Seamlessly spliced multilayer solid wood composite floor processing technology

Through seamless splicing of multi-layer solid wood composite flooring processing technology, natural plant-based glue liquid and nano-silicon dioxide are used to solve the problem of water absorption and expansion of the floor in humid environments and environmental protection standards not meeting, achieving safety and durability The improvement of aesthetics meets the health and environmental protection needs of modern consumers.

CN119017497AInactive Publication Date: 2024-11-26HOMONISIA HOME FURNISHING CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411136846.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-19
Publication Date
2024-11-26
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

In the processing process, the existing multi-layer solid wood composite floor has problems such as fall off of veneer layer, deformation of the underlying material, insufficient moisture-proof treatment and inconsistent environmental protection standards, resulting in water absorption and expansion, aesthetics and health risks of the floor in humid environments.

Method used

Using seamless splicing of multi-layer solid wood composite flooring, the process of using natural plant-based glue and nano-silicon dioxide through rotary cutting, drying, glue coating, pre-pressing, hot pressing, edge cutting and painting. Combined with polyurethane varnish, it forms a safe, legacy-free, not easy to absorb and expand, beautiful and seamless floor.

Benefits of technology

It has achieved improvements in the safety, durability and environmental protection of the floor, reduced the emission of harmful substances in the production process, reduced installation costs, and ensured the stability and aesthetics of the floor, and comply with modern environmental protection standards.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a processing technology of a seamlessly spliced multilayer solid wood composite floor, and belongs to the field of floor processing technologies, and the composite floor produced by the processing technology has the characteristics of safety, no formaldehyde, difficulty in water swelling, difficulty in cracking, attractiveness and no seam. A glue solution used in the gluing process is composed of natural rubber, pine resin, aromatic resin, purified water, rosin phenol, a sodium hydroxide solution, nano silicon dioxide and plant fibers. The glue solution used in the invention is natural plant components, does not contain harmful volatile chemical compounds, has small influence on environment and human health, does not contain chemical additives or harmful components, has small irritation on skin and respiratory system, and can also be used by chemically sensitive people; and nano silicon dioxide in the glue solution can be effectively filled in gaps of the plates to improve the bonding effect, so that the floor is more difficult to crack and deform in the daily use process, and the floor can still keep relatively good appearance in the long-time use process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of floor processing technology, and in particular relates to a seamlessly spliced ​​multi-layer solid wood composite floor processing technology. Background Art

[0002] Laminated flooring originated in the 1990s as an innovation and improvement of traditional solid wood flooring. It was originally designed to solve the problem of solid wood flooring's easy expansion and deformation in humid environments. The manufacturing process includes several key steps such as wood selection, drying, gluing, lamination, cutting and surface treatment. Modern technology enables the floor to better resist the effects of humidity and temperature changes while maintaining the advantages of traditional wood. Compared with traditional wooden floors, the multi-layer structure of solid wood composite flooring effectively reduces the expansion and contraction of wood caused by environmental changes. It is suitable for a wider range of installation environments and has lower manufacturing costs, but still provides similar appearance and performance. Overall, through continuous technological innovation and market adaptation, laminate flooring has developed from an initial substitute to a high-performance, highly decorative flooring option that meets the various needs of modern living and commercial environments.

[0003] At present, there are still some defects in the processing technology of multi-layer solid wood composite flooring. In the manufacture of composite flooring, the veneer layer usually uses glue to bond the solid wood veneer to the base layer. If the veneer bonding is not firm or the glue quality is not high, it is easy to cause the veneer layer to fall off or bubble during the use of the floor. The bottom layer of the composite floor often uses HDF or MDF boards. If the quality of these materials is uneven or the density is insufficient, it may cause the floor to deform, crack or warp easily. Insufficient moisture-proof treatment. The bottom material of the composite floor is often easy to absorb water. If the moisture-proof treatment is insufficient during the manufacturing process or the glue used is not waterproof, it may cause the floor to absorb water and swell in a humid environment, affecting the service life and aesthetics. The production process is imperfect. If the temperature and pressure control during the production process is not proper, the internal structure of the floor may be unstable, and it is easy to crack, break and other problems. Environmental protection standards do not meet the requirements. The glue and materials used in early composite floors may not meet modern environmental protection standards, contain harmful substances such as formaldehyde, affect indoor air quality, and do not meet the requirements of consumer health and environmental awareness.

