Ultrahigh-strength aluminum alloy profile, preparation method and application

By using the Si:Mg = 1:1 formula in the 6-series aluminum alloy, the Cu and Mn content is increased, and the rare earth elements La and Ce are added to inhibit the generation of β-AlFeMnSi, the aluminum alloy can be extruded when increasing its strength. The problem of reduced performance and insufficient resistance to high-temperature aging has achieved ultra-high strength and good resistance to high-temperature aging.

CN119020643APending Publication Date: 2024-11-26KUNSHAN JINGWEI NEW MATERIALS RES INST CO LTD +1
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411136469.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-19
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

When the existing 6-series aluminum alloys increase strength, the extrusion performance of the material is reduced and the high-temperature aging resistance is insufficient, making it difficult to meet the high-strength and high-temperature resistance requirements of new energy vehicles for body structural profiles.

Method used

Using the Si:Mg = 1:1 formula, the Cu and Mn content is increased, and the rare earth elements La and Ce are combined to form an Al-Mg-Si-Cu-Mn-La-Ce alloy, which inhibits needle-like β- by the formation of the rare earth phase. The generation of AlFeMnSi improves the resistance to high temperature aging of the alloy, and improves the mechanical properties and extrusionability of the alloy through specific heat treatment and cooling processes.

Benefits of technology

The ultra-high strength and good extrusion performance of the alloy are achieved, and the resistance to high-temperature aging is significantly improved. The mechanical properties reach yield strength > 390MPa and tensile strength > 410MPa, and both have excellent extrusion performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119020643A_ABST
    Figure CN119020643A_ABST
Patent Text Reader

Abstract

The invention provides an ultrahigh-strength aluminum alloy profile as well as a preparation method and application thereof. Relates to the field of aluminum alloy manufacturing. The ultrahigh-strength aluminum alloy profile comprises the following components in percentage by weight: 0.8 to 1.05 percent of Si, 0 to 0.2 percent of Fe, 0.3 to 0.55 percent of Cu, 0.3 to 0.55 percent of Mn, 0.8 to 1.05 percent of Mg, 0.1 to 0.2 percent of Cr, 0 to 0.2 percent of Zn, 0 to 0.1 percent of Ti, 0.1 to 0.225 percent of La, 0.1 to 0.225 percent of Ce and the balance of Al and inevitable impurities, wherein the ratio of Si to Mg in percentage by weight is 1 to 1. The profile cast and extruded according to the formula has ultrahigh mechanical properties and excellent high-temperature aging resistance, the yield strength is greater than 390 MPa, the tensile strength is greater than 410 MPa, the extrudable property is equivalent to that of conventional 6082, and the extrudable property is good.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of aluminum alloy manufacturing, and in particular to an ultra-high-strength aluminum alloy profile, a preparation method and application thereof. Background Art

[0002] Aluminum alloy profiles have been widely used in the manufacturing process of new energy vehicles due to their excellent properties such as light weight, high strength and corrosion resistance. With the continuous iteration and upgrading of new energy vehicle models, the requirements for aluminum alloy structural profiles of the body are getting higher and higher, especially for the parts of the body that bear loads, which also put forward higher requirements for the strength and high temperature aging resistance of the structural profiles.

[0003] 6 series aluminum alloys have been widely used in the field of automobile manufacturing due to their good mechanical properties and processing characteristics. 6 series aluminum alloys are a type of aluminum alloy composed of elements such as aluminum, magnesium, and silicon, including conventional grades such as 6063, 6005, 6061, and 6082. In 6 series aluminum alloys, the alloy strength is mainly related to the degree of alloying, that is, the total content of added alloying elements such as Si, Mg, Cu, and Mn. The higher the degree of alloying, the more strengthening phases are precipitated, and the corresponding strength is also higher. Therefore, improving the degree of alloying is an important way to break through the mechanical property limits of conventional 6 series aluminum alloys and achieve high strength. However, with the increase in the content of alloying elements, the extrudable performance of the material decreases, and the quenching sensitivity increases, which will lead to difficulty in extruding the material and serious deformation of the product. Therefore, it is urgent to develop an ultra-high-strength aluminum alloy profile with good extrusion performance. Summary of the invention

[0004] In view of the technical problems existing in the prior art, the present invention aims to provide an ultra-high-strength aluminum alloy profile, a preparation method and application.

