Ecological concrete based on fly ash and preparation method thereof
By deeply purifying the fly ash and combining it with active exciters and environmentally friendly additives, ecological concrete is prepared, which solves the problems of pollution and high carbon emissions in traditional concrete production environment, and realizes the safe resource utilization and construction of fly ash Green transformation of materials.
Patent Information
- Application Number
- CN202410946408.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-16
- Publication Date
- 2024-11-29
AI Technical Summary
Traditional concrete production relies on cement, which leads to high environmental pollution and carbon emissions, and the problem of handling harmful substances in fly ash in waste incineration limits its resource utilization.
By deeply purifying fly ash, including physical screening, chemical cleaning and heat treatment, removing heavy metals and harmful substances, and combining active exciters and environmentally friendly additives, an ecological concrete based on fly ash is prepared to enhance its mechanics Performance and environmentally friendly performance.
It has achieved safe and resource utilization of fly ash, reduced the carbon footprint and environmental impact of concrete production, provided new building materials with superior performance and high cost efficiency, and promoted the green transformation and sustainable development of building materials.
Smart Images

Figure CN119038916A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to an innovative technology for preparing building materials, and in particular to an ecological concrete that uses fly ash from garbage incineration, an industrial byproduct, as one of the main raw materials. This ecological concrete not only effectively utilizes fly ash that may have originally polluted the environment, but also improves the environmental protection performance and engineering performance of concrete through a series of advanced processing and formulation technologies. The technical field of the present invention includes but is not limited to the preparation of building materials, resource utilization of industrial waste, research and development of environmentally friendly concrete, and sustainable development construction practices. Through the application of this technology, it is intended to promote the green transformation of the concrete industry, reduce dependence on traditional cement, reduce the carbon footprint of the construction industry, and at the same time provide a new type of building material with superior performance and high cost-effectiveness. Background Art
[0002] As a widely used construction material, the impact of concrete production on the environment has attracted increasing attention. The production of traditional concrete relies on cement, which is one of the main sources of global CO2 emissions. In addition, with the acceleration of urbanization, the treatment of construction waste has also become a prominent issue, especially the fly ash produced during waste incineration, which contains heavy metals and other harmful substances, posing a potential threat to the environment and human health.
[0003] At present, the main methods for handling fly ash include landfill and resource utilization. Although the landfill method is simple, it occupies a large amount of land resources and has potential environmental risks. The resource utilization method of fly ash, such as using it as a substitute or additive for building materials, has potential, but is limited by the difficulty of handling harmful substances in fly ash and the requirements of concrete performance.
[0004] Therefore, a technology is needed that can effectively treat harmful substances in fly ash and improve the environmental protection and engineering performance of concrete. This requires the development of a new type of ecological concrete that can utilize the beneficial components in fly ash and, through innovative formulations and processes, reduce the negative impact on the environment and improve the mechanical properties and durability of concrete. It is in this context that the present invention proposes an ecological concrete based on fly ash and a preparation method thereof, aiming to address the deficiencies in the prior art and promote the sustainable development of building materials.
[0005] Technical Solution
[0006] The technical solution of the present invention is a method for preparing fly ash-based eco-concrete, which aims to transform waste incineration fly ash into environmentally friendly and high-performance building materials through a series of innovative process steps. This solution not only solves the environmental treatment problem of fly ash, but also improves the engineering application value of concrete.
[0007] 1. An eco-concrete based on fly ash, comprising the following raw materials, each raw material in the following proportions:
[0008] 50 parts of fly ash after purification, wherein the purification process involves at least one physical washing and chemical treatment to ensure the effective removal of heavy metals and harmful impurities, thereby obtaining a high-purity fly ash raw material that can partially replace traditional cement in concrete while providing the necessary micro-filling and reinforcement effects;
[0009] 40 parts of cement, preferably silicate cement, to provide the necessary bonding properties and chemically react with fly ash to form a high-strength cement stone structure;
[0010] 40 parts of aggregate, including fine aggregate and coarse aggregate, the ratio of fine aggregate to coarse aggregate is 1:2 to 1:4, so as to optimize the density and mechanical properties of concrete, the particle size of coarse aggregate is controlled between 5mm and 20mm, and the particle size of fine aggregate is controlled between 0.15mm and 0.6mm;
[0011] 20 parts of water, as the basic medium for concrete mixing, the amount of which is precisely calculated to ensure the workability and machinability of the concrete;
[0012] 5 parts of an active activator, used to increase the activity of fly ash and enhance the chemical reaction with cement. The active activator may be one or a combination of silane coupling agent, titanate coupling agent or aluminate activator;
[0013] 2 parts of environmentally friendly additives, used to improve the working performance of concrete, reduce cement dosage, and reduce CO2 emissions. The environmentally friendly additives can be one or a combination of superplasticizers, water reducers, or air introducing agents.
