Electrode plate and preparation method thereof
Through dry powder mixing, ultrasonic vibration and rolling treatment, the particle distribution of all-solid battery pole sheets is optimized, the problem of improving porosity and compaction density is solved, the energy density and cycle life of the battery are improved, and the battery performance and safety are ensured. sex.
Patent Information
- Application Number
- CN202411386497.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-30
- Publication Date
- 2024-11-26
AI Technical Summary
The existing all-solid-state battery pole plates are difficult to significantly reduce porosity, resulting in limited energy density improvement. The traditional compaction method is prone to cause wrinkles of the pole plates or cracks of active substances, affecting battery performance.
By mixing the active substance, solid electrolyte and conductive agent dry powder, and then spraying with ultrasonic vibration treatment and rolling treatment, the particle distribution is optimized, ensuring that the active substance and the solid electrolyte are in full contact, reducing porosity and improving compaction density.
It has achieved efficient use of the ion conduction capability of solid electrolytes, improved the capacity and cycle life of all-solid-state batteries, avoided the problems of solvent residues and cracked active substances, and improved production efficiency and safety.
Smart Images

Figure CN119029147A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of all-solid-state batteries, and in particular to an electrode plate and a method for preparing the same. Background Art
[0002] As the next generation of batteries, solid-state batteries use non-flammable solid electrolytes instead of flammable organic liquid electrolytes, which greatly improves the safety of the batteries. In addition, solid-state batteries can better adapt to high-energy positive and negative electrode materials and reduce system weight, achieving a simultaneous increase in energy density. It has become a consensus in the industry and the scientific community that solid-state batteries are the next generation technology closest to industrialization.
[0003] The pole pieces of traditional liquid lithium-ion batteries need to maintain a certain porosity to ensure that the electrolyte can infiltrate into the pole pieces, thereby conducting ion pathways. Solid-state batteries are different in that they use solid electrolytes for ion transmission. Therefore, solid-state batteries require as low a porosity as possible to ensure close contact between the active material and the solid electrolyte and reduce interface resistance. In addition to low porosity, the compaction density of the pole piece must also be increased to improve the energy density of the solid-state battery. In the prior art, the method of reducing the porosity of all-solid-state battery pole pieces is usually to use double-roll pressing equipment, isostatic pressing equipment or other external pressure equipment, but the pressure value of the roller pressing equipment is limited and cannot significantly reduce the porosity of the pole piece; and excessive pressure can cause problems such as pole piece wrinkles or active material particle rupture.
[0004] The density of the pole piece can be improved by compounding large and small particles. For example, the Chinese patent application with publication number CN106532033A discloses a "method for preparing a mixed lithium manganese oxide material", which prepares lithium manganese oxide materials of different sizes and then mixes them to obtain a high-compaction, high-rate lithium manganese oxide material. Although this method improves the compaction of lithium manganese oxide, the improvement effect is limited and there is no description of key cycle performance indicators.
[0005] For example, Chinese patent application publication number CN111933890A discloses "low-porosity all-solid-state battery electrode sheet and its preparation method and application". The method is to contact the solid-state battery electrode sheet with an organic solvent so that the organic solvent fills the voids in the solid electrode sheet. Although the inventive method can reduce the porosity, the introduced organic solvent will remain in the sheet or react with the solid electrolyte, posing a risk of battery failure. Summary of the invention
[0006] The present application provides an electrode plate and a preparation method thereof, which can produce an electrode plate with high compaction density and low porosity, efficiently exert the ion conduction ability of the solid electrolyte, and effectively improve the capacity and cycle life of the all-solid-state battery.
[0007] In one aspect, the present application provides a method for preparing an electrode sheet, the method comprising:
[0008] The active material, the solid electrolyte and the conductive agent are mixed and uniformly mixed to obtain a raw material mixture;
[0009] Evenly spraying the raw material mixture on the current collector to obtain an initial electrode sheet;
[0010] The initial electrode plate is vibrated by a conductive medium to obtain an intermediate electrode plate; wherein the vibration time corresponding to the vibration treatment is 0.1-5s and the vibration frequency is 10-40kHz;
[0011] The intermediate electrode plate is subjected to a rolling process to obtain the electrode plate; wherein the pressure of the rolling process is 0.10-0.50 MPa.
[0012] Furthermore, the vibrating treatment of the initial electrode plate with a conductive medium to obtain an intermediate electrode plate comprises:
[0013] The conductive medium is placed between the initial electrode plate and the vibration source; the conductive medium is a stainless steel plate; the vibration source is an ultrasonic generator;
[0014] Determining the vibration time and the vibration frequency corresponding to the vibration treatment according to the particle size of the solid electrolyte; the vibration time and the vibration frequency are both positively correlated with the particle size of the solid electrolyte;
[0015] The initial electrode plate is vibrated using the vibration time and the vibration frequency to obtain the intermediate electrode plate.
[0016] Furthermore, the active material, the solid electrolyte and the conductive agent are mixed and uniformly mixed to obtain a raw material mixture, comprising:
[0017] The active material and the solid electrolyte are mixed in a mass ratio of (60-90): (10-40) to obtain an initial raw material mixture after mixing evenly;
[0018] The initial raw material mixture and the conductive agent are mixed in a mass ratio of (70-130):(0-5), and the raw material mixture is obtained after mixing evenly.