[0004] The main defects of traditional multi-layer solid wood composite flooring in processing technology usually involve veneer quality, bottom material selection and processing, production process control, etc. With the advancement of technology and the improvement of consumers' quality requirements, a new multi-layer solid wood flooring processing technology is urgently needed to solve the above problems. Summary of the invention

[0005] The purpose of the present invention is to provide a processing technology for seamlessly spliced ​​multi-layer solid wood composite flooring. The composite flooring produced by the processing technology has the characteristics of being safe, formaldehyde-free, not easy to absorb water and expand, not easy to crack, and beautiful and seamless.

[0006] The technical solution of the invention is that a seamless multi-layer solid wood composite floor processing technology comprises the following specific steps:

[0007] Single board peeling: Use a peeling machine to peel the board, select the unqualified boards, and get the single board; the selected board standard is that it can withstand 2MPa pressure, 1.5MPa bending force without deformation, and has uniform color;

[0008] Veneer drying: After the veneer is dried with a dryer, the preliminarily dried board is placed in a drying kiln for 3-7 days, and then the boards are stacked for 2-9 days to select boards with unqualified moisture content; the dryer is set at a temperature of 65°C and a wind speed of 15km / h; the drying kiln temperature is set at 40°C and a wind speed of 5km / h; the selection standard for qualified boards is a moisture content of less than 10%.

[0009] Gluing and assembling: apply glue on the bottom of the surface plate, apply glue on the bottom plate, apply glue on both sides of the upper plate, the middle plate and the lower plate, and then glue the surface plate, the upper plate, the middle plate, the lower plate and the bottom plate together in order from top to bottom to obtain a plain plate 1; wherein the surface plate is made of a 1.2-2.5mm veneer made of ash board, the upper plate is made of a 2-3mm veneer made of birch board, the middle plate is made of a 6-8mm veneer made of birch board, the lower plate is made of a 0.5-1.2mm veneer made of eucalyptus board, and the bottom plate is made of a 0.8-2.2mm veneer made of camphor board.

[0010] Tissue culture pre-pressing: Use a press to pre-press the plain plate 1 at a constant temperature, and obtain the plain plate 2 after the pre-pressing is completed; wherein the temperature of the press is set to 45-75°C, the pressure is set to 0.8-1.2MPa, and the time is 45-55min.

[0011] Assembly hot pressing: Use a hot press to heat and hot press the plain plate 2, and obtain the plain plate 3 after the hot pressing is completed; the temperature of the hot press is set to 130-140°C, the pressure is set to 0.9-1.4MPa, and the time is set to 25-35min.

[0012] Finished product after trimming: After the plain board 3 is naturally cooled and stacked for 7 days, it is trimmed and sprayed with polyurethane varnish and dried for 3-7 days to obtain the finished floor. The size of the floor after trimming is 900mm in length and 120mm in width; there is a nano-glue coating covered with plastic at the bottom of the board, and the plastic can be torn off and pasted on the floor when it is needed.

[0013] Finished mortise and tenon product: Place the pre-finished baseboard into the mortise and tenon machine, set the left side of the floor as the tenon and the right side as the mortise. After the mortise and tenon are completed, seal the bottom surface of the floor with nano-glue to obtain the finished floor; the length of the left tenon is 15mm, and the depth of the right mortise is 14.8mm; during the installation process, insert the tenon into the mortise to achieve seamless splicing.