[0005] One of the purposes of the present invention is to provide an ultra-high strength aluminum alloy profile, wherein the ultra-high strength aluminum alloy profile comprises, by weight percentage: Si: 0.8~1.05%, Fe: 0~0.2%, Cu: 0.3~0.55%, Mn: 0.3~0.55%, Mg: 0.8~1.05%, Cr: 0.1~0.2%, Zn: 0~0.2%, Ti: 0~0.1%, La: 0.1~0.225%, Ce: 0.1~0.225%, the balance is Al and unavoidable impurities; Among them, Si:Mg =1:1 by weight percentage.

[0006] Preferably, the weight percentage of Si is 1.0-1.05%, and the weight percentage of Mg is 1.0-1.05%.

[0007] Preferably, the sum of the weight percentages of Mg and Si is 1.8-2.1%.

[0008] Preferably, the weight percentage of Cu is 0.5-0.55%, and the weight percentage of Mn is 0.5-0.55%.

[0009] Preferably, the weight percentage of La is 0.1-0.13%, and the weight percentage of Ce is 0.1-0.225%.

[0010] Preferably, the La and Ce are added in the form of an aluminum rare earth master alloy, and the aluminum rare earth master alloy components include, by weight percentage: La: 4.5-5.5%, Ce: 4.5-5.0%, Fe: 0.05-0.13%, and the balance is Al and unavoidable impurities.

[0011] A second object of the present invention is to provide a method for preparing an ultra-high-strength aluminum alloy profile, the preparation method comprising: S1 prepares the ingredients according to the weight percentage of the components, first melts the aluminum ingot, removes the slag and degases it, adds other metals to melt, and then adds a refining agent for online refining; S2 is cast at a temperature of 720°C to obtain a cast rod; the cast rod is first homogenized in a homogenizing furnace, then air-cooled, and finally water-mist-cooled; S3 aluminum alloy bar extrusion, water cooling is used during the extrusion process; After S4 extrusion, the sample was subjected to aging treatment and then air-cooled out of the furnace to obtain the finished aluminum alloy profile.

[0012] Preferably, the refining agent includes sodium chloride and potassium chloride, and the mass ratio of sodium chloride to potassium chloride is 4:6; the amount of the refining agent added is 2% of the mass of the aluminum liquid.

[0013] Preferably, the bar extrusion bar temperature is 500-530°C, the extrusion rod speed is 2.2-2.8 mm / s, and the discharge temperature is 510-550°C.

[0014] Preferably, the homogenization treatment temperature is 560-580°C, the time is 6-10 hours, and the water mist cooling time is 4-6 hours; the aging treatment temperature is 205-215°C, and the insulation time is 3-6 hours.

[0015] A third object of the present invention is to provide an ultra-high strength aluminum alloy profile for use in automobiles.

[0016] Beneficial effects of the present invention: The invention provides an ultra-high-strength aluminum alloy profile, the components of which, by weight percentage, include: Si: 0.8-1.05%, Fe: 0-0.2%, Cu: 0.3-0.55%, Mn: 0.3-0.55%, Mg: 0.8-1.05%, Cr: 0.1-0.2%, Zn: 0-0.2%, Ti: 0-0.1%, La: 0.1-0.225%, Ce: 0.1-0.225%, and the balance is Al and unavoidable impurities; wherein, by weight percentage, Si:Mg=1:1.

[0017] The strengthening phase of 6 series aluminum alloy is Mg2Si. When the Mg / Si mass ratio in the alloy decreases from Mg / Si>1 to Mg / Si<1, the precipitation fraction of the strengthening phase Mg2Si in the matrix increases first and then decreases with the decrease of temperature during the alloy solidification process. When Mg / Si is close to 1, the precipitation fraction of the strengthening phase Mg2Si in the matrix is ​​the largest and the strengthening effect is the best.

[0018] In the aluminum alloy formula, the increase in Cu percentage greatly improves the strength and hardness of the alloy through solid solution strengthening and precipitation hardening, and improves its heat treatment effect. The increase in Mn percentage increases the fine dispersed phase, enhances the strength and wear resistance of the alloy, and improves corrosion resistance and processing performance. Manganese can also improve the recrystallization structure of the alloy and improve high temperature strength.

[0019] However, in 6 series aluminum alloys, as the alloying elements Si, Mg, Cu, and Mn increase, the extrudability of the profile decreases, especially the increase in Cu and Mn content will significantly reduce the extrudability of the alloy. Therefore, in the case of Mg / Si=1, and Cu and Mn contents of 0.3~0.55%, the alloy has ultra-high strength and good extrudability.