[0019] Furthermore, the rolling process is room temperature rolling or high temperature rolling, wherein the temperature range of the high temperature rolling is 50-200°C.
[0020] Furthermore, a first active material layer, a second active material layer and a third active material layer are sequentially stacked on the current collector of the electrode plate;
[0021] The active material includes an active material of a first particle size and an active material of a second particle size, the first active material layer includes the active material of the first particle size and the solid electrolyte; the second active material layer includes the active material of the first particle size, the active material of the second particle size and the solid electrolyte; the third active material layer includes the active material of the second particle size and the solid electrolyte; the first particle size is smaller than the second particle size, and the second particle size is smaller than 20 μm.
[0022] Furthermore, the porosity of the electrode plate is 2-30%.
[0023] Furthermore, the particle size of the solid electrolyte is smaller than the particle size of the active material; the particle size of the solid electrolyte ranges from 0.5 to 15 μm.
[0024] Furthermore, the active material is a positive electrode material or a negative electrode material; wherein the positive electrode material is one or more of lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, lithium nickel cobalt manganese aluminum oxide, lithium cobalt oxide, lithium manganese oxide, lithium iron phosphate or lithium-rich manganese-based material; the negative electrode material is one or more of graphite, silicon-carbon composite material, and lithium titanate.
[0025] Furthermore, the solid electrolyte is one or more of a sulfide solid electrolyte, an oxide solid electrolyte, and a polymer solid electrolyte;
[0026] The conductive agent is one or more of acetylene black, vapor phase carbon fiber, carbon nanotube, nano carbon fiber and graphene.
[0027] On the other hand, an electrode plate is provided, and the electrode plate is prepared by the above preparation method.
[0028] On the other hand, an all-solid-state battery cell is provided, wherein the all-solid-state battery cell comprises an electrode plate prepared by the above-mentioned preparation method.
[0029] On the other hand, an all-solid-state battery is provided, which includes an electrode plate prepared by the above preparation method.
[0030] The electrode sheet and the preparation method thereof provided in this application have the following technical effects:
[0031] The present application mixes active material, solid electrolyte and conductive agent, and obtains raw material mixture after uniform mixing; sprays the raw material mixture evenly on the current collector to obtain initial electrode plate; vibrates the initial electrode plate with conductive medium to obtain intermediate electrode plate; wherein the vibration time corresponding to the vibration treatment is 0.1-5s, and the vibration frequency is 10-40kHz; rolls the intermediate electrode plate to obtain electrode plate; wherein the pressure of the roll pressing treatment is 0.10-0.50Mpa. The present application achieves a simple mixing process by mixing the active material, solid electrolyte and conductive agent in dry powder, thereby reducing the involvement of solvents in the processing of the electrode plate, avoiding the decrease in ionic conductivity caused by solvent volatilization, shortening the drying process, and improving production efficiency and safety; the particle distribution in the raw material mixture is optimized by vibration, so that the particles inside the electrode plate are more densely packed and have a low porosity, ensuring full contact between the active material and the solid electrolyte, and effectively exerting the ion conductivity of the solid electrolyte, thereby improving the rate performance and cycle life of the all-solid-state battery; by distributing the mixture of large particles of active material and solid electrolyte in the upper layer, i.e., away from the current collector, and the mixture of small particles of active material and solid electrolyte in the lower layer, i.e., close to the current collector, with the active material mixed with large and small particles in the middle, it is ensured that the large particles in the upper layer are not prone to particle rupture when subjected to high pressure, thereby avoiding the occurrence of active failure, and ensuring that each layer of active material on the electrode plate is dense enough, thereby effectively improving the compaction density of the electrode plate.
[0032] It should be understood that the foregoing general description and the following detailed description are exemplary and explanatory only and are not restrictive of the present application. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] In order to more clearly illustrate the technical solutions and advantages of the embodiments of this specification or the prior art, the drawings required for use in the embodiments or the prior art descriptions are briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0034] Figure 1 It is a schematic flow chart of a method for preparing an electrode sheet provided in an embodiment of this specification;
[0035] Figure 2 It is a schematic flow chart of a method for preparing a raw material mixture provided in an embodiment of this specification;
[0036] Figure 3 It is a schematic diagram of a vibration processing flow provided by an embodiment of this specification;
[0037] Figure 4 It is a schematic diagram of the structure of an electrode plate provided in an embodiment of this specification;
[0038] Figure 5 It is a schematic diagram of a device for preparing an electrode plate provided in an embodiment of this specification.
[0039] Among them, the corresponding marks in the drawings are as follows: 1-unwinding device, 2-guiding device, 3-spraying device, 4-ultrasonic vibration device, 5-rolling device, 6-thickness measuring device, 7-guiding device, 8-winding device. DETAILED DESCRIPTION
[0040] The following will be combined with the drawings in the embodiments of this specification to clearly and completely describe the technical solutions in the embodiments of this specification. Obviously, the described embodiments are only part of the embodiments of this application, not all of them. Based on the embodiments in this application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.
[0041] The following describes a method for preparing an electrode sheet of the present application, specifically: Figure 1 As shown, the method may include:
[0042] S1: The active material, the solid electrolyte and the conductive agent are mixed and uniformly obtained to obtain a raw material mixture.