[0014] The purified fly ash undergoes a series of sophisticated physical separation, chemical treatment and thermal treatment steps, including but not limited to flotation, sedimentation, filtration and pyrolysis, to remove heavy metals and other harmful substances in the fly ash, improve its safety and activity as a concrete raw material, and ensure that the final product meets ecological and environmental protection requirements.
[0015] The amount of the active activator added is accurately calculated according to its chemical properties and the specific requirements of concrete to achieve the best performance improvement. The addition of the active activator can significantly improve the early strength and long-term durability of concrete.
[0016] The addition of environmentally friendly additives is intended to improve the fluidity and plasticity of concrete while reducing the amount of cement used, thereby reducing CO2 emissions during concrete production. The addition of environmentally friendly additives can significantly improve the construction performance of concrete and reduce environmental impact.
[0017] The ratio of fine aggregate to coarse aggregate is 1:2 to 1:4. This ratio is optimized through multiple experiments based on the mechanical properties and durability requirements of concrete to ensure that the concrete has excellent engineering application performance and cost-effectiveness.
[0018] Cement is silicate cement or sulphoaluminate cement. Different types of cement can be selected according to different application scenarios and performance requirements of concrete to adapt to various engineering environments and improve the adaptability and application range of concrete.
[0019] The method for preparing ecological concrete is characterized by comprising the following steps:
[0020] Raw material preparation, weighing each raw material according to the number of portions as described in claim 1, ensuring the accuracy of the raw material ratio, and providing a basis for subsequent mixing and stirring;
[0021] Mixing: Mix the weighed raw materials evenly in a special concrete mixer to form a uniform mixture. The mixing time is controlled within 3 to 5 minutes to ensure that the various raw materials are fully dispersed;
[0022] Stirring: Stirring the mixed raw materials in a mixer until a uniform concrete slurry is formed, and the stirring speed is controlled at 100-200 rpm to ensure the uniformity and workability of the mixture;
[0023] Pouring: pour the mixed concrete slurry into the mold and shape it according to the engineering requirements. During the pouring process, care should be taken to avoid the mixing of air and the separation of the slurry;
[0024] Curing: Curing the poured concrete under suitable temperature and humidity conditions for the specified time to ensure the hardening and strength development of the concrete. The curing conditions are adjusted according to the specific performance requirements of the concrete.
[0025] During the mixing step, precise control of the mixing speed is crucial to the uniformity and final performance of the concrete. The mixing speed is controlled at 100-200 rpm to achieve the best mixing effect. The mixing time is adjusted according to the specific mix ratio and workability requirements of the concrete.
[0026] During the curing step, precise control of curing conditions is critical to the hardening and strength development of concrete. The curing temperature is controlled at 20-25°C, the humidity is controlled at 60-80%, and the curing time is 7 to 28 days to ensure that the concrete meets the designed performance requirements. The temperature and humidity of the concrete should be checked regularly during the curing process to ensure the stability of the curing conditions.
[0027] Prioritize deep purification of fly ash: This solution first conducts deep purification of fly ash to ensure its safety and stability as a concrete raw material. The specific steps include: Physical screening: Use a vibrating screen to remove large impurities and uneven particles in the fly ash. Chemical cleaning: Use chemical reagents to wash the fly ash multiple times to remove soluble salts and heavy metals. Thermal treatment: The cleaned fly ash is calcined at high temperature to further improve its activity and stabilize its chemical structure.
[0028] Preferentially, preparation and addition of active activators: In order to improve the activity of fly ash, the present solution involves the preparation and addition of one or more active activators. These activators can react chemically with elements such as silicon and aluminum in fly ash to form hydraulic compounds, thereby enhancing the mechanical properties of concrete. The preparation of active activators includes: Selecting activators: Selecting suitable activators according to the chemical composition of fly ash and the performance requirements of concrete. Accurate metering: Accurately meter the activators and evenly mix them into the fly ash according to the predetermined ratio.