[0014] The preparation method of the glue solution comprises the following steps:

[0015] A1: Raw material preparation: weigh 20-35 parts of natural rubber, 5-10 parts of pine resin, 5-10 parts of fragrant resin, 35-55 parts of purified water, 8-15 parts of 5% sodium hydroxide solution, 1-3 parts of nano-silicon dioxide, and 10-15 parts of plant fiber according to weight;

[0016] A2: Add purified water and natural rubber to the reactor, heat to 55-65℃, stir until completely dissolved and gradually add pine resin and fragrant resin and stir again;

[0017] A3: Add 5% sodium hydroxide solution dropwise to the product in step A2 at a drop rate of 1-2 drops / s, transfer to a magnetic stirrer, set the speed to 200-300 rpm, and react for 1-2 hours to obtain a base glue;

[0018] A4: After the base glue cools down to room temperature, add the plant fiber, heat to 55-65℃, set the stirrer speed to 500-600rpm and stir for 30min, then add nano silicon dioxide and keep the temperature unchanged, stir for 1-2h and wait for it to cool down to room temperature to obtain the required glue solution.

[0019] The beneficial effects of the present invention are:

[0020] The glue used in the present invention is a natural plant component and does not contain harmful volatile chemical compounds, which has little impact on the environment and human health. The glue used in the present invention reduces the negative impact on air quality during the production and use process. The glue used in the present invention has low sensitivity. Since it does not contain chemical additives and harmful components, it has little irritation to the skin and respiratory system, and can also be used by chemically sensitive people.

[0021] The present invention only requires two steps, pre-pressing and hot pressing, to achieve the gluing effect of the panels, which effectively reduces the steps of the traditional process and reduces the process complexity and cost. It not only facilitates the workmanship of manufacturers but also effectively reduces the emission of harmful substances during the production process, and is more in line with environmental protection requirements.

[0022] The nano-silicon dioxide in the adhesive of the present invention can effectively fill the gaps in the boards, thereby increasing the contact area between the adhesive and the boards, accelerating the curing efficiency and improving the bonding effect. It is less likely to crack and deform during daily use, and can keep the floor in a relatively good appearance during long-term use.

[0023] The bottom of the finished floor of the present invention is bonded with nano glue. During the installation process, it only needs to tear off the plastic seal and stick it on the ground to complete the installation, which greatly reduces the installation cost and can achieve seamless installation while ensuring good stability, which is both beautiful and practical.

[0024] The polyurethane varnish used in the painting process of the present invention has good wear resistance and durability and is suitable for high-intensity use floors. Through the above-mentioned combination, the formaldehyde emission of the present invention during daily use is far lower than the E1 grade index specified in the standard. DETAILED DESCRIPTION

[0025] In order to make the technical means, creative features, objectives and effects achieved by the present invention easy to understand, the present invention is further described below in conjunction with specific embodiments and diagrams.

[0026] The experimental methods in the following examples, unless otherwise specified, are conventional methods, and are performed according to the techniques or conditions described in the literature in the field or according to the product instructions. The materials and reagents used in the following examples, unless otherwise specified, can be obtained from commercial channels.

[0027] Example 1

[0028] 1. Raw material preparation: weigh 25g natural rubber, 5g pine resin, 5g fragrant resin, 40ml pure water, 10ml 5wt% sodium hydroxide solution, 3g nano-silicon dioxide, and 12g plant fiber.

[0029] 2: Add 40ml of pure water and 25g of natural rubber to the reactor, heat to 65°C, stir until completely dissolved and gradually add 5g of pine resin and 5g of fragrant resin and stir again;

[0030] 3: Add 10 ml of 5% sodium hydroxide solution dropwise to the product in step 2 at a drop rate of 2 drops / s, transfer to a magnetic stirrer, set the speed to 300 rpm, and react for 1 hour to obtain a base glue;

[0031] 4: After the base glue cools to room temperature, add 12g of plant fiber, heat to 65°C, set the stirrer speed to 600rpm and stir for 30min, then add nano-silicon dioxide and keep the temperature unchanged, stir for 2h and wait for it to cool to room temperature to obtain the required glue solution.

[0032] Example 2

[0033] 1. Raw material preparation: weigh 20g natural rubber, 10g pine resin, 10g fragrant resin, 38ml pure water, 10ml 5wt% sodium hydroxide solution, 2g nano-silicon dioxide, and 10g plant fiber.