[0043] Furthermore, the active material is a positive electrode material or a negative electrode material; wherein the positive electrode material is one or more of lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, lithium nickel cobalt manganese aluminum oxide, lithium cobalt oxide, lithium manganese oxide, lithium iron phosphate or lithium-rich manganese-based material; the negative electrode material is one or more of graphite, silicon-carbon composite material, and lithium titanate.
[0044] In the embodiment of the present application, the active material may be a positive electrode material or a negative electrode material. When it is necessary to prepare a positive electrode plate, a positive electrode material is used as the active material; when it is necessary to prepare a negative electrode plate, a negative electrode material is used as the active material. Among them, the positive electrode material may include lithium nickel cobalt manganese oxide NCM, lithium nickel cobalt aluminum oxide NCA, lithium nickel cobalt manganese aluminum oxide NCMA, lithium cobalt oxide LCO, lithium manganese oxide LMO, lithium iron phosphate LFP or lithium-rich manganese-based material; the negative electrode material may include graphite, silicon-carbon composite material, lithium titanate, etc., and one or more of them may be selected. In the embodiment of the present application, the positive electrode material is preferably lithium nickel cobalt manganese oxide NCM, and the negative electrode material is preferably graphite.
[0045] The embodiments of the present application select positive electrode materials or negative electrode materials as active materials in the electrode plates to provide channels for ion transmission and give full play to the ion conduction capacity of the solid electrolyte.
[0046] Furthermore, the solid electrolyte is one or more of a sulfide solid electrolyte, an oxide solid electrolyte, and a polymer solid electrolyte;
[0047] The conductive agent is one or more of acetylene black, vapor phase carbon fiber, carbon nanotube, nano carbon fiber and graphene.
[0048] In the embodiment of the present application, the solid electrolyte may include a sulfide solid electrolyte, an oxide solid electrolyte and a polymer solid electrolyte, and one or more thereof may be selected. In the embodiment of the present application, the solid electrolyte is preferably a sulfide solid electrolyte, specifically one of LGPS or LPSC.
[0049] In the embodiment of the present application, the conductive agent may include acetylene black, vapor grown carbon fiber, carbon nanotube, nano carbon fiber, graphene, etc., and any one or more thereof may be selected. In the embodiment of the present application, the conductive agent is preferably vapor grown carbon fiber (VGCF).
[0050] The embodiment of the present application uses a solid electrolyte to prepare an electrode plate with higher safety and stability; the conductive agent can effectively improve the conductivity of the electrode plate and fill the gaps in the electrode plate to obtain an electrode plate with lower porosity.
[0051] Furthermore, if Figure 2 As shown, the active material, the solid electrolyte and the conductive agent are mixed and uniformly mixed to obtain a raw material mixture, which may include:
[0052] S11: mixing the active material and the solid electrolyte in a mass ratio of (60-90):(10-40) to obtain an initial raw material mixture after mixing evenly;
[0053] S12: Mix the initial raw material mixture and the conductive agent in a mass ratio of (70-130): (0-5), and mix them evenly to obtain the raw material mixture.
[0054] In the embodiment of the present application, the active material, solid electrolyte and conductive agent are dry-powder mixed according to the mass ratio of (60-90): (10-40): (0-5). The three raw materials of active material, solid electrolyte and conductive agent can be directly weighed according to the mass ratio to mix the raw material mixture, or two of the raw materials can be mixed first, and then the other raw material can be mixed to obtain the raw material mixture. The mixing method can be high-speed shearing, ball milling or high-energy roller milling, etc., and the raw material mixture can be obtained after uniform mixing. Among them, if high-speed shearing is used for mixing, the corresponding rate range can be 2000-18000rpm; if ball milling is used for mixing, the corresponding ball milling speed range can be 20-200rpm; if high-energy roller milling is used for mixing, the corresponding speed range can be 200-500rpm. Compared with the wet slurry process, this dry powder mixing method adopts a simple process, does not require the use of any solvent in the preparation process, reduces the participation of solvents in the electrode processing process, avoids the solvent volatilization leading to a decrease in ionic conductivity, and shortens the drying process, thereby improving production efficiency and safety.
[0055] The embodiment of the present application directly mixes the three raw materials of active material, solid electrolyte and conductive agent into dry powder to obtain a uniformly mixed raw material mixture, which reduces the participation of solvent in the electrode plate processing process, avoids the decrease of ionic conductivity caused by solvent volatilization, and can effectively improve production efficiency and safety.
[0056] S2: spraying the raw material mixture uniformly on the current collector to obtain an initial electrode sheet.
[0057] In the embodiment of the present application, the raw material mixture is evenly spread on the surface of the current collector by spraying, and the spraying rate range can be 200-300m 2 / h. Compared with the existing coating technology, the spraying method can achieve close bonding between particles, greatly improve the interface contact, reduce the interface impedance, and thus optimize the cycle life of the sulfide solid-state battery.
[0058] The embodiment of the present application can evenly spread the raw material mixture on the surface of the current collector by spraying, thereby achieving close bonding between the raw material particles, improving the interface contact, and reducing the interface impedance.
[0059] S3: using a conductive medium to vibrate the initial electrode plate to obtain an intermediate electrode plate; wherein the vibration time corresponding to the vibration treatment is 0.1-5s, and the vibration frequency is 10-40kHz.