[0029] Prioritize the precise proportion of concrete raw materials: This solution determines the proportion of concrete raw materials through precise calculation, including purified fly ash, Portland cement, coarse and fine aggregates, and water reducing agent, etc. The proportion of each raw material is carefully designed to ensure that the final performance of the concrete meets the engineering requirements.
[0030] Prior to mixing and stirring process: the proportioned raw materials are mixed and stirred in a special concrete mixer. The mixing process is divided into two stages: dry mixing and wet mixing to ensure that the solid particles are fully dispersed and form a uniform mixture.
[0031] Prioritize the pouring and molding process: pour the evenly mixed concrete slurry into the mold under strictly controlled conditions. During the pouring process, care must be taken to avoid air mixing and slurry separation to ensure the uniformity and density of the concrete.
[0032] Preferably, curing process: After pouring, the concrete is cured under suitable temperature and humidity conditions to promote cement hydration and concrete hardening. Curing conditions are optimized according to the performance requirements of the concrete and environmental conditions.
[0033] Prioritize, performance testing and evaluation: After the curing period, a series of performance tests are carried out on the concrete samples, including compressive strength, flexural strength, impermeability, durability, etc., to ensure that the concrete meets the design requirements and relevant standards.
[0034] Prioritize, quality control system: During the entire preparation process, strict quality control measures are implemented, including quality inspection of raw materials, monitoring of the production process, and performance evaluation of the finished product, to ensure that each batch of eco-concrete meets the established quality standards.
[0035] Through the above-mentioned detailed process flow, this technical solution realizes the high-value utilization of fly ash and prepares ecological concrete with high mechanical properties and good durability, providing the construction industry with an environmentally friendly, economical, high-performance new building material with significant social and economic value.
[0036] The key technical problems addressed by the technical solution of the present invention include how to achieve deep purification of fly ash to remove harmful substances and ensure its safety as a concrete raw material; improve the activity of fly ash so that it can fully react with traditional cement and enhance the mechanical properties of concrete; accurately calculate and optimize the ratio of fly ash to other raw materials to meet the mechanical and durability requirements of high-performance concrete; ensure that concrete using fly ash has good workability and processability during mixing, pouring and molding; control curing conditions to adapt to different environments to ensure the hardening effect of concrete; conduct comprehensive performance evaluation and quality control to ensure that concrete meets design and standard requirements; select and apply environmentally friendly additives to reduce cement usage and CO2 emissions while maintaining cost-effectiveness; and ultimately achieve an environmentally friendly, economical, high-performance ecological concrete to solve the impact of traditional concrete production on the environment and promote the green transformation and sustainable development of building materials. Through this series of innovative processes and technical measures, the present invention successfully overcomes the above-mentioned difficulties and provides a practical solution for the resource utilization of fly ash and the commercial production of ecological concrete.
[0037] The core protection points of the present invention are mainly concentrated in two technical fields: first, the deep purification treatment technology of fly ash, which effectively removes heavy metals and harmful compounds in fly ash through a series of physical washing, chemical neutralization and heat treatment steps, ensuring the safety and stability of fly ash as a concrete raw material. This is the key technical link for the present invention to realize the resource utilization of fly ash; second, the innovative formula and preparation process of ecological concrete, which not only improves the mechanical properties and durability of concrete by accurately calculating the raw material ratio and combining the use of active stimulants and environmentally friendly additives, but also significantly reduces CO2 emissions in the production process, realizing the green transformation of building materials. These two protection points together constitute the technical core of the present invention and provide a solid innovation foundation and environmental value for its application in the field of construction.