[0034] 2: Add 38 ml of pure water and 20 g of natural rubber to the reactor, heat to 55 ° C, stir until completely dissolved and gradually add 10 g of pine resin and 10 g of fragrant resin and stir again;

[0035] 3: Add 10 ml of 5% sodium hydroxide solution dropwise to the product in step 2 at a drop rate of 1 drop / s, transfer to a magnetic stirrer, set the speed to 200 rpm, and react for 2 hours to obtain a base glue;

[0036] 4: After the base glue cools to room temperature, add 10g of plant fiber, heat to 65°C, set the stirrer speed to 600rpm and stir for 30min, then add nano-silicon dioxide and keep the temperature unchanged, stir for 2h and wait for it to cool to room temperature to obtain the required glue solution.

[0037] Example 3

[0038] 1. Raw materials preparation: weigh 27g natural rubber, 8g pine resin, 7g fragrant resin, 35ml pure water, 5ml 5wt% sodium hydroxide solution, 3g nano-silicon dioxide, and 15g plant fiber.

[0039] 2: Add 35 ml of pure water and 27 g of natural rubber to the reactor, heat to 55 ° C, stir until completely dissolved and gradually add 8 g of pine resin and 7 g of fragrant resin and stir again;

[0040] 3: Add 5 ml of 5% sodium hydroxide solution dropwise to the product in step 2 at a drop rate of 1 drop / s, transfer to a magnetic stirrer, set the speed to 300 rpm, and react for 2 h to obtain a base glue;

[0041] 4: After the base glue cools to room temperature, add 10g of plant fiber, heat to 65°C, set the stirrer speed to 600rpm and stir for 30min, then add nano-silicon dioxide and keep the temperature unchanged, stir for 2h and wait for it to cool to room temperature to obtain the required glue solution.

[0042] Aging performance test:

[0043] The damp heat aging test was carried out according to the GB / T2423.3 test method. Test conditions: +85°C, relative humidity 85%, 1000h.

[0044] Table 1, peel strength and aging performance test results of the adhesives prepared in Examples 1-3

[0045] Performance parameters Example 1 Example 2 Example 3 Peel strength before aging N / cm 2.35 2.62 2.28 Peel strength after constant humidity and heat aging for 1000h N / cm 2.11 2.27 2.03

[0046] From the analysis of the above table, it can be seen that the adhesives prepared in Examples 1-3 have strong peeling strength and anti-aging ability.

[0047] Example 4

[0048] Single board peeling: Use a peeling machine to peel the board, select the unqualified boards, and get the single board; the selected board standard is that it can withstand 2MPa pressure, 1.5MPa bending force without deformation, and has uniform color;

[0049] Veneer drying: After the veneer is dried with a dryer, the preliminarily dried boards are placed in a drying kiln for 3-7 days, and then the boards are stacked for 9 days to select boards with unqualified moisture content; the dryer is set at a temperature of 65°C and a wind speed of 15km / h; the drying kiln temperature is set at 40°C and a wind speed of 5km / h; the selection standard for qualified boards is a moisture content of less than 10%.

[0050] Glue coating and assembly: apply the glue prepared in Example 1 on the bottom of the surface plate, apply the glue prepared in Example 1 on the top of the bottom plate, apply the glue prepared in Example 1 on both sides of the upper plate, the middle plate and the lower plate, and then glue the surface plate, the upper plate, the middle plate, the lower plate and the bottom plate together in order from top to bottom to obtain a plain plate 1; wherein the surface plate is a 1.2 mm veneer made of elm wood board, the upper plate is a 2 mm veneer made of birch wood board, the middle plate is a 6 mm veneer made of birch wood board, the lower plate is a 0.5 mm veneer made of eucalyptus wood board, and the bottom plate is a 0.8 mm veneer made of camphor wood board.

[0051] Tissue culture pre-pressing: Use a press to pre-press the plain plate 1 at a constant temperature, and obtain the plain plate 2 after the pre-pressing is completed; the temperature of the press is set to 75°C, the pressure is set to 1.2MPa, and the time is 55min.