[0060] Furthermore, if Figure 3 As shown, the vibrating treatment of the initial electrode plate by using a conductive medium to obtain an intermediate electrode plate may include:
[0061] S31: placing the conductive medium between the initial electrode plate and the vibration source; the conductive medium is a stainless steel plate; the vibration source is an ultrasonic generator;
[0062] S32: determining the vibration time and the vibration frequency corresponding to the vibration treatment according to the particle size of the solid electrolyte; the vibration time and the vibration frequency are both positively correlated with the particle size of the solid electrolyte;
[0063] S33: vibrating the initial electrode plate using the vibration time and the vibration frequency to obtain the intermediate electrode plate.
[0064] In the embodiment of the present application, the internal particle distribution of the mixture on the surface of the current collector is optimized by vibration, and the vibration is transmitted through a conductive medium, which can be a stainless steel plate, and the vibration source can be an ultrasonic generator. If the current collector is directly vibrated, it will cause damage to the current collector or splashing of the surface material, affecting the forming of the pole piece. Through vibration treatment, the accumulation of active materials, solid electrolytes and conductive agents can be made closer, reducing internal pores, and a low-porosity dry pole piece can be obtained by rolling treatment without the need for an adhesive.
[0065] In an embodiment of the present application, after the current collector with a raw material mixture attached to its surface is vibrated, the active material mixed with large and small particles can be layered, so that large particles are on the top, small particles are on the bottom, and the middle is a state of large and small particles being mixed, that is, the active material with small particles is closest to the current collector, and the active material with large and small particles is above it, and the active material with large particles is above it; this distribution state can ensure that the large particles in the upper layer will not be inactivated due to particle rupture caused by the large rolling pressure, while the small particles in the lower layer are more likely to form a dense layer under the action of external force.
[0066] The embodiment of the present application can ensure that the solid electrolyte is fully filled between the active material particles through vibration treatment, so that the solid electrolyte and the active material particles can be fully contacted, which is easier to compact under the same external force conditions, providing sufficient ion transmission channels.
[0067] In an embodiment of the present application, the corresponding vibration time range during vibration treatment can be 0.1-5s, and the vibration frequency range can be 10-40kHz. Among them, the vibration time and vibration frequency can be appropriately adjusted according to the particle size of each material in the raw material mixture. The larger the particle size, the longer the vibration time and the higher the vibration frequency. Conversely, the smaller the particle size, the shorter the vibration time and the lower the vibration frequency. Selecting appropriate vibration time and vibration frequency can transfer the energy generated by the vibration to the inside of the raw material mixture as much as possible, so that all material particles vibrate, optimize the distribution state of the internal particles, effectively improve the packing density, and reduce the porosity, thereby obtaining a high-density all-solid-state battery pole piece.
[0068] The embodiment of the present application optimizes the particle distribution inside each material in the raw material mixture by means of vibration, which can effectively increase the packing density, thereby reducing the porosity of the electrode plate and obtaining a highly compacted electrode plate.
[0069] S4: rolling the intermediate electrode plate to obtain the electrode plate; wherein the pressure of the rolling process is 0.10-0.50 MPa.
[0070] Furthermore, the rolling process is room temperature rolling or high temperature rolling, wherein the temperature range of the high temperature rolling is 50-200°C.
[0071] In the embodiment of the present application, the intermediate electrode plate is subjected to roller pressing after vibration treatment, and the pressure range of the roller pressing treatment can be 0.10-0.50Mpa. Normal temperature roller pressing or hot pressing treatment can be adopted, and the temperature range of the hot pressing treatment can be 50-200°C.
[0072] The embodiment of the present application can obtain a highly compacted electrode sheet after rolling the intermediate electrode sheet, so that the particles in the electrode sheet are more densely stacked, ensuring more complete contact between the active material and the solid electrolyte, and effectively exerting the ion conduction capacity of the solid electrolyte.
[0073] Furthermore, a first active material layer, a second active material layer and a third active material layer are sequentially stacked on the current collector of the electrode plate;
[0074] The active material includes an active material of a first particle size and an active material of a second particle size, the first active material layer includes the active material of the first particle size and the solid electrolyte; the second active material layer includes the active material of the first particle size, the active material of the second particle size and the solid electrolyte; the third active material layer includes the active material of the second particle size and the solid electrolyte; the first particle size is smaller than the second particle size, and the second particle size is smaller than 20 μm.
[0075] In the embodiment of the present application, the current collector of the electrode plate is sequentially superimposed with the first active material layer, the second active material layer and the third active material layer. The first active material layer is close to the current collector, which is a mixture of small particles of active material and solid electrolyte; the second active material layer is a mixture of large particles of active material, small particles of active material and solid electrolyte; and the third active material layer is a mixture of large particles of active material, small particles of active material and solid electrolyte. This distribution method can ensure that the large particles on the top layer can withstand higher pressure and are not prone to particle rupture during the roller pressing process, avoiding active failure; and this distribution method can ensure that each layer on the plate is dense enough, improve the interface contact between the active material and the solid electrolyte, and build sufficient and rich ion transmission channels.
[0076] In the embodiment of the present application, the active materials on the current collector are distributed in sequence according to the particle size, which can ensure that during the roller pressing process, the large particle material on the upper layer can withstand a larger rolling pressure to avoid particle rupture and inactivation. The small particle material on the lower layer is more likely to form a dense layer under the action of external force, thereby constructing sufficient and rich ion transmission channels and ensuring the excellent ion transmission performance of the electrode plate.