[0038] The beneficial effects of the present invention are reflected in many aspects: first, by deeply purifying fly ash, the present invention effectively solves the environmental risks of harmful substances in fly ash, converts it into a safe and beneficial building material, and realizes the resource utilization of industrial by-products; secondly, the innovative ecological concrete formula and preparation process significantly improve the mechanical properties and durability of concrete, while reducing the dependence on traditional cement, reducing the carbon footprint and environmental impact of the construction industry; furthermore, by optimizing the raw material ratio and adding active stimulants, the ecological concrete of the present invention has better workability and processability while improving engineering performance, improving construction efficiency and application scope; finally, the use of the environmentally friendly additives of the present invention further reduces the energy consumption and CO2 emissions in the concrete production process, and promotes the green and sustainable development of the building materials industry. In general, the present invention not only improves the environmental protection performance and engineering application value of building materials, but also has significant social and economic benefits. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] Figure 1 The fly ash purification process of the present invention is
[0040] Figure 2 The process flow of concrete pouring and molding of the present invention Specific implementation 1:
[0042] The process of preparing eco-concrete based on fly ash from waste incineration is a comprehensive technical activity involving multiple stages, each of which has its own specific operational details and goals. The following is a detailed description of each step:
[0043] Fly ash collection and pretreatment
[0044] In waste incineration plants, fly ash is collected as one of the main by-products. The collection process is usually carried out immediately after the incineration process to reduce the exposure and potential environmental impact of fly ash. The collected fly ash is first transported to a dedicated treatment facility. Here, the fly ash is screened through a vibrating screen to remove particles larger than 2mm, such as unburned waste residues. This step is crucial for the subsequent deep purification of fly ash because it ensures the uniformity and processing efficiency of the fly ash.
[0045] Deep purification of fly ash
[0046] The deep purification process is designed to remove heavy metals and harmful organic matter, such as dioxins, from fly ash. First, fly ash is mixed with dilute sulfuric acid at a ratio of 5% of the fly ash mass and chemically cleaned at a pH of 3 to dissolve and remove heavy metals. This step requires precise control of the pH value and mixing ratio to ensure effective removal of heavy metals. Subsequently, the cleaned fly ash is heat treated at a high temperature of 600°C for 1 hour to further stabilize the fly ash structure and decompose residual organic matter.
[0047] Fly ash solidification treatment
[0048] The purpose of the solidification process is to improve the stability and safety of fly ash and make it suitable as a raw material for concrete. The purified fly ash is mixed with cement in a mass ratio of 3:7 to form a solidified body. In this step, cement not only acts as a curing agent, but also helps to improve the structural strength of the solidified body. The preparation of the solidified body needs to be carried out in a special mixing equipment to ensure a uniform mixture of fly ash and cement.
[0049] Concrete pouring preparation
[0050] At the construction site, the construction team first conducts a thorough inspection of the formwork and support system to ensure that all connections are stable and not loose. The formwork surface needs to be cleaned and, if necessary, a release agent is applied to prevent the concrete from adhering to the formwork, ensuring that the surface of the concrete is smooth and neat after forming.
[0051] Concrete transportation and inspection
[0052] After the concrete is mixed at the premix plant or on site, it is transported to the pouring site within 1 hour by a mixer truck or other transportation equipment. After arriving at the site, the construction personnel will test the workability of the concrete, especially the slump, to ensure that it meets the construction requirements of 160-200mm. The slump test is crucial to ensure the fluidity and pourability of the concrete.
[0053] Concrete pouring and vibrating
[0054] The concrete is poured in layers, and the thickness of each layer is strictly controlled within 300mm. After each layer of concrete is poured, a vibrating rod is used for vibration, and the vibration time is controlled within 20 seconds at each point to remove air, ensure the close combination between concrete and formwork, and improve the density of concrete.
[0055] Concrete leveling and finishing
[0056] After the vibration is completed, the concrete surface is initially leveled with a scraper to ensure that the concrete surface is flush with the top of the formwork. Afterwards, experienced workers use a trowel to perform a detailed plastering process to form a smooth and uniform concrete surface, providing a good foundation for subsequent maintenance and use.
[0057] Concrete curing
[0058] After pouring and plastering, the concrete should be covered immediately, such as with a wet cloth or special curing film, to reduce water evaporation. During the curing period, the concrete needs to be kept moist for no less than 7 days to ensure that the cement hydration reaction is fully carried out, thereby ensuring the strength and durability of the concrete.
[0059] Formwork removal and quality inspection
[0060] After the concrete strength reaches 75% of the design strength, usually within 7 to 14 days after the pouring is completed, the formwork can be removed. After removal, the concrete structure is subjected to detailed quality inspection, including compressive strength testing, to ensure that it meets the design and application requirements. The compressive strength test is carried out in accordance with GB / T 50081-2002 standard to ensure that the concrete compressive strength reaches or exceeds the design requirement of 30MPa.