[0020] In addition, the patent of the present invention also adds rare earths La and Ce on the basis of the new Al-Mg-Si-Cu-Mn alloy formula to form a new Al-Mg-Si-Cu-Mn-La-Ce alloy. The rare earth phase AlCuLa(Ce) (Al6Cu6La and Al8Cu4Ce) formed by adding rare earth elements La and Ce can inhibit the formation of needle-shaped β-AlFeMnSi, thereby improving the alloy's resistance to high-temperature aging.

[0021] The profiles extruded by melt casting of this alloy formula have ultra-high mechanical strength (yield strength>390MPa, tensile strength>410MPa), and the extrudable performance is equivalent to that of conventional 6082. It has good extrusion performance, ultra-high mechanical strength and excellent high temperature aging resistance. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 This is the SEM morphology of Example 6; Figure 2 This is the SEM morphology of Example 8; Figure 3 This is the SEM morphology of Comparative Example 3. DETAILED DESCRIPTION

[0023] According to the first aspect of the present invention, an ultra-high strength aluminum alloy profile is provided, wherein the ultra-high strength aluminum alloy profile components include, by weight percentage: Si: 0.8~1.05%, Fe: 0~0.2%, Cu: 0.3~0.55%, Mn: 0.3~0.55%, Mg: 0.8~1.05%, Cr: 0.1~0.2%, Zn: 0~0.2%, Ti: 0~0.1%, La: 0.2~0.225%, Ce: 0.2~0.225%, the balance is Al and unavoidable impurities; Among them, Si:Mg =1:1 by weight percentage.

[0024] In the present invention, the strengthening phase of the 6 series aluminum alloy is Mg2Si. When the Mg / Si mass ratio in the alloy is reduced from Mg / Si>1 to Mg / Si<1, the precipitation fraction of the strengthening phase Mg2Si in the matrix increases first and then decreases as the temperature decreases during the solidification of the alloy. When Mg / Si is close to 1, the precipitation fraction of the strengthening phase Mg2Si in the matrix is ​​the largest and the strengthening effect is the best.

[0025] In the aluminum alloy formula, increasing the content of Cu and Mn can significantly improve the performance of the alloy. The addition of Cu can greatly improve the strength and hardness of the alloy through solid solution strengthening and precipitation hardening, and improve its heat treatment effect. Mn enhances the strength and wear resistance of the alloy by forming a fine dispersed phase, while improving corrosion resistance and processing performance. Manganese can also improve the recrystallization structure of the alloy and improve high temperature strength.

[0026] However, in 6 series aluminum alloys, as the alloying elements Si, Mg, Cu, and Mn increase, the extrudability of the profile decreases, especially the increase in Cu and Mn content will significantly reduce the extrudability of the alloy. Therefore, in the case of Mg / Si=1, and Cu and Mn contents of 0.3~0.55%, the alloy has ultra-high strength and good extrudability.

[0027] The rare earth Ce and La are ranked first and second in the earth's crust, respectively, and La and Ce generally coexist in nature. LaCe mixed rare earth has lower cost. In 6-series aluminum alloys, LaCe microalloying can change the microstructure of Al-Si-Cu-Mn-Mg-Fe alloys, mainly manifested in the newly formed rare earth phase AlCuLa(Ce) (Al6Cu6La and Al8Cu4Ce) can significantly refine the main intermetallic compound AlFeMnSi phase in Al-Si-Cu-Mn-Mg-Fe alloys.

[0028] The AlFeMnSi phase is produced during the casting process of aluminum alloy. Because it is incoherent with the alloy matrix and has poor deformation ability, it will have a negative impact on the mechanical properties and high temperature aging resistance of the alloy. In particular, the lamellar and long needle-shaped β-AlFeMnSi phase in the AlFeMnSi phase has a more serious negative impact on the alloy than the irregular and dot-shaped α-AlFeMnSi phase. Adding LaCe mixed rare earth to 6xxx aluminum alloy, the rare earth phase AlCuLa(Ce) (Al6Cu6La and Al8Cu4Ce) formed can not only inhibit the formation of needle-shaped β-AlFeMnSi, but also refine the grains. Moreover, La and Ce are insoluble in iron-based intermetallic compounds, and can be adsorbed on the surface of α-AlFeMnSi phase to prevent the diffusion of Si and inhibit the formation of β-AlFeMnSi.