[0052] Assembly hot pressing: Use a hot press to heat and hot press the plain plate 2, and obtain the plain plate 3 after the hot pressing is completed; the temperature of the hot press is set to 140°C, the pressure is set to 1.4MPa, and the time is set to 35min.

[0053] Finished product after trimming: After the plain board 3 is naturally cooled and stacked for 7 days, it is trimmed and sprayed with polyurethane varnish and dried for 3-7 days to obtain the finished floor. The size of the floor after trimming is 900mm in length and 120mm in width; there is a nano-glue coating covered with plastic at the bottom of the board, and the plastic can be torn off and pasted on the floor when it is needed.

[0054] Finished mortise and tenon product: Place the pre-finished base plate into a mortise and tenon machine, set the left side of the floor as the tenon and the right side as the mortise. After the mortise and tenon are completed, plastic-seal the bottom surface of the floor with nano-glue to obtain Example 4; wherein the length of the left tenon is 15 mm, and the depth of the right mortise is 14.8 mm.

[0055] Example 5

[0056] Single board peeling: Use a peeling machine to peel the board, select the unqualified boards, and get the single board; the selected board standard is that it can withstand 2MPa pressure, 1.5MPa bending force without deformation, and has uniform color;

[0057] Veneer drying: After the veneer is dried with a dryer, the preliminarily dried boards are placed in a drying kiln for 3-7 days, and then the boards are stacked for 9 days to select boards with unqualified moisture content; the dryer is set at a temperature of 65°C and a wind speed of 15km / h; the drying kiln temperature is set at 40°C and a wind speed of 5km / h; the selection standard for qualified boards is a moisture content of less than 10%.

[0058] Glue coating assembly: apply the glue prepared in Example 2 on the bottom of the surface plate, apply the glue prepared in Example 2 on the top of the bottom plate, apply the glue prepared in Example 2 on the upper and lower surfaces of the upper plate, the middle plate, and the lower plate, and then glue the surface plate, the upper plate, the middle plate, the lower plate, and the bottom plate together in order from top to bottom to obtain a plain plate 1; wherein the surface plate is a 1.2 mm veneer made of elm wood board, the upper plate is a 2 mm veneer made of birch wood board, the middle plate is a 6 mm veneer made of birch wood board, the lower plate is a 0.5 mm veneer made of eucalyptus wood board, and the bottom plate is a 0.8 mm veneer made of camphor wood board.

[0059] Tissue culture pre-pressing: Use a press to pre-press the plain plate 1 at a constant temperature, and obtain the plain plate 2 after the pre-pressing is completed; the temperature of the press is set to 75°C, the pressure is set to 1.2MPa, and the time is 55min.

[0060] Assembly hot pressing: Use a hot press to heat and hot press the plain plate 2, and obtain the plain plate 3 after the hot pressing is completed; the temperature of the hot press is set to 140°C, the pressure is set to 1.4MPa, and the time is set to 35min.

[0061] Finished product after trimming: After the plain board 3 is naturally cooled and stacked for 7 days, it is trimmed and sprayed with polyurethane varnish and dried for 3-7 days to obtain the finished floor. The size of the floor after trimming is 900mm in length and 120mm in width; there is a nano-glue coating covered with plastic at the bottom of the board, and the plastic can be torn off and pasted on the floor when it is needed.

[0062] Finished mortise and tenon product: Place the pre-finished base plate into a mortise and tenon machine, set the left side of the floor as the tenon and the right side as the mortise. After the mortise and tenon are completed, plastic-seal the bottom surface of the floor with nano-glue to obtain Example 5; wherein the length of the left tenon is 15 mm, and the depth of the right mortise is 14.8 mm.

[0063] Example 6

[0064] Single board peeling: Use a peeling machine to peel the board, select the unqualified boards, and get the single board; the selected board standard is that it can withstand 2MPa pressure, 1.5MPa bending force without deformation, and has uniform color;

[0065] Veneer drying: After the veneer is dried with a dryer, the preliminarily dried boards are placed in a drying kiln for 3-7 days, and then the boards are stacked for 9 days to select boards with unqualified moisture content; the dryer is set at a temperature of 65°C and a wind speed of 15km / h; the drying kiln temperature is set at 40°C and a wind speed of 5km / h; the selection standard for qualified boards is a moisture content of less than 10%.