[0061] Through the above steps, fly ash is successfully converted into an important raw material for eco-concrete, realizing the resource utilization of fly ash. At the same time, the produced eco-concrete has good engineering performance and environmental protection characteristics, and is a green building material with broad application prospects.
[0062] Implementation 2: Preparation and application of fly ash-based ecological concrete
[0063] Step 1: Collection and classification of fly ash
[0064] In waste incineration power plants, fly ash is collected by the flue gas purification system. The collected fly ash is first classified according to its physical and chemical properties for subsequent treatment and application.
[0065] Step 2: Initial treatment of fly ash
[0066] The classified fly ash is initially processed, including mechanical screening to remove large impurities and magnetic separation to remove metal particles. This step is to ensure the purity of the fly ash and lay a good foundation for subsequent chemical treatment.
[0067] Step 3: Chemical Cleaning and Heavy Metal Removal
[0068] The fly ash was mixed with 5% by mass of dilute sulfuric acid and chemically cleaned at a pH of 4 to remove heavy metals. The cleaned fly ash was heat treated at 600°C for 1 hour to further stabilize the fly ash structure.
[0069] Step 4: Decomposition of dioxins
[0070] The fly ash is treated with high temperature pyrolysis technology at 850℃ for 1.5 hours to decompose dioxins in the fly ash. This step is carried out in an oxygen-free or low-oxygen environment to ensure the complete decomposition of dioxins.
[0071] Step 5: Activation of fly ash
[0072] In order to improve the activity of fly ash in concrete, 2% by mass of sodium silicate is added to the fly ash as an activity activator. This step helps to improve the interaction between fly ash and cement and improve the mechanical properties of concrete.
[0073] Step 6: Mixing of concrete ingredients
[0074] The activated fly ash, ordinary Portland cement, fine aggregate and coarse aggregate are mixed in a mass ratio of 30%, 35%, 20% and 15%. At the same time, appropriate amounts of water reducing agent and air introducing agent are added as needed to improve the workability of the concrete.
[0075] Step 7: Mixing the concrete
[0076] In a forced mixer, the mixed raw materials are stirred for 3-5 minutes to ensure uniform mixing of the raw materials.
[0077] Step 8: Concrete pouring
[0078] The mixed concrete is transported to the pouring site and poured in layers. The thickness of each layer does not exceed 500mm, and each layer is compacted after pouring to ensure the density of the concrete.
[0079] Step 9: Curing of Concrete
[0080] After pouring, the concrete surface is immediately covered and maintained to maintain moisture. The maintenance time is determined according to environmental conditions and concrete strength development, usually not less than 14 days.
[0081] Step 10: Concrete Performance Testing
[0082] After the curing period, the concrete samples are subjected to performance tests, including compressive strength, flexural strength, impermeability and durability tests, to evaluate whether the performance of the concrete meets the design requirements.
[0083] Step 11: Application of Concrete
[0084] Eco-concrete that passes the performance test will be used in building structures, road paving and other projects to achieve resource utilization of fly ash and green development of the concrete industry.
[0085] Through implementation method 2, waste incineration fly ash is successfully converted into an important raw material for ecological concrete, achieving high-value utilization of fly ash. The prepared ecological concrete has good mechanical properties and durability, and has low environmental impact, and is a green building material with broad application prospects.
Claims
1. An ecological concrete based on fly ash, It is characterized in that It is composed of the following ingredients, the number of parts of each ingredient is: 50 parts of fly ash after purification, wherein the purification process involves at least one physical washing and chemical treatment to ensure the effective removal of heavy metals and harmful impurities, thereby obtaining a high-purity fly ash raw material that can partially replace traditional cement in concrete while providing the necessary micro-filling and reinforcement effects; 40 parts of cement, preferably silicate cement, to provide the necessary bonding properties and chemically react with fly ash to form a high-strength cement stone structure; 40 parts of aggregate, including fine aggregate and coarse aggregate, the ratio of fine aggregate to coarse aggregate is 1:2 to 1:4, so as to optimize the density and mechanical properties of concrete, the particle size of coarse aggregate is controlled between 5mm and 20mm, and the particle size of fine aggregate is controlled between 0.15mm and 0.6mm; 20 parts of water, as the basic medium for concrete mixing, the amount of which is precisely calculated to ensure the workability and machinability of the concrete; 5 parts of an active activator, used to increase the activity of fly ash and enhance the chemical reaction with cement. The active activator may be one or a combination of silane coupling agent, titanate coupling agent or aluminate activator; 2 parts of environmentally friendly additives, used to improve the working performance of concrete, reduce cement dosage, and reduce CO2 emissions. The environmentally friendly additives can be one or a combination of superplasticizers, water reducers, or air introducing agents.