[0029] The rare earth phase AlCuLa(Ce) exists in three forms in the alloy: independently in the matrix; partially around the AlFeMnSi phase; completely covering the AlFeMnSi phase. Since the melting point of the AlFeMnSi phase is higher than that of the AlCuLa(Ce) phase, the AlFeMnSi phase can serve as the nucleation point of the AlCuLa(Ce) phase during the nucleation process and promote the heterogeneous nucleation of the rare earth phase. With the continuous diffusion of elements such as Cu, Ce and La in the melt, the rare earth phase gradually grows along the surface of the AlFeMnSi phase, and finally forms a "core / shell" structure with the AlFeMnSi phase as the core and the rare earth phase as the shell. During the solidification process, the formation of this structure can effectively prevent elements such as Mn and Fe in the melt from diffusing around the AlFeMnSi particles, thereby effectively reducing the particle size of the AlFeMnSi intermetallic compound and inhibiting the formation of needle-shaped β-AlFeMnSi, thereby improving the high temperature aging resistance of the alloy.

[0030] In addition, the rare earth elements La and Ce can also play a role in modifying and purifying aluminum melt in aluminum alloys. Adding trace amounts of La and Ce rare earth elements to aluminum alloys can reduce the hydrogen content and porosity in the aluminum liquid. Rare earth elements La and Ce can absorb a large amount of hydrogen to generate stable refractory compounds such as LaH2 and CeH2, reduce the formation of bubbles, and precipitate in the form of residues during the smelting process, greatly reducing the hydrogen content of the aluminum alloy and achieving the role of purifying the matrix.

[0031] In a preferred embodiment of the present invention, the sum of the weight percentages of Mg and Si is 1.8-2.1%.

[0032] In the present invention, the sum of the weight percentages of Mg and Si is, for example, 1.8%, 1.9%, 2.0% or 2.1%.

[0033] In a preferred embodiment of the present invention, the weight percentage of Si is 1.0-1.05%, and the weight percentage of Mg is 1.0-1.05%.

[0034] In the present invention, the weight percentage of Si is, for example, 1.01%, 1.02%, 1.03%, 1.04% or 1.05%.

[0035] In a preferred embodiment of the present invention, the weight percentage of Cu is 0.5-0.55%, and the weight percentage of Mn is 0.5-0.55%.

[0036] In the present invention, the weight percentage of Cu is, for example, 0.50%, 0.51%, 0.52%, 0.53%, 0.54% or 0.55%, and the weight percentage of Mn is, for example, 0.50%, 0.51%, 0.52%, 0.53%, 0.54% or 0.55%.

[0037] In a preferred embodiment of the present invention, the weight percentage of La is 0.1-0.13%, and the weight percentage of Ce is 0.1-0.225%.

[0038] In the present invention, the weight percentage of La in the ultra-high strength aluminum alloy profile is, for example, 0.10%, 0.11%, 0.12%, 0.125%, 0.13%, 0.14%, 0.15%, 0.16%, 0.17%, 0.18%, 0.19%, 0.20%, 0.21%, 0.22% or 0.225%.

[0039] In a preferred embodiment of the present invention, the La and Ce are added in the form of an aluminum rare earth master alloy, and the aluminum rare earth master alloy components include, by weight percentage: La: 4.5-5.5%, Ce: 4.5-5.0%, Fe: 0.05-0.13%, and the balance is Al and unavoidable impurities.

[0040] In the present invention, the weight percentage of La in the aluminum rare earth master alloy component is, for example, 4.5%, 4.6%, 4.7%, 4.8%, 4.9%, 5.0%, 5.1%, 5.2%, 5.3%, 5.4% or 5.5%; the weight percentage of Ce is, for example, 4.5%, 4.6%, 4.7%, 4.8%, 4.9% or 5.0%; the weight percentage of Fe is, for example, 0.05%, 0.06%, 0.07%, 0.08%, 0.09%, 0.10%, 0.11%, 0.12% or 0.13%.

[0041] According to a second aspect of the present invention, a method for preparing an ultra-high-strength aluminum alloy profile is provided, the preparation method comprising: S1 batches the ingredients according to the weight percentage of the components, first melts the aluminum ingot, removes the slag and gasses it, adds other metals to melt, and then adds a refining agent for online refining; S2 is cast at a temperature of 720°C to obtain a cast rod; the cast rod is first homogenized in a homogenizing furnace, then air-cooled, and finally water-mist-cooled; S3 aluminum alloy bar extrusion, water cooling is used during the extrusion process; After S4 extrusion, the sample was subjected to aging treatment and then air-cooled out of the furnace to obtain the finished aluminum alloy profile.