[0077] Furthermore, the particle size of the solid electrolyte is smaller than the particle size of the active material; the particle size of the solid electrolyte ranges from 0.5 to 15 μm.
[0078] In the embodiment of the present application, the microstructure of the active material used is a mixture of large particles and small particles, and the particle size of the solid electrolyte needs to be smaller than the particle size of the small particles in the active material. The particle size range of the solid electrolyte can be 0.5-15 μm.
[0079] The embodiment of the present application selects a material of mixed large and small particles as the active material and ensures that the particle size of the solid electrolyte is smaller than the particle size of the active material, so that the solid electrolyte can be evenly filled between the active materials, avoiding uneven distribution of the solid electrolyte and the active material in the electrode plate due to the large particle size of the solid electrolyte, thereby affecting the capacity of the battery.
[0080] Furthermore, the porosity of the electrode plate is 2-30%.
[0081] In an embodiment of the present application, the active material, solid electrolyte and conductive agent are dry-mixed to obtain a raw material mixture, and then the raw material mixture is sprayed, vibrated and roll-formed on the current collector to finally obtain a dry electrode plate. The porosity of the electrode plate obtained by the above steps is 2-30%, and preferably 2-10% in the embodiment of the present application. This tightly stacked and low-porosity electrode plate can make the active material fully contact with the solid electrolyte, and efficiently exert the ion conduction ability of the solid electrolyte, thereby improving the rate performance and cycle life of the all-solid-state battery.
[0082] The low-porosity electrode plate in the embodiment of the present application can ensure the close stacking of the raw material particles, and the active material and the solid electrolyte can be fully contacted, so that the ion conduction capacity of the solid electrolyte can be fully utilized, thereby improving the cycle life of the all-solid-state battery.
[0083] The present application also provides a device for preparing the electrode sheet, the schematic diagram of which is shown in FIG. Figure 5 As shown, the device includes an unwinding device 1, a guiding device 2, a spraying device 3, an ultrasonic vibration device 4, a rolling device 5, a thickness measuring device 6, a guiding device 7 and a winding device 8. The operation process is as follows: the current collector passes through the unwinding device 1 and the guiding device 2 to reach the spraying device 3; the spraying device is turned on to evenly spread the raw material mixture on the surface of the current collector; the current collector is vibrated by the ultrasonic vibration device 4; the current collector is rolled by the rolling device 5; the current collector is tested by the thickness measuring device 6, and if the current collector does not meet the requirements, the rolling parameters can be adjusted until the electrode sheet meets the requirements; the current collector is rolled by the guiding device 7 and the winding device 8 to complete the preparation of the electrode sheet.
[0084] The embodiment of the present application also provides an all-solid-state battery cell, which includes an electrode pole piece prepared by the above-mentioned preparation method.
[0085] An embodiment of the present application also provides an all-solid-state battery, which includes an electrode plate prepared by the above-mentioned preparation method.
[0086] Embodiment 1:
[0087] This embodiment provides a method for preparing a positive electrode sheet. This embodiment uses 9 series high nickel (wherein the large particles D50 is 8 μm and the small particles D50 is 4 μm) in nickel cobalt manganese oxide materials as the positive electrode material, LPSC (D50 is 0.5 μm) as the solid electrolyte, and vapor-phase carbon fiber (VGCF) as the conductive agent.
[0088] The specific preparation method includes:
[0089] Active material, solid electrolyte and conductive agent were weighed in a mass ratio of 85:14.5:0.5, and mixed by ball milling (ball-to-material mass ratio of 1:5) to obtain a positive electrode raw material mixture;
[0090] The cathode raw material mixture is sprayed on aluminum foil with a surface capacity of 3 mAh / cm 2 , obtaining an initial positive electrode sheet;
[0091] Apply 35kHz vibration for 1s to the initial positive electrode sheet to obtain an intermediate positive electrode sheet;
[0092] The middle positive electrode sheet is subjected to hot pressing treatment to obtain a positive electrode sheet; wherein the hot pressing temperature is 120° C. and the curing pressure is 0.30 MPa.
[0093] Embodiment 2:
[0094] This embodiment provides a method for preparing a positive electrode sheet. This embodiment uses 9 series high nickel (wherein the large particles D50 is 8 μm and the small particles D50 is 4 μm) as the positive electrode material, LPSC (D50 is 0.5 μm) as the solid electrolyte, and vapor-phase carbon fiber (VGCF) as the conductive agent.
[0095] The specific preparation method includes:
[0096] Active material, solid electrolyte and conductive agent were weighed in a mass ratio of 85:14.5:0.5, and mixed by ball milling (ball-to-material mass ratio of 1:5) to obtain a positive electrode raw material mixture;
[0097] The cathode raw material mixture is sprayed on aluminum foil with a surface capacity of 3 mAh / cm 2 , obtaining an initial positive electrode sheet;
[0098] Apply 35kHz vibration for 1s to the initial positive electrode sheet to obtain an intermediate positive electrode sheet;
[0099] The middle positive electrode sheet is rolled at room temperature to obtain a positive electrode sheet; wherein the curing pressure is 0.50 MPa.