2. The ecological concrete as claimed in claim 1, It is characterized in that The purified fly ash undergoes a series of fine physical separation, chemical treatment and thermal treatment steps, including but not limited to flotation, sedimentation, filtration and pyrolysis, to remove heavy metals and other harmful substances in the fly ash, improve its safety and activity as a concrete raw material, and ensure that the final product meets the requirements of ecological and environmental protection.
3. The ecological concrete as claimed in claim 1, It is characterized in that The amount of the active activator added is accurately calculated according to its chemical properties and the specific requirements of concrete to achieve optimal performance improvement. The addition of the active activator can significantly improve the early strength and long-term durability of concrete.
4. The ecological concrete as claimed in claim 1, It is characterized in that The addition of the environmentally friendly additive is intended to improve the fluidity and plasticity of concrete, while reducing the amount of cement used, thereby reducing CO2 emissions during the concrete production process. The addition of the environmentally friendly additive can significantly improve the construction performance of concrete and reduce environmental impact.
5. The ecological concrete as claimed in claim 1, It is characterized in that The ratio of fine aggregate to coarse aggregate in the aggregate is 1:2 to 1:
4. This ratio is obtained through multiple experiments and optimization based on the mechanical properties and durability requirements of concrete to ensure that the concrete has excellent engineering application performance and cost-effectiveness.
6. The ecological concrete according to claim 1, It is characterized in that The cement is silicate cement or sulphoaluminate cement. Different types of cement can be selected according to different application scenarios and performance requirements of concrete to adapt to various engineering environments and improve the adaptability and application range of concrete.
7. The method for preparing ecological concrete according to claim 1, It is characterized in that The following steps are involved: Raw material preparation, weighing each raw material according to the number of portions as described in claim 1, ensuring the accuracy of the raw material ratio, and providing a basis for subsequent mixing and stirring; Mixing: Mix the weighed raw materials evenly in a special concrete mixer to form a uniform mixture. The mixing time is controlled within 3 to 5 minutes to ensure that the various raw materials are fully dispersed; Stirring: Stirring the mixed raw materials in a mixer until a uniform concrete slurry is formed, and the stirring speed is controlled at 100-200 rpm to ensure the uniformity and workability of the mixture; Pouring: pour the mixed concrete slurry into the mold and shape it according to the engineering requirements. During the pouring process, care should be taken to avoid the mixing of air and the separation of the slurry; Curing: Curing the poured concrete under suitable temperature and humidity conditions for the specified time to ensure the hardening and strength development of the concrete. The curing conditions are adjusted according to the specific performance requirements of the concrete.
8. The preparation method according to claim 7, It is characterized in that In the mixing step, precise control of the mixing speed is crucial to the uniformity and final performance of the concrete. The mixing speed is controlled at 100-200 rpm to achieve the best mixing effect. The mixing time is adjusted according to the specific mix ratio and workability requirements of the concrete.
9. The preparation method according to claim 7, It is characterized in that In the curing step, precise control of curing conditions is critical to the hardening and strength development of concrete. The curing temperature is controlled at 20-25°C, the humidity is controlled at 60-80%, and the curing time is 7 to 28 days to ensure that the concrete meets the designed performance requirements. The temperature and humidity of the concrete should be checked regularly during the curing process to ensure the stability of the curing conditions.
10. The ecological concrete according to claim 1, It is characterized in that It has a compressive strength of at least 40MPa to 60MPa, impermeability of P8 to P12 levels, and durability that meets the national standard GB / T 50081-2002. These performance indicators are achieved through carefully designed raw material ratios and preparation processes, ensuring the engineering application value of concrete. At the same time, compared with traditional concrete, the ecological concrete of the present invention has a reduction of CO2 emissions by at least 30%, showing significant environmental friendliness, and providing a new solution for the green transformation and sustainable development of the concrete industry.
Citation Information
Cited By
Low-carbon concrete preparation method based on low-temperature pyrolysis fly ash
CN121850523A