[0042] In a preferred embodiment of the present invention, preferably, the refining agent includes sodium chloride and potassium chloride, and the mass ratio of sodium chloride to potassium chloride is 4:6; and the amount of the refining agent added is 2% of the mass of the aluminum liquid.

[0043] In a preferred embodiment of the present invention, the bar extrusion bar temperature is 500-530°C, the extrusion rod speed is 2.2-2.8 mm / s, and the discharge temperature is 510-550°C.

[0044] In the present invention, the rod extrusion rod temperature is, for example, 500°C, 505°C, 510°C, 515°C, 520°C, 525°C or 530°C; the pressing rod speed is, for example, 2.2mm / s, 2.3mm / s, 2.4mm / s, 2.5mm / s, 2.6mm / s, 2.7mm / s or 2.8mm / s; the discharge temperature is, for example, 510°C, 520°C, 530°C, 540°C or 550°C.

[0045] In a preferred embodiment of the present invention, the homogenization treatment temperature is 560-580°C, the time is 6-10 hours, and the water mist cooling time is 4-6 hours; the aging treatment temperature is 205-215°C, and the insulation time is 3-6 hours.

[0046] In the present invention, the homogenization treatment temperature is, for example, 560°C, 565°C, 570°C, 575°C or 580°C; the homogenization treatment time is, for example, 6h, 7h, 8h, 9h or 10h; the water mist cooling time is, for example, 4h, 5h or 6h; the aging treatment temperature is, for example, 205°C, 206°C, 207°C, 208°C, 209°C, 210°C, 211°C, 212°C, 213°C, 214°C or 215°C; and the insulation time is 3h, 4h, 5h or 6h.

[0047] According to the third aspect of the present invention, there is provided an application of an ultra-high strength aluminum alloy profile in automobiles.

[0048] Example The present invention provides 7 embodiments and 5 comparative examples, and Table 1 shows the weight percentages of embodiments 1 to 7 and comparative examples 1 to 5. Among them, in embodiments 1 to 6 and comparative examples 1 to 3, by weight percentage, Fe: 0.2%, Cr: 0.2%, Zn: 0.2%, Ti: 0.1%.

[0049] Comparative Example 4 is a GB / T 3190 6082 aluminum alloy, with Fe: 0.5% and Cr: 0.25% by weight, and Comparative Example 5 is a GB / T 3190 6061 aluminum alloy, with Fe: 0.7%, Cr: 0.35%, Zn: 0.25%, and Ti: 0.15% by weight. The weight percentages of Examples 1 to 8 and Comparative Examples 1 to 5 are shown in Table 1.

[0050] The specific preparation method is: S1 prepares the ingredients according to the weight percentage of the components, first melts the aluminum ingot, removes the slag and degases it, adds other metals to melt, and then adds 2% of refining agent for online refining; S2 is cast at a temperature of 720°C for aluminum liquid to obtain a cast rod; the cast rod is first homogenized at 560-580°C in a homogenizing furnace for 6-10 hours, then air-cooled, and finally water-mist-cooled for 4-6 hours; S3 aluminum alloy bar material temperature is 500~530℃, extrusion rod speed is 2.2~2.8mm / s, discharge temperature is 510~550℃, and water cooling is used during extrusion; After S4 extrusion, the sample was subjected to aging treatment at a temperature of 205-215°C for 3-6 hours, and then air-cooled out of the furnace to obtain a finished aluminum alloy profile.

[0051] Table 1 Weight percentage of Examples 1 to 8 and Comparative Examples 1 to 5

[0052] The alloy samples of Examples 1 to 8 and Comparative Examples 1 to 5 were sampled, and the mechanical properties and bending properties of the samples were tested.

[0053] The samples of Example 6, Example 7, Example 8 and Comparative Example 3 were used for high temperature aging test. The temperature was kept constant at 120°C for 100h, 200h, 400h, 600h, 800h and 1000h, and then the mechanical properties and bending properties were tested.

[0054] The samples of Example 6, Example 8 and Comparative Example 3 were subjected to SEM scanning electron microscopy to obtain SEM morphology images, as shown in FIG. Figure 1 , Figure 2 and Figure 3 shown.

[0055] like Figure 1 As shown, the matrix structure of the alloy sample of Example 6 is mainly composed of irregular and dot-shaped α-AlFeMnSi phases.

[0056] like Figure 2 As shown, the matrix structure of the alloy sample of Example 8 is still mainly composed of α-AlFeMnSi phase, but the α-AlFeMnSi phase is coarsened.