[0100] Embodiment 3:
[0101] This embodiment provides a method for preparing a positive electrode sheet. This embodiment uses 9 series high nickel (wherein the large particles D50 is 8 μm and the small particles D50 is 4 μm) as the positive electrode material, LPSC (D50 is 0.5 μm) as the solid electrolyte, and vapor-phase carbon fiber (VGCF) as the conductive agent.
[0102] The specific preparation method includes:
[0103] Active material, solid electrolyte and conductive agent were weighed in a mass ratio of 85:14.5:0.5, and mixed by ball milling (ball-to-material mass ratio of 1:5) to obtain a positive electrode raw material mixture;
[0104] The cathode raw material mixture is sprayed on aluminum foil with a surface capacity of 3 mAh / cm 2 , obtaining an initial positive electrode sheet;
[0105] Apply 35kHz vibration for 8s to the initial positive electrode sheet to obtain an intermediate positive electrode sheet;
[0106] The middle positive electrode sheet is rolled at room temperature to obtain a positive electrode sheet; wherein the curing pressure is 0.50 MPa.
[0107] Embodiment 4:
[0108] This embodiment provides a method for preparing a positive electrode sheet. This embodiment uses 9 series high nickel (wherein the large particles D50 is 8 μm and the small particles D50 is 4 μm) as the positive electrode material, LPSC (D50 is 0.5 μm) as the solid electrolyte, and vapor-phase carbon fiber (VGCF) as the conductive agent.
[0109] The specific preparation method includes:
[0110] Active material, solid electrolyte and conductive agent were weighed in a mass ratio of 85:14.5:0.5, and mixed by ball milling (ball-to-material mass ratio of 1:5) to obtain a positive electrode raw material mixture;
[0111] The cathode raw material mixture is sprayed on aluminum foil with a surface capacity of 3 mAh / cm 2 , obtaining an initial positive electrode sheet;
[0112] Apply 1 kHz vibration for 1 s to the initial positive electrode sheet to obtain an intermediate positive electrode sheet;
[0113] The middle positive electrode sheet is rolled at room temperature to obtain a positive electrode sheet; wherein the curing pressure is 0.50 MPa.
[0114] Embodiment 5:
[0115] This embodiment provides a method for preparing a positive electrode sheet. This embodiment uses 9 series high nickel (wherein the large particles D50 is 8 μm and the small particles D50 is 4 μm) as the positive electrode material, LPSC (D50 is 0.5 μm) as the solid electrolyte, and vapor-phase carbon fiber (VGCF) as the conductive agent.
[0116] The specific preparation method includes:
[0117] Active material, solid electrolyte and conductive agent were weighed in a mass ratio of 85:14.5:0.5, and mixed by ball milling (ball-to-material mass ratio of 1:5) to obtain a positive electrode raw material mixture;
[0118] The cathode raw material mixture is sprayed on aluminum foil with a surface capacity of 3 mAh / cm 2 , obtaining an initial positive electrode sheet;
[0119] Apply 35kHz vibration for 1s to the initial positive electrode sheet to obtain an intermediate positive electrode sheet;
[0120] The middle positive electrode sheet is rolled at room temperature to obtain a positive electrode sheet; wherein the curing pressure is 0.1 MPa.
[0121] Comparative Example 1:
[0122] This comparative example provides a method for preparing a positive electrode sheet. This comparative example uses 9 series high nickel (wherein the large particles D50 is 8 μm and the small particles D50 is 4 μm) as the positive electrode material, LPSC (D50 is 0.5 μm) as the solid electrolyte, and vapor-phase carbon fiber (VGCF) as the conductive agent.
[0123] The specific preparation method includes:
[0124] Active material, solid electrolyte and conductive agent were weighed in a mass ratio of 85:14.5:0.5, and mixed by ball milling (ball-to-material mass ratio of 1:5) to obtain a positive electrode raw material mixture;
[0125] The cathode raw material mixture is sprayed on aluminum foil with a surface capacity of 3 mAh / cm 2 , obtaining an initial positive electrode sheet;
[0126] The initial positive electrode sheet is subjected to hot pressing treatment to obtain a positive electrode sheet; wherein the hot pressing temperature is 120° C. and the curing pressure is 0.30 MPa.
[0127] Comparative Example 2:
[0128] This comparative example provides a method for preparing a positive electrode sheet. This comparative example uses 9 series high nickel (wherein the large particles D50 is 8 μm and the small particles D50 is 4 μm) as the positive electrode material, LPSC (D50 is 0.5 μm) as the solid electrolyte, and vapor-phase carbon fiber (VGCF) as the conductive agent.
[0129] The specific preparation method includes:
[0130] Active material, solid electrolyte and conductive agent were weighed in a mass ratio of 85:14.5:0.5, and mixed by ball milling (ball-to-material mass ratio of 1:5) to obtain a positive electrode raw material mixture;
[0131] The cathode raw material mixture is sprayed on aluminum foil with a surface capacity of 3 mAh / cm 2 , obtaining an initial positive electrode sheet;
[0132] Apply 50kHz vibration for 1s to the initial positive electrode sheet to obtain an intermediate positive electrode sheet;
[0133] The middle positive electrode sheet is subjected to hot pressing treatment to obtain a positive electrode sheet; wherein the hot pressing temperature is 120° C. and the curing pressure is 0.30 MPa.