[0066] Glue coating and assembly: apply the glue prepared in Example 3 on the bottom of the surface plate, apply the glue prepared in Example 3 on the top of the bottom plate, apply the glue prepared in Example 3 on both sides of the upper plate, the middle plate and the lower plate, and then glue the surface plate, the upper plate, the middle plate, the lower plate and the bottom plate together in order from top to bottom to obtain a plain plate 1; wherein the surface plate is a 1.2 mm veneer made of ash board, the upper plate is a 2 mm veneer made of birch board, the middle plate is a 6 mm veneer made of birch board, the lower plate is a 0.5 mm veneer made of eucalyptus board, and the bottom plate is a 0.8 mm veneer made of camphor board.

[0067] Tissue culture pre-pressing: Use a press to pre-press the plain plate 1 at a constant temperature, and obtain the plain plate 2 after the pre-pressing is completed; the temperature of the press is set to 75°C, the pressure is set to 1.2MPa, and the time is 55min.

[0068] Assembly hot pressing: Use a hot press to heat and hot press the plain plate 2, and obtain the plain plate 3 after the hot pressing is completed; the temperature of the hot press is set to 140°C, the pressure is set to 1.4MPa, and the time is set to 35min.

[0069] Finished product after trimming: After the plain board 3 is naturally cooled and stacked for 7 days, it is trimmed and sprayed with polyurethane varnish and dried for 3-7 days to obtain the finished floor. The size of the floor after trimming is 900mm in length and 120mm in width; there is a nano-glue coating covered with plastic at the bottom of the board, and the plastic can be torn off and pasted on the floor when it is needed.

[0070] Finished mortise and tenon product: Place the pre-finished base plate into a mortise and tenon machine, set the left side of the floor as the tenon and the right side as the mortise. After the mortise and tenon are completed, plastic-seal the bottom surface of the floor with nano-glue to obtain Example 6; wherein the length of the left tenon is 15 mm, and the depth of the right mortise is 14.8 mm.

[0071] Comparative Example 1

[0072] 1. Single board peeling: Use a peeling machine to peel the board, select the unqualified boards, and get the single board; the selected board standard is that it can withstand 2MPa pressure, 1.5MPa bending force without deformation, and has uniform color;

[0073] 2. Veneer drying: After drying the veneer with a dryer, the preliminarily dried boards are placed in a drying kiln for 3-7 days, and then the boards are stacked for 9 days to select boards with unqualified moisture content; the dryer is set at a temperature of 65°C and a wind speed of 15km / h; the drying kiln temperature is set at 40°C and a wind speed of 5km / h; the standard for selecting qualified boards is a moisture content of less than 10%.

[0074] 3. Among the obtained veneers, the surface board used for the plywood is made of oak board, and the middle board and the bottom board are made of camphor board.

[0075] 4. Use a glue coating machine to glue the surface plate, middle plate and bottom plate and assemble them. The glue liquid is low-formaldehyde urea-formaldehyde resin glue, and the glue coating amount on one side is 220g / m 2 .

[0076] 5. Pre-press the assembled slab at a unit pressure of 0.9 MPa for 75 minutes.

[0077] 6. Use a hot press machine for hot pressing molding, the hot pressing pressure is 1.1MPa, the temperature is 130℃ for 20 minutes, and then sent to the balance warehouse for tempering.

[0078] 7. The above-mentioned slab is trimmed and then sanded to obtain a base material layer, and low-formaldehyde urea-formaldehyde resin glue is applied to the two outer surfaces of the above-mentioned base material. The bonded panels are then cold-pressed at a unit pressure of 0.9 MPa for 70 minutes; and then hot-pressed at a pressure of 1.1 MPa and a temperature of 130°C for 20 minutes.

[0079] 8. After the hot pressing, the plate was cooled to room temperature and then a layer of ammonium acetate was sprayed on the surface of the plate, which was allowed to dry naturally to obtain Comparative Example 1.