[0057] like Figure 3 As shown, the matrix structure of the alloy sample of Comparative Example 3 is mainly composed of lamellar and long needle-shaped β-AlFeMnSi phases.

[0058] It can be seen that the addition of LaCe mixed rare earth is conducive to the formation of irregular and dot-shaped α-AlFeMnSi phases, but the rare earth content should not be too high. If the rare earth content is added too much, the α-AlFeMnSi phase will coarsen, resulting in a decrease in the high temperature aging resistance of the alloy.

[0059] Performance Testing The mechanical properties test is carried out in accordance with GB / T228.1-2021, using A50 specimens.

[0060] The bending angle test standard is carried out in accordance with VDA238-100.

[0061] Table 2 Test results of Examples 1 to 8 and Comparative Examples 1 to 5

[0062] Table 3 Performance test of high temperature aging test of Example 6

[0063] Table 4 Performance test of high temperature aging test of Example 7

[0064] Table 5 Performance test of high temperature aging test of Example 8

[0065] Table 6 High temperature aging test performance test of comparative example 3

Claims

1. An ultra-high strength aluminum alloy profile, It is characterized in that The ultra-high-strength aluminum alloy profile components include, by weight percentage: Si: 0.8-1.05%, Fe: 0-0.2%, Cu: 0.3-0.55%, Mn: 0.3-0.55%, Mg: 0.8-1.05%, Cr: 0.1-0.2%, Zn: 0-0.2%, Ti: 0-0.1%, La: 0.1-0.225%, Ce: 0.1-0.225%, the balance is Al and unavoidable impurities; Among them, Si:Mg=1:1 in weight percentage.

2. The ultra-high strength aluminum alloy profile according to claim 1, It is characterized in that The sum of the weight percentages of Mg and Si is 1.8-2.1%.

3. The ultra-high strength aluminum alloy profile according to claim 1, It is characterized in that The weight percentage of Si is 1.0-1.05%, and the weight percentage of Mg is 1.0-1.05%.

4. The ultra-high strength aluminum alloy profile according to claim 1, It is characterized in that The weight percentage of Cu is 0.5-0.55%, and the weight percentage of Mn is 0.5-0.55%.

5. The ultra-high strength aluminum alloy profile according to claim 1, It is characterized in that The weight percentage of La is 0.1-0.13%, and the weight percentage of Ce is 0.1-0.225%.

6. The ultra-high strength aluminum alloy profile according to claim 1, It is characterized in that The La and Ce are added in the form of an aluminum rare earth master alloy, and the aluminum rare earth master alloy components include, by weight percentage: La: 4.5-5.5%, Ce: 4.5-5.0%, Fe: 0.05-0.13%, and the balance is Al and inevitable impurities.

7. The method for preparing the ultra-high strength aluminum alloy profile according to any one of claims 1 to 6, It is characterized in that The preparation method comprises: S1 prepares the ingredients according to the weight percentage of the components, first melts the aluminum ingot, removes the slag and degases it, adds other metals to melt, and then adds a refining agent for online refining; S2 is cast at a temperature of 720°C to obtain a cast rod; the cast rod is first homogenized in a homogenizing furnace, then air-cooled, and finally water-mist-cooled; S3 aluminum alloy bar extrusion, water cooling is used during the extrusion process; After S4 extrusion, the sample was subjected to aging treatment and then air-cooled out of the furnace to obtain the finished aluminum alloy profile.

8. The method for preparing the ultra-high strength aluminum alloy profile according to claim 7, It is characterized in that The refining agent includes sodium chloride and potassium chloride, and the mass ratio of sodium chloride to potassium chloride is 4:6; the amount of the refining agent added is 2% of the mass of the aluminum liquid.

9. The method for preparing the ultra-high strength aluminum alloy profile according to claim 7, It is characterized in that The rod extrusion temperature is 500-530°C, the extrusion rod speed is 2.2-2.8 mm / s, the discharge temperature is 510-550°C, the homogenization treatment temperature is 560-580°C, the time is 6-10 hours, the water mist cooling time is 4-6 hours; the aging treatment temperature is 205-215°C, and the insulation time is 3-6 hours.

10. Use of the ultra-high strength aluminum alloy profile according to any one of claims 1 to 6 in automobiles.

Citation Information

Cited By

  • Integrated machining process for high-strength aluminum alloy mobile phone middle frame

    CN119772523A

  • Aluminum alloy material suitable for photovoltaics and preparation method thereof

    CN119899963A