous casting ingot and subsequent hot-rolled materials. The specific process is:
[0029] The tundish covering agent is a metallurgical auxiliary material with CaO, SiO2 and Al2O3 as main components, which contains a certain amount of carbon, usually 4-6%. After being added to the surface of the molten steel in the tundish, the carbon will burn at high temperature to form liquid slag. Therefore, the present invention controls the carbon content of the tundish covering agent to be 1.5-3.0% (preferably 1.5-2.0%). During the adding process, the tundish covering agent is added slowly and continuously at a speed of 8-12 kg / min to prevent the liquid level from fluctuating, causing the carbon in the powder slag layer to contact with the molten steel and cause carburization.
[0030] The mold protection slag is a metallurgical auxiliary material with CaO, SiO2, Al2O3, MgO and alkaline oxide as main components. Its main functions are lubrication and heat preservation. The protection slag contains a certain amount of carbon, which plays a role in controlling the melting rate. The carbon content is 1.0% to 10.0%. After being added to the surface of the molten steel in the tundish, the carbon will form liquid slag after burning at high temperature, and a layer with a lower carbon content will exist on the upper layer of the liquid slag. Therefore, the present invention controls the crystallizer liquid level fluctuation to 3 to 5 mm (preferably 1 to 3 mm) to prevent the liquid level fluctuation from causing the molten steel to contact with the slag layer and cause carbon increase in the molten steel.
[0031] After the casting is demoulded by the crystallizer, a casting with a liquid core inside the surface shell is formed. After entering the secondary cooling section, the surface is covered with a protective slag film, and the outer layer of the slag film will entrain a part of the powder slag, which contains a certain amount of carbon. Therefore, the casting of the present invention adopts a high-pressure nozzle to spray water to remove slag in the secondary cooling section to remove the slag skin on the surface of the casting to prevent the residual protective slag from carburizing at high temperature, causing carbon increase on the surface of the casting, and the pressure is 10-20MPa and the water volume is 2.5-4L / kg.
[0032] During the heating process of the ingot, the carbon content of the surface layer will decrease with the changes of the atmosphere in the heating furnace, heating time and other conditions. This phenomenon is called decarburization. Therefore, the present invention adopts a control of the weak oxidizing atmosphere in the soaking furnace, the CO2+O2 content in the soaking furnace is 15% to 20% (preferably 15% to 17%) of the total content of the furnace atmosphere, and the O2 content accounts for 1 to 5% of the total content of CO2 and O2, which promotes decarburization of the surface layer of the ingot within the range of 100 to 500 μm, further balances the carbon increase of the surface layer of the ingot caused by improper process operation, and finally achieves the effect of stable composition.
[0033] Example
[0034] Aiming at the surface pearlite banding defects that appear after hot rolling of ultra-low carbon steel continuous casting billet in Wuhan Iron and Steel Co., Ltd.'s thin slab production line, a new process was designed using this method. The carbon content of the tundish covering agent was controlled at 1.6%, and it was added slowly and continuously at a rate of 10 kg / min, and there was no liquid level fluctuation during the addition process. The crystallizer protection slag was added multiple times and slowly. The immersion depth during the continuous casting process was 190mm, and the pulling speed was reduced to below 3-4m / min to ensure that the crystallizer liquid level fluctuation was 1-3mm; the secondary cooling zero stage used high-pressure water to remove slag, the secondary cooling water pressure was 10MPa, and the water volume was 2.5L / kg, ensuring that the residue on the surface of the billet after leaving the casting machine was cleaned. After the billet entered the heating furnace, the heating furnace was controlled to be a weak oxidizing atmosphere, and the CO2+O2 content in the heating furnace was controlled at 16%.
[0035] After this process, the pearlite on the surface of the hot-rolled plate basically disappears, showing a pure ferrite structure, which meets the product quality requirements.
Claims
1. A method for inhibiting the formation of pearlite on the surface of an ultra-low carbon steel hot-rolled plate, wherein the carbon content of the ultra-low carbon steel is less than 0.06%; characterized in that: Control the carbon content of the tundish covering agent to 1.5-3.0%; Control the crystallizer liquid level fluctuation to 1-5mm; In the secondary cooling section, high-pressure nozzles are used to spray water to remove slag from the ingot; During the heating process of the ingot casting, the CO2+O2 content in the soaking furnace is 15% to 20% of the total content of the furnace atmosphere.
2. The method for inhibiting the formation of pearlite on the surface of ultra-low carbon hot-rolled steel sheet according to claim 1, characterized in that: The adding speed of the tundish covering agent is 8 to 12 kg / min.
3. The method for inhibiting the formation of pearlite on the surface of ultra-low carbon hot-rolled steel sheet according to claim 1, characterized in that: The tundish covering agent includes CaO, SiO2 and Al2O3.
4. The method for inhibiting the formation of pearlite on the surface layer of ultra-low carbon hot-rolled steel sheet according to claim 1, characterized in that: The pressure of water spraying for deslagging of the cast billet in the secondary cooling section by high-pressure nozzles is 10-20 MPa.
5. The method for inhibiting the formation of pearlite on the surface of ultra-low carbon hot-rolled steel sheet according to claim 1, characterized in that: The casting blank is sprayed with water in the secondary cooling section with a water volume of 2.5-4 L / kg for slag removal by using a high-pressure nozzle.
6. The method for inhibiting the formation of pearlite on the surface of ultra-low carbon hot-rolled steel sheet according to claim 1, characterized in that: The content of O2 in the soaking furnace accounts for 1-5% of the total content of CO2 and O2.
7. The method for inhibiting the formation of pearlite on the surface of ultra-low carbon hot-rolled steel sheet according to claim 1, characterized in that: The protective slag of the crystallizer includes CaO, SiO2, Al2O3, MgO and basic oxides.
8. The method for inhibiting the formation of pearlite on the surface layer of ultra-low carbon hot-rolled steel sheet according to claim 1, characterized in that: The carbon content of the tundish covering agent is 1.5-2.0%.
9. The method for inhibiting the formation of pearlite on the surface of ultra-low carbon hot-rolled steel sheet according to claim 1, characterized in that: The crystallizer liquid level fluctuation is 1 to 3 mm.
10. The method for inhibiting the formation of pearlite on the surface layer of ultra-low carbon hot-rolled steel sheet according to claim 1, characterized in that: The CO2+O2 content in the soaking furnace is 15% to 17% of the total content of the atmosphere in the furnace.