[0080] Formaldehyde emission experiment:

[0081] The 1m3 climate chamber method of GB / T 17657-2013 "Test methods for physical and chemical properties of wood-based panels and veneer wood-based panels" was used to test Examples 6-10 and Comparative Example 1. During the test, the temperature of the climate chamber was adjusted to 5°C, 15°C, 25°C, 35°C, and 45°C.

[0082] Table 2, experimental comparison of formaldehyde release of Examples 4-6 and Comparative Example 1

[0083] Example 4 Example 5 Example 6 Comparative Example 1 5℃ 0.000 0.000 0.000 0.053 15℃ 0.000 0.000 0.000 0.057 25℃ 0.000 0.000 0.000 0.072 35℃ 0.000 0.000 0.000 0.106 45℃ 0.000 0.000 0.000 0.131

[0084] It can be seen from the analysis of the above table that the present invention has good environmental performance at different temperatures, and the formaldehyde emission of Example 1 is significantly increased during the temperature rise process.

[0085] Water resistance test:

[0086] The bonding strength was determined by referring to the rapid test method for Class II plywood specified in 4.15 of GB / T 17657-1999 “Test methods for physical and chemical properties of wood-based panels and veneered wood-based panels”.

[0087] The instrument used in this performance test is a microcomputer-controlled electronic universal testing machine code-named CMJ6104 produced by Shenzhen Xinsansi Material Testing Co., Ltd.

[0088] Table 3, water resistance test of Examples 4-6 and Comparative Example 1

[0089] Example 4 Example 5 Example 6 Comparative Example 1 Bonding strength / MPa 1.98 2.04 2.06 1.85

[0090] It can be seen from the above table that the present invention has higher bonding strength and better water resistance than traditional flooring technology.

[0091] Dip stripping test:

[0092] According to the national standard GB / T18103, Examples 4-6 and Comparative Example 1 were treated as follows: the test pieces were immersed in hot water at 70°C±3°C for 2 hours, taken out and dried in a drying oven at 60°C±3°C for 3 hours, and the debonding length was measured.

[0093] Table 4, Immersion stripping test results of Examples 4-6 and Comparative Example 1

[0094] Example 4 Example 5 Example 6 Comparative Example 1 Glue opening length / mm 2.43 2.37 2.56 3.18

[0095] According to the analysis in Table 4, the composite floors prepared in Examples 4-6 all meet the standards of excellent composite floors.

[0096] The above shows and describes the basic principles and main features of the present invention and the advantages of the present invention. It should be understood by those skilled in the art that the present invention is not limited to the above embodiments. The above embodiments and descriptions are only for explaining the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, which fall within the scope of the present invention to be protected. The scope of protection of the present invention is defined by the attached claims and their equivalents.

Claims

1. A seamless multi-layer solid wood composite floor processing technology, characterized in that: The processing technology includes a series of steps of peeling the plate into single board and drying it, then applying glue to the single board, combining it into blanks, cold pressing and hot pressing it, and then trimming and mortising it; The method for preparing the glue solution used for gluing the veneers to form blanks comprises the following steps: A1: Raw material preparation: weigh 20-35 parts of natural rubber, 5-10 parts of pine resin, 5-10 parts of fragrant resin, 35-55 parts of purified water, 8-15 parts of 5% sodium hydroxide solution, 1-3 parts of nano-silicon dioxide, and 10-15 parts of plant fiber according to weight; A2: Add purified water and natural rubber to the reactor, heat to 55-65℃, stir until completely dissolved and gradually add pine resin and fragrant resin and stir again; A3: Add 5% sodium hydroxide solution dropwise to the product in step A2 at a drop rate of 1-2 drops / s, transfer to a magnetic stirrer, set the speed to 200-300 rpm, and react for 1-2 hours to obtain a base glue; A4: After the base glue cools down to room temperature, add the plant fiber, heat to 55-65℃, set the stirrer speed to 500-600rpm and stir for 30min, then add nano silicon dioxide and keep the temperature unchanged, stir for 1-2h and wait for it to cool down to room temperature to obtain the required glue solution.