[0134] Comparative Example 3:
[0135] This comparative example provides a method for preparing a positive electrode sheet. This comparative example uses 9 series high nickel (wherein the large particles D50 is 8 μm and the small particles D50 is 4 μm) as the positive electrode material, LPSC (D50 is 6 μm) as the solid electrolyte, and vapor-phase carbon fiber (VGCF) as the conductive agent.
[0136] The specific preparation method includes:
[0137] Active material, solid electrolyte and conductive agent were weighed in a mass ratio of 85:14.5:0.5, and mixed by ball milling (ball-to-material mass ratio of 1:5) to obtain a positive electrode raw material mixture;
[0138] The cathode raw material mixture is sprayed on aluminum foil with a surface capacity of 3 mAh / cm 2 , obtaining an initial positive electrode sheet;
[0139] Apply 35kHz vibration for 1s to the initial positive electrode sheet to obtain an intermediate positive electrode sheet;
[0140] The middle positive electrode sheet is subjected to hot pressing treatment to obtain a positive electrode sheet; wherein the hot pressing temperature is 120° C. and the curing pressure is 0.30 MPa.
[0141] Comparative Example 4;
[0142] This comparative example provides a method for preparing a positive electrode sheet. This comparative example uses two different particle sizes of 9 series high nickel (the two particle sizes are 8μm and 4μm respectively) as positive electrode materials, LPSC (D50 is 0.5μm) as solid electrolyte, and vapor-phase carbon fiber (VGCF) as conductive agent.
[0143] The specific preparation method includes:
[0144] Active material, solid electrolyte and conductive agent were weighed in a mass ratio of 85:14.5:0.5, and mixed by ball milling (ball-to-material mass ratio 1:5) to obtain a mixture of two positive electrode raw materials;
[0145] The two positive electrode raw material mixtures were sprayed on aluminum foil respectively. The small-particle positive electrode raw material mixture was sprayed first, and then the large-particle positive electrode raw material mixture was covered. The surface capacity was 3 mAh / cm 2 , and roll pressing is performed at room temperature to obtain a positive electrode sheet; wherein the curing pressure is 0.50MPa.
[0146] In the examples of the present application, the electrode plates obtained in the above-mentioned examples and comparative examples were subjected to a plate porosity test and an electrochemical performance test, and the test results are shown in Table 1. The plate porosity test is to test the porosity of the electrode plates at room temperature using a fully automatic mercury intrusion pore size instrument; the electrochemical performance test is to perform a cycle performance test on a 3*3cm single-piece soft-pack battery cell, with a voltage window of 3.0-4.25V and a test condition of 0.5C / 0.5C.
[0147] Table 1 Performance test results of different electrode plates
[0148] Electrode Porosity (%) Cycle number (capacity decay to 80%) Example 1 3.6 228 Example 2 4.1 225 Example 3 16.2 50 Example 4 14.3 126 Example 5 13.8 114 Comparative Example 1 17.5 66 Comparative Example 2 16.1 45 Comparative Example 3 20.4 35 Comparative Example 4 16.1 52
[0149] In the embodiments of the present application, Figure 4 Schematic diagram of the structure of the positive electrode sheet prepared in the above-mentioned embodiment 1. Figure 4 It can be obtained that after vibration and rolling treatment, each layer of positive electrode active material particles and solid electrolyte particles are tightly combined, indicating that the preparation method provided in the embodiment of the present application can effectively reduce the porosity of the electrode plate, and the prepared electrode plate has high density, which can effectively solve the problem that the all-solid-state battery plate is difficult to compact and the porosity is difficult to reduce by external pressure, and effectively improve the cycle performance of the all-solid-state battery.
[0150] In the embodiments of the present application, it can be obtained through the test results of Examples 2 and 3 that a long ultrasonic time will destroy the uniform distribution of active materials and solid electrolytes inside the electrode plates, and some active materials cannot contact the solid electrolyte, resulting in the inability to transmit lithium ions, affecting the capacity of the electrode plates; through the test results of Examples 2, 4 and Comparative Example 1, it can be obtained that the ultrasonic vibration frequency is low or ultrasonic vibration is not performed, and the internal structure of the electrode plates is not rearranged. In this case, if the electrode plates are directly rolled, it is difficult for external force to eliminate the larger pores inside the electrode plates. Cracks will appear in these larger pores after pressurization, and lithium dendrites will appear in subsequent charge and discharge cycles, resulting in Harm to battery performance; It can be obtained from the test results of Examples 2 and 5 that insufficient pressure during rolling treatment will cause high porosity and poor battery cycle; It can be obtained from the test results of Comparative Example 3 that if the particle size of the solid electrolyte particles is larger than the particle size of the active material particles, the small particles of the active material will partially sink during vibration, and the solid electrolyte cannot be filled between the active material particles through vibration due to its large particle size, which will cause uneven distribution of the solid electrolyte and the active material in the electrode sheet, causing serious impact on the battery capacity; It can be obtained from the test results of Example 2 and Comparative Example 4 that ultrasonic vibration is conducive to uniform filling of the solid electrolyte between the active material particles, and a dense electrode electrode sheet can be formed after further rolling.