2. A seamless multi-layer solid wood composite floor processing technology according to claim 1, characterized in that: The specific steps of the processing technology are: Veneer peeling: Use a peeling machine to peel the board, select unqualified boards, and get veneers; Veneer drying: After drying the veneer in a dryer, the preliminarily dried veneer is placed in a drying kiln for 3-7 days, and then the veneer is stacked for 2-9 days to select the veneer with unqualified moisture content; Gluing and assembling: glue is applied on the bottom of the surface plate, glue is applied on the top of the bottom plate, glue is applied on both the top plate, the middle plate and the bottom plate, and then the surface plate, the top plate, the middle plate, the bottom plate and the bottom plate are glued together in order from top to bottom to obtain a plain plate 1; Tissue culture pre-pressing: Use a press to pre-press the plain plate 1 at a constant temperature, and obtain the plain plate 2 after the pre-pressing is completed; Assembly hot pressing: using a hot press machine to heat and hot press the plain board 2, and after the hot pressing is completed, a plain board 3 is obtained; Cutting the edges of the raw board: After the raw board 3 is naturally cooled and stacked for 7 days, it is cut and sprayed with polyurethane varnish and dried for 3-7 days to obtain the pre-finished floor; Finished mortise and tenon product: put the pre-finished bottom plate into the mortise and tenon machine, set the left side of the floor as the tenon and the right side as the mortise. After the mortise and tenon are completed, seal the bottom surface of the floor with nano glue to obtain the finished floor.

3. The seamless multi-layer solid wood composite floor processing technology according to claim 1 is characterized in that: The standard of the board selected in the single board peeling step is that the board can withstand 2MPa pressure, 1.5MPa bending force without deformation, and has uniform color.

4. The seamless multi-layer solid wood composite floor processing technology according to claim 1 is characterized in that: In the veneer drying step, the dryer is set to a temperature of 65°C and a wind speed of 15km / h; the drying kiln temperature is set to 40°C and a wind speed of 5km / h; the selection standard for qualified boards is a moisture content of less than 10%.

5. The seamless multi-layer solid wood composite floor processing technology according to claim 1 is characterized in that: In the glue coating and assembly step, the surface plate is made of 1.2-2.5mm veneer made from elm wood board, the upper plate is made of 2-3mm veneer made from birch wood board, the middle plate is made of 6-8mm veneer made from birch wood board, the lower plate is made of 0.5-1.2mm veneer made from eucalyptus wood board, and the bottom plate is made of 0.8-2.2mm veneer made from camphor wood board.

6. The seamless multi-layer solid wood composite floor processing technology according to claim 1 is characterized in that: In the pre-pressing step of the green sheet assembly, the temperature of the press is set to 45-75° C., the pressure is set to 0.8-1.2 MPa, and the time is 45-55 min.

7. A seamless multi-layer solid wood composite floor processing process according to claim 1, characterized in that, in the assembly hot pressing step, the temperature of the hot press is set to 130-140°C, the pressure is set to 0.9-1.4MPa, and the time is set to 25-35min.

8. The seamless multi-layer solid wood composite floor processing technology according to claim 1 is characterized in that: The dimensions of the floor pre-finished product after trimming in the raw board trimming step are 900 mm in length and 120 mm in width.

9. The seamless multi-layer solid wood composite floor processing technology according to claim 1 is characterized in that: In the mortising step, the length of the left tenon is 15 mm, and the depth of the right mortise is 14.8 mm; during the installation process, the tenon is inserted into the mortise to achieve seamless splicing.

Citation Information

Patent Citations

  • High-efficiency, low-toxicity and environment-friendly adhesive

    CN104388010A

  • Environmental-friendly and formaldehyde-free composite floor processing technology

    CN110281323A

  • Adhesive based on materials containing latex and lignin and process for producing same

    CN112469793A

  • Self-adhesive multi-layer macromolecule waterproof wood board

    CN211143601U

  • Resin composition, adhesive, resin molded article, and method for manufacturing resin molded article

    JP7138980B1