[0151] As can be seen from the above embodiments provided by the present application, the present application mixes the active material, the solid electrolyte and the conductive agent, and obtains a raw material mixture after uniform mixing; the raw material mixture is uniformly sprayed on the current collector to obtain an initial electrode plate; the initial electrode plate is vibrated by a conductive medium to obtain an intermediate electrode plate; wherein the vibration time corresponding to the vibration treatment is 0.1-5s, and the vibration frequency is 10-40kHz; the intermediate electrode plate is roll-pressed to obtain an electrode plate; wherein the pressure of the roll-pressing treatment is 0.10-0.50Mpa. The present application achieves a simple mixing process by mixing the active material, solid electrolyte and conductive agent in dry powder, thereby reducing the involvement of solvents in the processing of the electrode plate, avoiding the decrease in ionic conductivity caused by solvent volatilization, shortening the drying process, and improving production efficiency and safety; the particle distribution in the raw material mixture is optimized by vibration, so that the particles inside the electrode plate are more densely packed and have a low porosity, ensuring full contact between the active material and the solid electrolyte, and effectively exerting the ion conductivity of the solid electrolyte, thereby improving the rate performance and cycle life of the all-solid-state battery; by distributing the mixture of large particles of active material and solid electrolyte in the upper layer, i.e., away from the current collector, and the mixture of small particles of active material and solid electrolyte in the lower layer, i.e., close to the current collector, with the active material mixed with large and small particles in the middle, it is ensured that the large particles in the upper layer are not prone to particle rupture when subjected to high pressure, thereby avoiding the occurrence of active failure, and ensuring that each layer of active material on the electrode plate is dense enough, thereby effectively improving the compaction density of the electrode plate.
[0152] The above description is only a preferred embodiment of the present application and is not intended to limit the present application. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present application should be included in the protection scope of the present application.
Claims
1. A method for preparing an electrode sheet, characterized in that: The method comprises: The active material, the solid electrolyte and the conductive agent are mixed and uniformly mixed to obtain a raw material mixture; Evenly spraying the raw material mixture on the current collector to obtain an initial electrode sheet; The initial electrode plate is vibrated by a conductive medium to obtain an intermediate electrode plate; wherein the vibration time corresponding to the vibration treatment is 0.1-5s and the vibration frequency is 10-40kHz; The intermediate electrode plate is subjected to a rolling process to obtain the electrode plate; wherein the pressure of the rolling process is 0.10-0.50 MPa.
2. The method according to claim 1, characterized in that The vibrating treatment of the initial electrode plate by using a conductive medium to obtain an intermediate electrode plate comprises: The conductive medium is placed between the initial electrode plate and the vibration source; the conductive medium is a stainless steel plate; the vibration source is an ultrasonic generator; Determining the vibration time and the vibration frequency corresponding to the vibration treatment according to the particle size of the solid electrolyte; the vibration time and the vibration frequency are both positively correlated with the particle size of the solid electrolyte; The initial electrode plate is vibrated using the vibration time and the vibration frequency to obtain the intermediate electrode plate.
3. The method according to claim 1, characterized in that: The active material, the solid electrolyte and the conductive agent are mixed and uniformly mixed to obtain a raw material mixture, comprising: The active material and the solid electrolyte are mixed in a mass ratio of (60-90): (10-40) to obtain an initial raw material mixture after mixing evenly; The initial raw material mixture and the conductive agent are mixed in a mass ratio of (70-130):(0-5), and the raw material mixture is obtained after mixing evenly.
4. The method according to claim 1, characterized in that: The rolling process is room temperature rolling or high temperature rolling, wherein the temperature range of the high temperature rolling is 50-200°C.
5. The method according to claim 1, characterized in that The current collector of the electrode plate is sequentially stacked with a first active material layer, a second active material layer and a third active material layer; The active material includes an active material of a first particle size and an active material of a second particle size, the first active material layer includes the active material of the first particle size and the solid electrolyte; the second active material layer includes the active material of the first particle size, the active material of the second particle size and the solid electrolyte; the third active material layer includes the active material of the second particle size and the solid electrolyte; the first particle size is smaller than the second particle size, and the second particle size is smaller than 20 μm.
6. The method according to claim 1, characterized in that The porosity of the electrode plate is 2-30%.
7. The method according to claim 1, characterized in that The particle size of the solid electrolyte is smaller than that of the active material; the particle size of the solid electrolyte ranges from 0.5 to 15 μm.
8. The method according to claim 1, characterized in that The active material is a positive electrode material or a negative electrode material; wherein the positive electrode material is one or more of lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, lithium nickel cobalt manganese aluminum oxide, lithium cobalt oxide, lithium manganese oxide, lithium iron phosphate or lithium-rich manganese-based material; the negative electrode material is one or more of graphite, silicon-carbon composite material, and lithium titanate.
9. The method according to claim 1, characterized in that: The solid electrolyte is one or more of a sulfide solid electrolyte, an oxide solid electrolyte, and a polymer solid electrolyte; The conductive agent is one or more of acetylene black, vapor phase carbon fiber, carbon nanotube, nano carbon fiber and graphene.
10. An electrode plate, characterized in that: The electrode plate is prepared by the preparation method according to any one of claims 1 to 9.
Citation Information
Patent Citations
Preparation method for mixed lithium manganate material
CN106532033A
Low-porosity all-solid-state battery electrode plate as well as preparation method and application thereof
CN111933890A
Cited By
Lithium battery composite positive electrode based on multi-stage particle size electrolyte and preparation method and application of lithium battery composite positive electrode